Optical adhesive sheet
By using liquid antistatic agents and ionic liquids in optical adhesive sheets, the problems caused by static electricity and thermal shock during rework of the image display panel are solved, and the high-difference absorption and heat resistance are achieved, ensuring the visual of the image display device Effect.
Patent Information
- Application Number
- CN202380030941.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-29
- Filing Date
- 2023-03-23
- Publication Date
- 2024-11-12
AI Technical Summary
During the reworking process of the image display panel, static electricity is easily generated when the adhesive sheet is peeled, resulting in poor display, and thermal shock causes gaps or haze to increase in the interface between the adhesive sheet and the panel, affecting visual recognition.
It adopts an optical adhesive sheet with liquid antistatic agent, the surface resistance value of the adhesive layer is less than 1010Ω and contains ionic liquid, which can maintain excellent antistatic effect and transparency in high-difference absorption and heat shock resistance environment. Reduce static electricity generation and visual recognition.
It effectively suppresses the generation of static electricity during rework of the image display panel, prevents the reduction of visual recognition caused by thermal shock, maintains the adhesion and transparency of the adhesive layer, and ensures high-quality display of the image display device.
Smart Images

Figure CN118946644A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an optical pressure-sensitive adhesive sheet and, more particularly, to an optical pressure-sensitive adhesive sheet suitable for production of image display devices. Background Art
[0002] Liquid crystal display devices and organic EL display devices are widely used as various image display devices such as smart phones, monitors for personal computers, and televisions. In such image display devices, in order to prevent damage to the image display panel caused by external impact, a transparent front plate such as a transparent resin plate or a glass plate is provided on the visual recognition side of the image display panel. In addition, image display devices having a touch panel on the visual recognition side of the image display panel are also becoming popular.
[0003] As a method of configuring the front transparent plate or touch panel, etc. on the front side of the image display panel, an "interlayer filling structure" (for example, Patent Document 1) is proposed in which the image display panel is bonded to the front transparent plate, touch panel, etc. by an adhesive sheet. In addition, an adhesive sheet is sometimes also provided between the front transparent plate and the touch panel. In the interlayer filling structure, the gaps between the components are filled with an adhesive, so that the refractive index difference of the interface is reduced, and the reduction in visual recognition caused by reflection or scattering can be suppressed. In addition, in the interlayer filling structure, since the components are bonded and fixed by using an adhesive sheet, it has the advantage that it is not easy to produce peeling of the components caused by impacts such as falling, compared with the case where the components are fixed only in the shell.
[0004] When the adhesive sheet is attached to the image display panel, sometimes poor attachment such as mixing of bubbles and offset of the attachment position occurs. In the case of poor attachment, it is desirable to peel off the adhesive sheet from the image display panel and reuse the image display panel (sometimes referred to as "rework" in this specification).
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2014-125524 Summary of the invention
[0008] Problems to be solved by the invention
[0009] In the case of poor lamination, when the adhesive sheet is peeled off from the image display panel for rework of the image display panel, static electricity is generated on the adhesive sheet. The generated static electricity affects the orientation of the display unit of the image display panel, etc., and becomes a cause of poor display. In particular, in an image display panel with a higher number of pixels for high image quality, it is difficult to separately provide a ground wiring for discharging static electricity, and a countermeasure for discharging static electricity is required.
[0010] In addition, due to thermal shock (cyclical heating and cooling) caused by repeatedly turning the power of the image display device on and off, gaps are generated at the interface between the adhesive sheet and the image display panel, or the haze of the adhesive sheet increases, there is a problem that the visual recognition of the image display device decreases over time.
[0011] The present invention is conceived based on the above situation, and an object of the present invention is to provide an optical adhesive sheet that can suppress the generation of static electricity when the adhesive sheet is peeled off from an image display panel for rework of the image display panel. In addition, another object of the present invention is to provide an optical adhesive sheet that can suppress the time-dependent reduction in the visual recognition of an image display device caused by thermal shock.
[0012] It should be noted that a transparent and conductive printed layer such as patterned ITO (indium tin oxide) is formed on the surface of the touch panel, and then silver and copper wiring (return wiring) is formed in the peripheral portion. In addition, a black shielding portion is usually printed in a frame shape on the peripheral portion of the front transparent plate. In the case where there are such uneven shapes of printed layers, wiring, etc. on various components such as image display panels, front transparent plates, touch panels, etc., the adhesive sheet that joins them is also required to have the property that the adhesive layer fully follows the height difference and can fill it without leaving bubbles (sometimes referred to as "height difference absorption" in this specification).
[0013] Means used to solve problems
[0014] That is, the first aspect of the present invention provides an optical adhesive sheet having a laminated structure in which a substrate and an adhesive layer are laminated, the substrate having a first surface and a second surface, and the adhesive layer is laminated on the first surface of the substrate. In this specification, the optical adhesive sheet of the first aspect of the present invention is sometimes referred to as "the optical adhesive sheet of the present invention". In addition, the above-mentioned adhesive layer constituting the optical adhesive sheet of the present invention is sometimes referred to as "the adhesive layer of the present invention", and the above-mentioned substrate is sometimes referred to as "the substrate of the present invention".
[0015] The optical adhesive sheet of the present invention can be suitable for the manufacture of an image display device. That is, the adhesive layer of the present invention can be suitable for laminating a front transparent plate, a touch panel, and other optical components (polarizing film, phase difference film, etc.) on the image display panel constituting the image display device. In addition, the substrate of the present invention can be various optical components for manufacturing an image display device, such as a front transparent plate, a touch panel, and other optical components (polarizing film, phase difference film, etc.).
[0016] In the optical adhesive sheet of the present invention, the adhesive layer of the present invention contains a liquid antistatic agent. The above-mentioned antistatic agent is suitable from the following aspects: antistatic property is given to the adhesive layer of the present invention, and in the case of poor lamination to the image display panel, the generation of static electricity can be suppressed when the adhesive sheet is peeled off from the image display panel for rework. In addition, the above-mentioned antistatic agent is suitable in the form of a liquid from the following aspects: the adhesive layer of the present invention can be given an excellent antistatic effect without damaging the adhesive properties of the adhesive layer of the present invention, so the adhesion between the adhesive layer of the present invention and the substrate of the present invention is improved, for example, even in harsh environments such as thermal shock (periodically repeated heating and cooling), it is possible to prevent the generation of voids at the interface of the adhesive layer of the present invention and the substrate and reduce transparency, and obtain the characteristics that can maintain excellent optical properties (in this specification, such characteristics are sometimes referred to as "heat shock resistance").
[0017] In the optical adhesive sheet of the present invention, the surface resistance value of the adhesive layer of the present invention is less than 10 10 Ω. The surface resistance of the adhesive layer of the present invention is less than 10 10 The structure of Ω is suitable from the following aspects: the adhesive layer of the present invention exhibits an excellent antistatic effect, and when poor lamination to the image display panel occurs, the generation of static electricity can be suppressed when the adhesive sheet is peeled off from the image display panel for rework.
[0018] The optical pressure-sensitive adhesive sheet of the present invention has a haze of 1% or less after the following heat shock test.
[0019] Thermal shock test
[0020] The optical pressure-sensitive adhesive sheet of the present invention was subjected to 200 cycles of exposure to an atmosphere of −40° C. for 30 minutes and then to an atmosphere of 80° C. for 30 minutes using a heat shock tester.
[0021] The optical pressure-sensitive adhesive sheet of the present invention preferably has a haze of 1% or less after the heat shock test because the image display device of the present invention can maintain excellent visibility even under a severe environment such as a heat shock.
[0022] In the optical adhesive sheet of the present invention, the antistatic agent is preferably an ionic liquid. The antistatic agent being an ionic liquid is suitable from the following aspects: it can impart an excellent antistatic effect to the adhesive layer of the present invention without damaging the adhesive properties of the adhesive layer of the present invention, thereby improving the adhesion between the adhesive layer of the present invention and the substrate of the present invention, and obtaining excellent heat shock resistance.
[0023] In the optical adhesive sheet of the present invention, the ionic liquid preferably contains an anionic component having a fluorine atom number of 10 or less. The configuration in which the ionic liquid contains an anionic component having a fluorine atom number of 10 or less is suitable from the following aspects: improving the compatibility of the ionic liquid with the adhesive layer of the present invention, suppressing the increase in haze caused by separation of the ionic liquid from the adhesive layer, and improving the visual recognition of the image display device.
[0024] The difference in haze of the optical adhesive sheet of the present invention before and after the thermal shock test (haze of the optical adhesive sheet after the thermal shock test - haze of the optical adhesive sheet before the thermal shock test) is preferably 2% or less. The configuration in which the difference in haze of the optical adhesive sheet of the present invention before and after the thermal shock test is 2% or less is preferred from the following aspects: the excellent visual recognition of the image display device of the present invention can be maintained even in a harsh environment such as thermal shock.
[0025] The absolute value of the difference in surface resistance of the pressure-sensitive adhesive layer of the present invention before and after the heat shock test represented by the following formula is preferably 1 logΩ or less.
[0026] |Log 10 B-Log 10 A|
[0027] A: Surface resistance value before thermal shock test
[0028] B: Surface resistance value after thermal shock test
[0029] The configuration in which the difference in surface resistance value of the adhesive layer of the present invention before and after the above-mentioned thermal shock test is less than 1 logΩ is suitable from the following aspects: the excellent antistatic effect of the adhesive layer of the present invention can be maintained even in a harsh environment such as thermal shock. For example, when a malfunction such as a light-emitting element not lighting up occurs in the use environment of an image display device, the generation of static electricity can be suppressed when the adhesive sheet is peeled off from the image display panel for repair.
[0030] In the optical adhesive sheet of the present invention, the second surface of the substrate is preferably subjected to an anti-reflection treatment and / or an anti-glare treatment. The configuration in which the second surface of the substrate is subjected to an anti-reflection treatment and / or an anti-glare treatment is preferred from the following aspects: it can prevent reflection caused by metal wiring, ITO wiring, etc. disposed on the substrate of the image display device and can improve visual recognition.
[0031] In the optical pressure-sensitive adhesive sheet of the present invention, the pressure-sensitive adhesive layer is preferably an acrylic pressure-sensitive adhesive layer containing an acrylic polymer. This configuration is suitable from the viewpoint of adjusting the above-mentioned properties (particularly the step absorption property) of the pressure-sensitive adhesive layer.
[0032] The second aspect of the present invention provides an image display device in which the optical pressure-sensitive adhesive sheet of the present invention and an image display panel are laminated. In this specification, the image display device of the second aspect of the present invention may be referred to as "the image display device of the present invention".
[0033] The image display device of the present invention has the optical adhesive sheet of the present invention in a laminated structure, and therefore is suitable from the following aspects: when poor lamination to the image display panel occurs, the generation of static electricity can be suppressed when the adhesive sheet is peeled off from the image display panel for rework. In addition, it is suitable from the following aspects: it is possible to prevent the visual recognition of the image display device from decreasing over time due to the generation of gaps at the interface between the adhesive sheet and the image display panel or the increase in the haze of the adhesive sheet caused by thermal shock.
[0034] In addition, the third aspect of the present invention provides a spliced display formed by arranging a plurality of image display devices of the present invention. In this specification, the spliced display of the third aspect of the present invention is sometimes referred to as "the spliced display of the present invention". The spliced display of the present invention is suitable as an image display device for large screens such as advertising displays or signs such as bulletin boards.
[0035] Effects of the Invention
[0036] By using the optical adhesive sheet of the present invention for the manufacture of an image display device, it is suitable from the following aspects: in the case of poor lamination to the image display panel, the generation of static electricity can be suppressed when the adhesive sheet is peeled off from the image display panel for rework. In addition, it is suitable from the following aspects: the adhesive layer of the present invention can be given an excellent antistatic effect without damaging the adhesive properties of the adhesive layer of the invention, so the adhesion between the adhesive layer of the present invention and the substrate of the present invention is improved, and excellent heat shock resistance can be obtained, and gaps are generated at the interface between the adhesive sheet and the image display panel, or the haze of the adhesive sheet increases, which can prevent the visual recognition of the image display device from decreasing over time. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 It is a schematic diagram (cross-sectional view) showing one embodiment of the optical pressure-sensitive adhesive sheet of the present invention.
[0038] Figure 2 It is a schematic diagram (cross-sectional view) showing another embodiment of the optical pressure-sensitive adhesive sheet of the present invention.
[0039] Figure 3 To indicate the stacking Figure 2 A schematic diagram (cross-sectional view) of one embodiment of the image display device of the present invention comprising an optical pressure-sensitive adhesive sheet.
[0040] Figure 4It is a schematic diagram (stereoscopic diagram) showing one embodiment of the spliced display of the present invention. DETAILED DESCRIPTION
[0041] The optical adhesive sheet of the present invention has a laminated structure in which a substrate and an adhesive layer are laminated, wherein the substrate has a first surface and a second surface, and the adhesive layer is laminated on the first surface of the substrate. It should be noted that "adhesive sheet" includes the meaning of "adhesive tape". That is, the optical adhesive sheet of the present invention can be an adhesive sheet having a tape-shaped form.
[0042] The image display device of the present invention is an image display device in which the optical pressure-sensitive adhesive sheet of the present invention and an image display panel are laminated. In addition, the spliced display of the present invention is a spliced display in which a plurality of image display devices of the present invention are arranged.
[0043] Hereinafter, embodiments of the present invention will be described with reference to the drawings, but the present invention is not limited thereto and is merely illustrative.
[0044] Figure 1 It is a schematic diagram (cross-sectional view) showing one embodiment of the optical pressure-sensitive adhesive sheet of the present invention.
[0045] exist Figure 1 In the embodiment, the optical pressure-sensitive adhesive sheet 10A has a laminated structure in which a substrate 1 and a pressure-sensitive adhesive layer 2 are laminated. The substrate 1 has a first surface 1 a and a second surface 1 b , and the pressure-sensitive adhesive layer 2 is laminated on the first surface 1 a of the substrate 1 .
[0046] exist Figure 2 In the embodiment, the optical adhesive sheet 10B has a laminated structure in which a substrate 1 and an adhesive layer 2 are laminated. The substrate 1 has a first surface 1a and a second surface 1b, and the adhesive layer 2 is laminated on the first surface 1a of the substrate 1. The second surface 1b of the substrate 1 is subjected to an anti-reflection treatment and / or an anti-glare treatment 3.
[0047] Figure 3 Schematic diagram (cross-sectional view) showing one embodiment of the image display device of the present invention. Figure 3 In the image display device 20 , the image display panel 4 is laminated on the pressure-sensitive adhesive layer 2 of the optical pressure-sensitive adhesive sheet 10B.
[0048] Figure 4 Schematic diagram (stereoscopic diagram) showing one embodiment of the spliced display of the present invention. Figure 4 In the figure, the spliced display 30 is formed by arranging nine image display devices 20 (the stacked structure is not shown) in a 3×3 arrangement on a supporting substrate 31 in a tile shape.
[0049] Hereinafter, each configuration will be described.
[0050] <Optical Adhesive Sheet>
[0051] The "optical" in the optical adhesive sheet of the present invention refers to optical applications, and more specifically, refers to products (optical products) used to manufacture optical components. Examples of optical products include image display devices, input devices such as touch panels, etc., and are suitable for the manufacture of liquid crystal image display devices, self-luminous image display devices (such as organic EL (electroluminescent) image display devices, LED image display devices), etc. In particular, the optical adhesive sheet of the present invention is suitable for the manufacture of self-luminous image display devices.
[0052] As long as the optical adhesive sheet of the present invention is laminated with the adhesive layer of the present invention on the first surface of the substrate of the present invention, its form is not particularly limited.For example, it can be a single-sided adhesive sheet with only one side as an adhesive surface, or it can be a double-sided adhesive sheet with two sides as adhesive surfaces.In addition, in the case where the optical adhesive sheet of the present invention is a double-sided adhesive sheet, the optical adhesive sheet of the present invention can have a form in which two adhesive surfaces are provided by the adhesive layer of the present invention, or it can have a form in which one adhesive surface is provided by the adhesive layer of the present invention, and another adhesive surface is provided by the adhesive layer (other adhesive layer) other than the adhesive layer of the present invention.In the case where the optical adhesive sheet of the present invention constitutes the outermost surface of an optical product, a single-sided adhesive sheet is preferably used, and in the case where adherends (optical components) are bonded to each other, a double-sided adhesive sheet is preferably used.
[0053] The optical adhesive sheet of the present invention may have other layers on the surface or between any layers, in addition to the substrate of the present invention and the adhesive layer of the present invention, within the range not impairing the effects of the present invention, such as a substrate other than the substrate of the present invention, an adhesive layer other than the adhesive layer of the present invention, an intermediate layer, a primer layer, an antistatic layer, a release liner, a surface protective film, etc.
[0054] The haze of the optical adhesive sheet of the present invention is not particularly limited, and is preferably 1% or less. The haze of the optical adhesive sheet of the present invention is 1% or less, and is preferably considered to be excellent in visual recognition of the image display device of the present invention. Considering that the image display device of the present invention shows excellent visual recognition, the haze of the optical adhesive sheet of the present invention is preferably 0.8% or less, more preferably 0.5% or less, or 0.4% or less. The lower limit of the haze of the optical adhesive sheet of the present invention is not particularly limited, and the lower the better, but it can be 0.01% or more.
[0055] The optical pressure-sensitive adhesive sheet of the present invention has a haze of 1% or less after the following heat shock test.
[0056] Thermal shock test
[0057] The optical pressure-sensitive adhesive sheet of the present invention was subjected to 200 cycles of exposure to a −40° C. atmosphere for 30 minutes and then to an 80° C. atmosphere for 30 minutes using a heat shock tester.
[0058] The optical adhesive sheet of the present invention has a haze of 1% or less after the thermal shock test, which is preferred from the following aspects: the image display device of the present invention can maintain excellent visual recognition even in a harsh environment such as thermal shock. Considering that the image display device of the present invention can further maintain visual recognition, the haze of the optical adhesive sheet of the present invention after the thermal shock test is preferably 0.8% or less, more preferably 0.5% or less, or 0.4% or less. The lower limit of the haze of the optical adhesive sheet of the present invention after the thermal shock test is not particularly limited, and the lower the better, but it can be 0.01% or more.
[0059] The haze difference of the optical adhesive sheet of the present invention before and after the above-mentioned thermal shock test (haze of the optical adhesive sheet after the thermal shock test - haze of the optical adhesive sheet before the thermal shock test) is preferably 2% or less. The configuration in which the difference in haze of the optical adhesive sheet of the present invention before and after the above-mentioned thermal shock test is 2% or less is preferred from the following aspects: the image display device of the present invention can also maintain excellent visual recognition under harsh environments such as thermal shock. From the aspect that the image display device of the present invention can further maintain excellent visual recognition, the difference in haze of the optical adhesive sheet of the present invention before and after the above-mentioned thermal shock test is more preferably 1.8% or less, further preferably 1.5% or less, or it can also be 1 or less.
[0060] The haze of the optical adhesive sheet of the present invention, the haze of the optical adhesive sheet of the present invention after the above-mentioned heat shock test, and the difference thereof can be measured according to JIS K7136, and specifically, can be measured by the method described in the embodiments described later. The haze of the optical adhesive sheet of the present invention, the haze of the optical adhesive sheet of the present invention after the above-mentioned heat shock test, and the difference thereof can be adjusted by the type and thickness of the resin and glass constituting the substrate of the present invention, the type and thickness of the resin constituting the adhesive layer of the present invention, the type and amount of the antistatic agent, and the anti-reflection treatment and / or anti-glare treatment of the substrate surface.
[0061] The visible light transmittance of the optical adhesive sheet of the present invention is not particularly limited, but is preferably 90% or more. The visible light transmittance of the optical adhesive sheet of the present invention is preferably 90% or more from the perspective of obtaining excellent visual recognition in the image display device of the present invention, more preferably 90.5% or more, and may be 91% or more. The upper limit of the visible light transmittance of the optical adhesive sheet of the present invention is not particularly limited, but may be 95% or less.
[0062] The visible light transmittance of the optical adhesive sheet of the present invention can be measured according to JIS K 7361-1. The visible light transmittance of the optical adhesive sheet of the present invention can be adjusted by the type and thickness of the resin and glass constituting the substrate of the present invention, the type and thickness of the resin constituting the adhesive layer of the present invention, the type and amount of the antistatic agent, and the anti-reflection treatment and / or anti-glare treatment of the substrate surface.
[0063] The optical adhesive sheet of the present invention has a * a * b * L specified in the color system * There is no particular limitation, but from the perspective of obtaining excellent visual recognition of the image display device of the present invention, it is preferably 90 or more, preferably 92 or more, and preferably 94 or more. * and b * There is no particular limitation and they may be the same or different, but are preferably in the range of -5 to 5, more preferably -3 to 3, and particularly preferably in the range of -1 to 1 (wherein, it is 0 or approximately 0).
[0064] The L of the optical adhesive sheet of the present invention before and after the above-mentioned heat shock test * a * b * b in the color system * The change in (Δb * ) is not particularly limited, but is preferably 0.1 or less, and preferably 0.05 or less, from the perspective that the optical adhesive sheet of the present invention exhibits excellent heat shock resistance.
[0065] L * a * b * The color system refers to the color space called the International Commission on Illumination (CIE) 1976 color system, which can be measured according to JIS Z8781-4 (2013). * a * b * L specified in the color system * 、a * 、b * , and Δb * The thickness of the resin and glass constituting the substrate of the present invention, the thickness of the resin constituting the adhesive layer of the present invention, the type and amount of the antistatic agent, and the anti-reflection treatment and / or anti-glare treatment of the substrate surface can be used to adjust the surface.
[0066] The adhesive force of the optical adhesive sheet of the present invention to the acrylic plate when peeled off at 23°C, a peeling speed of 300mm / min and a peeling angle of 180° is not particularly limited. From the perspective of sufficient adhesion between the substrate and the image display panel of the present invention, it is preferably 3N / 25mm or more, more preferably 5N / 25mm or more, and further preferably 7N / 25mm or more. When the adhesive force of the optical adhesive sheet of the present invention to the acrylic plate when peeled off at 23°C, a peeling speed of 300mm / min and a peeling angle of 180° is 3N / 25mm, it is easy to obtain good adhesion to the substrate of the present invention and good suppression of the bulge of the height difference, so it is preferred. It should be noted that the upper limit of the adhesive force of the optical adhesive sheet of the present invention to the acrylic plate when peeled off at 23°C, a peeling speed of 300mm / min and a peeling angle of 180° is not particularly limited, for example, 40N / 20mm, more preferably 60N / 20mm.
[0067] The optical adhesive sheet of the present invention has no particular restriction on the peeling charge when peeled from the acrylic plate at 23°C, a peeling speed of 5 mm / min and a peeling angle of 150°. From the perspective of suppressing the generation of static electricity when the adhesive sheet is peeled from the image display panel for rework in the event of poor bonding to the image display panel, the peeling charge is preferably within ±2 kV, more preferably within ±1.5 kV, and even more preferably within ±1 kV.
[0068] The adhesive force of the optical adhesive sheet of the present invention when peeled to an acrylic plate at 23°C, a peeling speed of 300 mm / min and a peeling angle of 180° and the peeling charge when peeled at 23°C, a peeling speed of 5 mm / min and a peeling angle of 150° are measured by the adhesive force and peeling charge measurement in the examples described below. The adhesive force of the adhesive layer of the present invention when peeled to an acrylic plate at 23°C, a peeling speed of 300 mm / min and a peeling angle of 180° and the peeling charge when peeled at 23°C, a peeling speed of 5 mm / min and a peeling angle of 150° can be adjusted by the composition of the adhesive composition used to form the adhesive layer of the present invention (e.g., the type, molecular weight, amount used, monomer composition, type and amount of functional groups, type and amount of antistatic agent, type and amount of crosslinking agent), curing conditions (heating conditions, radiation irradiation conditions), etc.
[0069] The thickness of the optical pressure-sensitive adhesive sheet of the present invention is not particularly limited. For example, when considering dimensional stability, strength, workability, thin-layer properties, etc., it is preferably in the range of 10 μm to 500 μm, more preferably in the range of 20 μm to 300 μm, and most preferably in the range of 30 μm to 200 μm.
[0070] <Base Material>
[0071] Examples of the material constituting the substrate of the present invention include glass and plastic films. Examples of the plastic film include polyester resins such as polyethylene terephthalate (PET) and polyethylene naphthalate (PEN), cyclic olefin polymers (COP) (e.g., trade name "ARTON" (manufactured by JSR Corporation), trade name "ZEONOR" (manufactured by ZEON Corporation of Japan), etc.), acrylic resins such as polymethyl methacrylate (PMMA), polycarbonate (PC), triacetyl cellulose (TAC), polysulfone, polyarylate, polyetheretherketone (PEEK), polyimide (PI), transparent polyimide (CPI), polyvinyl chloride, polyvinyl acetate, polyethylene, polypropylene, ethylene-propylene copolymer and other plastic materials. Polyester resins such as polyethylene terephthalate (PET) and polyethylene naphthalate (PEN), cyclic olefin polymers (COP), polycarbonate (PC), polyetheretherketone (PEEK), and transparent polyimide (CPI) that are excellent in dimensional stability and not easy to shrink are preferred. It should be noted that these plastic materials can be used alone or in combination of two or more. The substrate of the present invention is a portion that is attached to an adherend together with the adhesive layer when the optical adhesive sheet of the present invention is attached to an adherend (image display panel, etc.). The release liner that is peeled off when using the optical adhesive sheet of the present invention (when pasting) is not included in the "substrate".
[0072] The substrate of the present invention has a film-like (substrate-like) form having a first surface and a second surface. The substrate of the present invention is not particularly limited as long as it is a component constituting the image display device of the present invention, and various optical films such as a front transparent plate, a touch panel, and other optical components (polarizing film, phase difference film, etc.) can be cited, preferably used as a front transparent plate. In the case where the substrate of the present invention is a front transparent plate, the second surface is the outermost surface of the image display device of the present invention.
[0073] The glass transition temperature (Tg) of the substrate of the present invention is not particularly limited, and is preferably above 60°C. The configuration in which the glass transition temperature of the substrate of the present invention is above 60°C is preferred from the following aspects: the mechanical properties of the image display device of the present invention are stable under the use environment. From the aspect of the stability of the mechanical properties of the image display device of the present invention, the glass transition temperature of the above-mentioned substrate may be above 63°C or above 65°C. In addition, there is no particular limitation on the upper limit of the glass transition temperature of the above-mentioned substrate. From the aspect of being able to simplify the molding process of the substrate, the glass transition temperature of the above-mentioned substrate is preferably below 350°C, and may be below 250°C, below 200°C, below 140°C, below 130°C or below 125°C.
[0074] The glass transition temperature (Tg) of the substrate of the present invention can be measured in accordance with JIS K 7121. The glass transition temperature (Tg) of the substrate of the present invention can be adjusted by the type of resin constituting the substrate of the present invention and the like.
