Conductive film and display device

By using multi-layer metal layer and grain boundary structure in the conductive film, and adding inorganic particles to the resin layer, the problem of insufficient adhesion between metal layers in the conductive film is solved, and high adhesion and excellent conductivity are achieved performance.

CN118946455AActive Publication Date: 2024-11-12TDK CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202380030271.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-29
Filing Date
2023-03-06
Publication Date
2024-11-12
Estimated Expiration
2043-03-06

AI Technical Summary

Technical Problem

In the conventional conductive film, the conductive layer composed of a plurality of metal layers is insufficiently adhered to the metal layer, which affects its conductive properties.

Method used

A conductive film consisting of a multi-layer metal layer is adopted, wherein the first metal layer includes a grain boundary, the second metal layer exists in the grain boundary, and a third metal layer is provided between the first metal layer and the second metal layer, through The anchoring effect improves the adhesion between metal layers and adds inorganic particles to the resin layer to enhance adhesion and transparency.

Benefits of technology

The adhesion and conductivity between metal layers are significantly improved, the transparency and conductivity of the conductive layer are enhanced, and excellent conductivity and transparency are achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118946455A_ABST
    Figure CN118946455A_ABST
Patent Text Reader

Abstract

This conductive film is provided with a film-like substrate and a conductive layer provided on one main surface side of the substrate. The conductive layer has a first metal layer containing a first metal and a second metal layer containing a second metal different from the first metal, which are provided in this order from the base material side. The first metal layer includes a grain boundary.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a conductive film and a display device. Background Art

[0002] A transparent antenna having a transparent and conductive conductive substrate (conductive film) is sometimes mounted on the surface of a touch panel or display. Recently, with the increase in size and diversification of touch panels and displays, the conductive film is required to have high transparency and conductivity, as well as flexibility.

[0003] As a conductive substrate, for example, Patent Document 1 discloses a conductive substrate comprising a base material, a base layer, a groove forming layer, and a conductive pattern layer, wherein the base layer has a mixed region formed from the surface of the conductive pattern layer side of the base layer to the inner side thereof, containing a metal constituting the conductive pattern layer and containing metal particles entering the base layer. It is also disclosed that the conductive pattern layer can be formed of a plurality of metal layers.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2019-29658 Summary of the invention

[0007] Technical problem to be solved by the invention

[0008] In a conductive film having a conductive layer composed of a plurality of metal layers, it is desired that the adhesion between the metal layers is high.

[0009] Technical solutions for solving technical problems

[0010] One aspect of the present disclosure relates to a conductive film including a film-shaped substrate and a conductive layer provided on one main surface side of the substrate. In the conductive film, the conductive layer includes a first metal layer and a second metal layer provided in order from the substrate side. The first metal layer includes a grain boundary.

[0011] Another aspect of the present disclosure relates to a display device including a conductive film.

[0012] Effects of the Invention

[0013] In the conductive film having a conductive layer composed of a plurality of metal layers, the adhesion between the metal layers can be improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 It is a schematic plan view showing a conductive film according to one embodiment.

[0015] Figure 2 It is along Figure 1 Cross-sectional view along line II-II.

[0016] Figure 3 yes Figure 2 A partial enlarged view of the conductive film shown.

[0017] Figure 4 It is a schematic representation Figure 1 A cross-sectional view showing a method for manufacturing a conductive film.

[0018] Figure 5 It is a schematic representation Figure 1 A cross-sectional view showing a method for manufacturing a conductive film.

[0019] Figure 6 It is a schematic representation Figure 1 A cross-sectional view showing a method for forming a metal layer of a conductive film.

[0020] Figure 7 It is a cross-sectional view showing one embodiment of a display device. DETAILED DESCRIPTION

[0021] The present disclosure is not limited to the following examples.

[0022] Figure 1 It is a schematic plan view showing a conductive film according to one embodiment. Figure 2 It is along Figure 1 Cross-sectional view along line II-II. Figure 1 and Figure 2 The conductive film 100 shown in the figure comprises: a film-shaped substrate 1; a first resin layer 10 provided on the substrate 1; a second resin layer 20 provided on the first resin layer 10 and having a linear groove 25 opened on the surface on the side opposite to the first resin layer 10; and a conductive layer 30 provided in the groove 25. Figure 1 and Figure 2 In the example of , a plurality of linear grooves 25 extending in two directions intersect each other to form a mesh pattern. The conductive layer 30 in the grooves 25 also forms a mesh pattern. The conductive layer 30 having a mesh pattern can function well as a radiation element of an antenna, for example. The grooves 25 and the conductive layer 30 are provided over a portion of the surface 10S of the first resin layer 10.

[0023] Figure 3 yes Figure 2 FIG. 1 is an enlarged view of a region R in a cross-sectional view of the conductive film 100 shown in FIG. Figure 3As shown, the conductive layer 30 has a first metal layer 30a containing a first metal, a third metal layer 30c containing a third metal, and a second metal layer 30b containing a second metal, which are arranged in sequence from the substrate 1 side. The first metal, the second metal and the third metal are metals of different types. The first metal, the second metal and the third metal can be a single metal or a combination of two or more metals. The first metal layer 30a can also contain the second metal and / or the third metal, the second metal layer 30b can also contain the first metal and / or the third metal, and the third metal layer 30c can also contain the first metal and / or the second metal. The first metal layer 30a, the second metal layer 30b and the third metal layer 30c can also contain non-metallic elements such as phosphorus within the range of maintaining conductivity.

[0024] The first metal constituting the first metal layer 30 a may be, for example, at least one selected from nickel, gold, silver, copper, and palladium, or may be nickel.

[0025] The first metal layer 30a includes a plurality of crystal grains, and a crystal grain boundary 31 as the boundary between them is formed in the first metal layer 30a. If the crystal grain boundary 31 is formed, the surface area of ​​the first metal layer 30a becomes larger, which can contribute to improving the adhesion between the first metal layer 30a and other metal layers. For example, the formation of the crystal grain boundary 31 can be confirmed by observing the cross section of the conductive film 100 along the thickness direction with a TEM (transmission electron microscope). In the element mapping of the first metal layer 30a, the crystal grain boundary 31 is sometimes observed as a linear area in which the first metal is not substantially observed in the first metal layer 30a. In this case, the first metal layer 30a can also be divided into a plurality of regions by the crystal grain boundary 31. It is also considered that each region divided by the crystal grain boundary 31 is equivalent to a crystal grain, and its maximum width can be, for example, more than 10nm or more than 20nm, or less than 100nm or less than 80nm.