[0075] The humidity expansion coefficient of the substrate of the present invention is not particularly limited, but is preferably 5×10 -5 / %RH or less. The humidity expansion coefficient of the substrate of the present invention is 5×10 -5 The structure of less than 3×10 / %RH is suitable from the following aspects: the dimensional stability of the substrate of the present invention is improved due to humidity changes, the shrinkage or expansion of the image display device of the present invention in the use environment is suppressed, and the transparency can be maintained without change. From the aspects of dimensional stability of the substrate of the present invention, small shrinkage or expansion, and the transparency can be maintained without change, the humidity expansion coefficient of the substrate of the present invention is preferably 3×10 -5 / %RH or less, and can also be 2×10 -5 / %RH or less.
[0076] The lower limit of the humidity expansion coefficient of the substrate of the present invention is not particularly limited, and the lower the value, the better. However, it may be 0.001×10 -5 / %RH and above.
[0077] The humidity expansion coefficient of the substrate of the present invention can be adjusted by the type of resin constituting the substrate of the present invention, the conditions during the production of the substrate (temperature, extrusion speed, etc.), and the like.
[0078] The haze of the substrate of the present invention is not particularly limited, and is more preferably 1% or less, more preferably 0.8% or less, further preferably 0.5% or less, or 0.4% or less from the perspective of showing the excellent visual recognition of the image display device of the present invention. The lower limit of the haze of the substrate of the present invention is not particularly limited, and the lower the more preferred, but it may also be 0.01% or more.
[0079] The haze of the substrate of the present invention can be measured according to JIS K 7136. The haze of the substrate of the present invention can be adjusted by the type and thickness of the resin constituting the substrate of the present invention, antireflection treatment and / or antiglare treatment of the substrate surface, and the like.
[0080] The reflectivity of the substrate of the present invention is not particularly limited, and is preferably 5% or less. The constitution that the reflectivity of the substrate of the present invention is 5% or less is preferred from the following aspects: it is possible to prevent the reflection caused by the metal wiring, ITO wiring, etc. configured on the substrate of the image display panel in the image display device of the present invention, and the reflectivity of the substrate of the present invention is more preferably 3% or less, and may also be 1.5% or less. The lower limit of the reflectivity of the substrate of the present invention is not particularly limited, but may be 0.1% or more or 0.3% or more.
[0081] The reflectance of the substrate of the present invention can be measured according to JIS K 7361-1. The reflectance of the substrate of the present invention can be adjusted by the type and thickness of the resin constituting the substrate of the present invention, anti-reflection treatment and / or anti-glare treatment of the substrate surface, and the like.
[0082] The thickness of the substrate of the present invention is not particularly limited, for example, when considering the workability such as dimensional stability, strength, operability, thin layer properties, etc., it is preferably in the range of 10 μm to 500 μm, more preferably in the range of 20 μm to 300 μm, and most preferably in the range of 30 μm to 200 μm. The refractive index of the substrate of the present invention is not particularly limited, for example, it is in the range of 1.30 to 1.80, preferably in the range of 1.40 to 1.70.
[0083] The second side of the substrate of the present invention is preferably subjected to a reflective surface treatment and / or an anti-glare treatment. The second side of the substrate of the present invention is preferably subjected to a reflective surface treatment and / or an anti-glare treatment from the following aspects: the reflection caused by the metal wiring, ITO wiring, etc., which can be prevented from being configured on the substrate of the image display device of the present invention.
[0084] As the antireflection treatment, a known antireflection treatment can be used without particular limitation, and an example thereof is an antireflection (AR) treatment.
[0085] As the above-mentioned anti-reflection (AR) treatment, a known AR treatment can be applied without particular limitation. Specifically, it can be implemented by forming an optical film having a strictly controlled thickness and refractive index on the second surface of the substrate of the present invention or by laminating the above-mentioned optical film in two or more layers to obtain an anti-reflection layer (AR layer). The AR layer utilizes the interference effect of light to cancel out the inverted phases of the incident light and the reflected light, thereby exhibiting an anti-reflection function. The wavelength region of visible light exhibiting the anti-reflection function is, for example, 380nm to 780nm, and the wavelength region with high visual sensitivity is in the range of 450nm to 650nm. It is preferred to design the AR layer in such a way that the reflectivity of 550nm as its central wavelength is minimized.
[0086] As the AR layer, a multilayer antireflection layer having a structure of 2 to 5 optical thin layers (thin films with strictly controlled thickness and refractive index) can be generally cited. By forming multiple layers with components having different refractive indices at a predetermined thickness, the freedom of optical design of the AR layer is increased, the antireflection effect can be further improved, and the spectral reflection characteristics can be made uniform (flat) in the visible light region. In the optical thin film, in order to require high thickness accuracy, the formation of each layer is usually implemented by vacuum evaporation, sputtering, CVD, etc. as a dry method.
[0087] The AR layer may be formed by a coating liquid for forming an antireflection layer. The coating liquid for forming an antireflection layer may contain, for example, a resin, a fluorine-containing additive, hollow particles, solid particles, and a diluent solvent, and may be produced by mixing them.
[0088] Examples of the resin include thermosetting resins and ionizing radiation curable resins that are cured by ultraviolet rays or light. As the resin, commercially available thermosetting resins, ultraviolet curable resins, and the like can be used.
[0089] As the above-mentioned thermosetting resin and ultraviolet curing resin, for example, a curing compound having at least one group of an acrylate group and a methacrylate group that is cured by heat, light (ultraviolet rays, etc.) or an electron beam, etc. can be used, for example, oligomers or prepolymers such as acrylates or methacrylates of polyfunctional compounds such as polysiloxane resins, polyester resins, polyether resins, epoxy resins, urethane resins, alkyd resins, spiroacetal resins, polybutadiene resins, polythiol polyene resins, and polyols, etc., can be cited. They can be used alone or in combination of two or more.
[0090] The above-mentioned resin can use a reactive diluent having at least one of an acrylate group and a methacrylate group. The above-mentioned reactive diluent can use, for example, the reactive diluent recorded in Japanese Patent Publication No. 2008-88309, for example, including monofunctional acrylates, monofunctional methacrylates, multifunctional acrylates, multifunctional methacrylates, etc. As the above-mentioned reactive diluent, trifunctional or higher acrylates and trifunctional or higher methacrylates are preferred. This is because the hardness of the second surface of the substrate of the present invention can be made excellent. As the above-mentioned reactive diluent, for example, butanediol glycerol ether diacrylate, isocyanuric acid acrylate, isocyanuric acid methacrylate, etc. can be listed. They can be used alone or in combination of two or more. The weight average molecular weight of the resin before curing can be, for example, more than 100, more than 300, more than 500, more than 1000, or more than 2000, and can be less than 100000, less than 70000, less than 50000, less than 30000, or less than 10000. If the weight average molecular weight before curing is high, the hardness decreases, but there is a tendency that cracking is less likely to occur when bending. On the other hand, if the weight average molecular weight before curing is low, there is a tendency that the intermolecular crosslinking density increases and the hardness becomes higher.
[0091] As the above-mentioned resin, it is preferable to contain a multifunctional acrylate (for example, pentaerythritol triacrylate).
[0092] In order to cure the curable resin, for example, a curing agent may be added. The curing agent is not particularly limited, and for example, a known polymerization initiator (such as a thermal polymerization initiator, a photopolymerization initiator, etc.) may be appropriately used. The amount of the curing agent added is not particularly limited, and relative to 100 parts by weight of the resin in the anti-reflection layer forming coating solution, for example, it may be 0.5 parts by weight or more, 1.0 parts by weight or more, 1.5 parts by weight or more, 2.0 parts by weight or more, or 2.5 parts by weight or less, and may be 15 parts by weight or less, 13 parts by weight or less, 10 parts by weight or less, 7 parts by weight or less, or 5 parts by weight or less.
[0093] The above-mentioned fluorine-containing element additive is not particularly limited, for example, it can be an organic compound or an inorganic compound containing fluorine in the molecule. The above-mentioned organic compound is not particularly limited, for example, it can be listed as: fluorine-containing antifouling coating agent, fluorine-containing acrylic compound, acrylic compound containing fluorine and silicon, etc. Specifically, the organic compound can be listed as: the trade name "KY-1203" manufactured by Shin-Etsu Chemical Co., Ltd., the trade name "MEGAFAC" manufactured by DIC Corporation, etc. The above-mentioned inorganic compound is also not particularly limited. The amount of the above-mentioned fluorine-containing element additive added is not particularly limited, for example, relative to the weight of the entire solid component in the above-mentioned anti-reflection layer forming coating liquid, the weight of the fluorine element in the above-mentioned solid component can be, for example, 0.05 weight% or more, 0.1 weight% or more, 0.15 weight% or more, 0.20 weight% or more, or 0.25 weight% or more, and can be 20 weight% or less, 15 weight% or less, 10 weight% or less, 5 weight% or less, or 3 weight% or less. In addition, for example, relative to 100 parts by weight of the above-mentioned resin in the above-mentioned anti-reflection layer forming coating liquid, the weight of the above-mentioned fluorine-containing element additive can be, for example, greater than 0.05 weight %, greater than 0.1 weight %, greater than 0.15 weight %, greater than 0.20 weight % or greater than 0.25 weight %, and can be less than 20 weight %, less than 15 weight %, less than 10 weight %, less than 5 weight % or less than 3 weight %.
[0094] The hollow particles are not particularly limited, for example, they can be silica particles, acrylic resin particles, acrylic-styrene copolymer particles, etc. The silica particles can be, for example, trade names "Thrulya 5320", "Thrulya 4320" manufactured by JGC Catalysts & Chemicals Co., Ltd. The weight-average particle size of the hollow particles is not particularly limited, for example, it can be more than 30nm, more than 40nm, more than 50nm, more than 60nm or more than 70nm, and can be less than 150nm, less than 140nm, less than 130nm, less than 120nm or less than 110nm. The shape of the hollow particles is not particularly limited, for example, it can be a bead-like roughly spherical shape, or it can be a particle of an indefinite shape such as a powder, preferably a roughly spherical particle, more preferably a roughly spherical particle with an aspect ratio of less than 1.5, and most preferably a spherical particle. By adding the hollow particles, for example, a low refractive index of the anti-reflection layer, good anti-reflection properties, etc. can be achieved. The amount of the hollow particles added is not particularly limited, and relative to 100 parts by weight of the resin in the anti-reflection layer forming coating solution, for example, it can be 30 parts by weight or more, 50 parts by weight or more, 70 parts by weight or more, 90 parts by weight or more, or 100 parts by weight or less, 300 parts by weight or less, 270 parts by weight or less, 250 parts by weight or less, 200 parts by weight or less, or 180 parts by weight or less. From the viewpoint of low refractive index of the anti-reflection layer, it is preferred that the amount of the hollow particles added is not too little, and from the viewpoint of ensuring the mechanical properties of the anti-reflection layer, it is preferred that the amount of the hollow particles added is not too much.
[0095] The solid particles are not particularly limited, for example, they can be silica particles, zirconium oxide particles, titanium-containing particles (such as titanium oxide particles), etc. The silica particles can be listed, for example, as trade names "MEK-2140Z-AC", "MIBK-ST", "IPA-ST" manufactured by Nissan Chemical Industry Co., Ltd. The weight-average particle size of the solid particles is not particularly limited, for example, it can be more than 5nm, more than 10nm, more than 15nm, more than 20nm or more than 25nm, and can be less than 300nm, less than 250nm, less than 200nm, less than 150nm or less than 100nm. The shape of the solid particles is not particularly limited, for example, it can be a bead-like roughly spherical shape, or it can be an amorphous particle such as a powder, preferably a roughly spherical particle, more preferably a roughly spherical particle with an aspect ratio of less than 1.5, and most preferably a spherical particle. By adding the solid particles, for example, the fluorine-containing additive is easily concentrated on the surface of the anti-reflection layer-forming coating solution applied, and the anti-reflection layer has excellent scratch resistance, and can achieve low refractive index, good anti-reflection characteristics, etc. The amount of the solid particles added is not particularly limited, and can be, for example, 5 parts by weight or more, 10 parts by weight or more, 15 parts by weight or more, 20 parts by weight or more, or 25 parts by weight or more, and can be 150 parts by weight or less, 120 parts by weight or less, 100 parts by weight or less, or 80 parts by weight or less, relative to 100 parts by weight of the resin in the anti-reflection layer-forming coating solution.
[0096] The dilution solvent may be, for example, a mixed solvent containing MIBK (methyl isobutyl ketone) and PMA (propylene glycol monomethyl ether acetate). The mixing ratio in this case is not particularly limited, and when the weight of MIBK is set to 100 weight %, the weight of PMA may be, for example, 20 weight % or more, 50 weight % or more, 100 weight % or more, 150 weight % or more, or 200 weight % or less, and may be 400 weight % or less, 350 weight % or less, 300 weight % or less, or 250 weight % or less.
[0097] The above-mentioned dilution solvent may be, for example, a mixed solvent containing TBA (tert-butyl alcohol) in addition to MIBK and PMA. The mixing ratio in this case is not particularly limited. When the weight of MIBK is set to 100% by weight, the weight of PMA may be, for example, 10% by weight or more, 30% by weight or more, 50% by weight or more, 80% by weight or more, or 100% by weight or less, or 200% by weight or less, 180% by weight or less, 150% by weight or less, 130% by weight or less, or 110% by weight or less. In addition, when the weight of MIBK is set to 100% by weight, the weight of TBA may be, for example, 10% by weight or more, 30% by weight or more, 50% by weight or more, 80% by weight or more, or 100% by weight or less, or 200% by weight or less, 180% by weight or less, 150% by weight or less, 130% by weight or less, or 110% by weight or less.
[0098] The amount of the diluent added is not particularly limited. For example, the weight of the solid component relative to the weight of the anti-reflection layer forming coating solution as a whole can be, for example, 0.1% by weight or more, 0.3% by weight or more, 0.5% by weight or more, 1.0% by weight or more, or 1.5% by weight or less, 20% by weight or less, 15% by weight or less, 10% by weight or less, 5% by weight or less, or 3% by weight or less. From the viewpoint of ensuring coating properties (wetting, leveling), it is preferred that the content of the solid component is not too high, and from the viewpoint of preventing poor appearance caused by drying such as uneven air drying and whitening, it is preferred that the content of the solid component is not too low.
[0099] Next, the coating liquid for forming the anti-reflection layer is applied on the second surface of the substrate of the present invention (the coating step). The coating method is not particularly limited, and for example, known coating methods such as jet coating, die coating, spin coating, spray coating, gravure coating, roller coating, and rod coating can be appropriately used. The coating amount of the coating liquid for forming the anti-reflection layer is not particularly limited, and the thickness of the anti-reflection layer formed can be, for example, 0.1 μm or more, 0.3 μm or more, 0.5 μm or more, 1.0 μm or more, or 2.0 μm or more, and can be 50 μm or less, 40 μm or less, 30 μm or less, 20 μm or less, or 10 μm or less.
[0100] Next, the applied anti-reflection layer-forming coating liquid is dried to form a coating film (the coating film forming step). The drying temperature is not particularly limited, and may be, for example, in the range of 30°C to 200°C. The drying temperature may be, for example, 40°C or more, 50°C or more, 60°C or more, 70°C or more, 80°C or more, 90°C or more, or 100°C or less, 190°C or less, 180°C or less, 170°C or less, 160°C or less, 150°C or less, 140°C or less, 135°C or less, 130°C or less, 120°C or less, or 110°C or less. The drying time is not particularly limited, and may be, for example, 30 seconds or more, 40 seconds or more, 50 seconds or more, or 60 seconds or more, and may be 150 seconds or less, 130 seconds or less, 110 seconds or less, or 90 seconds or less.
[0101] In addition, the coating film may be cured (curing step). The curing may be performed, for example, by heating, light irradiation, etc. The light is not particularly limited, and may be, for example, ultraviolet light. The light source of the light irradiation is also not particularly limited, and may be, for example, a high-pressure mercury lamp. The irradiation amount of the energy ray source in the ultraviolet curing is preferably 50 mJ / cm in terms of the cumulative exposure at an ultraviolet wavelength of 365 nm. 2 ~500mJ / cm 2 If the irradiation dose is 50mJ / cm 2 If the irradiation dose is 500 mJ / cm 2 Then, the formed anti-reflection layer can be prevented from being colored.
[0102] As the anti-glare (AG) treatment, known AG treatment can be applied without particular limitation, for example, by forming an anti-glare layer on the second surface of the substrate of the present invention. As the anti-glare layer, known anti-glare layers can be adopted without particular limitation, usually, formed as a layer in which inorganic or organic particles as anti-glare agents are dispersed in a resin.
[0103] The anti-glare layer is not particularly limited, and can be formed, for example, using an anti-glare layer-forming material including a resin, particles, and a thixotropy-imparting agent, and the particles and the thixotropy-imparting agent are agglomerated to form convex portions on the surface of the anti-glare layer. With this configuration, the anti-glare layer has excellent display characteristics that take into account both anti-glare properties and prevention of white blur, and even if the anti-glare layer is formed by agglomeration of particles, the generation of protrusions on the surface of the anti-glare layer that become appearance defects can be prevented, thereby improving the yield rate of the product.
[0104] Examples of the resin include thermosetting resins and ionizing radiation curable resins that are cured by ultraviolet rays or light. Commercially available thermosetting resins, ultraviolet curable resins, and the like may also be used as the resin.
[0105] As the above-mentioned thermosetting resin and ultraviolet curing resin, for example, a curing compound having at least one group of an acrylate group and a methacrylate group that is cured by heat, light (ultraviolet rays, etc.) or an electron beam, etc. can be used, for example, oligomers or prepolymers such as acrylates or methacrylates of polyfunctional compounds such as polysiloxane resins, polyester resins, polyether resins, epoxy resins, urethane resins, alkyd resins, spiroacetal resins, polybutadiene resins, polythiol polyene resins, and polyols, etc., can be cited. They can be used alone or in combination of two or more.
[0106] The above-mentioned resin can use a reactive diluent having at least one group of an acrylate group and a methacrylate group. The above-mentioned reactive diluent can use, for example, the reactive diluent recorded in Japanese Patent Publication No. 2008-88309, for example, including monofunctional acrylate, monofunctional methacrylate, multifunctional acrylate, multifunctional methacrylate, etc. As the above-mentioned reactive diluent, trifunctional or higher acrylate and trifunctional or higher methacrylate are preferred. This is because the hardness of the anti-glare layer can be made excellent. As the above-mentioned reactive diluent, for example, butanediol glyceryl ether diacrylate, isocyanuric acid acrylate, isocyanuric acid methacrylate, etc. can be cited. They can be used alone or in combination of two or more.
[0107] As the resin, a urethane acrylate resin is preferably included, and a copolymer of a curable urethane acrylate resin and a multifunctional acrylate (for example, pentaerythritol triacrylate) is more preferred.
[0108] The main function of the particles used to form the anti-glare layer is to make the surface of the anti-glare layer formed into a concavo-convex shape to impart anti-glare properties and to control the haze value of the anti-glare layer. The haze value of the anti-glare layer can be designed by controlling the refractive index difference between the particles and the resin. As the particles, for example, there are inorganic particles and organic particles. There is no particular restriction on the inorganic particles, and for example, silicon oxide particles, titanium oxide particles, aluminum oxide particles, zinc oxide particles, tin oxide particles, zirconium oxide particles, calcium carbonate particles, barium sulfate particles, talc particles, kaolin particles and calcium sulfate particles can be listed. In addition, there is no particular restriction on the organic particles, and for example, polymethyl methacrylate resin powder (PMMA particles), polysiloxane resin powder, polystyrene resin powder, polycarbonate resin powder, acrylic styrene resin powder, benzoguanamine resin powder, melamine resin powder, polyolefin resin powder, polyester resin powder, polyamide resin powder, polyimide resin powder, polyvinyl fluoride resin powder, etc. These inorganic particles and organic particles can be used alone or in combination of two or more.
[0109] The weight average particle size (D) of the above-mentioned particles is preferably in the range of 2.5μm to 10μm. By setting the weight average particle size of the particles within the range, for example, the anti-glare property is better and white blur can be prevented. The weight average particle size of the above-mentioned particles is more preferably in the range of 3μm to 7μm. It should be noted that the weight average particle size of the above-mentioned particles can be measured, for example, by the Coulter counting method. For example, using a particle size distribution measuring device using a pore resistance method (trade name: Coulter Multisizer, manufactured by Beckman Coulter), the resistance of the electrolyte equivalent to the volume of the particles when the particles pass through the above-mentioned pores is measured, thereby measuring the number and volume of the above-mentioned particles, and calculating the weight average particle size.
[0110] The shape of the particles is not particularly limited, and may be, for example, roughly spherical beads or particles of irregular shape such as powder. Preferred particles are roughly spherical particles, more preferably roughly spherical particles with an aspect ratio of less than 1.5, and most preferably spherical particles.
[0111] The ratio of the particles in the anti-glare layer is preferably in the range of 0.2 to 12 parts by weight, more preferably in the range of 0.5 to 12 parts by weight, and further preferably in the range of 1 to 7 parts by weight relative to 100 parts by weight of the resin. By setting it within the above range, for example, the anti-glare property is more excellent and white blur can be prevented.
[0112] The anti-glare layer may contain a thixotropy-imparting agent. By including the thixotropy-imparting agent, the aggregation state of the particles can be easily controlled. Examples of the thixotropy-imparting agent used to form the anti-glare layer include organic clay, oxidized polyolefin, and modified urea.
[0113] In order to improve the affinity with the resin, the organoclay is preferably clay that has been subjected to an organic treatment. Examples of the organoclay include layered organoclay. The organoclay may be prepared by itself or a commercial product may be used. Examples of the commercially available products include Lucentite SAN, Lucentite STN, Lucentite SEN, Lucentite SPN, Somasif ME-100, Somasif MAE, Somasif MTE, Somasif MEE, and Somasif MPE (trade names, all manufactured by Co-op Chemical Co., Ltd.); ESBEN, ESBEN C, ESBEN E, SBEN W, ESBEN P, ESBEN WX, ESBEN N-400, ESBEN NX, ESBEN NX80, ESBEN NO12S, ESBEN NEZ, ESBEN NO12, ESBEN NE, ESBEN NZ, ESBEN NZ70, ORGANITE, ORGANITE D, and ORGANITE T (trade names, all manufactured by Hojun Co., Ltd.); KUNIPIA F, KUNIPIA G, and KUNIPIA G4 (trade names, all manufactured by Kunimine Industries, Ltd.); TIXOGEL VZ, Kraton HT, Kraton 40 (trade names, all manufactured by Rockwood Additives), etc.
[0114] The oxidized polyolefin may be prepared by itself or a commercial product may be used. Examples of the commercial product include Disparlon 4200-20 (trade name, manufactured by Kusumoto Chemicals Co., Ltd.) and Flownon SA300 (trade name, manufactured by Kyoeisha Chemical Co., Ltd.).
[0115] The modified urea is a reaction product of an isocyanate monomer or an adduct thereof with an organic amine. The modified urea can be prepared by itself or a commercial product can be used. Examples of the commercial product include BYK410 (manufactured by BYK-Chemie).
[0116] The above-mentioned thixotropy-imparting agents may be used alone or in combination of two or more.
[0117] The height of the convex portion from the roughness average line of the anti-glare layer is preferably less than 0.4 times the thickness of the anti-glare layer. More preferably, it is in the range of greater than or equal to 0.01 times and less than 0.4 times, and further preferably in the range of greater than or equal to 0.01 times and less than 0.3 times. If within this range, it is possible to appropriately prevent the formation of protrusions that become appearance defects on the convex portion. The anti-glare layer can be less prone to appearance defects by having a convex portion of such a height. Here, the height from the average line can be measured, for example, by the method described in Japanese Patent Gazette No. 2017-138620.
[0118] The ratio of the thixotropy-imparting agent in the antiglare layer is preferably in the range of 0.1 to 5 parts by weight, and more preferably in the range of 0.2 to 4 parts by weight, based on 100 parts by weight of the resin.
[0119] The thickness (d) of the anti-glare layer is not particularly limited, and is preferably in the range of 3 μm to 12 μm. By setting the thickness (d) of the anti-glare layer within the above range, for example, the optical adhesive sheet of the present invention can be prevented from curling, and problems of reduced productivity such as poor transportability can be avoided. In addition, when the thickness (d) is within the above range, as described above, the weight-average particle size (D) of the particles is preferably in the range of 2.5 μm to 10 μm. By making the thickness (d) of the anti-glare layer and the weight-average particle size (D) of the particles the above combination, the anti-glare property can be made better. The thickness (d) of the anti-glare layer is more preferably in the range of 3 μm to 8 μm.
[0120] The relationship between the thickness (d) of the anti-glare layer and the weight average particle size (D) of the particles is preferably in the range of 0.3≤D / d≤0.9. With such a relationship, an anti-glare layer with better anti-glare properties and prevention of white blurring can be made, and further, an anti-glare layer without appearance defects can be made.
[0121] In the optical adhesive sheet of the present invention, as described above, the anti-glare layer forms convex portions on the surface of the anti-glare layer by agglomeration of the particles and the thixotropy imparting agent. In the agglomerated portion forming the convex portion, the particles exist in a state of being aggregated in the surface direction of the anti-glare layer. Thus, the convex portion has a gentle shape. The anti-glare layer can prevent white blurring while maintaining anti-glare properties by having convex portions of such a shape, and thus can be less likely to produce appearance defects.
[0122] The surface shape of the anti-glare layer can be arbitrarily designed by controlling the coagulation state of the particles contained in the anti-glare layer forming material. The coagulation state of the particles can be controlled, for example, by the material of the particles (e.g., the chemical modification state of the particle surface, the affinity to the solvent or resin, etc.), the type and combination of the resin (adhesive) or the solvent. Here, the coagulation state of the particles can be controlled by the thixotropy imparting agent contained in the anti-glare layer forming material. As a result, the coagulation state of the particles can be made as described above, and the convex portion can be made into a gentle shape.
[0123] In the optical adhesive sheet of the present invention, when the substrate of the present invention is formed by a resin or the like, it is preferred that a permeation layer is provided at the interface between the substrate of the present invention and the anti-glare layer. The permeation layer is formed by the resin component contained in the material forming the anti-glare layer penetrating into the substrate of the present invention. When a permeation layer is formed, it is preferred because the adhesion between the substrate of the present invention and the anti-glare layer can be improved. The thickness of the permeation layer is preferably in the range of 0.2 μm to 3 μm, and more preferably in the range of 0.5 μm to 2 μm. For example, when the substrate of the present invention is a polyester resin and the resin contained in the anti-glare layer is an acrylic resin, the permeation layer can be formed. The permeation layer can be confirmed, for example, by observing the cross section of the optical adhesive sheet of the present invention using a transmission electron microscope (TEM), and its thickness can be measured.
[0124] Even when applied to the optical adhesive sheet of the present invention having such a permeable layer, it is possible to easily form a desired gentle surface concave-convex shape that takes into account both anti-glare properties and prevention of white blur. The more the substrate lacks adhesion to the above-mentioned anti-glare layer, the more the above-mentioned permeable layer improves adhesion, so it is preferably formed thicker.
[0125] In the above anti-glare layer, it is preferred that the number of appearance defects with a maximum diameter of 200 μm or more is 1 m2 per 1 m2 of the anti-glare layer. 2 More preferably, there is no such appearance defect.
[0126] In the concavo-convex shape of the anti-glare layer surface, the average tilt angle θa (°) is preferably in the range of 0.1 to 5.0, more preferably in the range of 0.3 to 4.5, further preferably in the range of 1.0 to 4.0, and particularly preferably in the range of 1.6 to 4.0. Here, the average tilt angle θa is a value defined by the following mathematical formula (1). The average tilt angle θa is, for example, a value measured by the method described in Japanese Patent Application Laid-Open No. 2017-138620.
[0127] Average tilt angle θa = tan-1Δa (1)
[0128] In the mathematical formula (1), Δa is a value obtained by dividing the sum of the differences (height h) between the apex of adjacent peaks and the lowest points of troughs (h1+h2+h3···+hn) by the reference length L of the roughness curve specified in JIS B0601 (1994 edition), as shown in the following mathematical formula (2). The roughness curve is a curve obtained by removing surface undulation components longer than a specified wavelength from a profile curve using a phase difference compensation type high-pass filter. In addition, the profile curve refers to a contour that appears at the cut when the target surface is cut by a plane at right angles to the target surface.
[0129] Δa=(h1+h2+h3···+hn) / L (2)
[0130] When θa is within the above range, the anti-glare property is more excellent and white blurring can be prevented.
[0131] When forming the antiglare layer of the present invention, the prepared antiglare layer-forming material (coating solution) preferably exhibits thixotropy, and the Ti value specified below is preferably in the range of 1.3 to 3.5, and more preferably in the range of 1.3 to 2.8.
[0132] Ti value = β1 / β2
[0133] Here, β1 is the viscosity measured at a shear rate of 20 (1 / s) using Rheo stress 6000 manufactured by HAAKE, and β2 is the viscosity measured at a shear rate of 200 (1 / s) using Rheo stress 6000 manufactured by HAAKE.
[0134] When the Ti value is less than 1.3, appearance defects are likely to occur, and the anti-glare property and white blur properties are deteriorated. On the other hand, when the Ti value is greater than 3.5, the particles are unlikely to aggregate and are likely to be in a dispersed state.
[0135] The method for producing the anti-glare layer of the present invention is not particularly limited, and the anti-glare layer can be produced by any method, for example, by preparing an anti-glare layer-forming material (coating solution) containing the above-mentioned resin, the above-mentioned particles, the above-mentioned thixotropy imparting agent and a solvent, applying the above-mentioned anti-glare layer-forming material (coating solution) on the second surface of the substrate of the present invention to form a coating film, and curing the above-mentioned coating film to form an anti-glare layer. A transfer method using a mold, a method of imparting a concave-convex shape by a suitable method such as sandblasting or an embossing roller, etc. can also be used together.
[0136] The above-mentioned solvent is not particularly limited, and various solvents can be used, one alone or two or more solvents can be used in combination. According to the composition of the resin, the type and content of the particles and the thixotropy imparting agent, there are optimal solvent types and solvent ratios. As solvents, there are no particular restrictions, for example, they can be listed: alcohols such as methanol, ethanol, isopropanol, butanol, 2-methoxyethanol; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone; esters such as methyl acetate, ethyl acetate, butyl acetate; ethers such as diisopropyl ether and propylene glycol monomethyl ether; glycols such as ethylene glycol and propylene glycol; cellosolves such as ethyl cellosolve and butyl cellosolve; aliphatic hydrocarbons such as hexane, heptane, octane; aromatic hydrocarbons such as benzene, toluene, xylene, etc.
[0137] When the permeable layer is formed of a polyester resin as the substrate of the present invention, a good solvent for the polyester resin can be preferably used. Examples of the solvent include ethyl acetate, methyl ethyl ketone, and cyclopentanone.
[0138] By appropriately selecting the above solvent, the thixotropy of the thixotropy imparting agent to the anti-glare layer forming material (coating solution) can be well expressed. For example, when using organoclay, toluene and xylene can be appropriately used alone or in combination, for example, when using oxidized polyolefin, methyl ethyl ketone, ethyl acetate, propylene glycol monomethyl ether can be appropriately used alone or in combination, for example, when using modified urea, butyl acetate and methyl isobutyl ketone can be appropriately used alone or in combination.
[0139] Various leveling agents can be added to the above-mentioned anti-glare layer forming material. As the above-mentioned leveling agent, in order to prevent uneven coating (uniformization of the coating surface), for example, a fluorine-containing type or silicone-based leveling agent can be used. The leveling agent can be appropriately selected according to the situation that the surface of the above-mentioned anti-glare layer requires antifouling properties, or the situation that an anti-reflection layer (low refractive index layer) and a layer containing an interlayer filler are formed on the anti-glare layer. For example, by including the above-mentioned thixotropy imparting agent, the coating liquid can be made to exhibit thixotropy, so uneven coating is not easy to occur. Therefore, for example, there is an advantage of expanding the selection range of the above-mentioned leveling agent.
[0140] The amount of the leveling agent blended is, for example, 5 parts by weight or less, and preferably within a range of 0.01 to 5 parts by weight, relative to 100 parts by weight of the resin.
[0141] The anti-glare layer forming material may be added with pigments, fillers, dispersants, plasticizers, ultraviolet absorbers, surfactants, antifouling agents, antioxidants, etc. as needed within a range that does not impair performance. These additives may be used alone or in combination of two or more.
[0142] As the anti-glare layer forming material, for example, a conventionally known photopolymerization initiator described in Japanese Patent Application Laid-Open No. 2008-88309 can be used.
[0143] As a method for coating the anti-glare layer forming material on the second surface of the substrate of the present invention, for example, a coating method such as inkjet coating, die coating, spin coating, spray coating, gravure coating, roll coating, and bar coating can be used.
[0144] The anti-glare layer forming material is applied to form a coating on the substrate of the present invention, and the coating is cured. Preferably, the coating is dried before curing. The drying may be, for example, natural drying, air drying by blowing, heating drying, or a combination of these.
[0145] The curing method of the coating of the anti-glare layer forming material is not particularly limited, but ultraviolet curing is preferred. The irradiation amount of the energy ray source is preferably 50 mJ / cm in terms of cumulative exposure at an ultraviolet wavelength of 365 nm. 2 ~500mJ / cm 2 If the irradiation dose is 50mJ / cm 2 If the irradiation dose is 500 mJ / cm 2 The following can prevent the formed anti-glare layer from being colored.
[0146] By operating as above, the anti-glare layer can be formed on the second surface of the substrate of the present invention. It should be noted that the anti-glare layer can also be formed by a manufacturing method other than the above method. The hardness of the anti-glare layer is also affected by the thickness of the layer in terms of pencil hardness, but preferably has a hardness of more than 2H.
[0147] The anti-glare layer may have a multi-layer structure of two or more layers stacked together.
[0148] The AR layer (low refractive index layer) can also be configured on the anti-glare layer. For example, when the optical adhesive sheet is installed in an image display device, one of the main reasons for reducing the visual recognition of the image can be the reflection of light at the interface between air and the anti-glare layer. The AR layer reduces its surface reflection. It should be noted that the anti-glare layer and the anti-reflection layer can be a multilayer structure with two or more layers stacked.
[0149] In order to prevent the adhesion of contaminants and improve the ease of removal of adhered contaminants, it is preferred to stack a contamination prevention layer composed of a fluorine-containing silane compound or a fluorine-containing organic compound on the antireflection layer and / or antiglare layer.
[0150] Preferably, at least one of the substrate of the present invention and the anti-glare layer is surface treated. If the surface of the substrate of the present invention is surface treated, the adhesion to the anti-glare layer is further improved. In addition, if the surface of the anti-glare layer is surface treated, the adhesion to the AR layer is further improved.
[0151] In order to prevent the substrate of the present invention from curling, the other side of the anti-glare layer may be subjected to solvent treatment. In addition, in order to prevent curling, a transparent resin layer may be formed on the other side of the anti-glare layer.
[0152] <Adhesive Layer>
[0153] The adhesive layer of the present invention may be an adhesive layer without a substrate (substrate layer), or an adhesive layer of a type having a substrate. It should be noted that in this specification, an adhesive layer without a substrate (substrate layer) is sometimes referred to as a "substrate-free adhesive layer", and an adhesive layer of a type having a substrate is sometimes referred to as a "substrate-without adhesive layer". As the above-mentioned substrate-free adhesive layer, for example, an adhesive layer including only a single layer of the adhesive layer of the present invention, an adhesive layer including the adhesive layer of the present invention and other adhesive layers (adhesive layers other than the adhesive layer of the present invention), etc. can be cited. In addition, as the above-mentioned adhesive layer with a substrate, an adhesive layer having the adhesive layer of the present invention on both sides of the substrate can be cited; an adhesive layer having the adhesive layer of the present invention on one side of the substrate and other adhesive layers on the other side, etc. As the "substrate (substrate layer)" constituting the "adhesive layer with a substrate", a plastic film similar to the substrate of the present invention can be used.
[0154] The surface resistance of the adhesive layer of the present invention is less than 10 10 Ω. The surface resistance of the adhesive layer of the present invention is less than 10 10 The structure of Ω is suitable from the following aspects: the adhesive layer of the present invention exhibits excellent antistatic effect and suppresses the generation of static electricity when the adhesive sheet is peeled off from the image display panel for rework when the image display panel of the present invention has poor lamination. From the aspect that the adhesive layer of the present invention exhibits a more excellent antistatic effect and can more effectively suppress the generation of static electricity during rework of the image display device of the present invention, the surface resistance value of the adhesive layer of the present invention is preferably 0.97×10 10 Ω or less, more preferably 0.96×10 10 Ω or less, more preferably 0.95×10 10 The lower limit of the surface resistance value of the adhesive layer of the present invention is not particularly limited, and the lower the value, the better, but it can be 10 7 Ω or more.
[0155] The surface resistance value of the adhesive layer of the present invention after the following heat shock test is preferably less than 10 10 Ω.
[0156] Thermal shock test
[0157] The optical pressure-sensitive adhesive sheet was subjected to 200 cycles of exposure to an atmosphere of −40° C. for 30 minutes and then to an atmosphere of 80° C. for 30 minutes using a heat shock tester.
[0158] The surface resistance of the adhesive layer of the present invention after the above-mentioned thermal shock test is less than 10 10 The structure of Ω is suitable from the following aspects: the adhesive layer of the present invention can maintain excellent antistatic effect even in harsh environments such as thermal shock. For example, when a light-emitting element fails to light up in the use environment of an image display device, the generation of static electricity can be suppressed when the adhesive sheet is peeled off from the image display panel for repair. From the perspective of maintaining a more excellent antistatic effect in the use environment of the image display device and more effectively suppressing the generation of static electricity when reworking the image display device of the present invention, the surface resistance value of the adhesive layer of the present invention after the above thermal shock test is preferably 0.97×10 10 Ω or less, more preferably 0.96×10 10 Ω or less, more preferably 0.95×10 10 The lower limit of the surface resistance value of the adhesive layer of the present invention after the above-mentioned heat shock test is not particularly limited, and the lower the better, but it can be 10 7 Ω or more.
[0159] The absolute value of the difference in surface resistance of the adhesive layer of the present invention before and after the heat shock test was calculated according to the following formula.
[0160] |Log 10 B-Log 10 A|
[0161] A: Surface resistance value before thermal shock test
[0162] B: Surface resistance value after thermal shock test
[0163] The absolute value of the difference in surface resistance of the adhesive layer of the present invention before and after the thermal shock test (|Log 10 B-Log 10A|) is preferably 1 logΩ or less. The configuration in which the difference in the surface resistance value of the adhesive layer of the present invention before and after the above-mentioned thermal shock test is 1 logΩ or less is suitable from the following aspects: the adhesive layer of the present invention can also maintain an excellent antistatic effect under a harsh environment such as thermal shock. For example, in the case of a failure such as a light-emitting element not lighting up in the use environment of an image display device, the generation of static electricity can be suppressed when the adhesive sheet is peeled off from the image display panel for repair. From the perspective that the adhesive layer of the present invention maintains a more excellent antistatic effect in the use environment of the image display device, and can more effectively suppress the generation of static electricity when rework is performed to repair the image display device of the present invention, the difference in the surface resistance value of the adhesive layer of the present invention before and after the above-mentioned thermal shock test is more preferably 0.9 logΩ or less, further preferably 0.8 logΩ or less, and particularly preferably 0.7 logΩ or less.
[0164] The surface resistivity of the adhesive layer of the present invention, the surface resistance value before and after the above-mentioned heat shock test, and the difference thereof are measured by the surface resistance value measurement in the examples described later. The surface resistivity of the adhesive layer of the present invention, the surface resistance value before and after the above-mentioned heat shock test, and the difference thereof can be adjusted by the composition of the adhesive composition used to form the adhesive layer of the present invention (e.g., the type, molecular weight, usage amount, monomer composition, type and amount of functional groups, type and amount of antistatic agent, type and amount of crosslinking agent), curing conditions (heating conditions, radiation irradiation conditions), etc.
[0165] The hardness H [kPa] of the adhesive layer of the present invention measured by the nanoindentation method is preferably less than 60 kPa. The hardness H [kPa] of the adhesive layer of the present invention measured by the nanoindentation method is less than 60 kPa. The structure of the adhesive layer of the present invention having a hardness H [kPa] of less than 60 kPa is suitable from the following aspects: in the case of a height difference of a concave-convex shape such as a printed layer or wiring in an image display panel, an optical component, etc., the adhesive layer of the present invention fully follows the height difference and can be filled without residual bubbles, that is, it shows excellent height difference absorption, and thus can prevent the above-mentioned poor lamination. From the aspect that the adhesive layer of the present invention shows a more excellent height difference absorption, the hardness H [kPa] of the adhesive layer of the present invention measured by the nanoindentation method is preferably 55 kPa or less, more preferably 50 kPa or less, and can also be 45 kPa or less. From the viewpoint of processability such as the unfavorable situation that the adhesive layer protrudes from the end when the optical adhesive sheet of the present invention is stored, the lower limit of the hardness H [kPa] of the adhesive layer of the present invention measured by the nanoindentation method is preferably 1 kPa or more, and can also be 5 kPa or more.
[0166] The hardness H of the adhesive layer of the present invention measured by the above-mentioned nanoindentation method can be specifically measured by the method of the embodiment described later. The hardness H of the adhesive layer of the present invention measured by the above-mentioned nanoindentation method can be adjusted by the composition of the adhesive composition used to form the adhesive layer of the present invention (for example, the type, molecular weight, usage amount, monomer composition, type and amount of functional groups, type and amount of antistatic agent, type and amount of crosslinking agent), curing conditions (heating conditions, radiation irradiation conditions), etc.
[0167] The glass transition temperature (Tg) of the adhesive layer of the present invention is preferably 10°C or less. The configuration in which the Tg of the adhesive layer of the present invention is 10°C or less is preferred from the following aspects: the excellent height difference absorption of the adhesive layer of the present invention can be maintained even in a low temperature environment. From the perspective of being able to maintain the more excellent height difference absorption of the adhesive layer of the present invention even in a low temperature environment, the glass transition temperature of the adhesive layer of the present invention is preferably -15°C or less, and may also be -20°C or less. There is no particular restriction on the lower limit of the Tg of the adhesive layer of the present invention, but from the perspective of processability such as the adhesive layer not easily protruding from the end when the optical adhesive sheet of the present invention is stored, it is preferably -50°C or more, and may also be -40°C or more.
[0168] The glass transition temperature (Tg) of the adhesive layer of the present invention is measured by the dynamic viscoelasticity measurement in the examples described later. The glass transition temperature (Tg) of the adhesive layer of the present invention can be adjusted by the composition of the adhesive composition used to form the adhesive layer of the present invention (e.g., the type, molecular weight, usage, monomer composition, type and amount of functional groups, type and amount of antistatic agent, type and amount of crosslinking agent), curing conditions (heating conditions, radiation irradiation conditions), etc.
[0169] The storage modulus of the adhesive layer of the present invention at 25°C and 1Hz is preferably less than 200kPa. The configuration in which the storage modulus of the adhesive layer of the present invention at 25°C and 1Hz is less than 200kPa is preferred from the following aspects: the adhesive layer of the present invention fully follows the contraction or expansion in the use environment of the image display device of the present invention, and can suppress bulging and peeling. In addition, it is suitable from the following aspects: in the case where there is a height difference of a concave-convex shape such as a printed layer or wiring on an image display panel or an optical component, etc., it shows excellent height difference absorption, thereby being able to prevent the above-mentioned poor bonding. From the perspective of suppressing the bulging, peeling, and height difference absorption of the optical adhesive sheet of the present invention, the storage modulus of the adhesive layer of the present invention at 25°C and 1Hz is preferably 180kPa or less, more preferably 160kPa or less, further preferably 140kPa or less, and can also be 120kPa or less. The lower limit of the storage elastic modulus of the adhesive layer of the present invention at 25°C and 1 Hz is not particularly limited, but is preferably 1 kPa or more, and may be 5 kPa or more, from the viewpoint of processability such as preventing the adhesive layer from protruding from the edge during storage of the optical adhesive sheet of the present invention.
[0170] The storage modulus of the adhesive layer of the present invention at 85°C and 1Hz is preferably less than 100kPa. The configuration in which the storage modulus of the adhesive layer of the present invention at 85°C and 1Hz is less than 100kPa is preferred from the following aspects: the adhesive layer of the present invention fully follows the contraction or expansion in the use environment of the image display device of the present invention, and can suppress bulging and peeling. In addition, it is suitable from the following aspects: in the case where there is a height difference of a concave-convex shape such as a printed layer or wiring on an image display panel or an optical component, it shows excellent height difference absorption, thereby preventing the above-mentioned poor bonding. From the perspective of suppressing the bulging, peeling, and height difference absorption of the optical adhesive sheet of the present invention, the storage modulus of the adhesive layer of the present invention at 85°C and 1Hz is preferably 97kPa or less, more preferably 95kPa or less, further preferably 92kPa or less, and may also be 90kPa or less. The lower limit of the storage elastic modulus of the adhesive layer of the present invention at 85°C and 1 Hz is not particularly limited, but is preferably 1 kPa or more, and may be 5 kPa or more, from the viewpoint of processability such as preventing the adhesive layer from protruding from the edge when the optical adhesive sheet of the present invention is stored.
[0171] The storage modulus of the adhesive layer of the present invention at 25°C or 85°C and 1 Hz is measured by the dynamic viscoelasticity measurement in the examples described later. The storage modulus of the adhesive layer of the present invention at 25°C or 85°C and 1 Hz can be adjusted by the composition of the adhesive composition used to form the adhesive layer of the present invention (e.g., the type, molecular weight, usage, monomer composition, type and amount of functional groups, type and amount of antistatic agent, type and amount of crosslinking agent), curing conditions (heating conditions, radiation irradiation conditions), etc.
[0172] The 300% tensile residual stress value of the adhesive layer of the present invention is not particularly limited, but is preferably 25 N / cm 2 The 300% tensile residual stress value of the adhesive layer of the present invention is 25N / cm 2 The following configuration is preferred from the following perspectives: the adhesive layer of the present invention fully follows the contraction or expansion in the use environment of the image display device of the present invention, and can suppress bulging and peeling. In addition, it is suitable from the following perspectives: when there is a height difference of a concave-convex shape such as a printed layer or wiring on an image display panel or an optical component, it shows excellent height difference absorption, thereby being able to prevent the above-mentioned poor bonding. From the perspective of suppressing bulging, peeling, and better height difference absorption of the optical adhesive sheet of the present invention, the 300% tensile residual stress value of the adhesive layer of the present invention is more preferably 20N / cm 2 Below, more preferably 18N / cm 2 Below, can also be 15N / cm 2 The lower limit of the 300% tensile residual stress value of the adhesive layer of the present invention is not particularly limited, but is preferably 1 N / cm2 from the viewpoint of processability such as the difficulty in causing the adhesive layer to protrude from the end when the optical adhesive sheet of the present invention is stored. 2 Above, it can also be 1.5N / cm 2 above.
[0173] The 300% tensile residual stress value of the adhesive layer of the present invention is measured by the 300% tensile residual stress value measurement in the examples described later. The 300% tensile residual stress value of the adhesive layer of the present invention can be adjusted by the composition of the adhesive composition used to form the adhesive layer of the present invention (e.g., the type, molecular weight, usage, monomer composition, type and amount of functional groups, type and amount of antistatic agent, type and amount of crosslinking agent), curing conditions (heating conditions, radiation irradiation conditions), etc.
[0174] As the adhesive constituting the adhesive layer of the present invention, there is no particular limitation, and for example, acrylic adhesives, rubber adhesives, vinyl alkyl ether adhesives, polysiloxane adhesives, polyester adhesives, polyamide adhesives, polyurethane adhesives, fluorine-containing adhesives, epoxy adhesives, etc. can be cited. Among them, as the adhesive constituting the adhesive layer, acrylic adhesives are preferred from the viewpoints of transparency, adhesion, weather resistance, cost, and ease of design of the adhesive. That is, the adhesive layer of the present invention is preferably an acrylic adhesive layer consisting of an acrylic adhesive. The above-mentioned adhesives can be used alone or in combination of two or more.
[0175] The acrylic adhesive layer contains an acrylic polymer as a base polymer. The acrylic polymer is a polymer containing an acrylic monomer (a monomer having a (meth)acryloyl group in the molecule) as a monomer component constituting the polymer. The acrylic polymer is preferably a polymer containing an alkyl (meth)acrylate as a monomer component constituting the polymer. It should be noted that the acrylic polymer can be used alone or in combination of two or more.
[0176] The adhesive composition forming the adhesive layer of the present invention can be in any form. For example, the adhesive composition can be an emulsion type, a solvent type (solution type), an active energy ray curing type, a hot melt type (hot melt type), etc. Among them, from the aspect of productivity, it is easy to obtain an adhesive layer with excellent optical properties and appearance, preferably a solvent type, an active energy ray curing type adhesive composition. In particular, from the viewpoint of being easy to control the above-mentioned various characteristics (especially the height difference absorption) of the adhesive layer within a specified range, preferably an active energy ray curing type adhesive composition.
[0177] That is, the adhesive layer of the present invention is an acrylic adhesive layer containing an acrylic polymer as a base polymer, and is preferably formed from an active energy ray-curable acrylic adhesive composition. In addition, the adhesive layer of the present invention is an acrylic adhesive layer containing an acrylic polymer as a base polymer, and is preferably formed from a solvent-based acrylic adhesive composition.
[0178] Examples of the active energy rays include ionizing radiation such as α rays, β rays, γ rays, neutron rays, electron rays, and ultraviolet rays, and ultraviolet rays are particularly preferred. That is, the active energy ray-curable adhesive composition is preferably an ultraviolet-curable adhesive composition.
[0179] As the adhesive composition (acrylic adhesive composition) forming the above-mentioned acrylic adhesive layer, for example, there can be mentioned: an acrylic adhesive composition having an acrylic polymer as an essential component, or an acrylic adhesive composition having a mixture of monomers (monomers) constituting acrylic polymers (sometimes referred to as a "monomer mixture") or a partial polymer thereof as an essential component. As the former, for example, the so-called solvent-based acrylic adhesive composition can be mentioned. In addition. As the latter, for example, the so-called active energy ray-curable acrylic adhesive composition can be mentioned. The above-mentioned "monomer mixture" refers to a mixture containing monomer components constituting a polymer. In addition, the above-mentioned "partial polymer" is sometimes also referred to as a "prepolymer", which refers to a composition formed by partial polymerization of one or more monomer components among the monomer components in the above-mentioned monomer mixture.
[0180] The acrylic polymer is a polymer composed (formed) of an acrylic monomer as an essential monomer component (monomer component). The acrylic polymer is preferably a polymer composed (formed) of an alkyl (meth)acrylate as an essential monomer component. That is, the acrylic polymer preferably contains an alkyl (meth)acrylate as a structural unit. In this specification, "(meth)acrylic acid" means "acrylic acid" and / or "methacrylic acid" (either or both of "acrylic acid" and "methacrylic acid"), and the same applies to others. It should be noted that the acrylic polymer is composed of one or more monomer components.
[0181] The (meth)acrylic acid alkyl ester as the essential monomer component preferably includes a (meth)acrylic acid alkyl ester having a linear or branched alkyl group. The (meth)acrylic acid alkyl ester may be used alone or in combination of two or more.
[0182] The (meth)acrylic acid alkyl ester having a linear or branched alkyl group is not particularly limited, and examples thereof include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, pentyl (meth)acrylate, isopentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, nonyl (meth)acrylate, propyl ...tert-butyl (meth)acrylate, tert-butyl (meth)acrylate, tert-butyl (meth)acrylate, tert-butyl (meth)acrylate, tert-butyl (meth)acrylate, tert-butyl (meth)acrylate, tert-butyl (meth)acrylate, tert-butyl (meth)acrylate, tert-butyl ( Alkyl (meth)acrylates having a linear or branched alkyl group having 1 to 20 carbon atoms, such as isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate (stearyl (meth)acrylate), isostearyl (meth)acrylate, nonadecyl (meth)acrylate, eicosyl (meth)acrylate. Among them, the alkyl (meth)acrylates having a linear or branched alkyl group are preferably alkyl (meth)acrylates having a linear or branched alkyl group having 4 to 18 carbon atoms, and more preferably 2-ethylhexyl acrylate (2EHA), isostearyl acrylate (ISTA), lauryl acrylate (LA), and butyl acrylate (BA). The above-mentioned alkyl (meth)acrylates having a linear or branched alkyl group may be used alone or in combination of two or more.
[0183] The proportion of the alkyl (meth)acrylate in all monomer components (100 wt %) constituting the acrylic polymer is not particularly limited, but is preferably 50 wt % or more (e.g., 50 to 100 wt %), more preferably 53 to 100 wt %, and further preferably 55 to 100 wt %.
[0184] In addition, the acrylic adhesive composition may contain the above-mentioned alkyl (meth)acrylate in addition to the acrylic polymer. When the acrylic adhesive composition contains the alkyl (meth)acrylate in addition to the acrylic polymer, the content (compounding amount) of the alkyl (meth)acrylate is preferably 10 parts by weight or more (e.g., 10 to 100 parts by weight), more preferably 20 to 90 parts by weight, and even more preferably 30 to 80 parts by weight, relative to 100 parts by weight of the acrylic polymer.
[0185] The acrylic polymer may contain a copolymerizable monomer together with the (meth)acrylic acid alkyl ester as a monomer component constituting the polymer. That is, the acrylic polymer may contain a copolymerizable monomer as a structural unit. It should be noted that the copolymerizable monomer may be used alone or in combination of two or more.