[0026] From the viewpoint of high adhesion between the first metal layer 30a and other metal layers (e.g., the third metal layer 30c), the thickness of the first metal layer 30a may be 10 nm or more, 20 nm or more, or 30 nm or more. From the viewpoint of high conductivity as the conductive layer 30, the thickness of the first metal layer 30a may be 200 nm or less, 100 nm or less, or 90 nm or less. The thickness of the portion containing the first metal in the conductive layer 30 can be regarded as the thickness of the first metal layer 30a.

[0027] The second metal constituting the second metal layer 30 b may be, for example, at least one selected from copper, gold, silver, and palladium, or may be copper.

[0028] The second metal may also be present at the grain boundary 31 in the first metal layer 30a. That is, the metal component of the second metal may also invade the grain boundary 31 in the first metal layer 30a. The second metal may also be continuously distributed from the second metal layer 30b to the grain boundary 31 in the first metal layer 30a. The second metal present at the grain boundary 31 can be regarded as a part of the first metal layer 30a. By making the second metal present at the grain boundary 31, for example, the adhesion between the first metal layer 30a and the second metal layer 30b can be further improved by utilizing the anchoring effect. The presence of the second metal at the grain boundary 31 can be confirmed by element mapping using EDS-STEM.

[0029] From the viewpoint of high conductivity, the thickness of the second metal layer 30b may be 1.5 μm or more, 1.8 μm or more, or 2.0 μm or more. The thickness of the second metal layer 30b may be 10 μm or less, 8 μm or less, or 6 μm or less. The thickness of the portion containing the second metal in the conductive layer 30 can be regarded as the thickness of the second metal layer 30b. However, the thickness of the second metal present at the grain boundary 31 is not included in the thickness of the second metal layer 30b.

[0030] The conductive layer 30 may be Figure 3 The third metal layer 30c is further provided between the first metal layer 30a and the second metal layer 30b, or may not be provided. The third metal constituting the third metal layer 30c may be, for example, at least one selected from palladium, gold, silver, and copper, or may be palladium. The third metal layer 30c may also be formed of metal particles containing the third metal.

[0031] The third metal may also exist at the grain boundary 31. That is, the metal component of the third metal may also invade the grain boundary 31 in the first metal layer 30a. The third metal may also be distributed continuously from the third metal layer 30c to the grain boundary 31 in the first metal layer 30a. The third metal existing at the grain boundary 31 can be regarded as a part of the first metal layer 30a. By making the third metal exist at the grain boundary 31, for example, the adhesion between the first metal layer 30a and the third metal layer 30c can be improved by utilizing the anchor effect. The presence of the third metal at the grain boundary 31 can be confirmed by element mapping using EDS-STEM analysis.

[0032] From the viewpoint of better adhesion between the first metal layer 30a and the third metal layer 30c, the maximum depth of the third metal present at the grain boundary 31 from the surface of the first metal layer 30a may be 40 nm or more, 30 nm or more, or 20 nm or more. From the viewpoint of high conductivity as the conductive layer 30, the depth of the third metal present at the grain boundary 31 from the surface of the first metal layer 30a may be 200 nm or less, or 150 nm or less.

[0033] From the perspective of making it easy to grow a metal plating layer on the third metal layer 30c and from the perspective of higher adhesion between the third metal layer 30c and the second metal layer 30b, the thickness of the third metal layer 30c may be greater than 10nm, greater than 15nm, or greater than 20nm. From the perspective of high conductivity as the conductive layer 30, the thickness of the third metal layer 30c may be less than 30nm, less than 25nm, or less than 20nm. The thickness of the portion containing the third metal in the conductive layer 30 can be regarded as the thickness of the third metal layer 30c. However, the thickness of the third metal present at the grain boundary 31 is not included in the thickness of the third metal layer 30c.

[0034] The third metal layer 30c may have a thickness smaller than either the thickness of the first metal layer 30a or the thickness of the second metal layer 30b. The first metal layer 30a may have a thickness smaller than the thickness of the second metal layer 30b. Thus, the conductive film 100 easily has better adhesion between the metal layers and better conductivity.

[0035] The electrical conductivity of the second metal of the second metal layer 30b, the electrical conductivity of the first metal of the first metal layer 30a, and the electrical conductivity of the third metal of the third metal layer 30c may be successively higher. Thus, the conductive film 100 is likely to have excellent electrical conductivity.

[0036] The conductive layer 30 may further include a fourth metal layer including a metal different from the second metal on the second metal layer 30b. The metal constituting the fourth metal layer may include at least one of gold and palladium, for example.

[0037] The conductive layer 30 may have a pattern including linear portions. The conductive layer 30 may have a pattern including a plurality of linear portions arranged while extending in a certain direction. The conductive layer 30 may have a mesh pattern including linear portions.

[0038] The width of the linear portion of the conductive layer 30 may be 1 μm or more, 10 μm or more, or 20 μm or more, or 90 μm or less, 70 μm or less, or 30 μm or less. In this specification, the width of the linear portion of the conductive layer 30 is referred to as the maximum width in the extension direction of the linear portion. From the viewpoint of improving the transparency of the conductive film 100, the width of the linear portion of the conductive layer 30 may be 0.3 μm or more, 0.5 μm or more, or 1.0 μm or more, or 5.0 μm or less, 4.0 μm or less, or 3.0 μm or less.

[0039] The thickness of the conductive layer 30 may be 0.1 μm or more, 1.0 μm or more, or 10.0 μm or less, 5.0 μm or less, or 3.0 μm or less. The width and thickness of the conductive layer 30 can be adjusted by changing the design of the mold 50 described later and changing the width and thickness of the groove 25.

[0040] The aspect ratio of the conductive layer 30 may be, for example, 0.1 or more, 0.5 or more, or 1.0 or less, 10.0 or less, 7.0 or less, or 4.0 or less. The aspect ratio of the conductive layer 30 refers to the ratio of the thickness of the conductive layer 30 to the width of the conductive layer 30 (thickness / width).

[0041] The substrate 1 may also be a transparent substrate, in particular, a transparent resin film. The resin film may be, for example, a film of polyethylene terephthalate (PET), polycarbonate (PC), polyethylene naphthalate (PEN), cycloolefin polymer (COP) or polyimide (PI). The substrate 1 may also be glass or Si wafer, etc. The substrate 1 may also have a degree of light transmittance required when the conductive film 100 is installed in a display device. Specifically, the total light transmittance of the substrate may also be 90 to 100%. The haze of the substrate may also be 0 to 5%.

[0042] The thickness of the substrate 1 may be 10 μm or more, 20 μm or more, or 35 μm or more, or 500 μm or less, 200 μm or less, or 100 μm or less.

[0043] The first resin portion 12 constituting the first resin layer 10 may also be a cured product of a curable resin composition containing a curable resin. The first resin layer 10 may also be transparent. Examples of curable resins include amino resins, cyanate resins, isocyanate resins, polyimide resins, epoxy resins, oxetane resins, polyesters, allyl resins, phenolic resins, benzoxazine resins, xylene resins, ketone resins, furan resins, COPNA resins, silicone resins, dicyclopentadiene resins, benzocyclobutene resins, episulfide resins, ene-thiol resins, polyazomethine resins, polyvinyl benzyl ether compounds, acenaphthylene, and ultraviolet curing resins containing functional groups such as unsaturated double bonds, cyclic ethers, and vinyl ethers that undergo polymerization reactions due to ultraviolet rays. The curable resin may be a single one or a combination of two or more.

[0044] The first inorganic particles 11 are dispersed in the first resin portion 12. Examples of the first inorganic particles 11 include silicon dioxide, aluminum oxide, titanium dioxide, tantalum oxide, zirconium oxide, silicon nitride, barium titanate, barium carbonate, magnesium carbonate, aluminum hydroxide, magnesium hydroxide, lead titanate, lead zirconate titanate, lead lanthanum zirconate titanate, gallium oxide, spinel, molite, cordierite, talc, aluminum titanate, barium silicate, boron nitride, calcium carbonate, barium sulfate, calcium sulfate, zinc oxide, magnesium titanate, hydrotalcite, mica, calcined kaolin, and carbon. The first inorganic particles 11 may be one alone or a combination of two or more.

[0045] The shape of the first inorganic particles 11 is not particularly limited, and may be, for example, spherical, ellipsoidal, polyhedral, plate-like, scaly, or columnar.

[0046] A portion of the plurality of first inorganic particles 11 may also be present in the first metal layer 30a. The first inorganic particles 11a present in the first metal layer 30a may partially protrude from the first resin portion 12, or may be separated from the first resin portion 12 and distributed in the first metal layer 30a. The first inorganic particles 11a partially protruding from the first resin portion 12 or the first inorganic particles 11a leaving the first resin portion 12 are located in the first metal layer 30a, and the first metal of the first metal layer 30a exists around the protruding portion or the leaving portion. That is, a portion of the plurality of first inorganic particles 11 may also be partially protruding from the first resin portion 12 and / or separated from the first resin portion 12 in a manner partially surrounded by the first metal and surrounded by the first metal in the first metal layer 30a. In addition, being surrounded by the first metal includes not only the case of being surrounded by the first metal alone, but also the case of being surrounded by the first metal, the grain boundary 31 contained in the first metal layer 30a, and the second metal and the third metal present in the grain boundary 31. The first inorganic particles 11a separated from the first resin portion 12 can be regarded as part of the first metal layer 30a. By making the first inorganic particles 11a exist in the first metal layer 30a, the adhesion between the first resin layer 10 and the first metal layer 30a can be further improved. In addition, if the first inorganic particles 11a exist in the first metal layer 30a, it is easy to form a grain boundary 31 in the first metal layer 30a.

[0047] At least a portion of the plurality of first inorganic particles 11 may partially protrude from the first resin portion 12 to the second resin layer 20 side. "The first inorganic particles 11 partially protrude from the first resin portion 12 to the second resin layer 20 side" means a state in which a portion of the surface of the first inorganic particle 11 protrudes from the first resin portion 12 to the second resin layer 20 side and is in contact with the second resin layer 20. That is, the plurality of first inorganic particles 11 partially protruding to the second resin layer 20 side may also be in a state in which the portion protruding to the second resin layer 20 side is not covered by the first resin portion 12 (the portion protruding to the second resin layer 20 side is exposed from the first resin portion 12). Hereinafter, such first inorganic particles are also referred to as "exposed first inorganic particles". The exposed first inorganic particles 11a can contribute to improving the adhesion between the first resin layer 10 and the second resin layer 20. For example, the presence of the exposed first inorganic particles 11a can be confirmed by observing a cross section of the conductive film 100 along the thickness direction with a TEM. The first inorganic particles 11 may include first inorganic particles 11 b that are buried in the first resin portion 12 and do not protrude to the second resin layer 20 side (do not protrude from the first resin portion 12 ).

[0048] From the viewpoint of excellent adhesion between the first resin layer 10 and the second resin layer 20 of the conductive film 100, the ratio of the number of exposed first inorganic particles 11a to the total number of first inorganic particles 11 may be 10% or more. The ratio of the number of exposed first inorganic particles 11a to the total number of first inorganic particles 11 may be, for example, 40% or less. By observing a cross section of the conductive film 100 along the thickness direction with TEM, the number of exposed first inorganic particles 11a in the cross-sectional image of the first resin layer 10 in a range of 1.5 μm and the number of all first inorganic particles 11 in the cross-sectional image of the first resin layer 10 in the range are measured in any extending direction of the conductive film 100, thereby calculating the ratio of the number of exposed first inorganic particles 11a.

[0049] The plurality of first inorganic particles 11 may be localized on the second resin layer 20 side in the first resin layer 10. By observing a cross section of the conductive film 100 along the thickness direction with TEM, it can be confirmed that the first inorganic particles 11 are localized on the second resin layer 20 side in the first resin layer 10.