[0186] As the copolymerizable monomer, there is no particular restriction. From the viewpoint of easily controlling the various properties (especially the height difference absorbency) of the adhesive layer within the specified range, suppressing the cloudiness under high humidity environment, improving durability, adhesion reliability, compatibility with various additives such as ultraviolet absorbers, and transparency, preferably a monomer having a nitrogen atom in the molecule and a monomer having a hydroxyl group in the molecule are listed. That is, the acrylic polymer preferably contains a monomer having a nitrogen atom in the molecule as a structural unit. In addition, the acrylic polymer preferably contains a monomer having a hydroxyl group in the molecule as a structural unit.
[0187] The monomer having a nitrogen atom in the molecule is a monomer having at least one nitrogen atom in the molecule (in one molecule). In this specification, the "monomer having a nitrogen atom in the molecule" is sometimes referred to as a "nitrogen atom-containing monomer". There are no particular restrictions on the nitrogen atom-containing monomer, and preferably cyclic nitrogen-containing monomers, (meth)acrylamides, etc. are listed. It should be noted that the nitrogen atom-containing monomer can be used alone or in combination of two or more.
[0188] The cyclic nitrogen-containing monomer is not particularly limited as long as it is a monomer having a polymerizable functional group having an unsaturated double bond such as a (meth)acryloyl group or a vinyl group and having a cyclic nitrogen structure. The cyclic nitrogen structure preferably has a nitrogen atom in the cyclic structure.
[0189] Examples of the cyclic nitrogen-containing monomer include N-vinyl cyclic amide (lactam-based vinyl monomer) and vinyl-based monomers having a nitrogen-containing heterocyclic ring.
[0190] Examples of the N-vinyl cyclic amide include N-vinyl cyclic amides represented by the following formula (1).
[0191]
[0192] (In formula (1), R 1 represents a divalent organic group. )
[0193] In the above formula (1), R 1 It is a divalent organic group, preferably a divalent saturated hydrocarbon group or an unsaturated hydrocarbon group, and more preferably a divalent saturated hydrocarbon group (for example, an alkylene group having 3 to 5 carbon atoms).
[0194] Examples of the N-vinyl cyclic amide represented by the formula (1) include N-vinyl-2-pyrrolidone, N-vinyl-2-piperidone, N-vinyl-3-morpholinone, N-vinyl-2-caprolactam, N-vinyl-1,3- Oxazine-2-one, N-vinyl-3,5-morpholinedione, etc.
[0195] Examples of the vinyl monomer having a nitrogen-containing heterocyclic ring include acrylic monomers having a nitrogen-containing heterocyclic ring such as a morpholine ring, a piperidine ring, a pyrrolidine ring, and a piperazine ring.
[0196] The vinyl monomer having a nitrogen-containing heterocyclic ring is not particularly limited, and examples thereof include (meth)acryloylmorpholine, N-vinylpiperazine, N-vinylpyrrole, N-vinylimidazole, N-vinylpyrazine, N-vinylmorpholine, N-vinylpyrazole, vinylpyridine, vinylpyrimidine, vinyl Azoles, vinyl isocyanates oxazole, vinylthiazole, vinylisothiazole, vinylpyridazine, (meth)acryloylpyrrolidone, (meth)acryloylpyrrolidine, (meth)acryloylpiperidine and the like.
[0197] As the vinyl monomer having a nitrogen-containing heterocyclic ring, an acrylic monomer having a nitrogen-containing heterocyclic ring is preferred, and (meth)acryloylmorpholine, (meth)acryloylpyrrolidine, and (meth)acryloylpiperidine are more preferred.
[0198] Examples of the (meth)acrylamides include (meth)acrylamide, N-alkyl (meth)acrylamide, N,N-dialkyl (meth)acrylamide, etc. Examples of the N-alkyl (meth)acrylamide include N-ethyl (meth)acrylamide, N-isopropyl (meth)acrylamide, N-n-butyl (meth)acrylamide, N-octyl (meth)acrylamide, etc. In addition, the N-alkyl (meth)acrylamide also includes (meth)acrylamide having an amino group, such as dimethylaminoethyl (meth)acrylamide, diethylaminoethyl (meth)acrylamide, and dimethylaminopropyl (meth)acrylamide. Examples of the N,N-dialkyl(meth)acrylamide include N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N,N-dipropyl(meth)acrylamide, N,N-diisopropyl(meth)acrylamide, N,N-di(n-butyl)(meth)acrylamide, and N,N-di(tert-butyl)(meth)acrylamide.
[0199] In addition, the (meth)acrylamides include, for example, various N-hydroxyalkyl (meth)acrylamides. Examples of the N-hydroxyalkyl (meth)acrylamides include N-methylol (meth)acrylamide, N-(2-hydroxyethyl) (meth)acrylamide, N-(2-hydroxypropyl) (meth)acrylamide, N-(1-hydroxypropyl) (meth)acrylamide, N-(3-hydroxypropyl) (meth)acrylamide, N-(2-hydroxybutyl) (meth)acrylamide, N-(3-hydroxybutyl) (meth)acrylamide, N-(4-hydroxybutyl) (meth)acrylamide, and N-methyl-N-2-hydroxyethyl (meth)acrylamide.
[0200] The (meth)acrylamides include, for example, various N-alkoxyalkyl (meth)acrylamides, such as N-methoxymethyl (meth)acrylamide and N-butoxymethyl (meth)acrylamide.
[0201] In addition, examples of nitrogen-containing monomers other than the above-mentioned cyclic nitrogen-containing monomers and the above-mentioned (meth)acrylamides include amino-containing monomers, cyano-containing monomers, imide-containing monomers, isocyanate-containing monomers, etc. Examples of the above-mentioned amino-containing monomers include aminoethyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, dimethylaminopropyl (meth)acrylate, tert-butylaminoethyl (meth)acrylate, etc. Examples of the cyano-containing monomers include acrylonitrile, methacrylonitrile, etc. Examples of the imide group-containing monomer include maleimide monomers (e.g., N-cyclohexylmaleimide, N-isopropylmaleimide, N-laurylmaleimide, N-phenylmaleimide, etc.), itaconimide monomers (e.g., N-methylitaconimide, N-ethylitaconimide, N-butylitaconimide, N-octylitaconimide, N-2-ethylhexylitaconimide, N-laurylitaconimide, N-cyclohexylitaconimide, etc.), succinimide monomers (e.g., N-(meth)acryloyloxymethylenesuccinimide, N-(meth)acryloyl-6-oxyhexamethylenesuccinimide, N-(meth)acryloyl-8-oxyoctamethylenesuccinimide, etc.), etc. Examples of the isocyanate group-containing monomer include 2-(meth)acryloyloxyethyl isocyanate, etc.
[0202] Among them, as the nitrogen atom-containing monomer, a cyclic nitrogen-containing monomer is preferred, and N-vinyl cyclic amide is more preferred. More specifically, N-vinyl-2-pyrrolidone (NVP) is particularly preferred.
[0203] In the case where the acrylic polymer contains the nitrogen-containing monomer as the monomer component constituting the polymer, the ratio of the nitrogen-containing monomer in all monomer components (100% by weight) constituting the acrylic polymer is not particularly limited, preferably more than 1% by weight, more preferably more than 3% by weight, and further preferably more than 5% by weight. When the above ratio is more than 1% by weight, the suppression and durability of the whitening under a high humidity environment can be further improved, and high adhesive reliability can be obtained, which is preferred. In addition, from the viewpoint of obtaining an adhesive layer with appropriate softness, the viewpoint of obtaining an adhesive layer with excellent transparency, and the viewpoint of easily controlling the various characteristics (especially the height difference absorbency) of the adhesive layer to a specified range, the upper limit of the ratio of the nitrogen-containing monomer is preferably less than 30% by weight, more preferably less than 25% by weight, and further preferably less than 20% by weight.
[0204] The monomer having a hydroxyl group in the above-mentioned molecule is a monomer having at least one hydroxyl group (hydroxyl group) in the molecule (in one molecule), preferably a monomer having a polymerizable functional group having an unsaturated double bond such as a (meth)acryloyl group or a vinyl group and having a hydroxyl group. Among them, the above-mentioned nitrogen atom-containing monomer is not included in the monomer having a hydroxyl group in the above-mentioned molecule. That is, in the present specification, a monomer having both a nitrogen atom and a hydroxyl group in the molecule is included in the above-mentioned "nitrogen atom-containing monomer". In the present specification, the above-mentioned "monomer having a hydroxyl group in the molecule" is sometimes referred to as a "hydroxyl-containing monomer". It should be noted that the hydroxyl-containing monomer can be used alone or in combination of two or more.
[0205] Examples of the hydroxyl-containing monomer include hydroxyl-containing (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, hydroxyoctyl (meth)acrylate, hydroxydecyl (meth)acrylate, hydroxylauryl (meth)acrylate, and (meth)acrylate (4-hydroxymethylcyclohexyl); vinyl alcohol; allyl alcohol, and the like.
[0206] Among them, as the hydroxyl group-containing monomer, hydroxyl group-containing (meth)acrylate is preferred, and 2-hydroxyethyl acrylate (HEA) and 4-hydroxybutyl acrylate (4HBA) are more preferred.
[0207] In the case where the acrylic polymer contains the hydroxy-containing monomer as a monomer component constituting the polymer, the proportion of the hydroxy-containing monomer in all monomer components (100% by weight) constituting the acrylic polymer is not particularly limited, and is preferably 0.5% by weight or more, more preferably 0.8% by weight or more, and further preferably 1% by weight or more from the viewpoint of suppressing turbidity under high humidity environment and improving durability, and obtaining high adhesive reliability. In addition, from the viewpoint of easily controlling the various characteristics (especially the height difference absorbency) of the adhesive layer within a specified range, the upper limit of the proportion of the hydroxy-containing monomer is preferably 30% by weight or less, more preferably 25% by weight or less, and further preferably 20% by weight or less.
[0208] In addition, in order to further enhance the above-mentioned effect brought by the hydroxyl-containing monomer, the acrylic adhesive composition may also contain a hydroxyl-containing monomer in addition to the above-mentioned acrylic polymer. In the case where the acrylic adhesive composition also contains a hydroxyl-containing monomer in addition to the acrylic polymer, the content (compounding amount) of the hydroxyl-containing monomer is preferably more than 1 part by weight, more preferably more than 3 parts by weight, and more preferably more than 5 parts by weight relative to 100 parts by weight of the acrylic polymer. When the above-mentioned content is more than 5 parts by weight, the suppression and durability of the white turbidity under a high humidity environment can be further improved, and higher adhesive reliability can be obtained, which is preferred. In addition, from the viewpoint of easily obtaining cohesive force, adhesiveness, adhesive reliability, and the viewpoint of easily controlling the above-mentioned various characteristics (especially the height difference absorbency) of the adhesive layer within a specified range, the upper limit of the content (compounding amount) of the above-mentioned hydroxyl-containing monomer is more preferably less than 30 parts by weight, more preferably less than 25 parts by weight, more preferably less than 20 parts by weight, and particularly preferably less than 17 parts by weight.
[0209] The total ratio of the nitrogen-atom-containing monomer and the hydroxyl-containing monomer in all monomer components (100% by weight) constituting the acrylic polymer is not particularly limited. From the viewpoint of suppressing turbidity under high humidity environment and improving durability, and obtaining high adhesive reliability, it is preferably 5% by weight or more, more preferably 10% by weight or more, and further preferably 15% by weight or more. In addition, from the viewpoint of obtaining an adhesive layer with appropriate flexibility, the viewpoint of obtaining an adhesive layer with excellent transparency, and the viewpoint of easily controlling the various characteristics (especially the height difference absorbency) of the adhesive layer within a specified range, the upper limit of the total ratio is preferably 50% by weight or less, more preferably 40% by weight or less, and further preferably 35% by weight or less.
[0210] As copolymerizable monomers other than nitrogen-containing monomers and hydroxyl-containing monomers, carboxyl-containing monomers can also be cited. As long as the above-mentioned carboxyl-containing monomers are monomers having polymerizable functional groups with unsaturated double bonds such as (meth)acryloyl or vinyl and having carboxyl groups, there is no particular limitation. As carboxyl-containing monomers, for example, (meth)acrylic acid, itaconic acid, maleic acid, fumaric acid, crotonic acid, isocrotonic acid, etc. can be cited. In addition, for example, acid anhydride-containing monomers such as maleic anhydride and itaconic anhydride are also included. It should be noted that the carboxyl-containing monomers can be used alone or in combination of two or more.
[0211] In the case where the acrylic polymer contains the above-mentioned carboxyl-containing monomer as the monomer component constituting the polymer, the ratio of the above-mentioned carboxyl-containing monomer in the whole monomer components (100 wt %) constituting the above-mentioned acrylic polymer is not particularly limited, and from the viewpoint of obtaining high adhesive reliability, it is preferably more than 0.5 wt %, more preferably more than 0.8 wt %, and further preferably more than 1 wt %. In addition, from the viewpoint of easily controlling the above-mentioned various characteristics (particularly the height difference absorbency) of the adhesive layer to the prescribed scope, the upper limit of the ratio of the above-mentioned carboxyl-containing monomer is preferably less than 30 wt %, more preferably less than 25 wt %, and further preferably less than 20 wt %.
[0212] As copolymerizable monomers other than nitrogen-containing monomers and hydroxyl-containing monomers, alicyclic structure-containing monomers can also be cited. The above-mentioned alicyclic structure-containing monomers are not particularly limited as long as they are monomers having a polymerizable functional group having an unsaturated double bond such as a (meth)acryloyl group or a vinyl group and having an alicyclic structure. For example, (meth)acrylic acid alkyl esters having a cycloalkyl group are included in the above-mentioned alicyclic structure-containing monomers. It should be noted that the alicyclic structure-containing monomers can be used alone or in combination of two or more.
[0213] The alicyclic structure in the alicyclic structure-containing monomer is a cyclic hydrocarbon structure, and preferably has 5 or more carbon atoms, more preferably 6 to 24 carbon atoms, further preferably 6 to 15 carbon atoms, and particularly preferably 6 to 10 carbon atoms.
[0214] Examples of the above-mentioned alicyclic structure-containing monomers include (meth)acrylic acid-based monomers such as cyclopropyl (meth)acrylate, cyclobutyl (meth)acrylate, cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, cycloheptyl (meth)acrylate, cyclooctyl (meth)acrylate, isobornyl (meth)acrylate, tetrahydrodicyclopentadienyl (meth)acrylate, HPMPA represented by the following formula (2), TMA-2 represented by the following formula (3), and HCPA represented by the following formula (4). It should be noted that in the following formula (4), there is no particular limitation on the bonding position of the cyclohexyl ring connected by a line to the structural formula in the brackets. Among them, cyclohexyl (meth)acrylate and isobornyl (meth)acrylate are preferred.
[0215]
[0216]
[0217]
[0218] In the case where the acrylic polymer contains the alicyclic structure-containing monomer as a monomer component constituting the polymer, the proportion of the alicyclic structure-containing monomer in all monomer components (100% by weight) constituting the acrylic polymer is not particularly limited, but is preferably 10% by weight or more from the viewpoint of improving durability and obtaining high adhesive reliability. In addition, from the viewpoint of obtaining an adhesive layer with moderate flexibility and facilitating the control of the various properties (especially the height difference absorption) of the adhesive layer within a specified range, the upper limit of the proportion of the alicyclic structure-containing monomer is preferably 50% by weight or less, more preferably 40% by weight or less, and further preferably 30% by weight or less.
[0219] In addition, as copolymerizable monomers, for example, multifunctional monomers can be cited. As the above-mentioned multifunctional monomers, for example, hexanediol di(meth)acrylate, butanediol di(meth)acrylate, (poly)ethylene glycol di(meth)acrylate, (poly)propylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, trimethylolpropane tri(meth)acrylate, tetramethylolmethane tri(meth)acrylate, allyl (meth)acrylate, vinyl (meth)acrylate, divinylbenzene, epoxy acrylate, polyester acrylate, urethane acrylate, etc. It should be noted that the multifunctional monomers can be used alone or in combination of two or more.
[0220] In the case where the acrylic polymer contains the multifunctional monomer as a monomer component constituting the polymer, the proportion of the multifunctional monomer in all the monomer components (100 wt %) constituting the acrylic polymer is not particularly limited, but is preferably 0.5 wt % or less (for example, greater than 0 wt % and less than or equal to 0.5 wt %), and more preferably 0.2 wt % or less (for example, greater than 0 wt % and less than or equal to 0.2 wt %), from the viewpoint of easily controlling the various properties (especially the height difference absorbency) of the adhesive layer within a specified range.
[0221] In addition, the above-mentioned multifunctional monomer can be formulated in addition to the above-mentioned acrylic polymer and can also be formulated in an acrylic adhesive composition. In the case where the acrylic adhesive composition contains the multifunctional monomer in addition to the acrylic polymer, from the viewpoint of easily controlling the above-mentioned various properties of the adhesive layer (especially the height difference absorption) within the specified range, the content (compounding amount) of the multifunctional monomer is preferably 0.5 parts by weight or less (for example, greater than 0 parts by weight and less than or equal to 0.5 parts by weight) relative to 100 parts by weight of the acrylic polymer, and more preferably 0.2 parts by weight or less (for example, greater than 0 parts by weight and less than or equal to 0.2 parts by weight).
[0222] In addition, as the copolymerizable monomer, alkoxyalkyl (meth)acrylate can be cited. As the alkoxyalkyl (meth)acrylate, there is no particular limitation, and examples thereof include 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, methoxytriethylene glycol (meth)acrylate, 3-methoxypropyl (meth)acrylate, 3-ethoxypropyl (meth)acrylate, 4-methoxybutyl (meth)acrylate, 4-ethoxybutyl (meth)acrylate, etc. Among them, the alkoxyalkyl (meth)acrylate is preferably an alkoxyalkyl acrylate, and more preferably 2-methoxyethyl acrylate (MEA). It should be noted that the alkoxyalkyl (meth)acrylate can be used alone or in combination of two or more.
[0223] In the case where the acrylic polymer contains the alkoxyalkyl (meth)acrylate as a monomer component constituting the polymer, the ratio of the alkyl (meth)acrylate to the alkoxyalkyl (meth)acrylate is not particularly limited, but is preferably 100: greater than 0 to 25:75 or less, and more preferably 100: greater than 0 to 50:50 or less in terms of [former:latter] (weight ratio).
[0224] In addition, examples of the copolymerizable monomers include epoxy-containing monomers, sulfonic acid-containing monomers, phosphoric acid-containing monomers, (meth)acrylates having aromatic hydrocarbon groups, vinyl esters, aromatic vinyl compounds, olefins or dienes, vinyl ethers, and vinyl chloride. Examples of the epoxy-containing monomers include glycidyl (meth)acrylate and methyl glycidyl (meth)acrylate. Examples of the sulfonic acid-containing monomers include sodium vinyl sulfonate. Examples of the phosphoric acid-containing monomers include 2-hydroxyethyl acryloyl phosphate. Examples of the (meth)acrylates having aromatic hydrocarbon groups include phenyl (meth)acrylate, phenoxyethyl (meth)acrylate, and benzyl (meth)acrylate. Examples of the vinyl esters include vinyl acetate and vinyl propionate. Examples of the aromatic vinyl compounds include styrene and vinyl toluene. Examples of the olefins or dienes include ethylene, propylene, butadiene, isoprene, and isobutylene. Examples of the vinyl ether include vinyl alkyl ether and the like.
[0225] The content of the base polymer (especially acrylic polymer) in the adhesive layer of the present invention is not particularly limited, and is preferably 50 wt % or more (e.g., 50 wt % to 100 wt %), more preferably 80 wt % or more (e.g., 80 wt % to 100 wt %), and further preferably 90 wt % or more (e.g., 90 wt % to 100 wt %), relative to the total weight of 100 wt % of the adhesive layer of the present invention.
[0226] The weight average molecular weight (Mw) of the acrylic polymer is 100,000 to 5,000,000, preferably 500,000 to 4,000,000, and more preferably 750,000 to 3,000,000. A configuration in which the weight average molecular weight of the acrylic polymer is 100,000 or more is preferred from the perspective of improved adhesive force and improved foaming and peeling resistance. On the other hand, a configuration in which the weight average molecular weight of the acrylic polymer is 5,000,000 or less is preferred from the perspective of easy improvement of adhesive force and improved foaming and peeling resistance.
[0227] The weight average molecular weight (Mw) of the acrylic polymer can be determined in terms of polystyrene by GPC, for example, using a high-speed GPC device "HPLC-8120 GPC" manufactured by Tosoh Corporation, under the following conditions.
[0228] Column: TSKgel Super HZM-H / HZ4000 / HZ3000 / HZ2000
[0229] Solvent: Tetrahydrofuran
[0230] Flow rate: 0.6mL / min
[0231] The glass transition temperature (Tg) of the acrylic polymer is not particularly limited, but is preferably -70°C to -10°C, more preferably -65°C to -15°C, and further preferably -60°C to -20°C. When the glass transition temperature of the acrylic polymer is -70°C or higher, the cohesive force is improved and the foaming and peeling resistance is easily improved, so it is preferred. In addition, a configuration in which the glass transition temperature of the acrylic polymer is -10°C or lower is preferred from the following aspects: the stress relaxation of the adhesive layer is maintained even in a low temperature environment, the adhesive layer fully follows the contraction or expansion in the use environment of the image display device of the present invention, and can suppress swelling and peeling, and can fully ensure adhesion to the adherend.
[0232] The glass transition temperature (Tg) of the acrylic polymer is a glass transition temperature (theoretical value) represented by the following FOX equation.
[0233] 1 / Tg=W1 / Tg1+W2 / Tg2+···+W n / Tg n
[0234] In the above formula, Tg represents the glass transition temperature of the acrylic polymer (unit: K), Tg i represents the glass transition temperature (unit: K) when monomer i forms a homopolymer, W i It represents the weight fraction of monomer i in the total amount of monomer components (i=1, 2, ... n).
[0235] As Tg of the homopolymer of the monomer constituting the acrylic polymer, the following values can be adopted.
[0236] 2-Ethylhexyl acrylate -70℃
[0237] n-Hexyl acrylate-65℃
[0238] n-Octyl acrylate-65℃
[0239] Isononyl acrylate-60℃
[0240] Nonyl acrylate-58℃
[0241] n-Butyl acrylate-55℃
[0242] Ethyl acrylate -20℃
[0243] Lauryl acrylate 0℃
[0244] 2-Ethylhexyl Methacrylate -10℃
[0245] Methyl acrylate 8℃
[0246] Butyl Methacrylate 20℃
[0247] Methyl methacrylate 105℃
[0248] Acrylic acid 106℃
[0249] Methacrylic acid 228℃
[0250] Vinyl acetate 32℃
[0251] Styrene 100℃
[0252] In addition, as the Tg of the homopolymer of the monomer not described above, the value described in "Polymer Handbook" (3rd edition, John Wiley & Sons, Inc, 1989) can be used. In addition, as the Tg of the homopolymer of the monomer not described in the above literature, the value obtained by the above-mentioned measurement method (the peak temperature of tan δ in the viscoelasticity test) can be used.
[0253] The base polymer such as the acrylic polymer contained in the adhesive layer of the present invention is obtained by polymerizing monomer components. There are no particular restrictions on the polymerization method, and examples thereof include: solution polymerization method, emulsion polymerization method, bulk polymerization method, polymerization method using active energy ray irradiation (active energy ray polymerization method), etc. Among them, from the perspective of transparency and cost of the adhesive layer, solution polymerization method and active energy ray polymerization method are preferred, and active energy ray polymerization method is more preferred.
[0254] In addition, various common solvents can be used in the polymerization of the above-mentioned monomer components. Examples of the above-mentioned solvents include esters such as ethyl acetate and n-butyl acetate; aromatic hydrocarbons such as toluene and benzene; aliphatic hydrocarbons such as n-hexane and n-heptane; alicyclic hydrocarbons such as cyclohexane and methylcyclohexane; ketones such as methyl ethyl ketone and methyl isobutyl ketone, and other organic solvents. It should be noted that the solvents can be used alone or in combination of two or more.
[0255] In the polymerization of the above-mentioned monomer components, a polymerization initiator such as a thermal polymerization initiator or a photopolymerization initiator (photoinitiator) may be used depending on the type of the polymerization reaction. The polymerization initiator may be used alone or in combination of two or more.
[0256] As the above-mentioned thermal polymerization initiator, there is no particular limitation, and examples thereof include azo polymerization initiators, peroxide polymerization initiators (e.g., dibenzoyl peroxide, tert-butyl permaleate, etc.), redox polymerization initiators, etc. Among them, the azo polymerization initiators disclosed in Japanese Patent Publication No. 2002-69411 are preferred. As the above-mentioned azo polymerization initiators, examples thereof include: 2,2'-azobisisobutyronitrile (hereinafter sometimes referred to as "AIBN"), 2,2'-azobis(-2-methylbutyronitrile) (hereinafter sometimes referred to as "AMBN"), 2,2'-azobis(2-methylpropionic acid) dimethyl ester, 4,4'-azobis(4-cyanovaleric acid), etc. It should be noted that the thermal polymerization initiator can be used alone or in combination of two or more.
[0257] When the azo polymerization initiator is used in the polymerization of the acrylic polymer, the amount of the azo polymerization initiator used is not particularly limited, and for example, it is preferably 0.05 parts by weight or more, more preferably 0.1 parts by weight or more, and is preferably 0.5 parts by weight or less, more preferably 0.3 parts by weight or less, relative to 100 parts by weight of all monomer components constituting the acrylic polymer.
[0258] As the above-mentioned photopolymerization initiator, there is no particular limitation, and examples thereof include benzoin ether photopolymerization initiators, acetophenone photopolymerization initiators, α-ketol photopolymerization initiators, aromatic sulfonyl chloride photopolymerization initiators, photoactive oxime photopolymerization initiators, benzoin photopolymerization initiators, benzyl photopolymerization initiators, benzophenone photopolymerization initiators, ketal photopolymerization initiators, thioxanthone photopolymerization initiators, etc. In addition, acylphosphine oxide photopolymerization initiators and titanocene photopolymerization initiators can be listed. As the above-mentioned benzoin ether photopolymerization initiators, for example, benzoin methyl ether, benzoin ethyl ether, benzoin propyl ether, benzoin isopropyl ether, benzoin isobutyl ether, 2,2-dimethoxy-1,2-diphenylethane-one, anisole methyl ether, etc. can be listed. Examples of the acetophenone-based photopolymerization initiator include 2,2-diethoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 1-hydroxycyclohexylphenyl ketone, 4-phenoxydichloroacetophenone, and 4-(tert-butyl)dichloroacetophenone. Examples of the α-ketoalcohol-based photopolymerization initiator include 2-methyl-2-hydroxypropiophenone and 1-[4-(2-hydroxyethyl)phenyl]-2-methylpropane-1-one. Examples of the aromatic sulfonyl chloride-based photopolymerization initiator include 2-naphthalenesulfonyl chloride and the like. Examples of the photoactive oxime-based photopolymerization initiator include 1-phenyl-1,2-propanedione-2-(O-ethoxycarbonyl)-oxime. Examples of the benzoin-based photopolymerization initiator include benzoin and the like. Examples of the benzyl-based photopolymerization initiator include benzyl. As the above-mentioned benzophenone-based photopolymerization initiator, for example, benzophenone, benzoylbenzoic acid, 3,3'-dimethyl-4-methoxybenzophenone, poly(vinylbenzophenone) and α-hydroxycyclohexylphenyl ketone can be listed. As the above-mentioned ketal-based photopolymerization initiator, for example, benzildimethylketal can be listed. As the above-mentioned thioxanthone-based photopolymerization initiator, for example, thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, 2,4-dimethylthioxanthone, isopropylthioxanthone, 2,4-diisopropylthioxanthone and dodecylthioxanthone can be listed. As the above-mentioned acylphosphine oxide-based photopolymerization initiator, for example, 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, etc. As the above-mentioned titanocene-based photopolymerization initiator, for example, bis(η 5 -2,4-cyclopentadien-1-yl)-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)-phenyl)titanium, etc. In addition, the photopolymerization initiator can be used alone or in combination of two or more.