[0050] “The plurality of first inorganic particles 11 are biased toward the second resin layer 20 in the first resin layer 10” means, for example, that in a cross section along the thickness direction of the conductive film 100, when the region from the center in the thickness direction of the first resin layer 10 to the second resin layer 20 is defined as region A, the ratio of the number of the first inorganic particles 11 (including the exposed first inorganic particles 11a) present in region A exceeds 50% relative to the total number of the first inorganic particles 11 in the entire first resin layer 10. The ratio may be 60% or more, 70% or more, 75% or more, or 80% or more.

[0051] The average particle size of the first inorganic particles 11 may be, for example, 10 nm or more, 15 nm or more, or 20 nm or less, or 400 nm or less, 300 nm or less, or 200 nm or less. The average particle size of the first inorganic particles 11 is calculated by observing a cross section of the conductive film 100 along the thickness direction with a TEM, measuring the maximum length of each of the first inorganic particles 11 within a range of 1.5 μm in any extension direction of the conductive film 100 in the TEM image of the cross section, and averaging the maximum lengths.

[0052] The thickness of the first resin layer 10 or the first resin portion 12 may be, for example, 30 nm or more, 50 nm or more, or 100 nm or less, or 500 nm or less, 400 nm or less, or 300 nm or less.

[0053] The second resin layer 20 is a resin layer mainly composed of the second resin portion 22. The second resin portion 22 may also be transparent. The second resin portion 22 may also be a cured product of a photocurable resin or a thermosetting resin. Examples of photocurable resins or thermosetting resins include acrylic resins, amino resins, cyanate resins, isocyanate resins, polyimide resins, epoxy resins, oxetane resins, polyesters, allyl resins, phenolic resins, benzoxazine resins, xylene resins, ketone resins, furan resins, COPNA resins, silicone resins, dicyclopentadiene resins, benzocyclobutene resins, episulfide resins, ene-thiol resins, polyazomethine resins, polyvinyl benzyl ether compounds, acenaphthylene, and ultraviolet curing resins containing unsaturated double bonds, cyclic ethers, and vinyl ethers, etc., which undergo polymerization reactions due to ultraviolet rays. These photocurable resins or thermosetting resins may be a single one or a combination of two or more.

[0054] The second resin layer 20 may also contain second inorganic particles. The second inorganic particles may be one or more inorganic particles selected from Pd, Cu, Ni, Co, Au, Ag, Pd, Rh, Pt, In and Sn, and may also contain Pd. The second inorganic particles may be a single inorganic particle or a combination of two or more inorganic particles. The second inorganic particles may also be included in the first metal layer 30a.

[0055] The shape of the second inorganic particles is not particularly limited, and may be, for example, spherical, ellipsoidal, polyhedral, plate-like, scaly, or columnar.

[0056] From the viewpoint of excellent transparency of the conductive film 100, the average particle size of the second inorganic particles may be 10 nm or less, 8 nm or less, or 5 nm or less. The average particle size of the second inorganic particles may be, for example, 0.1 nm or more, 0.5 nm or more, or 1 nm or more. By observing the cross section of the conductive film 100 along the thickness direction with TEM, the maximum length of each of the second inorganic particles existing in the range of 1.5 μm in any extension direction of the conductive film 100 is measured in the TEM image of the cross section and averaged, thereby calculating the average particle size of the second inorganic particles.

[0057] The average particle size of the second inorganic particles may be smaller than the average particle size of the first inorganic particles 11. The ratio of the average particle size of the second inorganic particles to the average particle size of the first inorganic particles 11 (average particle size of the second inorganic particles / average particle size of the first inorganic particles 11) may be 0.3 or less, or 0.1 or less, or 0.01 or more, 0.02 or more, or 0.05 or more.

[0058] The plurality of second inorganic particles may be biased toward the first resin layer 10 in the second resin layer 20. “The plurality of second inorganic particles are biased toward the first resin layer 10 in the second resin layer 20” means, for example, that in an observation image when a cross section along the thickness direction of the conductive film 100 is observed by TEM, when a region from the center in the thickness direction of the second resin layer 20 to the first resin layer 10 side is defined as region B, the ratio of the number of second inorganic particles in region B exceeds 50% relative to the total number of second inorganic particles in the entire second resin layer 20. The ratio may be 80% or more, 90% or more, or 95% or more.

[0059] From the viewpoint of excellent transparency of the conductive film 100, the second inorganic particles, which are 80% or more of the total number of the second inorganic particles, may be distributed in a region where the distance from the interface between the first resin layer 10 and the second resin layer 20 is less than 1 / 3, less than 1 / 4, or less than 1 / 5 of the thickness of the first resin layer 10. The second inorganic particles, which are 90% or more or 95% or more of the total number of the second inorganic particles, may be distributed in a region where the distance from the interface between the first resin layer 10 and the second resin layer 20 is less than 1 / 3, less than 1 / 4, or less than 1 / 5 of the thickness of the first resin layer 10. The "interface between the first resin layer 10 and the second resin layer 20" refers to the interface between the first resin portion 12 and the second resin portion 22, and the interface between the exposed first inorganic particles 11a and the second resin portion 22.

[0060] From the viewpoint of excellent transparency of the conductive film 100, the second inorganic particles whose number is 80% or more relative to the total number of the second inorganic particles may be distributed in a region whose distance from the interface between the first resin layer 10 and the second resin layer 20 is 70 nm or less, 65 nm or less, 60 nm or less, 55 nm or less, 50 nm or less, 45 nm or less, 40 nm or less, 35 nm or less, 30 nm or less, 25 nm or less, 20 nm or less, 15 nm or less, or 10 nm or less. The second inorganic particles whose number is 90% or more or 95% or more relative to the total number of the second inorganic particles may be distributed in a region whose distance from the interface between the first resin layer 10 and the second resin layer 20 is 70 nm or less, 65 nm or less, 60 nm or less, 55 nm or less, 50 nm or less, 45 nm or less, 40 nm or less, 35 nm or less, 30 nm or less, 25 nm or less, 20 nm or less, 15 nm or less, or 10 nm or less.

[0061] A plurality of second inorganic particles may also be present around the portion of each of the exposed plurality of first inorganic particles 11a protruding (exposed) toward the second resin layer 20. In this case, the adhesion between the first resin layer 10 and the second resin layer 20 can be further improved. "The portion of each of the first inorganic particles 11a protruding toward the second resin layer 20" may also be a region within 10 nm from the surface of the portion of the first inorganic particle 11a protruding toward the second resin layer 20. The plurality of second inorganic particles may also be in contact with the portion of one of the exposed first inorganic particles 11a protruding toward the second resin layer 20.

[0062] The groove 25 opens on the surface on the side opposite to the first resin layer 10 and extends on the second resin layer 20. The groove 25 includes a portion where a pattern corresponding to the pattern of the conductive layer 30 is formed. Figure 2 As shown, the width of the groove 25 may be narrowed from the side of the second resin layer 20 opposite to the first resin layer 10 side toward the first resin layer 10 side, and the width of the groove 25 may be substantially constant in the depth direction.

[0063] The width and depth of the groove 25 are generally substantially the same as the width and thickness of the conductive layer 30. In this specification, the width of the groove 25 refers to the maximum width in the direction perpendicular to the thickness direction of the conductive film 100 (the extension direction of the conductive film 100), and the depth of the groove 25 refers to the maximum depth in the thickness direction of the conductive film 100. The ratio of the depth of the groove 25 to the width of the groove 25 may be the same as the aspect ratio of the conductive layer 30 described above.

[0064] The thickness of the second resin layer 20 or the second resin portion 22 may be, for example, 1 μm or more, 1.5 μm or more, or 2 μm or less, or 5 μm or less, 4 μm or less, or 3 μm or less.

[0065] Figures 4 to 6 It is a schematic representation of the manufacturing Figure 1 100 is a cross-sectional view of an example of a method for forming a conductive film 100. In the method of this embodiment, first, as Figure 4 As shown in (a), a first resin layer 10 including first inorganic particles 11 is formed on one surface 1S of a film-like substrate 1. The first resin layer 10 is formed, for example, by a method including the steps of applying a coating liquid including a resin component forming a first resin portion 12, first inorganic particles 11, and a solvent on the substrate 1; and removing the solvent from the coating film on the substrate 1. Figure 4 The step (a) may be a step of preparing a laminate including the substrate 1 and the first resin layer 10 formed on the substrate 1 .

[0066] like Figure 4 As shown in (b), a layer 40 containing second inorganic particles is formed on a surface 10S of the first resin layer 10 on the side opposite to the substrate 1. The layer 40 containing second inorganic particles is a layer containing second inorganic particles 21 and a third resin portion 41. The third resin portion 41 may also contain the same material as the second resin portion 22. Figure 4 The step (b) may be a step of preparing a laminated body including the substrate 1 , the first resin layer 10 , and the second inorganic particle-containing layer 40 in this order.

[0067] like Figure 4 As shown in (c), the first inorganic particles 11 are exposed from the surface 10S of the first resin layer 10. As a method for exposing the first inorganic particles 11 from the surface 10S, for example, Figure 4 (b) The laminated body is subjected to an ashing treatment to remove a portion of the third resin portion 41 in the second inorganic particle-containing layer 40 and a portion of the first resin portion 12 in the first resin layer 10. By the ashing treatment, the first resin layer 10 becomes thinner than Figure 4The moment (b) is thin. A portion of the first resin portion 12 is removed by the ashing treatment, but the first inorganic particles 11 present in the first resin portion 12 are not removed and remain on the side of the first resin layer 10 opposite to the substrate 1. Therefore, a first resin layer 10 in which the first inorganic particles 11 are biased toward the side opposite to the substrate 1 can be formed. The third resin portion 41 in the layer 40 containing the second inorganic particles can be completely removed by the ashing treatment, or a portion of it can remain on the surface 10S of the first resin layer 10. By removing the third resin portion 41 in the layer 40 containing the second inorganic particles, the second inorganic particles 21 in the layer 40 containing the second inorganic particles are deposited on the surface 10S of the first resin layer 10. The deposited second inorganic particles 21 may also be attached to the first resin portion 12 or the exposed first inorganic particles 11a. Figure 4 The step (c) may be a step of removing a portion of the first resin portion 12 in the first resin layer 10 and the third resin portion 41 in the second inorganic particle-containing layer 40 to expose the plurality of first inorganic particles 11 on the surface 10S of the first resin layer 10 .

[0068] like Figure 4 As shown in (d), the second resin layer 20 is formed on the surface 10S of the first resin layer 10. Specifically, the second resin layer 20 containing the second resin part 22 and the second inorganic particles 21 is formed by applying a resin composition containing a resin component forming the second resin part 22 on the surface 10S of the first resin layer 10 on which the second inorganic particles 21 are deposited. Here, in the case where a part of the third resin part 41 in the layer 40 containing the second inorganic particles remains on the surface 10S of the first resin layer 10, the remaining third resin part 41 becomes a part of the second resin part 22 of the second resin layer 20. Figure 4 The step (d) may be a step of preparing a laminated body including the substrate 1 , the first resin layer 10 , and the second resin layer 20 in this order.

[0069] like Figure 5 As shown in (a) and (b) of FIG. 1 , a groove (groove portion) 25 is formed in the second resin layer 20 by an imprinting method using a mold 50 having a convex portion 50a. In this step, the mold 50 having a convex portion 50a of a predetermined shape is moved in the direction indicated by the arrow A, so that the mold 50 is pressed into the second resin layer 20 ( Figure 5 (a)). Alternatively, the mold 50 may be pressed in until the tip of the protrusion 50a reaches the first resin layer 10. In this state, the second resin portion 22 is cured as required. When the second resin portion 22 before curing includes a photocurable resin, the second resin portion 22 is cured by irradiating light such as ultraviolet rays. Thereafter, by removing the mold 50, a groove 25 ( Figure 5(b)). The method for forming the groove 25 is not limited to the imprint method, for example, the groove 25 may be formed by laser, dry etching or photolithography. The groove 25 extends on the first resin layer 10 in a manner to form a pattern corresponding to the conductive layer 30. In order to expose the second inorganic particles 21 at the bottom surface of the groove 25, the second resin portion 22 remaining on the first resin layer 10 in the groove 25 may be removed by etching such as dry etching after the mold 50 is removed. Figure 5 Steps (a) and (b) may be steps of forming a groove 25 opening on the surface of the second resin layer 20 on the side opposite to the first resin layer 10 in a laminate including the substrate 1, the first resin layer 10, and the second resin layer 20 in that order.