[0259] When the photopolymerization initiator is used in the polymerization of the acrylic polymer, the amount of the photopolymerization initiator used is not particularly limited. For example, it is preferably 0.01 parts by weight or more, more preferably 0.1 parts by weight or more, relative to 100 parts by weight of all monomer components constituting the acrylic polymer. It is also preferably 3 parts by weight or less, more preferably 1.5 parts by weight or less.
[0260] The adhesive layer of the present invention contains a liquid antistatic agent. The above antistatic agent is suitable from the following aspects: it imparts antistatic properties to the adhesive layer of the present invention, and in the case of poor lamination to the image display panel, it suppresses the generation of static electricity when the adhesive sheet is peeled off from the image display panel for rework. In addition, the above antistatic agent is suitable in the form of a liquid from the following aspects: it can impart an excellent antistatic effect to the adhesive layer of the present invention without damaging the adhesive properties of the adhesive layer of the present invention, so that the adhesion between the adhesive layer of the present invention and the substrate of the present invention is improved, and excellent heat shock resistance is obtained.
[0261] As the above-mentioned liquid antistatic agent, there is no particular limitation as long as it is a liquid antistatic agent at room temperature (e.g., 25° C.), and examples thereof include: ionic liquids, alkali metal salts, silicones containing ionic groups, etc. From the perspective of being able to impart an excellent antistatic effect to the adhesive layer of the present invention without damaging the adhesive properties of the adhesive layer of the present invention, thereby improving the adhesion between the adhesive layer of the present invention and the substrate of the present invention, and obtaining excellent heat shock resistance, ionic liquids are preferred. It should be noted that the liquid antistatic agent can be used alone or in combination of two or more.
[0262] The ionic liquid is a molten salt (ionic compound) that is liquid at room temperature (25° C.) It is believed that the ionic liquid is easy to add, disperse or dissolve in the adhesive layer of the present invention, facilitates molecular movement, does not impair adhesive properties, and can obtain excellent antistatic ability.
[0263] As the ionic liquid, an ionic liquid containing an anionic component and an organic cationic component represented by the following formulae (A) to (E) is preferably used. An ionic liquid containing these cationic components can provide a pressure-sensitive adhesive layer having a more excellent antistatic property.
[0264]
[0265] In the above formula (A), R a represents a divalent hydrocarbon group having 4 to 20 carbon atoms, a part of which may be a functional group substituted with a heteroatom (e.g., an oxygen atom, a nitrogen atom, a sulfur atom, etc.; the same applies hereinafter), R b and R cmay be the same or different and represent hydrogen or a hydrocarbon group having 1 to 16 carbon atoms, and a portion of the hydrocarbon group may be a functional group substituted with a heteroatom. However, when the nitrogen atom (N) contains a double bond, R is absent. c .
[0266] In the above formula (B), R d represents a divalent hydrocarbon group having 2 to 20 carbon atoms, a part of which may be a functional group substituted with a heteroatom, R e , R f and R g They may be the same or different and represent hydrogen or a hydrocarbon group having 1 to 16 carbon atoms, and a part of the hydrocarbon group may be a functional group substituted with a heteroatom.
[0267] In the above formula (C), R h represents a divalent hydrocarbon group having 2 to 20 carbon atoms, a part of which may be a functional group substituted with a heteroatom, R i , R j and R k They may be the same or different and represent hydrogen or a hydrocarbon group having 1 to 16 carbon atoms, and a part of the hydrocarbon group may be a functional group substituted with a heteroatom.
[0268] In the above formula (D), Z represents a nitrogen, sulfur or phosphorus atom, and R l , R m , R n and R o may be the same or different and represent a hydrocarbon group having 1 to 20 carbon atoms, a part of which may be a functional group substituted by a heteroatom. In the case where Z is a sulfur atom, R o .
[0269] In the above formula (E), R P It represents a hydrocarbon group having 1 to 18 carbon atoms, and a part of the hydrocarbon group may be a functional group substituted with a heteroatom.
[0270] Examples of the cation represented by formula (A) include pyridine Cation, piperidine Cation, pyrrolidine Cation, cation having a pyrroline skeleton, cation having a pyrrole skeleton, morpholine Cations, etc.
[0271] Specific examples of the cation represented by formula (A) include: 1-ethylpyridine Cation, 1-butylpyridine Cation, 1-hexylpyridine Cation, 1-butyl-3-methylpyridine Cation, 1-butyl-4-methylpyridine Cation, 1-hexylpyridinium-3-methylpyridine Cation, 1-butyl-3,4-dimethylpyridine Cation, 1,1-dimethylpyrrolidine Cation, 1-ethyl-1-methylpyrrolidine Cation, 1-methyl-propylpyrrolidine Cation, 1-methyl-butylpyrrolidine Cation, 1-methyl-pentylpyrrolidine Cation, 1-methyl-1-hexylpyrrolidine Cation, 1-methyl-heptylpyrrolidine Cation, 1-ethyl-1-propylpyrrolidine Cation, 1-ethyl-1-butylpyrrolidine Cation, 1-ethyl-1-pentylpyrrolidine Cation, 1-ethyl-1-hexylpyrrolidine Cation, 1-ethyl-1-heptylpyrrolidine Cation, 1,1-dipropylpyrrolidine Cationic, 1-propyl-butylpyrrolidine Cation, 1,1-dibutylpyrrolidine Cation, pyrrolidine -2-Keto cation, 1-propylpiperidin Cation, 1-pentylpiperidinium Cation, 1,1-dimethylpiperidinium Cation, 1-methyl-1-ethylpiperidin Cation, 1-methyl-1-propylpiperidinium Cation, 1-methyl-butylpiperidinium Cation, 1-methyl-1-pentylpiperidinium Cation, 1-methyl-1-hexylpiperidinium Cation, 1-methyl-1-heptylpiperidinium Cation, 1-ethyl-1-propylpiperidinium Cation, 1-ethyl-1-butylpiperidinium Cation, 1-ethyl-1-pentylpiperidinium Cation, 1-ethyl-1-hexylpiperidinium Cation, 1-ethyl-1-heptylpiperidinium Cation, 1,1-dipropylpiperidinium Cation, 1-propyl-butylpiperidinium Cation, 1,1-dibutylpiperidinium cation, 2-methyl-1-pyrrolinium cation, 1-ethyl-2-phenylindole cation, 1,2-dimethylindole cation, 1-ethylcarbazole cation, N-ethyl-N-methylmorpholine Cations, etc.
[0272] Examples of the cation represented by formula (B) include imidazole Cation, Tetrahydropyrimidine Cations and dihydropyrimidines Cations, etc.
[0273] Specific examples of the cation represented by formula (B) include: 1,3-dimethylimidazole Cation, 1,3-diethylimidazole Cation, 1-ethyl-3-methylimidazole Cation, 1-butyl-3-methylimidazole Cation, 1-hexyl-3-methylimidazole Cation, 1-octyl-3-methylimidazole Cation, 1-decyl-3-methylimidazole Cation, 1-dodecyl-3-methylimidazole Cation, 1-tetradecyl-3-methylimidazole Cation, 1,2-dimethyl-3-propylimidazole Cation, 1-ethyl-2,3-dimethylimidazole Cation, 1-butyl-2,3-dimethylimidazole Cation, 1-hexyl-2,3-dimethylimidazole Cation, 1-(2-methoxyethyl)-3-methylimidazole Cation, 1,3-dimethyl-1,4,5,6-tetrahydropyrimidine Cation, 1,2,3-trimethyl-1,4,5,6-tetrahydropyrimidine Cation, 1,2,3,4-tetramethyl-1,4,5,6-tetrahydropyrimidine Cation, 1,2,3,5-tetramethyl-1,4,5,6-tetrahydropyrimidine Cation, 1,3-dimethyl-1,4-dihydropyrimidine Cation, 1,3-dimethyl-1,6-dihydropyrimidine Cation, 1,2,3-trimethyl-1,4-dihydropyrimidine Cation, 1,2,3-trimethyl-1,6-dihydropyrimidine Cation, 1,2,3,4-tetramethyl-1,4-dihydropyrimidine Cation, 1,2.3,4-tetramethyl-1,6-dihydropyrimidine Cations, etc.
[0274] Examples of the cation represented by the formula (C) include pyrazoles. Cationic, pyrazoline Cations, etc.
[0275] Specific examples of the cation represented by formula (C) include: 1-methylpyrazole Cation, 3-methylpyrazole Cation, 1-ethyl-2-methylpyrazoline Cation, 1-ethyl-2,3,5-trimethylpyrazole Cation, 1-propyl-2,3,5-trimethylpyrazole Cation, 1-butyl-2,3,5-trimethylpyrazole Cation, 1-ethyl-2,3,5-trimethylpyrazoline Cationic, 1-propyl-2,3,5-trimethylpyrazoline Cationic, 1-butyl-2,3,5-trimethylpyrazoline Cations, etc.
[0276] Examples of the cation represented by the formula (D) include tetraalkylammonium cations, trialkylsulfonium cations, tetraalkyl A cation, a cation in which a part of the alkyl group is substituted with an alkenyl group or an alkoxy group, and further with an epoxy group, and the like.
[0277] Specific examples of the cation represented by the formula (D) include tetramethylammonium cation, tetraethylammonium cation, tetrabutylammonium cation, tetrapentylammonium cation, tetrahexylammonium cation, tetraheptylammonium cation, triethylmethylammonium cation, tributylethylammonium cation, trimethyldecylammonium cation, N,N-diethyl-N-methyl-N-(2-methoxyethyl)ammonium cation, glycidyltrimethylammonium cation, trimethylsulfonium cation, triethylsulfonium cation, tributylsulfonium cation, trihexylammonium cation, diethylmethylsulfonium cation, dibutylethylsulfonium cation, dimethyldecylammonium cation, tetramethyl Cationic, tetraethyl Cationic, Tetrabutyl Cation, Tetrahexyl Cationic, Tetraoctyl Cation, triethylmethyl Cation, tributyl ethyl Cationic, trimethyldecyl Cation, diallyldimethylammonium cation, tributyl-(2-methoxyethyl) Among them, triethylmethylammonium cation, tributylethylammonium cation, trimethyldecylammonium cation, diethylmethylsulfonium cation, dibutylethylsulfonium cation, dimethyldecylsulfonium cation, triethylmethyl Cation, tributyl ethyl Cationic, trimethyldecyl Cations such as asymmetric tetraalkylammonium cations, trialkylsulfonium cations, tetraalkyl cation, N, N-diethyl-N-methyl-N-(2-methoxyethyl)ammonium cation, glycidyltrimethylammonium cation, diallyldimethylammonium cation, N,N-dimethyl-N-ethyl-N-propylammonium cation, N,N-dimethyl-N-ethyl-N-butylammonium cation, N,N-dimethyl-N-ethyl-N-pentylammonium cation, N,N-dimethyl-N-ethyl-N-hexylammonium cation, N,N-dimethyl-N-ethyl-N-heptylammonium cation, N,N-dimethyl-N-ethyl-N-nonylammonium cation, N,N-dimethyl-N,N-dipropylammonium cation, N,N-diethyl-N-propyl-N-butylammonium cation, N,N-dimethyl-N-propyl-N-pentylammonium cation, N,N-dimethyl-N-propyl-N-hexylammonium cation, N,N-dimethyl N,N-dipropyl-N-methyl-N-pentylammonium cation, N,N-diethyl-N-methyl-N-pentylammonium cation, N,N-diethyl-N-propyl-N-pentylammonium cation, triethylpropylammonium cation, triethylpentylammonium cation, triethylheptylammonium cation, N,N-dipropyl-N-methyl-N-ethylammonium cation, N,N-dipropyl-N-methyl-N-pentylammonium cation, N,N-dipropyl-N-butyl-N-hexylammonium cation, N,N-dipropyl-N,N-dihexylammonium cation, N,N-dibutyl-N-methyl-N-pentylammonium cation, N,N-dibutyl-N-methyl-N-hexylammonium cation, trioctylmethylammonium cation, N-methyl-N-ethyl-N-propyl-N-pentylammonium cation.
[0278] Examples of the cation represented by formula (E) include sulfonium cations. P Specific examples of include methyl, ethyl, propyl, butyl, hexyl, octyl, nonyl, decyl, dodecyl, tridecyl, tetradecyl, and octadecyl.
[0279] On the other hand, the anion component is not particularly limited as long as it satisfies the requirement of forming an ionic liquid. For example, the following can be used: Cl - Br - ,I - 、AlCl4- 、Al2Cl7 - 、BF4 - PF6 - 、ClO4 - 、NO3 - 、CH3COO - CF3COO - 、CH3SO3 - CF3SO3 - 、C4F9SO3 - 、(CF3SO2)2N - 、(C2F5SO2)2N - 、(C3F7SO2)2N - 、(C4F9SO2)2N - 、(CF3SO2)3C - 、AsF6 - 、SbF6 - 、NbF6 - 、TaF6 - 、F(HF) n - 、(CN)2N - 、C4F9SO3 - 、(C2F5SO2)2N - 、C3F7COO - 、(CF3SO2)(CF3CO)N - 、C9H 19 COO - 、(CH3)2PO4 - 、(C2H5)2PO4 - 、C2H5OSO3 - 、C6H 13 OSO3 - 、C8H 17 OSO3 - 、CH3(OC2H4)2OSO3 - 、C6H4(CH3)SO3 - 、(C2F5)3PF3 - 、CH3CH(OH)COO - , and (FSO2)2N - wait.
[0280] In addition, as the anion component, an anion represented by the following formula (F) or the like can also be used.
[0281]
[0282] Among them, it is particularly preferable to use an anion component containing a fluorine atom as the anion component because an ionic liquid having a low melting point can be obtained.
[0283] The ionic liquid preferably contains an anionic component having 10 or less fluorine atoms. The structure in which the ionic liquid contains an anionic component having 10 or less fluorine atoms is preferred from the following aspects: improving the compatibility of the ionic liquid with the adhesive layer of the present invention, suppressing the increase in haze caused by the separation of the ionic liquid from the adhesive layer, and improving the visual recognition of the image display device. From the viewpoint of improving the compatibility of the ionic liquid with the adhesive layer of the present invention and suppressing the increase in haze of the adhesive layer, the number of fluorine atoms contained in the anionic component of the ionic liquid is more preferably 8 or less, and further preferably 6 or less. From the viewpoint of obtaining an ionic liquid with a low melting point, the lower limit of the number of fluorine atoms contained in the anionic component of the ionic liquid is preferably 4 or more.
[0284] Specific examples of the ionic liquid used in the present invention can be appropriately selected from the combination of the above-mentioned cationic components and anionic components, for example: 1-butylpyridine Tetrafluoroborate, 1-butylpyridine Hexafluorophosphate, 1-butyl-3-methylpyridine Tetrafluoroborate, 1-butyl-3-methylpyridine Trifluoromethanesulfonate, 1-butyl-3-methylpyridine Bis(trifluoromethanesulfonyl)imide, 1-butyl-3-methylpyridine Bis(pentafluoroethanesulfonyl)imide, 1-hexylpyridine Tetrafluoroborate, 1,1-dimethylpyrrolidine Bis(trifluoromethylsulfonyl)imide, 1-methyl-1-ethylpyrrolidine Bis(trifluoromethylsulfonyl)imide, 1-methyl-1-propylpyrrolidine Bis(trifluoromethylsulfonyl)imide, 1-methyl-butylpyrrolidine Bis(trifluoromethylsulfonyl)imide, 1-methyl-1-pentylpyrrolidine Bis(trifluoromethylsulfonyl)imide, 1-methyl-1-hexylpyrrolidine Bis(trifluoromethylsulfonyl)imide, 1-methyl-1-heptylpyrrolidine Bis(trifluoromethylsulfonyl)imide, 1-ethyl-1-propylpyrrolidine Bis(trifluoromethylsulfonyl)imide, 1-ethyl-1-butylpyrrolidine Bis(trifluoromethylsulfonyl)imide, 1-ethyl-1-pentylpyrrolidine Bis(trifluoromethylsulfonyl)imide, 1-ethyl-1-hexylpyrrolidine Bis(trifluoromethylsulfonyl)imide, 1-ethyl-1-heptylpyrrolidine Bis(trifluoromethylsulfonyl)imide, 1,1-dipropylpyrrolidine Bis(trifluoromethylsulfonyl)imide, 1-propyl-1-butylpyrrolidine Bis(trifluoromethylsulfonyl)imide, 1,1-dibutylpyrrolidine Bis(trifluoromethylsulfonyl)imide, 1-propylpiperidine Bis(trifluoromethylsulfonyl)imide, 1-pentylpyridine Bis(trifluoromethylsulfonyl)imide, 1,1-dimethylpiperidine Bis(trifluoromethylsulfonyl)imide, 1-methyl-1-ethylpiperidine Bis(trifluoromethylsulfonyl)imide, 1-methyl-1-propylpiperidine Bis(trifluoromethylsulfonyl)imide, 1-methyl-1-butylpiperidine Bis(trifluoromethylsulfonyl)imide, 1-methyl-1-pentylpiperidine Bis(trifluoromethylsulfonyl)imide, 1-methyl-1-hexylpiperidine Bis(trifluoromethylsulfonyl)imide, 1-methyl-1-heptylpiperidine Bis(trifluoromethylsulfonyl)imide, 1-ethyl-1-propylpiperidine Bis(trifluoromethylsulfonyl)imide, 1-ethyl-1-butylpiperidine Bis(trifluoromethylsulfonyl)imide, 1-ethyl-1-pentylpiperidine Bis(trifluoromethylsulfonyl)imide, 1-ethyl-1-hexylpiperidine Bis(trifluoromethylsulfonyl)imide, 1-ethyl-1-heptylpiperidine Bis(trifluoromethylsulfonyl)imide, 1,1-dipropylpiperidine Bis(trifluoromethylsulfonyl)imide, 1-propyl-butylpiperidine Tris(trifluoromethylsulfonyl)imide, 1,1-dibutylpiperidine Bis(trifluoromethylsulfonyl)imide, 1,1-dimethylpyrrolidine Bis(pentafluoroethylsulfonyl)imide, 1-methyl-1-ethylpyrrolidine Bis(pentafluoroethylsulfonyl)imide, 1-methyl-1-propylpyrrolidine Bis(pentafluoroethylsulfonyl)imide, 1-methyl-butylpyrrolidine Bis(pentafluoroethylsulfonyl)imide, 1-methyl-1-pentylpyrrolidine Bis(pentafluoroethylsulfonyl)imide, 1-methyl-1-hexylpyrrolidine Bis(pentafluoroethylsulfonyl)imide, 1-methyl-1-heptylpyrrolidine Bis(pentafluoroethylsulfonyl)imide, 1-ethyl-1-propylpyrrolidine Bis(pentafluoroethylsulfonyl)imide, 1-ethyl-1-butylpyrrolidine Bis(pentafluoroethylsulfonyl)imide, 1-ethyl-1-pentylpyrrolidine Bis(pentafluoroethylsulfonyl)imide, 1-ethyl-1-hexylpyrrolidine Bis(pentafluoroethylsulfonyl)imide; 1-ethyl-1-heptylpyrrolidine Bis(pentafluoroethylsulfonyl)imide, 1,1-dipropylpyrrolidine Bis(pentafluoroethylsulfonyl)imide, 1-propyl-1-butylpyrrolidine Bis(pentafluoroethylsulfonyl)imide, 1,1-dibutylpyrrolidine Bis(pentafluoroethylsulfonyl)imide, 1-propylpiperidine Bis(pentafluoroethylsulfonyl)imide, 1-pentylpiperidine Bis(pentafluoroethylsulfonyl)imide, 1,1-dimethylpiperidine Bis(pentafluoroethylsulfonyl)imide, 1-methyl-1-ethylpiperidine Bis(pentafluoroethylsulfonyl)imide, 1-methyl-1-propylpiperidine Bis(pentafluoroethylsulfonyl)imide, 1-methyl-1-butylpiperidine Bis(pentafluoroethylsulfonyl)imide, 1-methyl-1-pentylpiperidine Bis(pentafluoroethylsulfonyl)imide, 1-methyl-1-hexylpiperidine Bis(pentafluoroethylsulfonyl)imide, 1-methyl-1-heptylpiperidine Bis(pentafluoroethylsulfonyl)imide, 1-ethyl-1-propylpiperidine Bis(pentafluoroethylsulfonyl)imide, 1-ethyl-1-butylpiperidine Bis(pentafluoroethylsulfonyl)imide, 1-ethyl-1-pentylpiperidine Bis(pentafluoroethylsulfonyl)imide, 1-ethyl-1-hexylpiperidine Bis(pentafluoroethylsulfonyl)imide, 1-ethyl-1-heptylpiperidine Bis(pentafluoroethylsulfonyl)imide, 1,1-dipropylpiperidine Bis(pentafluoroethylsulfonyl)imide, 1-propyl-1-butylpiperidine Bis(pentafluoroethylsulfonyl)imide, 1,1-dibutylpiperidine Bis(pentafluoroethylsulfonyl)imide, 2-methyl-1-pyrroline tetrafluoroborate, 1-ethyl-2-phenylindole tetrafluoroborate, 1,2-dimethylindole tetrafluoroborate, 1-ethylcarbazole tetrafluoroborate, 1-ethyl-3-methylimidazole Tetrafluoroborate, 1-ethyl-3-methylimidazole Acetate, 1-ethyl-3-methylimidazole Trifluoroacetate, 1-ethyl-3-methylimidazole Heptafluorobutyrate, 1-ethyl-3-methylimidazole Trifluoromethanesulfonate, 1-ethyl-3-methylimidazole Perfluorobutanesulfonate, 1-ethyl-3-methylimidazole Dicyanamide, 1-ethyl-3-methylimidazole Bis(trifluoromethylsulfonyl)imide, 1-ethyl-3-methylimidazolium bis(pentafluoroethylsulfonyl)imide, 1-ethyl-3-methylimidazole Bis(nonafluorobutylsulfonyl)imide, 1-ethyl-3-methylimidazole Tris(trifluoromethylsulfonyl) methide, 1-butyl-3-methylimidazole Tetrafluoroborate, 1-butyl-3-methylimidazole Hexafluorophosphate, 1-butyl-3-methylimidazole Trifluoroacetate, 1-butyl-3-methylimidazole Heptafluorobutyrate, 1-butyl-3-methylimidazole Trifluoromethanesulfonate, 1-butyl-3-methylimidazole Perfluorobutanesulfonate, 1-butyl-3-methylimidazole Bis(trifluoromethylsulfonyl)imide, 1-hexyl-3-methylimidazole Bromide, 1-hexyl-3-methylimidazole Chloride, 1-hexyl-3-methylimidazole Tetrafluoroborate, 1-hexyl-3-methylimidazole Hexafluorophosphate, 1-hexyl-3-methylimidazole Trifluoromethanesulfonate, 1-octyl-3-methylimidazole Tetrafluoroborate, 1-octyl-3-methylimidazole Hexafluorophosphate, 1-hexyl-2,3-dimethylimidazole Tetrafluoroborate, 1,2-dimethyl-3-propylimidazole Bis(trifluoromethanesulfonyl)imide, 1-methylpyrazole Tetrafluoroborate, 2-methylpyrazole Tetrafluoroborate, 1-ethyl-2,3,5-trimethylpyrazole Bis(trifluoromethylsulfonyl)imide, 1-propyl-2,3,5-trimethylpyrazole Bis(trifluoromethylsulfonyl)imide, 1-butyl-2,3,5-trimethylpyrazole Bis(trifluoromethylsulfonyl)imide, 1-ethyl-2,3,5-trimethylpyrazole Bis(pentafluoroethylsulfonyl)imide, 1-propyl-2,3,5-trimethylpyrazole Bis(pentafluoroethylsulfonyl)imide, 1-butyl-2,3,5-trimethylpyrazole Bis(pentafluoroethylsulfonyl)imide, 1-ethyl-2,3,5-trimethylpyrazole Bis(trifluoromethylsulfonyl)trifluoroacetamide, 1-propyl-2,3,5-trimethylpyrazole Bis(trifluoromethylsulfonyl)trifluoroacetamide, 1-butyl-2,3,5-trimethylpyrazole Bis(trifluoromethylsulfonyl)trifluoroacetamide, 1-ethyl-2,3,5-trimethylpyrazoline Bis(trifluoromethylsulfonyl)imide, 1-propyl-2,3,5-trimethylpyrazoline Bis(trifluoromethylsulfonyl)imide, 1-butyl-2,3,5-trimethylpyrazoline Bis(trifluoromethylsulfonyl)imide, 1-ethyl-2,3,5-trimethylpyrazoline Bis(pentafluoroethylsulfonyl)imide, 1-propyl-2,3,5-trimethylpyrazoline Bis(pentafluoroethylsulfonyl)imide, 1-butyl-2,3,5-trimethylpyrazoline Bis(pentafluoroethylsulfonyl)imide, 1-ethyl-2,3,5-trimethylpyrazoline Bis(trifluoromethylsulfonyl)trifluoroacetamide, 1-propyl-2,3,5-trimethylpyrazoline Bis(trifluoromethylsulfonyl)trifluoroacetamide, 1-butyl-2,3,5-trimethylpyrazoline Bis(trifluoromethylsulfonyl)trifluoroacetamide, tetrapentylammonium trifluoromethanesulfonate, tetrapentylammonium bis(trifluoromethylsulfonyl)imide, tetrahexylammonium trifluoromethanesulfonate, tetrahexylammonium bis(trifluoromethylsulfonyl)imide, tetraheptylammonium trifluoromethanesulfonate, tetraheptylammonium bis(trifluoromethylsulfonyl)imide, diallyldimethylammonium tetrafluoroborate, diallyldimethylammonium trifluoromethanesulfonate, diallyldimethylammonium bis(trifluoromethylsulfonyl)imide, diallyldimethylammonium bis(pentafluoroethylsulfonyl)imide, N,N-diethyl-N-methyl-N-(2 -methoxyethyl)ammonium tetrafluoroborate, N,N-diethyl-N-methyl-N-(2-methoxyethyl)ammonium trifluoromethanesulfonate, N,N-diethyl-N-methyl-N-(2-methoxyethyl)ammonium bis(trifluoromethanesulfonyl)imide, N,N-diethyl-N-methyl-N-(2-methoxyethyl)ammonium bis(pentafluoroethylsulfonyl)imide, glycidyl trimethylammonium trifluoromethanesulfonate, glycidyl trimethylbis(trifluoromethylsulfonyl)imide, glycidyl trimethylammonium bis(pentafluoroethylsulfonyl)imide, tetraoctyl trifluoromethanesulfonate Salt, Tetraoctyl Bis(trifluoromethylsulfonyl)imide, N,N-dimethyl-N-ethyl-N-propylammonium bis(trifluoromethylsulfonyl)imide, N,N-dimethyl-N-ethyl-N-butylammonium bis(trifluoromethylsulfonyl)imide, N,N-dimethyl-N-ethyl-N-pentylammonium bis(trifluoromethylsulfonyl)imide, N,N-dimethyl-N-ethyl-N-hexylammonium bis(trifluoromethylsulfonyl)imide, N,N-dimethyl-N-ethyl-N-heptylammonium bis(trifluoromethylsulfonyl)imide, N,N-dimethyl-N-ethyl-N-nonylammonium bis(trifluoromethylsulfonyl)imide, N,N-dimethyl-N,N-dipropylammonium bis(trifluoromethylsulfonyl)imide, N,N-dimethyl-N-propyl-N-butylammonium bis(trifluoromethylsulfonyl)imide, N,N-dimethyl-N-propyl-N-pentylammonium bis(trifluoromethylsulfonyl)imide, N,N-dimethyl-N-propyl-N-hexylammonium bis(trifluoromethylsulfonyl)imide, N,N-dimethyl-N-propyl-N-heptylammonium bis(trifluoromethylsulfonyl)imide, N,N-dimethyl-N-butyl-N-hexylammonium bis(trifluoromethylsulfonyl)imide, N,N-dimethyl-N-butyl-N-heptylammonium bis(trifluoromethylsulfonyl)imide, N,N-dimethyl-N-pentyl-N-hexylammonium bis(trifluoromethylsulfonyl)imide, N,N-dimethyl-N,N-dihexyl ammonium bis(trifluoromethylsulfonyl)imide, trimethylheptyl ammonium bis(trifluoromethylsulfonyl)imide, N,N-diethyl-N-methyl-N-propyl ammonium bis(trifluoromethylsulfonyl)imide, N,N-diethyl-N-methyl-N-pentylammonium bis(trifluoromethylsulfonyl)imide, N,N-diethyl-N-methyl-N-heptyl ammonium bis(trifluoromethylsulfonyl)imide, N,N-diethyl-N-propyl-N-pentylammonium bis(trifluoromethylsulfonyl)imide, triethylpropyl ammonium bis(trifluoromethylsulfonyl)imide, triethylpentylammonium bis(trifluoromethylsulfonyl)imide, triethylheptyl ammonium bis(trifluoromethylsulfonyl)imide, N,N-dipropyl-N-methyl- N-Ethylammonium bis(trifluoromethylsulfonyl)imide, N,N-dipropyl-N-methyl-N-pentylammonium bis(trifluoromethylsulfonyl)imide, N,N-dipropyl-N-butyl-N-hexylammonium bis(trifluoromethylsulfonyl)imide, N,N-dipropyl-N,N-dihexylammonium bis(trifluoromethylsulfonyl)imide, N,N-dibutyl-N-methyl-N-pentylammonium bis(trifluoromethylsulfonyl)imide, N,N-dibutyl-N-methyl-N-hexylammonium bis(trifluoromethylsulfonyl)imide, trioctylmethylammonium bis(trifluoromethylsulfonyl)imide, N-methyl-N-ethyl-N-propyl-N-pentylammonium bis(trifluoromethylsulfonyl)imide, 1-butylpyridine (Trifluoromethylsulfonyl)trifluoroacetamide, 1-butyl-3-methylpyridine (Trifluoromethylsulfonyl)trifluoroacetamide, 1-ethyl-3-methylimidazole (Trifluoromethylsulfonyl)trifluoroacetamide, N-ethyl-N-methylmorpholine Thiocyanate, 4-ethyl-4-methylmorpholine Methyl carbonate, etc. The above ionic liquids may be used alone or in combination of two or more.
[0285] The content of the liquid antistatic agent in the adhesive layer (especially the acrylic adhesive layer) of the present invention is not particularly limited. From the perspective of being able to effectively suppress the generation of static electricity when the adhesive sheet is peeled off from the image display panel for rework in the case of poor lamination to the image display panel, it is preferably 0.5 parts by weight or more, more preferably 1 part by weight or more, and further preferably 1.5 parts by weight or more relative to 100 parts by weight of the base polymer. In addition, the upper limit of the content of the liquid antistatic agent is not particularly limited. From the perspective of visual recognition of the image display device, it is preferably 20 parts by weight or less, and more preferably 15 parts by weight or less relative to 100 parts by weight of the base polymer.
[0286] The acrylic adhesive composition preferably contains an acrylic oligomer having a weight average molecular weight of 1,000 to 30,000 together with the acrylic polymer. When the acrylic oligomer is contained, the adhesiveness to the adherend at the interface in the optical adhesive sheet of the present invention is improved, so that strong adhesiveness is easily obtained, and excellent resistance to foaming and peeling is easily obtained. It should be noted that in this specification, "acrylic oligomer having a weight average molecular weight of 1,000 to 30,000" is sometimes referred to as "acrylic oligomer".
[0287] As the acrylic oligomer, preferably, an acrylic polymer comprising a (meth)acrylate having a cyclic structure in the molecule as an essential monomer component is cited, and more preferably, an acrylic polymer comprising a (meth)acrylate having a cyclic structure in the molecule and an alkyl (meth)acrylate having a linear or branched alkyl group as essential monomer components is cited. That is, as the acrylic oligomer, preferably, an acrylic polymer comprising a (meth)acrylate having a cyclic structure in the molecule as a monomer unit is cited, and more preferably, an acrylic polymer comprising a (meth)acrylate having a cyclic structure in the molecule and an alkyl (meth)acrylate having a linear or branched alkyl group as a monomer unit is cited.
[0288] The cyclic structure (ring) of the (meth)acrylate having a cyclic structure in the above-mentioned molecule (in one molecule) (hereinafter, sometimes referred to as "ring-containing (meth)acrylate") may be any of an aromatic ring and a non-aromatic ring, and is not particularly limited. Examples of the above-mentioned aromatic ring include aromatic carbocycles [e.g., monocyclic carbocycles such as benzene rings, condensed carbocycles such as naphthalene rings, etc.], various aromatic heterocycles, etc. Examples of the non-aromatic ring include a non-aromatic aliphatic ring (non-aromatic alicyclic ring) [e.g., cycloalkane rings such as cyclopentane ring, cyclohexane ring, cycloheptane ring, cyclooctane ring, and cycloalkene rings; cycloalkene rings such as cyclohexene ring, etc.], a non-aromatic bridged ring [e.g., bicyclic hydrocarbon rings in pinane, pinene, camphane, norbornene, norbornene, etc.; aliphatic hydrocarbon rings with three or more rings (bridged hydrocarbon rings) in adamantane, etc.], and a non-aromatic heterocyclic ring [e.g., an epoxy ring, a tetrahydrofuran ring, an oxetane ring, etc.], etc.
[0289] Examples of the above-mentioned tricyclic or higher aliphatic hydrocarbon rings (tricyclic or higher bridged hydrocarbon rings) include a tetrahydrodicyclopentadienyl group represented by the following formula (5a), a dihydrodicyclopentadienyl group represented by the following formula (5b), an adamantyl group represented by the following formula (5c), a tetrahydrotricyclopentadienyl group represented by the following formula (5d), and a dihydrotricyclopentadienyl group represented by the following formula (5e).
[0290]
[0291] That is, examples of the ring-containing (meth)acrylate include cycloalkyl (meth)acrylates such as cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, cycloheptyl (meth)acrylate, and cyclooctyl (meth)acrylate; (meth)acrylates having a bicyclic aliphatic hydrocarbon ring such as isobornyl (meth)acrylate; (meth)acrylates having a tricyclic or higher aliphatic hydrocarbon ring such as tetrahydrodicyclopentadienyl (meth)acrylate, tetrahydrodicyclopentadienyloxyethyl (meth)acrylate, tetrahydrotricyclopentadienyl (meth)acrylate, 1-adamantyl (meth)acrylate, 2-methyl-2-adamantyl (meth)acrylate, and 2-ethyl-2-adamantyl (meth)acrylate; (meth)acrylates having an aromatic ring such as aryl (meth)acrylate such as phenyl (meth)acrylate, aryloxyalkyl (meth)acrylate such as phenoxyethyl (meth)acrylate, and arylalkyl (meth)acrylate such as benzyl (meth)acrylate. Among them, as the above-mentioned ring-containing (meth)acrylate, a (meth)acrylate containing a non-aromatic ring is particularly preferred, and cyclohexyl acrylate (CHA), cyclohexyl methacrylate (CHMA), tetrahydrodicyclopentadienyl acrylate (DCPA), and tetrahydrodicyclopentadienyl methacrylate (DCPMA) are more preferred, and tetrahydrodicyclopentadienyl acrylate (DCPA) and tetrahydrodicyclopentadienyl methacrylate (DCPMA) are further preferred. It should be noted that the ring-containing (meth)acrylate can be used alone or in combination of two or more.
[0292] Among the above-mentioned (meth)acrylates containing non-aromatic rings, when using (meth)acrylates having aliphatic hydrocarbon rings of three or more rings (especially bridged hydrocarbon rings of three or more rings), it is particularly preferred from the viewpoint of being less likely to cause polymerization inhibition. In addition, when using (meth)acrylates having tetrahydrodicyclopentadienyl represented by the above formula (5a) without unsaturated bonds, adamantyl represented by the above formula (5c), and tetrahydrotricyclopentadienyl represented by the above formula (5d), the foaming and peeling resistance can be further improved, and the adhesion to low-polar adherends such as polyethylene and polypropylene can be significantly improved.
[0293] The content (ratio) of the above-mentioned ring-containing (meth) acrylate in all monomer units of the acrylic oligomer (the total amount of monomer components constituting the acrylic oligomer) is not particularly limited, and is preferably 10 to 90 parts by weight, and more preferably 20 to 80 parts by weight, relative to the total amount of monomer components constituting the acrylic oligomer (100 parts by weight). When the content of the above-mentioned ring-containing (meth) acrylate is 10 parts by weight or more, the foaming and peeling resistance is easily improved, so it is preferred. In addition, when the content is 90 parts by weight or less, the adhesive layer has moderate flexibility, and the adhesive force, height difference absorption, etc. are easily improved, so it is preferred.
[0294] In addition, the (meth)acrylic acid alkyl ester having a linear or branched alkyl group as the monomer unit of the acrylic oligomer includes, for example, methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, pentyl (meth)acrylate, isopentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, pentyl (meth)acrylate, isopentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, propyl (meth)acrylate, Alkyl (meth)acrylates having an alkyl group with 1 to 20 carbon atoms, such as isooctyl (meth)acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, nonadecyl (meth)acrylate, eicosyl (meth)acrylate, etc. Among them, methyl methacrylate (MMA) is preferred from the viewpoint of good compatibility with acrylic polymers. It should be noted that the above-mentioned alkyl (meth)acrylates can be used alone or in combination of two or more.
[0295] The content (ratio) of the above-mentioned (meth) alkyl ester having a straight or branched alkyl group in all monomer units of the acrylic oligomer (the total amount of monomer components constituting the acrylic oligomer) is not particularly limited. From the viewpoint of foaming and peeling resistance, it is preferably 10 to 90 parts by weight, more preferably 20 to 80 parts by weight, and further preferably 20 to 60 parts by weight relative to the total amount of monomer components constituting the acrylic oligomer (100 parts by weight). When the content is 10 parts by weight or more, the adhesive force to an adherend made of an acrylic resin or a polycarbonate is easily improved, so it is preferred.
[0296] The monomer units of the acrylic oligomer may include, in addition to the above-mentioned (meth)acrylates having a ring and (meth)alkyl acrylates having a straight or branched alkyl group, monomers (copolymerizable monomers) that can copolymerize with these monomers. It should be noted that the content (ratio) of the above-mentioned copolymerizable monomers in all monomer units of the acrylic oligomer (the total amount of monomer components constituting the acrylic oligomer) is not particularly limited, and is preferably 49.9 parts by weight or less (for example, 0 to 49.9 parts by weight), and more preferably 30 parts by weight or less, relative to the total amount of monomer components constituting the acrylic oligomer (100 parts by weight). In addition, the copolymerizable monomers may be used alone or in combination of two or more.
[0297] The copolymerizable monomers as the monomer units of the acrylic oligomer (the copolymerizable monomers constituting the acrylic oligomer) include, for example, alkoxyalkyl (meth)acrylates [e.g., 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, methoxytriethylene glycol (meth)acrylate, 3-methoxypropyl (meth)acrylate, 3-ethoxypropyl (meth)acrylate, 4-methoxybutyl (meth)acrylate, 4-ethoxybutyl (meth)acrylate, etc.]; hydroxyl (hydroxyl) group-containing monomers [e.g., 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, etc.]; hydroxyalkyl (meth)acrylates [e.g., 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, etc.]; vinyl alcohol, allyl alcohol, etc.]; amide group-containing monomers [such as (meth)acrylamide, N,-dimethyl (meth)acrylamide, N-hydroxymethyl (meth)acrylamide, N-methoxymethyl (meth)acrylamide, N-butoxymethyl (meth)acrylamide, N-hydroxyethyl (meth)acrylamide, etc.]; amino group-containing monomers [such as aminoethyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, tert-butylaminoethyl (meth)acrylate, etc.]; cyano group-containing monomers [such as acrylonitrile, methacrylonitrile, etc.]; sulfonic acid group-containing monomers [such as sodium vinyl sulfonate, etc.]; phosphoric acid group-containing monomers [such as 2-hydroxyethyl acryloyl phosphate, etc.]; isocyanate group-containing monomers [such as 2-methacryloyloxyethyl isocyanate, etc.], imide group-containing monomers [cyclohexylmaleimide, isopropylmaleimide, etc.], etc.
[0298] As described above, the acrylic oligomer is preferably an acrylic polymer containing a (meth)acrylate having a cyclic structure in the molecule and a (meth)acrylate alkyl ester having a linear or branched alkyl group as monomer units. Among them, an acrylic polymer containing a (meth)acrylate containing a ring as a monomer unit, and the above-mentioned (meth)acrylate alkyl ester having a linear or branched alkyl group is preferred. In the acrylic polymer containing a (meth)acrylate containing a ring and a (meth)acrylate alkyl ester having a linear or branched alkyl group as the above-mentioned monomer units, the amount of the (meth)acrylate containing a ring is not particularly limited relative to the total amount of the monomer components constituting the acrylic oligomer (100 parts by weight), and is preferably 10 parts by weight to 90 parts by weight, and more preferably 20 parts by weight to 80 parts by weight. In addition, the content of the (meth)acrylate alkyl ester having a linear or branched alkyl group is not particularly limited, and is preferably 10 parts by weight to 90 parts by weight, more preferably 20 parts by weight to 80 parts by weight, and further preferably 20 parts by weight to 60 parts by weight.
[0299] In addition, as a particularly preferred specific structure of the acrylic oligomer, there can be cited: an acrylic polymer containing at least one monomer selected from the group consisting of (1) tetrahydrodicyclopentadienyl acrylate, tetrahydrodicyclopentadienyl methacrylate, cyclohexyl acrylate and cyclohexyl methacrylate as a monomer unit, and (2) methyl methacrylate. The content of (1) tetrahydrodicyclopentadienyl acrylate, tetrahydrodicyclopentadienyl methacrylate, cyclohexyl acrylate and cyclohexyl methacrylate (the total amount thereof when two or more are included) in all monomer units of the acrylic oligomer in the acrylic oligomer of the above particularly preferred specific structure is preferably 30 to 70 parts by weight relative to the total amount (100 parts by weight) of the monomer components constituting the acrylic oligomer, and the content of (2) methyl methacrylate is preferably 30 to 70 parts by weight. However, the acrylic oligomer is not limited to the above specific structure.
[0300] The acrylic oligomer can be obtained by polymerizing the above-mentioned monomer components using a known or customary polymerization method. Examples of the polymerization method for the acrylic oligomer include a solution polymerization method, an emulsion polymerization method, a bulk polymerization method, a polymerization method using active energy ray irradiation (active energy ray polymerization method), etc. Among them, the bulk polymerization method and the solution polymerization method are preferred, and the solution polymerization method is more preferred.
[0301] Various common solvents can be used in the polymerization of acrylic oligomers. Examples of the above-mentioned solvents include esters such as ethyl acetate and n-butyl acetate; aromatic hydrocarbons such as toluene and benzene; aliphatic hydrocarbons such as n-hexane and n-heptane; alicyclic hydrocarbons such as cyclohexane and methylcyclohexane; ketones such as methyl ethyl ketone and methyl isobutyl ketone, and other organic solvents. It should be noted that such solvents can be used alone or in combination of two or more.
[0302] In the polymerization of the acrylic oligomer, a known or commonly used polymerization initiator (eg, a thermal polymerization initiator, a photopolymerization initiator, etc.) may be used. The polymerization initiator may be used alone or in combination of two or more.
[0303] Examples of the thermal polymerization initiator include 2,2'-azobisisobutyronitrile (AIBN), 2,2'-azobis-2-methylbutyronitrile (AMBN), 2,2'-azobis(2-methylpropionic acid) dimethyl ester, 4,4'-azobis-4-cyanovaleric acid, 2,2'-azobis(4-methoxyphenyl-2,4-dimethylvaleronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 1,1 Azo initiators such as '-azobis(cyclohexane-1-carbonitrile), 2,2'-azobis(2,4,4-trimethylpentane); peroxide initiators such as benzoyl peroxide, tert-butyl hydroperoxide, di-tert-butyl peroxide, tert-butyl peroxybenzoate, diisopropylbenzene peroxide, 1,1-bis(tert-butylperoxide)-3,3,5-trimethylcyclohexane, 1,1-bis(tert-butylperoxide)cyclododecane, etc. It should be noted that, in the case of solution polymerization, an oil-soluble polymerization initiator is preferably used. In addition, the thermal polymerization initiator can be used alone or in combination of two or more.
[0304] The amount of the thermal polymerization initiator used is not particularly limited, but is, for example, 0.1 to 15 parts by weight based on 100 parts by weight of all monomer units of the acrylic oligomer (the total amount of monomer components constituting the acrylic oligomer).
[0305] The photopolymerization initiator is not particularly limited, and examples thereof include the same photopolymerization initiators as those used in the polymerization of the acrylic polymers listed above. The amount of the photopolymerization initiator used is not particularly limited and can be appropriately selected.
[0306] In the polymerization of the acrylic oligomer, a chain transfer agent may be used to adjust the molecular weight (specifically, to adjust the weight average molecular weight to 1000 to 30000). Examples of the chain transfer agent include 2-mercaptoethanol, α-thioglycerol, 2,3-dimercapto-1-propanol, octyl mercaptan, tert-nonyl mercaptan, dodecyl mercaptan (lauryl mercaptan), tert-dodecyl mercaptan, glycidyl mercaptan, thioglycolic acid, methyl thioglycolate, ethyl thioglycolate, propyl thioglycolate, butyl thioglycolate, tert-butyl thioglycolate, 2-ethylhexyl thioglycolate, octyl thioglycolate, isooctyl thioglycolate, decyl thioglycolate, dodecyl thioglycolate, thioglycolate of ethylene glycol, thioglycolate of neopentyl glycol, thioglycolate of pentaerythritol, and α-methylstyrene dimer. Among them, from the viewpoint of suppressing whitening of the optical adhesive sheet of the present invention due to humidification, α-thioglycerol and methyl thioglycolate are preferred, and α-thioglycerol is particularly preferred. The chain transfer agent may be used alone or in combination of two or more.
[0307] The content (usage amount) of the chain transfer agent is not particularly limited, but is preferably 0.1 to 20 parts by weight, more preferably 0.2 to 15 parts by weight, and further preferably 0.3 to 10 parts by weight, relative to 100 parts by weight of all monomer units of the acrylic oligomer (the total amount of monomer components constituting the acrylic oligomer). By making the content (usage amount) of the chain transfer agent within the above range, an acrylic oligomer having a weight average molecular weight controlled to 1,000 to 30,000 can be easily obtained.
[0308] The weight average molecular weight (Mw) of the acrylic oligomer is 1000 to 30000, preferably 1000 to 20000, more preferably 1500 to 10000, and further preferably 2000 to 8000. Since the weight average molecular weight of the acrylic oligomer is 1000 or more, the adhesive force and the holding property are improved, and the foaming and peeling resistance is improved. On the other hand, since the weight average molecular weight of the acrylic oligomer is 30000 or less, the adhesive force is easily improved, and the foaming and peeling resistance is improved.
[0309] The weight average molecular weight (Mw) of the acrylic oligomer can be determined by GPC in terms of polystyrene. For example, it can be measured under the following conditions using a high-speed GPC apparatus "HPLC-8120 GPC" manufactured by Tosoh Corporation.
[0310] Column: TSKgel SuperHZM-H / HZ4000 / HZ3000 / HZ2000
[0311] Solvent: Tetrahydrofuran
[0312] Flow rate: 0.6mL / min
[0313] The glass transition temperature (Tg) of the acrylic oligomer is not particularly limited, but is preferably 20°C to 300°C, more preferably 30°C to 300°C, and further preferably 40°C to 300°C. When the glass transition temperature of the acrylic oligomer is 20°C or higher, the foaming and peeling resistance is easily improved, which is preferred. In addition, when the glass transition temperature of the acrylic oligomer is 300°C or lower, the adhesive layer has moderate flexibility, and it is easy to obtain good adhesive strength and good step absorption, and it is easy to obtain excellent adhesion reliability, which is preferred.
[0314] The glass transition temperature (Tg) of the acrylic oligomer is a glass transition temperature (theoretical value) expressed by the above-mentioned FOX equation.
[0315] As the Tg of the homopolymer of the monomer constituting the above-mentioned acrylic oligomer, the value described in the following Table 1 can be adopted. In addition, as the Tg of the homopolymer of the monomer not described in Table 1, the value described in "Polymer Handbook" (3rd edition, John Wiley & Sons, Inc, 1989) can be adopted. In addition, as the Tg of the homopolymer of the monomer not described in the above-mentioned literature, the value obtained by the above-mentioned measurement method (the peak top temperature of tan δ in the viscoelasticity test) can be adopted.
[0316]
[0317] It should be noted that the copolymer of "DCPMA / MMA=60 / 40" in Table 1 refers to a copolymer of 60 parts by weight of DCPMA and 40 parts by weight of MMA.
[0318] When the acrylic adhesive composition contains an acrylic polymer and an acrylic oligomer, the content of the acrylic oligomer is not particularly limited, and is preferably 1 to 30 parts by weight, more preferably 2 to 20 parts by weight, and further preferably 2 to 10 parts by weight relative to 100 parts by weight of the acrylic polymer. That is, the content of the acrylic oligomer in the adhesive composition is not particularly limited, and is preferably 1 to 30 parts by weight, more preferably 2 to 20 parts by weight, and further preferably 2 to 10 parts by weight relative to 100 parts by weight of all monomer units of the acrylic polymer. The content of the acrylic oligomer in the acrylic adhesive composition is not particularly limited, for example, it is preferably 1 to 30 parts by weight, more preferably 2 to 20 parts by weight, and further preferably 2 to 10 parts by weight relative to 100 parts by weight of the monomer mixture. When the content of the acrylic oligomer is 1 part by weight or more, it is easy to obtain excellent adhesiveness and excellent foaming and peeling resistance, so it is preferred. In addition, when the content of the acrylic oligomer is 30 parts by weight or less, excellent transparency and adhesion reliability are easily obtained, so it is preferred. In addition, from the viewpoint of easily controlling the above-mentioned various properties (especially the height difference absorption) of the adhesive layer within a specified range, the content of the acrylic oligomer is preferably 10 parts by weight or less, and more preferably 8 parts by weight or less.
[0319] There is no particular limitation on the method for preparing the adhesive composition containing the acrylic polymer and the acrylic oligomer. For example, the adhesive composition can be prepared by adding an acrylic oligomer, an additive, etc. as needed to a mixture of monomer components constituting the acrylic polymer or a partial polymer of a mixture of monomer components constituting the acrylic polymer (a monomer mixture forming the acrylic polymer or a partial polymer thereof) and mixing them.
[0320] The adhesive layer of the present invention is not particularly limited, but preferably contains an ultraviolet absorber (UVA). When the adhesive layer of the present invention contains an ultraviolet absorber, it is preferred from the perspective of being able to suppress damage to the image display panel caused by ultraviolet rays. It should be noted that the ultraviolet absorber can be used alone or in combination of two or more.
[0321] The ultraviolet absorber is not particularly limited, and examples thereof include benzotriazole ultraviolet absorbers, hydroxyphenyltriazine ultraviolet absorbers, benzophenone ultraviolet absorbers, salicylate ultraviolet absorbers, cyanoacrylate ultraviolet absorbers, and hydroxybenzophenone ultraviolet absorbers.
[0322] Examples of the benzotriazole ultraviolet absorber (benzotriazole compound) include 2-(2-hydroxy-5-tert-butylphenyl)-2H-benzotriazole (trade name "TINUVIN PS", manufactured by BASF), an ester compound of phenylpropionic acid and 3-(2H-benzotriazol-2-yl)-5-(1,1-dimethylethyl)-4-hydroxy (C7-9 side chain and linear alkyl) (trade name "TINUVIN384-2", manufactured by BASF), a mixture of octyl 3-[3-tert-butyl-4-hydroxy-5-(5-chloro-2H-benzotriazol-2-yl)phenyl]propionate and 2-ethylhexyl 3-[3-tert-butyl-4-hydroxy-5-(5-chloro-2H-benzotriazol-2-yl)phenyl]propionate (trade name "TINUVIN109", manufactured by BASF), 2-(2H-benzotriazol-2-yl)- 4,6-bis(1-methyl-1-phenylethyl)phenol (trade name "TINUVIN900", manufactured by BASF), 2-(2H-benzotriazol-2-yl)-6-(1-methyl-1-phenylethyl)-4-(1,1,3,3-tetramethylbutyl)phenol (trade name "TINUVIN928", manufactured by BASF), 3-(3-(2H-benzotriazol-2-yl)-5-tert-butyl-4-hydroxyphenyl)propionic acid methyl ester / polyethylene glycol 300 reaction product (trade name "TINUVIN1130", manufactured by BASF), 2-(2H-benzotriazol-2-yl)-p-cresol (trade name "TINUVIN P", manufactured by BASF), 2-(2H-benzotriazol-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol (trade name "TINUVIN234", manufactured by BASF), 2-[5-chloro-2H-benzotriazol-2-yl]-4-methyl-6-(tert-butyl)phenol (trade name "TINUVIN326", manufactured by BASF), 2-(2H-benzotriazol-2-yl)-4,6-di-tert-amylphenol (trade name "TINUVIN328", manufactured by BASF), 2-(2H-benzotriazol-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol (trade name "TINUVIN IN329", manufactured by BASF), 2,2'-methylenebis[6-(2H-benzotriazol-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol] (trade name "TINUVIN360", manufactured by BASF), reaction product of methyl 3-(3-(2H-benzotriazol-2-yl)-5-tert-butyl-4-hydroxyphenyl)propionate and polyethylene glycol 300 (trade name "TINUVIN213", manufactured by BASF), 2-(2H-benzotriazol-2-yl)-6-dodecyl-4-methylphenol (trade name "TINUVIN571", manufactured by BASF), 2-[2-hydroxy-3-(3,4,5,6-tetrahydrophthalimidomethyl)-5-methylphenyl]benzotriazole (trade name "Sumisorb 250", manufactured by Sumitomo Chemical Co., Ltd.), 2,2'-methylenebis[6-(2H-benzotriazol-2-yl)-4-tert-octylphenol] (trade name "ADK STAB LA-31", manufactured by ADEKA Co., Ltd.), etc.