[0070] The mold 50 may also be formed of quartz, Ni, ultraviolet curing liquid silicone rubber (PDMS), etc. The shape of the convex portion 50 a of the mold 50 is designed according to the shape of the groove 25 to be formed.

[0071] like Figure 5 As shown in (c), a conductive layer 30 is formed to fill the groove 25. By forming the conductive layer 30 to fill the groove 25, the conductive film 100 can be obtained. The conductive layer 30 is formed, for example, as follows Figure 6 As shown in (a) to (c).

[0072] First, if Figure 6 As shown in (a), the first metal layer 30a is formed at the bottom of the groove 25 of the stacked body having the groove 25. The first metal layer 30a can be formed by immersing the stacked body having the groove 25 in a first chemical plating solution containing ions of the metal constituting the first metal layer 30a. Figure 6 The step (a) may be a step of preparing a stacked body which sequentially comprises a substrate 1, a first resin layer 10, a second resin layer 20 having a groove 25 opened on a surface opposite to the first resin layer 10, and a first metal layer 30a formed in the groove 25.

[0073] The first chemical plating solution contains ions of the metal constituting the first metal layer 30a. The first chemical plating solution may further contain phosphorus, boron, iron, and the like.

[0074] When the laminate is immersed in the first chemical plating solution, the temperature of the first chemical plating solution may be, for example, 40 to 80° C. The immersion time in the first chemical plating solution varies depending on the thickness of the first metal layer 30 a and the like, but may be, for example, 1 to 10 minutes.

[0075] like Figure 6As shown in (b), the third metal layer 30c is formed on the first metal layer 30a. The third metal layer 30c can be formed by immersing the laminated body on which the first metal layer 30a is formed in an aqueous solution containing a metal constituting the third metal layer 30c. Figure 6 The process (b) may also be a process of preparing a stacked body which sequentially comprises a substrate 1, a first resin layer 10, a second resin layer 20 having a groove 25 opened on a surface opposite to the first resin layer 10, a first metal layer 30a formed in the groove 25, and a third metal layer 30c formed on the first metal layer 30a.

[0076] The aqueous solution contains the metal constituting the third metal layer 30c. The temperature of the aqueous solution when the laminate is immersed in the aqueous solution may be, for example, 20 to 60°C. The immersion time in the aqueous solution varies depending on the thickness of the third metal layer 30c, etc., and may be, for example, 1 to 10 minutes.

[0077] like Figure 6 As shown in (c), the second metal layer 30b is formed on the third metal layer 30c. The second metal layer 30b can be formed by immersing the laminated body formed with the third metal layer 30c in a second chemical plating solution containing ions of the metal constituting the second metal layer 30b. Figure 6 The step (c) may also be a step of preparing a laminated body which sequentially includes a substrate 1, a first resin layer 10, a second resin layer 20 having a groove 25 opened on a surface opposite to the first resin layer 10, a first metal layer 30a formed in the groove 25, a third metal layer 30c formed on the first metal layer 30a, and a second metal layer 30b formed on the third metal layer 30c. In the case where the conductive layer 30 does not include the third metal layer 30c, the laminated body having the first metal layer 30a formed thereon may be immersed in a second chemical plating solution containing ions of a metal constituting the second metal layer 30b, thereby forming the second metal layer 30b on the first metal layer 30a.

[0078] The second chemical plating solution contains ions of the metal constituting the second metal layer 30 b. The second chemical plating solution may further contain formalin or the like.

[0079] When the laminate is immersed in the second chemical plating solution, the temperature of the second chemical plating solution may be, for example, 30 to 60° C. The immersion time in the second chemical plating solution varies depending on the thickness of the second metal layer 30 b and may be, for example, 2 to 20 minutes.

[0080] The conductive film described above can be incorporated into a display device as, for example, a planar transparent antenna. The display device may be, for example, a liquid crystal display device or an organic EL display device. Figure 7 It is a cross-sectional view showing one embodiment of a display device incorporating the conductive film 100 . Figure 7 The display device 500 shown includes an image display unit 60 having an image display region 60S, a conductive film 100, a polarizing plate 70, and a cover glass 80. The conductive film 100, the polarizing plate 70, and the cover glass 80 are stacked on the image display region 60S side of the image display unit 60 in this order from the image display unit 60 side.

[0081] The structure of the display device is not limited to Figure 7 The form can be appropriately changed as needed. For example, the polarizer 70 can also be provided between the image display unit 60 and the conductive film 100. The image display unit 60 can also be, for example, a liquid crystal display unit. As the polarizer 70 and the cover glass 80, the polarizer and cover glass commonly used in the display device can be used. The polarizer 70 and the cover glass 80 may not be provided.

[0082] Although a display device is exemplified as an application device of the conductive film, the conductive film can also be applied to devices other than display devices. For example, the conductive film can also be applied to glass of buildings, cars, etc. as a transparent antenna.

[0083] The technology disclosed herein includes the following configuration examples, but is not limited thereto.

[0084] The conductive film involved in one aspect of the present disclosure is a conductive film having a film-shaped substrate and a conductive layer arranged on one main surface side of the substrate, the conductive layer having a first metal layer containing a first metal and a second metal layer containing a second metal different from the first metal arranged in sequence from the substrate side, and the first metal layer includes a grain boundary.

[0085] According to the above-mentioned conductive film, since the first metal layer includes the grain boundary, the surface area of ​​the first metal layer is increased, and the adhesion between the first metal layer and other metal layers is improved.

[0086] In the above-mentioned conductive film, the second metal may also exist at the grain boundary, thereby improving the conductivity of the conductive layer and further improving the adhesion between the first metal layer and other metal layers due to the anchor effect of the second metal existing at the grain boundary.