[0323] Examples of the hydroxyphenyltriazine ultraviolet absorber (hydroxyphenyltriazine compound) include a reaction product of 2-(4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine-2-yl)-5-hydroxyphenyl and [(C10-C16 (mainly C12-C13) alkoxy)methyl]ethylene oxide (trade name "TINUVIN 400", manufactured by BASF), 2-[4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine-2-yl]-[3-(dodecyloxy)-2-hydroxypropoxy]phenol), a reaction product of 2-(2,4-dihydroxyphenyl)-4,6-bis-(2,4-dimethylphenyl)-1,3,5-triazine and glycidic acid (2-ethylhexyl) ester (trade name "TINUVIN 405", manufactured by BASF), 2,4 -bis(2-hydroxy-4-butoxyphenyl)-6-(2,4-dibutoxyphenyl)-1,3,5-triazine (trade name "TINUVIN 460", manufactured by BASF), 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-[(hexyl)oxy]-phenol (trade name "TINUVIN 1577", manufactured by BASF), 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-[2-(2-ethylhexanoyloxy)ethoxy]-phenol (trade name "ADKSTABLA-46", manufactured by ADEKA Corporation), 2-(2-hydroxy-4-[1-octyloxycarbonylethoxy]phenyl)-4,6-bis(4-phenylphenyl)-1,3,5-triazine (trade name "TINUVIN 479", manufactured by BASF), etc. In addition, a compound represented by the following formula (6) (trade name "TINUVIN 477", manufactured by BASF Corporation) can be mentioned.
[0324]
[0325] Examples of the benzophenone-based ultraviolet absorbers (benzophenone-based compounds) and hydroxybenzophenone-based ultraviolet absorbers (hydroxybenzophenone-based compounds) include 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-methoxybenzophenone-5-sulfonic acid (anhydride and trihydrate salt), 2-hydroxy-4-octyloxybenzophenone, 4-dodecyloxy-2-hydroxybenzophenone, 4-benzyloxy-2-hydroxybenzophenone, 2,2'-dihydroxy-4-methoxybenzophenone (trade name "KEMISORB111", manufactured by Chemipro Chemicals Co., Ltd.), 2,2',4,4'-tetrahydroxybenzophenone (trade name "SEESORB106", manufactured by Shipro Chemicals Co., Ltd.), and 2,2'-dihydroxy-4,4'-dimethoxybenzophenone.
[0326] Examples of the salicylate ultraviolet absorber (salicylate compound) include phenyl 2-acryloxybenzoate, phenyl 2-acryloxy-3-methylbenzoate, phenyl 2-acryloxy-4-methylbenzoate, phenyl 2-acryloxy-5-methylbenzoate, phenyl 2-acryloxy-3-methoxybenzoate, phenyl 2-hydroxybenzoate, phenyl 2-hydroxy-3-methylbenzoate, phenyl 2-hydroxy-4-methylbenzoate, phenyl 2-hydroxy-5-methylbenzoate, phenyl 2-hydroxy-3-methoxybenzoate, phenyl 2-hydroxybenzoate, phenyl 2-hydroxy-3-methylbenzoate, phenyl 2-hydroxy-4-methylbenzoate, phenyl 2-hydroxy-5-methylbenzoate, phenyl 2-hydroxy-3-methoxybenzoate, and phenyl 2,4-di-tert-butylphenyl 3,5-di-tert-butyl-4-hydroxybenzoate (trade name "TINUVIN 120", manufactured by BASF).
[0327] Examples of the cyanoacrylate ultraviolet absorber (cyanoacrylate compound) include 2-cyanoacrylate alkyl esters, 2-cyanoacrylate cycloalkyl esters, 2-cyanoacrylate alkoxyalkyl esters, 2-cyanoacrylate alkenyl esters, and 2-cyanoacrylate alkynyl esters.
[0328] As the above-mentioned ultraviolet absorber, from the viewpoint of further improving corrosion resistance (especially UV resistance) while having high ultraviolet absorbency, the viewpoint of obtaining an adhesive layer having excellent optical properties and high transparency, and the viewpoint of having excellent light stability, at least one ultraviolet absorber selected from the group consisting of benzotriazole ultraviolet absorbers, benzophenone ultraviolet absorbers, and hydroxyphenyltriazine ultraviolet absorbers is preferred, and benzotriazole ultraviolet absorbers and benzophenone ultraviolet absorbers are more preferred. In particular, a benzotriazole ultraviolet absorber having a group having 6 or more carbon atoms and a phenyl group having a hydroxyl group as a substituent bonded to a nitrogen atom constituting a benzotriazole ring is preferred.
[0329] Furthermore, from the viewpoint of obtaining higher ultraviolet absorbency and further improving corrosion resistance (especially UV resistance), the ultraviolet absorber preferably has an absorbance A determined as described below of 0.5 or less.
[0330] Absorbance A: The absorbance measured by irradiating a 0.08% toluene solution of the above-mentioned ultraviolet absorber with light of wavelength 400nm
[0331] In the case where the adhesive layer of the present invention contains an ultraviolet absorber, the content of the ultraviolet absorber in the adhesive layer of the present invention (especially the acrylic adhesive layer) is not particularly limited. From the viewpoint of further improving corrosion resistance (especially UV resistance), it is preferably 0.01 parts by weight or more, more preferably 0.05 parts by weight or more, and further preferably 0.1 parts by weight or more relative to 100 parts by weight of the base polymer. In addition, from the viewpoint of suppressing the yellowing phenomenon of the adhesive accompanying the addition of the ultraviolet absorber and obtaining excellent optical properties, high transparency and excellent appearance characteristics, the upper limit of the content of the ultraviolet absorber is preferably 10 parts by weight or less, more preferably 9 parts by weight or less, and further preferably 8 parts by weight or less relative to 100 parts by weight of the base polymer.
[0332] The adhesive layer of the present invention may contain a light stabilizer. When the adhesive layer of the present invention contains a light stabilizer, it is particularly preferred to contain the light stabilizer together with the above-mentioned ultraviolet absorber. The light stabilizer can capture free radicals generated by photooxidation, thereby improving the resistance of the adhesive layer to light (especially ultraviolet rays). It should be noted that the light stabilizer can be used alone or in combination of two or more.
[0333] The light stabilizer is not particularly limited, and examples thereof include phenolic light stabilizers (phenolic compounds), phosphorus-containing light stabilizers (phosphorus compounds), thioether light stabilizers (thioether compounds), amine light stabilizers (amine compounds) (particularly hindered amine light stabilizers (hindered amine compounds)), and the like.
[0334] Examples of the phenolic light stabilizer (phenolic compound) include 2,6-di-tert-butyl-4-methylphenol, 4-hydroxymethyl-2,6-di-tert-butylphenol, 2,6-di-tert-butyl-4-ethylphenol, butylated hydroxyanisole, 3-(4-hydroxy-3,5-di-tert-butylphenyl) propionate, (4-hydroxy-3-methyl-5-tert-butyl) benzylmalonate distearyl ester, tocopherol, 2,2'-methylenebis(4-methyl-6-tert-butylphenol), 2,2'-methylenebis(4-ethyl-6-tert-butylphenol), 4,4'-methylenebis(2,6-di-tert-butylphenol), 4,4'-butylenebis(6-tert-butyl-m-cresol), 4,4'-thiobis(6-tert-butyl-m-cresol), styrenated phenol, N,N'-hexamethylenebis(3,5-di-tert-butyl-4-hydroxyhydrocinnamic acid), bis(3, 5-di-tert-butyl-4-hydroxybenzylphosphonic acid ethyl ester) calcium, 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyloxymethyl]methane, 1,6-hexanediol-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 2,2'-methylenebis(4-methyl-6-cyclohexylphenol), 2,2'-methylenebis[ 6-(1-methylcyclohexyl)-p-cresol], 1,3,5-tris(4-tert-butyl-3-hydroxy-2,6-dimethylbenzyl)isocyanuric acid, 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanuric acid, triethylene glycol-bis[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionate], 2,2'-oxalamidebis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 6-(4-hydroxy-3,5-di-tert-butylanilino)-2,4-dioctylthio-1,3,5 -triazine, bis[2-tert-butyl-4-methyl-6-(2-hydroxy-3-tert-butyl-5-methylbenzyl)phenyl]terephthalate, 3,9-bis{2-[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]-1,1-dimethylethyl}-2,4,8,10-tetraoxaspiro[5.5]undecane, 3,9-bis{2-[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyloxy]-1,1-dimethylethyl}-2,4,8,10-tetraoxaspiro[5.5]undecane, and the like.
[0335] Examples of the phosphorus-containing light stabilizer (phosphorus compound) include trisnonylphenyl phosphite, tris(2,4-di-tert-butylphenyl)phosphite, tris[2-tert-butyl-4-(3-tert-butyl-4-hydroxy-5-methylphenylthio)-5-methylphenyl]phosphite, tridecylphosphite, octyldiphenylphosphite, di(decyl)monophenylphosphite, di(tridecyl)pentaerythritol diphosphite, distearylpentaerythritol diphosphite, di(nonylphenyl)pentaerythritol diphosphite, bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite, bis(2 ,4,6-tri-tert-butylphenyl) pentaerythritol diphosphite, tetra(tridecyl) isopropylidene diphenol diphosphite, tetra(tridecyl)-4,4'-n-butylidene bis(2-tert-butyl-5-methylphenol) diphosphite, hexa(tridecyl)-1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl) butane triphosphite, tetra(2,4-di-tert-butylphenyl) biphenylene diphosphite, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, tris(2-[(2,4,8,10-tetra-tert-butyldibenzo[d,f][1,3,2]dioxaphosphacycloheptane-6-yl)oxy]ethyl)amine, etc.
[0336] Examples of thioether light stabilizers (thioether compounds) include dialkyl thiodipropionate compounds such as dilauryl thiodipropionate, dimyristyl thiodipropionate, and distearyl thiodipropionate; and β-alkylmercaptopropionate compounds of polyhydric alcohols such as tetrakis[methylene(3-dodecylthio)propionate]methane.
[0337] Examples of the amine light stabilizer (amine compound) include a polymer of dimethyl succinate and 4-hydroxy-2,2,6,6-tetramethyl-1-piperidinol (trade name "TINUVIN 622", manufactured by BASF), a 1:1 reaction product of a polymer of dimethyl succinate and 4-hydroxy-2,2,6,6-tetramethyl-1-piperidinol and N,N',N",N"'-tetrakis(4,6-bis(butyl-(N-methyl-2,2,6,6-tetramethylpiperidin-4-yl)amino)-triazine-2-yl)-4,7-diazadecane-1,10-diamine (trade name "TINUVIN 119", manufactured by BASF), dibutylamine·1,3-triazine·N,N'- Condensation product of bis(2,2,6,6-tetramethyl-4-piperidinyl-1,6-hexamethylenediamine and N-(2,2,6,6-tetramethyl-4-piperidinyl)butylamine (trade name "TINUVIN 2020", manufactured by BASF), poly[{6-(1,1,3,3-tetramethylbutyl)amino-1,3,5-triazine-2,4-diyl}{2,2,6,6-tetramethyl-4-piperidinyl}imino]hexamethylene{(2,2,6,6-tetramethyl-4-piperidinyl)imino} (trade name "TINUVIN 944", manufactured by BASF), bis(1,2,2,6,6-pentamethyl-4-piperidinyl) sebacate and methyl 1,2,6,6-pentamethyl-4-piperidinyl) sebacate -piperidinyl ester mixture (trade name "TINUVIN765", manufactured by BASF), bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate (trade name "TINUVIN770", manufactured by BASF), bis(2,2,6,6-tetramethyl-1-(octyloxy)-4-piperidinyl) sebacate, reaction product of 1,1-dimethylethyl hydroperoxide and octane (trade name "TINUVIN123", manufactured by BASF), bis(1,2,2,6,6-pentamethyl-4-piperidinyl)[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]butylmalonate (trade name "TINUVIN144", manufactured by BASF) ), the reaction product of cyclohexane and N-butyl peroxide 2,2,6,6-tetramethyl-4-piperidinamine-2,4,6-trichloro-1,3,5-triazine and 2-aminoethanol (trade name "TINUVIN152", manufactured by BASF), a mixture of bis(1,2,2,6,6-pentamethyl-4-piperidinyl) sebacate and methyl sebacate 1,2,2,6,6-pentamethyl-4-piperidinyl ester (trade name "TINUVIN292", manufactured by BASF), 1,2,3,4-butanetetracarboxylic acid with 1,2,2,6,6-pentamethyl-4-piperidinol and 3,9-bis(2-hydroxy-1,1-dimethylethyl)-2,4,8,10-tetraoxaspiro[5.5] Undecane mixed ester (trade name "Adekastab LA-63P", manufactured by ADEKA Corporation), etc. As the amine stabilizer, hindered amine stabilizers are particularly preferred.
[0338] When the adhesive layer of the present invention contains a light stabilizer, the content of the light stabilizer in the adhesive layer of the present invention (particularly the acrylic adhesive layer) is not particularly limited. From the viewpoint of easily exhibiting light resistance, it is preferably 0.1 parts by weight or more, and more preferably 0.2 parts by weight or more, relative to 100 parts by weight of the base polymer. In addition, from the viewpoint of not easily causing coloring caused by the light stabilizer itself, easily obtaining high transparency, and from the viewpoint of optical properties, the upper limit of the above content is preferably 5 parts by weight or less, and more preferably 3 parts by weight or less, relative to 100 parts by weight of the base polymer.
[0339] The formation of the adhesive layer of the present invention is not particularly limited, and a crosslinking agent may be used. For example, the acrylic polymer in the acrylic adhesive layer can be crosslinked to control the gel fraction. It should be noted that the crosslinking agent may be used alone or in combination of two or more.
[0340] The crosslinking agent is not particularly limited, and examples thereof include isocyanate crosslinking agents, epoxy crosslinking agents, melamine crosslinking agents, peroxide crosslinking agents, urea crosslinking agents, metal alkoxide crosslinking agents, metal chelate crosslinking agents, metal salt crosslinking agents, carbodiimide crosslinking agents, Oxazoline crosslinking agents, aziridine crosslinking agents, amine crosslinking agents, etc. Among them, isocyanate crosslinking agents and epoxy crosslinking agents are preferred, and isocyanate crosslinking agents are more preferred.
[0341] Examples of the isocyanate crosslinking agent (polyfunctional isocyanate compound) include lower aliphatic polyisocyanates such as 1,2-ethylene diisocyanate, 1,4-butylene diisocyanate, and 1,6-hexamethylene diisocyanate; alicyclic polyisocyanates such as cyclopentylene diisocyanate, cyclohexylene diisocyanate, isophorone diisocyanate, hydrogenated toluene diisocyanate, and hydrogenated xylene diisocyanate; and aromatic polyisocyanates such as 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, 4,4′-diphenylmethane diisocyanate, and xylylene diisocyanate. In addition, examples of the isocyanate crosslinking agent include commercially available products such as trimethylolpropane / toluene diisocyanate adduct (trade name "CORONATE L", manufactured by Tosoh Corporation), trimethylolpropane / hexamethylene diisocyanate adduct (trade name "CORONATE HL", manufactured by Tosoh Corporation), and trimethylolpropane / xylylene diisocyanate adduct (trade name "TAKENATE D-110N", manufactured by Mitsui Chemicals, Inc.).
[0342] Examples of the epoxy crosslinking agent (polyfunctional epoxy compound) include N,N,N',N'-tetraglycidyl-m-xylylenediamine, diglycidyl aniline, 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, 1,6-hexanediol diglycidyl ether, neopentyl glycol diglycidyl ether, ethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, sorbitol polyol, Examples of the epoxy crosslinking agent include glycidyl ether, glycerol polyglycidyl ether, pentaerythritol polyglycidyl ether, polyglycerol polyglycidyl ether, sorbitan polyglycidyl ether, trimethylolpropane polyglycidyl ether, diglycidyl adipate, diglycidyl phthalate, tris(2-hydroxyethyl)isocyanurate triglycidyl ether, resorcinol diglycidyl ether, bisphenol-S-diglycidyl ether, and epoxy resins having two or more epoxy groups in the molecule. Examples of the epoxy crosslinking agent include commercial products such as "TETRAD C" (manufactured by Mitsubishi Gas Chemical Co., Ltd.).
[0343] When a cross-linking agent is used in the formation of the adhesive layer of the present invention, the amount of the cross-linking agent used is not particularly limited. From the perspective of obtaining sufficient adhesive reliability, it is preferably 0.001 parts by weight or more, and more preferably 0.01 parts by weight or more relative to 100 parts by weight of the base polymer. In addition, from the perspective of easily controlling the above-mentioned various properties of the adhesive layer (especially the height difference absorption) within a specified range, the upper limit of the above-mentioned amount used is preferably 10 parts by weight or less, and more preferably 5 parts by weight or less relative to 100 parts by weight of the base polymer.
[0344] From the viewpoint of improving the adhesive reliability under humidification conditions, especially the viewpoint of improving the adhesive reliability to glass, the adhesive layer of the present invention (especially the acrylic adhesive layer) may contain a silane coupling agent. It should be noted that the silane coupling agent may be used alone or in combination of two or more. When the above-mentioned adhesive layer contains a silane coupling agent, the adhesiveness under humidification conditions, especially the adhesiveness to glass, can be improved.
[0345] The silane coupling agent is not particularly limited, and examples thereof include γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane, γ-aminopropyltrimethoxysilane, N-phenyl-aminopropyltrimethoxysilane, etc. In addition, commercial products such as trade name "KBM-403" (manufactured by Shin-Etsu Chemical Co., Ltd.) can also be cited as silane coupling agents. Among them, γ-glycidoxypropyltrimethoxysilane is preferred as the silane coupling agent.
[0346] When the adhesive layer of the present invention contains a silane coupling agent, the content of the silane coupling agent in the adhesive layer of the present invention (particularly the acrylic adhesive layer) is not particularly limited, and is preferably 0.01 parts by weight or more, more preferably 0.02 parts by weight or more, relative to 100 parts by weight of the base polymer. In addition, the upper limit of the content of the silane coupling agent is preferably 1 part by weight or less, more preferably 0.5 parts by weight or less, relative to 100 parts by weight of the base polymer.
[0347] The adhesive layer of the present invention may contain a colorant. It should be noted that the colorant may be used alone or in combination of two or more. When the above-mentioned adhesive layer contains a colorant, it is preferred from the perspective of being able to prevent reflection caused by metal wiring, ITO wiring, etc. configured on the substrate of the image display device of the present invention.
[0348] As long as the above-mentioned coloring agent can be dissolved or dispersed in the adhesive layer of the present invention, it can be either a dye or a pigment. Even if a dye is added in a small amount, low haze can be achieved, and it will not have sedimentation like a pigment so as to be easily evenly distributed, so a dye is preferred. In addition, even if a pigment is added in a small amount, the color expression is also high, so a pigment is preferred. When a pigment is used as a coloring agent, it is preferred that the conductivity is low or there is no conductivity. In addition, when a dye is used, it is preferably used in combination with the above-mentioned light stabilizer, etc.
[0349] As the above-mentioned colorant, as long as it absorbs visible light (wavelength 400-700nm), a substance that is transmissive to ultraviolet rays (wavelength 330-400nm) or a substance that is absorptive to ultraviolet rays can be used without limitation, preferably a substance that absorbs visible light and has ultraviolet transmissivity. That is, the colorant is preferably a colorant whose maximum value of transmittance at a wavelength of 330nm-400nm is greater than the maximum value of transmittance at a wavelength of 400nm-700nm. In addition, the above-mentioned colorant preferably has an average transmittance at a wavelength of 330nm-400nm greater than the average transmittance at a wavelength of 400nm-700nm. The transmittance of the colorant is measured using a solution or dispersion diluted with an appropriate solvent such as tetrahydrofuran (THF) or a dispersion medium (an organic solvent with low absorption in the range of wavelengths 330nm-700nm) so that the transmittance at a wavelength of 400nm is about 50% to about 60%.
[0350] Carbon black and titanium black, which are commonly used as black colorants, absorb more ultraviolet light than visible light (ultraviolet transmittance is lower than visible light transmittance). Therefore, if a colorant such as carbon black is added to an active energy ray-curable acrylic adhesive composition, most of the ultraviolet light irradiated for photocuring is absorbed by the colorant, the amount of light absorbed by the photopolymerization initiator is small, and photocuring requires time (the cumulative amount of irradiated light increases). In addition, when the thickness of the adhesive layer is large, less ultraviolet light reaches the surface on the opposite side of the light irradiation surface, so even if long-term light irradiation is performed, photocuring tends to become insufficient. In contrast, by using a colorant whose ultraviolet transmittance is higher than that of visible light, it is possible to suppress the curing hindrance caused by the colorant.
[0351] Examples of ultraviolet-transmitting black pigments include "9050 BLACK" and "UVBK-0001" manufactured by TOKUSHIKI. Examples of ultraviolet-absorbing black dyes include "VALIFAST BLACK 3810" and "NUBIAN Black PA-2802" manufactured by Oriental Chemical Industry. Examples of ultraviolet-absorbing black pigments include carbon black and titanium black.
[0352] The content of the colorant in the adhesive layer of the present invention is, for example, about 0.01 to 20 parts by weight relative to 100 parts by weight of the base polymer, and can be appropriately set according to the type of the colorant, the color tone and light transmittance of the adhesive layer, etc. The colorant can be added to the composition as a solution or dispersion dissolved or dispersed in an appropriate solvent.
[0353] The adhesive layer of the present invention may further contain additives such as a crosslinking accelerator, a tackifying resin (rosin derivatives, polyterpene resins, petroleum resins, oil-soluble phenolic resins, etc.), an anti-aging agent, a filler, an antioxidant, a chain transfer agent, a plasticizer, a softener, and a surfactant as needed within the range that does not impair the effects of the present invention. In addition, such additives may be used alone or in combination of two or more.
[0354] The haze of the adhesive layer of the present invention is not particularly limited, but is preferably 1% or less, more preferably 0.8% or less, and further preferably 0.5% or less from the viewpoint of appearance characteristics, transparency, and optical characteristics. It should be noted that in this specification, the haze of the adhesive layer can be measured, for example, using a haze meter according to JIS K7136.
[0355] The visible light transmittance of the adhesive layer of the present invention is not particularly limited. From the perspective of appearance characteristics, transparency, and optical characteristics, it is preferably 90% or more, more preferably 90.5% or more, and further preferably 91% or more. It should be noted that in this specification, the visible light transmittance of the adhesive layer can be measured, for example, using a haze meter according to JIS K7361-1. It should be noted that the above-mentioned visible light transmittance is the transmittance of light (visible light) with a wavelength of 400nm to 780nm.
[0356] The thickness of the adhesive layer of the present invention is not particularly limited. From the perspective of obtaining sufficient adhesive reliability, it is preferably 12 μm or more, preferably 15 μm or more, more preferably 20 μm or more, and particularly preferably 25 μm or more. When the thickness is 12 μm or more, it is preferred from the following aspects: the adhesive layer fully follows the contraction or expansion in the use environment of the image display device of the present invention, can suppress bulging or peeling, and has excellent height difference absorption. In addition, from the perspective of optical properties, the thickness is preferably 500 μm or less, preferably 300 μm or less, and more preferably 200 μm or less.
[0357] <Manufacturing of Optical Adhesive Sheet>
[0358] The optical pressure-sensitive adhesive sheet of the present invention can be produced by laminating the pressure-sensitive adhesive layer of the present invention on the first surface of the substrate of the present invention.
[0359] The method for laminating the adhesive layer of the present invention on the first surface of the substrate of the present invention is not particularly limited, and can be carried out as follows: the above-mentioned adhesive composition is coated (applied) on a release liner, and the obtained adhesive composition layer is dried and cured; the above-mentioned adhesive composition is coated (applied) on a release liner, and the obtained adhesive composition layer is irradiated with active energy rays to cure it, thereby forming a sheet-shaped adhesive layer on the release liner, and the above-mentioned adhesive layer is attached to the first surface of the substrate of the present invention. In addition, heating and drying can be further performed as needed.
[0360] When curing is performed by irradiation with active energy rays, it is preferred to further attach a release liner to the surface of the coating film and irradiate with active energy rays while the pressure-sensitive adhesive composition is sandwiched between two release liners to prevent inhibition by oxygen.
[0361] Other methods for laminating the adhesive layer of the present invention on the first surface of the substrate of the present invention may be carried out as follows: the adhesive composition is applied (coated) on the first surface of the substrate of the present invention, and the obtained adhesive composition layer is dried and cured; the adhesive composition is applied (coated) on the first surface of the substrate of the present invention, and the obtained adhesive composition layer is irradiated with active energy rays to cure it. In addition, heating and drying may be further performed as needed.
[0362] When curing is performed by irradiation with active energy rays, it is preferred that a release liner is attached to the surface of the coating film and the active energy rays are irradiated with the pressure-sensitive adhesive composition sandwiched between the substrate of the present invention and the release liner to prevent inhibition by oxygen.
[0363] Before the active energy ray irradiation, the sheet-like coating film may be heated to remove the solvent, etc. When the solvent, etc. are removed by heating, it is preferably carried out before attaching a release liner.
[0364] Examples of the active energy rays include ionizing radiation such as α rays, β rays, γ rays, neutron rays, electron rays, and ultraviolet rays, and ultraviolet rays are particularly preferred. The irradiation energy, irradiation time, and irradiation method of the active energy rays are not particularly limited.
[0365] The above-mentioned adhesive composition can be prepared by a known or customary method. For example, a solvent-based acrylic adhesive composition can be prepared by mixing a liquid antistatic agent and an additive as required (such as an ultraviolet absorber, etc.) in a solution containing the above-mentioned acrylic polymer. For example, an active energy ray-curable acrylic adhesive composition can be prepared by mixing a liquid antistatic agent and an additive as required (such as an ultraviolet absorber, etc.) in a mixture of the above-mentioned acrylic monomers or a partial polymer thereof.