[0087] In the above-mentioned conductive film, the conductive layer may further include a third metal layer, which is provided between the first metal layer and the second metal layer and contains a third metal different from the first metal and the second metal. Accordingly, by multi-layering the conductive layer, the stress applied to the conductive film is dispersed, and the adhesion between the first metal layer and the third metal layer and between the second metal layer and the third metal layer is further improved.

[0088] In the above-mentioned conductive film, the third metal may be present at the grain boundary. In this way, the adhesion between the first metal layer and the third metal layer is further improved due to the anchor effect of the third metal present at the grain boundary.

[0089] In the above-mentioned conductive film, the conductivity of the second metal, the conductivity of the first metal, and the conductivity of the third metal may be successively higher. This allows the conductive film to easily have excellent conductivity.

[0090] In the above-mentioned conductive film, the third metal layer may have a thickness smaller than that of the first metal layer and the second metal layer. This makes it easier for the conductive film to have better adhesion between the metal layers and better conductivity.

[0091] The above-mentioned conductive film may further include a resin layer provided between the substrate and the conductive layer and containing a plurality of inorganic particles. This further improves the adhesion of the conductive layer to the substrate.

[0092] In the above-mentioned conductive film, a part of the plurality of inorganic particles may partially protrude from the resin portion in a manner partially surrounded by the first metal. In addition, a part of the plurality of inorganic particles may be separated from the resin portion and surrounded by the first metal in the first metal layer. Accordingly, the adhesion between the conductive layer and the resin layer is further improved.

[0093] In the above-mentioned conductive film, the conductive layer may have a pattern including a linear portion. This makes it easy for the conductive film to have excellent transparency.

[0094] Moreover, a display device according to one aspect of the present disclosure includes the above-mentioned conductive film.

[0095] According to the above display device, a display device including a conductive film having high adhesion between metal layers is obtained.

[0096] The present disclosure includes, for example, the following [1] to

[12] .

[0097] [1] A conductive film comprising a film-like substrate and a conductive layer provided on one main surface side of the substrate,

[0098] The conductive layer includes a first metal layer containing a first metal and a second metal layer containing a second metal different from the first metal, which are provided in order from the substrate side.

[0099] The first metal layer includes grain boundaries.

[0100] [2] The conductive film according to [1], wherein the second metal also exists in the grain boundary.

[0101] [3] The conductive film according to [1], wherein the conductive layer further includes a third metal layer, the third metal layer is provided between the first metal layer and the second metal layer, and contains a third metal different from the first metal and the second metal.

[0102] [4] The conductive film according to [3], wherein the third metal also exists in the grain boundary.

[0103] [5] The conductive film according to [2], wherein the conductive layer further includes a third metal layer, the third metal layer is provided between the first metal layer and the second metal layer, and contains a third metal different from the first metal and the second metal.

[0104] [6] The conductive film according to [5], wherein the third metal also exists in the grain boundary.

[0105] [7] The conductive film according to any one of [3] to [6], wherein the electrical conductivity of the second metal, the electrical conductivity of the first metal, and the electrical conductivity of the third metal are successively higher.

[0106] [8] The conductive film according to any one of [3] to [7], wherein the third metal layer has a thickness smaller than either the thickness of the first metal layer or the thickness of the second metal layer.

[0107] [9] The conductive film according to any one of [1] to [8], further comprising a resin layer provided between the substrate and the conductive layer and containing a resin portion and a plurality of inorganic particles.

[0108]

[10] A conductive film according to [9], wherein a portion of the plurality of inorganic particles partially protrude from the resin portion in a manner partially surrounded by the first metal, and / or a portion of the plurality of inorganic particles are separated from the resin portion and surrounded by the first metal in the first metal layer.

[0109]

[11] The conductive film according to any one of [1] to

[10] , wherein the conductive layer has a pattern including linear portions.

[0110]

[12] A display device comprising the conductive film described in

[11] .

[0111] Example

[0112] The present disclosure is not limited to the following examples.

[0113] [Example 1]

[0114] A coating liquid for forming a first resin layer containing silica particles (average particle size 100 nm), acrylic resin and solvent was prepared. The coating liquid was applied to a COP film (thickness 100 μm), and the solvent was removed from the coating film on the COP film in a hot air drying furnace. Next, the coating film was irradiated with ultraviolet rays using a UV treatment device to cure the coating film, and a first resin layer with a thickness of 300 μm containing a first resin portion and silica particles (first inorganic particles) was formed on the COP film.

[0115] A coating liquid for forming a layer containing second inorganic particles, which contains Pd particles (average particle size 5 nm), acrylic resin, and solvent, is prepared. The coating liquid is applied to the first resin layer, and the solvent is removed from the coating film on the first resin layer in a hot air drying furnace. Next, the coating film is irradiated with ultraviolet rays using a UV treatment device to cure the coating film, and a layer containing second inorganic particles with a thickness of 60 μm and containing Pd particles (second inorganic particles) is formed on the first resin layer to obtain a laminate.

[0116] The laminated body after forming the second inorganic particle-containing layer was placed in a vacuum device, and the surface of the second inorganic particle-containing layer was ashed to remove the resin portion in the second inorganic particle-containing layer and the resin portion of the surface layer of the first resin layer. The thickness of the first resin layer after ashing was 260 μm.

[0117] A UV curing resin is applied to the surface of the first resin layer after the ashing treatment to form a coating film with a thickness of 2 μm. Next, a mold having a convex portion is pressed into the coating film in such a manner that the front end of the convex portion of the mold reaches the surface of the first resin layer, and the coating film is irradiated with ultraviolet rays in this state to cure the coating film. The mold is removed from the cured coating film to form a second resin layer, in which linear grooves are formed that intersect with each other, open on the surface on the side opposite to the first resin layer, and have a mesh pattern.

[0118] The laminated body after the second resin layer is formed is placed in a vacuum device and subjected to an ashing process to remove the resin constituting the second resin layer remaining at the bottom of the groove.

[0119] Next, the laminated body is immersed in a chemical plating solution containing nickel sulfate and sodium hypophosphite to grow a Ni plating layer from the surface of the first resin layer, thereby forming a Ni layer (first metal layer) in the grooves.

[0120] The laminated body formed with the Ni layer is immersed in an aqueous solution containing Pd. Next, the obtained laminated body is immersed in a chemical plating solution containing copper sulfate and formalin, so that the Cu plating layer grows on the Ni layer starting from the Pd layer, and a Cu layer (second metal layer) is formed in the groove. Thus, a conductive layer having a Ni layer, a Pd layer and a Cu layer and having a mesh pattern is formed in the groove to obtain a conductive film. The thickness of the Ni layer, the Pd layer and the Cu layer is 100nm, 30nm and 2μm respectively.

[0121] In order to observe the cross section of the obtained conductive film along the thickness direction, the portion of the conductive film containing the conductive layer was cut into a plate shape using FIB (focused ion beam), and thinned to prepare a sample for TEM observation. The prepared sample was observed in bright field using TEM (device name JEM-2011F) under the condition of an acceleration voltage of 200 kV, and the result confirmed that a grain boundary was formed in the Ni layer. Through EDS-STEM analysis, it was confirmed that a part of the silica particles in the first resin layer existed in the Ni layer, and it was also confirmed that Pd and Cu existed in the grain boundaries of the Ni layer.

[0122] [Example 2]

[0123] A conductive film was prepared by the same method as in Example 1 except that the ashing treatment was not performed after the second resin layer was formed and before the first metal layer was formed. The cross section of the obtained conductive film in the thickness direction was observed by TEM, and it was confirmed that a grain boundary was formed in the Ni layer. In addition, by EDS-STEM analysis, it was confirmed that the silica particles were surrounded by Ni in the Ni layer, and that Pd and Cu were present at the grain boundary of the Ni layer.

[0124] [Example 3]

[0125] A conductive film was prepared by the same method as in Example 1 except that the ashing treatment was not performed after the formation of the layer containing the second inorganic particles and before the formation of the second resin layer. The cross section of the obtained conductive film in the thickness direction was observed by TEM, and it was confirmed that a grain boundary was formed in the Ni layer. In addition, by EDS-STEM analysis, it was confirmed that the silica particles were surrounded by Ni in the Ni layer, and Pd and Cu were also confirmed to be present at the grain boundary of the Ni layer.

[0126] [Comparative Example 1]

[0127] A conductive film was prepared by the same method as in Example 1, except that ashing was not performed after forming the layer containing the second inorganic particles and before forming the second resin layer, and ashing was not performed after forming the second resin layer and before forming the first metal layer. A cross section in the thickness direction of the obtained conductive film was observed by TEM, and as a result, a plurality of grain boundaries were not confirmed in the Ni layer.

[0128] <Evaluation of Adhesion>

[0129] The evaluation of the adhesion is performed by a cross-cut test specified in JIS K 5600. Specifically, an incision is made on the surface of the area including the second resin layer and the conductive layer using a cutting knife to form a right-angled grid pattern (25 squares). Next, a tape is pasted on the grid pattern to make the surface of the second resin layer and the conductive layer close to the tape, and then the tape is peeled off. The grid pattern after the tape is peeled off is observed under an optical microscope, and the situation where the peeling of the conductive layer is not confirmed is evaluated as A, and the situation where the peeling of the conductive layer is confirmed is evaluated as B. The results are shown in Table 1. In each embodiment, interlayer peeling in the conductive layer is not confirmed.

[0130] [Table 1]

[0131]

[0132] Explanation of symbols:

[0133] 1…substrate, 10…first resin layer, 11, 11a, 11b…first inorganic particles, 12…first resin portion, 20…second resin layer, 21…second inorganic particles, 22…second resin portion, 25…groove, 30…conductive layer, 30a…first metal layer, 30b…second metal layer, 30c…third metal layer, 31…grain boundary, 40…layer containing second inorganic particles, 41…third resin portion, 50…mold, 60…image display portion, 70…polarizer, 80…cover glass, 100…conductive film, 500…display device.

Claims

1. A conductive film, wherein: The conductive film includes a film-shaped substrate and a conductive layer provided on one main surface side of the substrate. The conductive layer includes a first metal layer containing a first metal and a second metal layer containing a second metal different from the first metal, which are provided in order from the substrate side. The first metal layer includes grain boundaries.

2. The conductive film according to claim 1, wherein The second metal is also present at the grain boundaries.

3. The conductive film according to claim 1, wherein The conductive layer further includes a third metal layer, which is disposed between the first metal layer and the second metal layer and contains a third metal different from the first metal and the second metal.

4. The conductive film according to claim 3, wherein The third metal also exists at the grain boundaries.

5. The conductive film according to claim 2, wherein The conductive layer further includes a third metal layer, which is disposed between the first metal layer and the second metal layer and contains a third metal different from the first metal and the second metal.

6. The conductive film according to claim 5, wherein The third metal also exists at the grain boundaries.

7. The conductive film according to any one of claims 3 to 6, wherein The electrical conductivity of the second metal, the electrical conductivity of the first metal, and the electrical conductivity of the third metal become higher in sequence.

8. The conductive film according to any one of claims 3 to 6, wherein The third metal layer has a thickness smaller than any of a thickness of the first metal layer and a thickness of the second metal layer.

9. The conductive film according to any one of claims 1 to 6, wherein The conductive film further includes a resin layer provided between the substrate and the conductive layer and including a resin portion and a plurality of inorganic particles.

10. The conductive film according to claim 9, wherein Some of the plurality of inorganic particles partially protrude from the resin portion so as to be partially surrounded by the first metal, and / or some of the plurality of inorganic particles are separated from the resin portion and surrounded by the first metal in the first metal layer.

11. The conductive film according to any one of claims 1 to 6, wherein The conductive layer has a pattern including linear portions.

12. A display device, wherein: A conductive film according to claim 11 is provided.

Citation Information

Patent Citations

  • Conductive substrate, electronic device, and display device

    JP2019029658A

  • Laminate body, panel for use in display device with support board, panel for use in display device, and display device

    CN103201104A

  • Metal alloy composites

    CN107849642A

  • Conductive substrate, electronic device, and method of manufacturing display device

    CN109309012A

  • Manufacture of semiconductor device and multi-layer wiring substrate and manufacture of the same