[0366] It should be noted that the adhesive composition can be applied by a known coating method, for example, a coating machine such as a gravure roll coater, a reverse roll coater, a lick coater, a dip roll coater, a rod coater, a knife coater, a spray coater, a comma coater, or a direct coater can be used.
[0367] In particular, when an adhesive layer is formed using an active energy ray-curable adhesive composition, the active energy ray-curable adhesive composition preferably contains a photopolymerization initiator. It should be noted that when the active energy ray-curable adhesive composition contains an ultraviolet absorber, as a photopolymerization initiator, it is preferred to contain at least a photopolymerization initiator having light absorption characteristics in a wide wavelength range. For example, it is preferred to contain at least a photopolymerization initiator having light absorption characteristics for visible light in addition to ultraviolet light. This is because: there is a concern that the curing caused by active energy rays is hindered by the action of the ultraviolet absorber, and when a photopolymerization initiator having light absorption characteristics in a wide wavelength range is contained, the adhesive composition is easy to obtain high photocurability.
[0368] <Antistatic Layer>
[0369] In the optical adhesive sheet of the present invention, an antistatic layer may be provided on the surface or between any layers. The optical adhesive sheet of the present invention has an antistatic layer, which is suitable from the following aspects: in the case of poor lamination to the image display panel, static electricity can be suppressed when the adhesive sheet is peeled off from the image display panel for rework. The above-mentioned antistatic layer is preferably formed between the substrate of the present invention and the adhesive layer of the present invention.
[0370] The antistatic layer is not particularly limited, and for example, it is an antistatic layer formed by coating a conductive coating liquid containing a conductive polymer on a release liner. Specifically, for example, it is an antistatic layer formed by coating a conductive coating liquid containing a conductive polymer on the first surface of the substrate of the present invention. Specific coating methods include roller coating, rod coating, gravure coating, etc.
[0371] Examples of the conductive polymer include conductive polymers obtained by doping polyanions in π-conjugated conductive polymers, etc. Examples of the π-conjugated conductive polymer include chain conductive polymers such as polythiophene, polypyrrole, polyaniline, and polyacetylene, etc. Examples of the polyanion include polystyrene sulfonic acid, polyisoprene sulfonic acid, polyvinyl sulfonic acid, polyallyl sulfonic acid, polyethyl acrylate sulfonic acid, and polymethacryloyl carboxylic acid, etc.
[0372] The thickness of the antistatic layer is preferably 1 nm to 1000 nm, and more preferably 5 nm to 900 nm. The antistatic layer may be a single layer or may be two or more layers.
[0373] <Release liner>
[0374] In the optical adhesive sheet of the present invention, the surface of the adhesive layer of the present invention (the adhesive surface of the adhesive layer of the present invention) may be protected by a release liner before use. The release liner is used as a protective material for the adhesive layer and is peeled off when the optical adhesive sheet of the present invention is attached to an adherend.
[0375] As the above-mentioned release liner, conventional release paper or the like can be used. Specifically, for example, in addition to a substrate having a release treatment layer treated with a release treatment agent on at least one surface, a low-adhesive substrate containing a fluorine-containing polymer (for example, polytetrafluoroethylene, polychlorotrifluoroethylene, polyvinyl fluoride, polyvinylidene fluoride, tetrafluoroethylene-hexafluoropropylene copolymer, chlorofluoroethylene-vinylidene fluoride copolymer, etc.), a low-adhesive substrate containing a non-polar polymer (for example, olefin resins such as polyethylene and polypropylene, etc.), etc. can also be used.
[0376] As the release liner, for example, a release liner having a release treatment layer formed on at least one side of the release liner substrate can be preferably used. As such a release liner substrate, in addition to plastic substrate films (synthetic resin films) such as polyester films (polyethylene terephthalate films, etc.), olefin resin films (polyethylene films, polypropylene films, etc.), polyvinyl chloride films, polyimide films, polyamide films (nylon films), and rayon films, and papers (high-quality paper, Japanese paper, kraft paper, glass paper, synthetic paper, lacquered paper, etc.), substrates (complexes of 2 to 3 layers) obtained by laminating or coextrusion can also be cited.
[0377] The release agent constituting the release layer is not particularly limited, and examples thereof include silicone release agents, fluorine-containing release agents, and long-chain alkyl release agents. The release agents may be used alone or in combination of two or more.
[0378] The thickness of the release liner is not particularly limited and can be appropriately selected from the range of 5 μm to 100 μm.
[0379] In order to prevent the damage of adherends such as image display panels, the release liner may be provided with an antistatic layer on at least one side of the release liner substrate. The antistatic layer may be formed on one side (release treated side or untreated side) of the release liner, or may be formed on both sides (release treated side and untreated side) of the release liner.
[0380] The antistatic layer is not particularly limited, and for example, it is an antistatic layer formed by coating a conductive coating liquid containing a conductive polymer on a release liner. Specifically, for example, it is an antistatic layer formed by coating a conductive coating liquid containing a conductive polymer on a release liner (release treated surface and / or untreated surface). Specific coating methods include roller coating, rod coating, gravure coating, etc.
[0381] As the conductive polymer, the same conductive polymer as the conductive polymer constituting the antistatic layer constituting the optical pressure-sensitive adhesive sheet of the present invention can be used.
[0382] The thickness of the antistatic layer is preferably 1 nm to 1000 nm, and more preferably 5 nm to 900 nm. The antistatic layer may be a single layer or may be two or more layers.
[0383] <Surface protection film>
[0384] In the optical adhesive sheet of the present invention, the second surface of the substrate of the present invention may be protected by a surface protective film. The surface protective film is used as a protective material for the second surface of the substrate of the present invention during the manufacture and transportation of the optical adhesive sheet of the present invention and the image display device of the present invention.
[0385] Examples of the material for forming the surface protection film include ester resins such as polyethylene terephthalate resins, cycloolefin resins such as norbornene resins, olefin resins such as polypropylene, polyamide resins, polycarbonate resins, and copolymer resins thereof, etc. Ester resins (particularly polyethylene terephthalate resins) are preferred.
[0386] The thickness of the surface protection film is typically 20 μm to 250 μm, and preferably 30 μm to 150 μm.
[0387] The surface protective film is releasably attached to the second surface of the substrate of the present invention via any appropriate adhesive. It is preferred to form a surface protective film having an adhesive layer, and to attach it to the second surface of the substrate of the present invention of the optical adhesive sheet of the present invention. As the adhesive used in the lamination of the surface protective film, for example, the following adhesive composition can be cited: an adhesive composition obtained by using acrylic resin, styrene resin, polysiloxane resin, etc. as a base resin, and a crosslinking agent selected from isocyanate compounds, epoxy compounds, aziridine compounds, etc., and a silane coupling agent, etc. in the base resin. The thickness of the adhesive layer is usually 1μm to 60μm, preferably 3μm to 30μm. When the adhesive layer is too thin, it is possible to produce undesirable conditions such as reduced adhesion and easy mixing of bubbles. When the adhesive layer is too thick, it is possible to produce undesirable conditions such as adhesive protrusion. From the viewpoints of chemical resistance and adhesion, it is preferred to use an acrylic adhesive.
[0388] <Image Display Device>
[0389] The image display device of the present invention has a laminated structure in which the optical pressure-sensitive adhesive sheet of the present invention and an image display panel are laminated. Figure 3 In the image display device 20 , the image display panel 4 is laminated on the pressure-sensitive adhesive layer 1 of the optical pressure-sensitive adhesive sheet 10B.
[0390] The image display device of the present invention has the optical adhesive sheet of the present invention in the laminated structure, so it is suitable from the following aspects: in the case of poor lamination to the image display panel, the generation of static electricity can be suppressed when the adhesive sheet is peeled off from the image display panel for rework, and the damage of the image display panel can be suppressed. In addition, it is also suitable from the following aspects: it is possible to impart an excellent antistatic effect to the adhesive layer of the present invention without damaging the adhesive properties of the adhesive layer of the invention, so the adhesion between the adhesive layer of the present invention and the substrate of the present invention is improved, and excellent thermal shock resistance is obtained. In addition, it is also suitable from the following aspects: even in a harsh environment such as thermal shock, the adhesive layer of the present invention maintains an excellent antistatic effect, and in the case of a failure such as a light-emitting element not lighting up in the use environment of the image display device, the generation of static electricity can be suppressed when the adhesive sheet is peeled off from the image display panel for repair. In addition, the rise, contraction or expansion of the haze of the optical adhesive sheet of the present invention caused by the thermal shock in the use environment can be suppressed, and the transparency can be maintained without change. In addition, the adhesive layer of the present invention fully follows the contraction or expansion of the image display device, and is not easy to produce bulges or peeling. Furthermore, when there are uneven shapes due to wiring or the like in the image display panel, the pressure-sensitive adhesive layer of the present invention can sufficiently follow the uneven shapes and fill them without leaving any bubbles, that is, it has excellent uneven absorption properties.
[0391] The image display panel is not particularly limited, and examples thereof include a liquid crystal image display panel, a self-luminous image display panel (eg, an organic EL (electroluminescence) image display panel, an LED image display panel), and the like.
[0392] The image display panel is formed by alternately arranging RGB elements. In order to improve the contrast, black matrix (BM) is preferably used to fill the gaps between the RGB elements.
[0393] The image display device of the present invention may have an optical component other than the optical adhesive sheet of the present invention and the image display panel on the surface or in any interlayer. As the above-mentioned optical component, there is no particular limitation, and examples thereof include: a polarizing plate, a phase difference plate, an anti-reflection film, a field of view adjustment film, an optical compensation film, etc. It should be noted that the above-mentioned optical component also includes a component (appearance film, decorative film, surface protection plate, etc.) that plays a decorative and protective role while maintaining the visual recognition of the image display device and the input device.
[0394] The image display device of the present invention can be produced by bonding the above-mentioned image display panel to the pressure-sensitive adhesive layer of the optical pressure-sensitive adhesive sheet of the present invention.
[0395] Specifically, the image display panel and the optical adhesive sheet of the present invention can be pasted by laminating under heating and / or pressure. After laminating under heating and / or pressure, active energy rays can be irradiated for curing. The irradiation of active energy rays can be carried out in the same manner as the formation of the adhesive layer of the present invention.
[0396] <Splicing Display>
[0397] The spliced display of the present invention is formed by arranging a plurality of image display devices of the present invention. Figure 4 In the figure, the spliced display 30 is formed by arranging 9 image display devices 20 (the stacked structure is not shown) in a 3×3 arrangement on a supporting substrate 31 in a tile shape, and the image display devices 20 are in contact with each other at the gap 32. As the above-mentioned supporting substrate, a glass plate or a plastic film similar to the base material of the present invention can be used.
[0398] The image display device of the present invention suppresses shrinkage or expansion in the use environment, so it is difficult to generate gaps or overlaps between the multiple image display devices in the spliced display of the present invention, and the gaps are not conspicuous, so that a good appearance is maintained. In addition, the shrinkage or expansion is small, and the transparency can be maintained without change. In addition, the adhesive layer of the present invention can fully follow the shrinkage or expansion of the image display device, and can prevent the undesirable conditions caused by the generation of bulges or peeling.
[0399] In addition, in the spliced display of the present invention, when the second surface of the substrate of the present invention is subjected to anti-reflection treatment and / or anti-glare treatment, it is preferred from the following aspects: it is possible to prevent reflection caused by metal wiring, ITO wiring, etc. disposed on the substrate of the image display device of the present invention. In addition, it is also preferred from the following aspects: in the spliced display, it is not easy to visually identify the gap between the image display devices of the present invention.
[0400] The spliced display of the present invention may also include components other than the image display device of the present invention and the supporting substrate. Such components are not particularly limited, and examples thereof include a backlight, a touch sensor, and the like.
[0401] The spliced display of the present invention can be manufactured by arranging a plurality of the image display devices of the present invention without gaps on the supporting substrate and fixing them by sealing the outermost surfaces with glass or the like.
[0402] Example
[0403] Hereinafter, the present invention will be described in more detail based on Examples, but the present invention is not limited to these Examples.
[0404] <Example 1>
[0405] [Preparation of (meth)acrylic polymer solution 1]
[0406] In a four-necked flask equipped with a stirring blade, a thermometer, a nitrogen inlet tube, and a cooler, 95 parts by mass of butyl acrylate (BA), 5 parts by mass of acrylic acid (AA), 0.2 parts by mass of 2,2'-azobisisobutyronitrile (AIBN) as a polymerization initiator, and 234 parts by mass of ethyl acetate were added, and nitrogen was introduced while slowly stirring, and the liquid temperature in the flask was maintained at around 65°C for 6 hours to perform a polymerization reaction, thereby preparing a (meth)acrylic polymer solution 1 (30% by mass). The weight average molecular weight (Mw) of the above-mentioned (meth)acrylic polymer is 600,000, the molecular weight distribution (Mw / Mn) is 4.0, and the glass transition temperature (Tg) is -47°C.
[0407] Preparation of acrylic adhesive composition 1
[0408] The (meth)acrylic polymer solution 1 (30% by mass) was diluted to 20% by mass with ethyl acetate, and to 500 parts by mass of the solution (100 parts by mass of solid content), 0.075 parts by mass of an epoxy crosslinking agent (manufactured by Mitsubishi Gas Chemical Co., Ltd., trade name "TETRAD-C", 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, epoxy equivalent: 110, number of functional groups: 4) and a liquid antistatic agent (manufactured by Nippon Carlit Co., Ltd., trade name "CIL312"), 1-butyl-3-methylpyridine were added. 3 parts by mass of bis(trifluoromethylsulfonyl)imide) (actual mass: 3 parts by mass) were added, and then mixed and stirred to prepare an acrylic pressure-sensitive adhesive composition 1 (acrylic pressure-sensitive adhesive solution).
[0409] [Preparation of Adhesive Sheet 1]
[0410] The acrylic adhesive composition 1 was applied to the surface of a 75 μm thick polyethylene terephthalate film (PET film, transparent substrate, release liner) treated with a silicone release agent, air-dried for 3 minutes, and then heated at 145° C. for 90 seconds to form a 50 μm thick adhesive layer 1. Next, a non-anti-glare layer of an anti-glare film (manufactured by DNP Co., Ltd., trade name "DSG23", PET film) having an anti-glare layer formed on one side was bonded to the surface of the adhesive layer 1, thereby obtaining an adhesive sheet 1 comprising an anti-glare film / adhesive layer 1 / release liner.
[0411] <Example 2>
[0412] Preparation of acrylic adhesive composition 2
[0413] To 556 parts by mass (100 parts by mass of solid content) of a (meth)acrylic polymer solution 2 (a copolymer of 99 parts by mass of butyl acrylate (BA) and 1 part by mass of 4-hydroxybutyl acrylate (HBA), 18% by mass, manufactured by Soken Chemical Co., Ltd.), 0.27 parts by mass (0.2 parts by mass of a solid content) of an isocyanate crosslinking agent (trimethylolpropane xylylene diisocyanate, manufactured by Mitsui Chemicals, Ltd., under the trade name “TAKENATE D110N”), and a peroxide crosslinking agent (NYPER manufactured by NOF Corporation, under the trade name “Takenate D110N”) were added. BMT", 0.75 parts by weight (0.3 parts by weight of solid content) of benzoyl peroxide), 3 parts by weight (actual weight: 3 parts by weight) of a liquid antistatic agent (manufactured by Mitsubishi Materials Electronic Chemicals Co., Ltd., trade name "MTOATFSI", trioctylmethylammonium bis(trifluoromethylsulfonyl)imide), and then mixed and stirred to prepare an acrylic adhesive composition 2.
[0414] [Preparation of Adhesive Sheet 2]
[0415] A pressure-sensitive adhesive sheet 1 including an antiglare film / pressure-sensitive adhesive layer 1 / release liner was obtained in the same manner as in Example 1 except that the acrylic pressure-sensitive adhesive composition 2 was used.
[0416] <Example 3>
[0417] [Preparation of Acrylic Adhesive Composition 3]
[0418] As monomer components for forming a prepolymer, 67 parts by mass of butyl acrylate (BA), 14 parts by mass of cyclohexyl acrylate (manufactured by Osaka Organic Chemical Industry Co., Ltd., trade name "Viscoat #155"), 19 parts by mass of 4-hydroxybutyl acrylate (4HBA), 0.09 parts by mass of a photopolymerization initiator (manufactured by BASF, trade name "Omnirad 184"), and 0.09 parts by mass of a photopolymerization initiator (manufactured by BASF, trade name "Omnirad 651") were mixed, and polymerization was performed by irradiation with ultraviolet rays to obtain a prepolymer composition. 3 parts by mass of a liquid antistatic agent (manufactured by Mitsubishi Materials Electronic Chemicals Co., Ltd., trade name "MTOATFSI", trioctylmethylammonium bis (trifluoromethylsulfonyl) imide) were added to 100 parts by weight of the prepolymer composition, and then they were uniformly mixed to prepare an acrylic adhesive composition 3.
[0419] [Preparation of Adhesive Layer 3]
[0420] A polyethylene terephthalate (PET) film ("Diafoil MRF75" manufactured by Mitsubishi Chemical) with a thickness of 75 μm and a silicone release layer on the surface was used as a substrate (also serving as a heavy release liner), and the acrylic adhesive composition 3 was applied to the release layer of the substrate in a thickness of 50 μm to form a coating layer. A release layer of a PET film ("DIAFOIL MRE75" manufactured by Mitsubishi Chemical) with a thickness of 75 μm and a silicone release treatment on one side was attached to the coating layer as a cover sheet (also serving as a light release liner). The irradiation intensity of the irradiation surface directly below the lamp was 5 mW / cm 2 The laminate was irradiated with ultraviolet rays from the cover sheet side for photocuring using a black light lamp whose position was adjusted in a manner of , thereby obtaining an adhesive layer 3 having a thickness of 50 μm.
[0421] [Preparation of Adhesive Sheet 3]
[0422] The non-anti-glare layer of an anti-glare film (manufactured by DNP Co., Ltd., trade name "DSG23", PET film) having an anti-glare layer formed on one side is adhered to the adhesive surface exposed by peeling off one release liner from the above-obtained adhesive layer 3, thereby obtaining an adhesive sheet 3 comprising anti-glare film / adhesive layer 3 / release liner.
[0423] <Example 4>
[0424] As the liquid antistatic agent, IL220 manufactured by Daiichi Kogyo Seiyaku Co., Ltd., 1-methyl-1-propylpyrrolidine A pressure-sensitive adhesive sheet 4 including an antiglare film / pressure-sensitive adhesive layer 4 / release liner was obtained in the same manner as in Example 3 except that 3 parts by mass of bis(trifluoromethylsulfonyl)imide was used.
[0425] <Example 5>
[0426] As liquid antistatic agents, CIL612 manufactured by Nippon Carlit Co., Ltd., 1-ethyl-3-methylimidazole A pressure-sensitive adhesive sheet 5 including an antiglare film / pressure-sensitive adhesive layer 5 / release liner was obtained in the same manner as in Example 3 except that 3 parts by mass of bis(trifluoromethylsulfonyl)imide was used.
[0427] <Example 6>
[0428] As the liquid antistatic agent, CIL312 manufactured by Nippon Carlit Co., Ltd., 1-butyl-3-methylpyridine A pressure-sensitive adhesive sheet 6 including an antiglare film / pressure-sensitive adhesive layer 6 / release liner was obtained in the same manner as in Example 1 except that 2 parts by mass of bis(trifluoromethylsulfonyl)imide was used.
[0429] <Example 7>
[0430] As the liquid antistatic agent, CIL312 manufactured by Nippon Carlit Co., Ltd., 1-butyl-3-methylpyridine A pressure-sensitive adhesive sheet 7 including an antiglare film / pressure-sensitive adhesive layer 7 / release liner was obtained in the same manner as in Example 1 except that 5 parts by mass of bis(trifluoromethylsulfonyl)imide was used.
[0431] <Example 8>
[0432] As the liquid antistatic agent, CIL312 manufactured by Nippon Carlit Co., Ltd., 1-butyl-3-methylpyridine A pressure-sensitive adhesive sheet 8 including an antiglare film / pressure-sensitive adhesive layer 8 / release liner was obtained in the same manner as in Example 1 except that 10 parts by mass of bis(trifluoromethylsulfonyl)imide was used.
[0433] <Comparative Example 1>
[0434] As the liquid antistatic agent, CIL312 manufactured by Nippon Carlit Co., Ltd., 1-butyl-3-methylpyridine A pressure-sensitive adhesive sheet 9 including an antiglare film / pressure-sensitive adhesive layer 9 / release liner was obtained in the same manner as in Example 1 except that 0.1 parts by mass of bis(trifluoromethylsulfonyl)imide was added.
[0435] <Comparative Example 2>
[0436] A pressure-sensitive adhesive sheet 10 including an antiglare film / pressure-sensitive adhesive layer 10 / release liner was obtained in the same manner as in Example 1 except that 3 parts by mass of bis(trifluoromethylsulfonyl)imide (trade name "LiTFSI" manufactured by Mitsubishi Materials Electronic Chemicals Co., Ltd.) was used as a solid antistatic agent.
[0437] <Comparative Example 3>
[0438] As the liquid antistatic agent, Mitsubishi Materials Electronic Chemicals Co., Ltd., trade name "EMIN441", 1-ethyl-3-methylimidazole A pressure-sensitive adhesive sheet 11 including an antiglare film / pressure-sensitive adhesive layer 11 / release liner was obtained in the same manner as in Example 3 except that 3 parts by mass of bis(nonafluorobutylsulfonyl)imide was used.
[0439] (evaluate)
[0440] The following evaluations were performed using the PSA sheets obtained in the above Examples and Comparative Examples. The evaluation methods are as follows. The results are shown in Table 2.
[0441] (1) Determination of surface resistance
[0442] The release liner was peeled off from the adhesive sheet obtained in the above-mentioned Examples and Comparative Examples, and the surface resistance value was measured under the conditions of a temperature of 23° C. and a relative humidity of 50% by using a resistivity meter (“Model 152-1” manufactured by TREK) and bringing a probe (“Model 152P-2P” manufactured by TREK) into contact with the adhesive surface, and applying a voltage of 100 V for 10 seconds.
[0443] (2) Determination of surface resistance after thermal shock test
[0444] After the PSA sheet was removed from the heat shock test described below, it was left to stand in an environment of a temperature of 23° C. and a relative humidity of 50% for more than 2 hours, and the surface resistance value was measured using a resistivity meter (“Model 152-1” manufactured by TREK) by bringing a probe (“Model 152P-2P” manufactured by TREK) into contact with the PSA surface from which the release liner had been peeled off, under the conditions of an applied voltage of 100 V and a voltage application time of 10 seconds.
[0445] Thermal shock test
[0446] The PSA sheets obtained in Examples and Comparative Examples were subjected to 200 cycles of exposure to -40°C atmosphere for 30 minutes and then to 80°C atmosphere for 30 minutes using a thermal shock tester.
[0447] The absolute value of the difference in surface resistance value of the adhesive layer before and after the heat shock test was calculated according to the following formula.
[0448] |Log 10 B-Log 10 A|
[0449] A: Surface resistance value before thermal shock test
[0450] B: Surface resistance value after thermal shock test
[0451] (3) Measurement of Hardness of Adhesive Layer by Nanoindentation Method
[0452] The adhesive layers of Examples and Comparative Examples were cut into approximately 1 cm squares and fixed to a support (slide glass, manufactured by Matsunami Glass Industries, Ltd.) as nanoindentation measurement samples. Nanoindentation measurement was performed under the following conditions to obtain load-displacement curves.
[0453] Nanoindentation measurement conditions
[0454] Device: Triboindenter manufactured by Hysitron Inc.
[0455] Use indenter: Berkovich (triangular pyramid)
[0456] Measurement method: Single indentation measurement
[0457] Measuring temperature: room temperature
[0458] Indentation depth: 100nm
[0459] The hardness H is determined by the load (maximum load P) when the indenter is pressed to the above-mentioned depth. max) and the contact area between the indenter and the sample at this time (contact projection area Ac) are calculated by the following formula (1).
[0460]
[0461] (4) Storage modulus and glass transition temperature of adhesive layer
[0462] The release liner was peeled off from the adhesive layer obtained in each embodiment and comparative example, and a plurality of adhesive layers were stacked to prepare a test sample with a thickness of about 2 mm. The test sample was punched into a disc with a diameter of 7.9 mm and sandwiched between parallel plates. The dynamic viscoelasticity was measured under the following conditions using the "Advanced Rheological Expansion System (ARES)" manufactured by Rheometric Scientific, and the storage modulus G' at 25°C and 85°C was read from the measurement results. In addition, the temperature at which tanδ is maximum is taken as the glass transition temperature of the adhesive layer.
[0463] (Measurement conditions)
[0464] Deformation mode: Twist
[0465] Measuring frequency: 1Hz
[0466] Measuring temperature: -70℃~150℃
[0467] (5) 300% tensile residual stress value of adhesive layer
[0468] The adhesive layer obtained in each embodiment and comparative example was cut into a size of 40 mm × 40 mm, and after peeling off the release liner on one side, it was folded once in a manner that the adhesive surfaces were bonded to each other, and the release liner on one side was peeled off again, and the adhesive surfaces were bonded to each other again, thereby preparing an adhesive layer sample with a size of about 10 mm × 40 mm and a thickness of about 400 μm. The above-mentioned adhesive layer sample was set in a tensile testing machine with a chuck spacing set to 20 mm, and stretched 60 mm (300%) at a stretching speed of 200 mm / min (the chuck spacing after stretching was 80 mm). The position stretched by 60 mm was fixed and maintained for 300 seconds, and the stress value thereafter was measured, and the "300% tensile residual stress value" was calculated by the following formula.
[0469] 300% tensile residual stress value (N / cm 2 ) = stress value after 300 seconds of fixation (N) / (4 × adhesive sheet thickness (mm) / 10)
[0470] (6) Haze
[0471] The pressure-sensitive adhesive sheets obtained in each example and each comparative example were measured at room temperature (23° C.) using a haze measuring device (HR-100 manufactured by Murakami Color Laboratory). The measurement was repeated three times, and the average value was used as the measured value.
[0472] (7) Haze after thermal shock test
[0473] The PSA sheets obtained in each example and each comparative example were subjected to the above-mentioned heat shock test and then measured at room temperature (23° C.) using a haze meter (HR-100 manufactured by Murakami Color Laboratory). The test was repeated three times and the average value was taken as the measured value.
[0474] The difference in haze before and after the heat shock test (haze after the heat shock test - haze before the heat shock test) was calculated.
[0475] (8) Visible light transmittance
[0476] The pressure-sensitive adhesive sheets obtained in each example and each comparative example were measured at room temperature (23° C.) using a haze meter (HR-100 manufactured by Murakami Color Laboratory). The measurement was repeated three times, and the average value was used as the measured value.
[0477] (9)L * a * b * Color system
[0478] The adhesive sheets obtained in each example and comparative example were attached to a slide glass (trade name "MICRO SLIDEGLASS", white polish, No. 2, thickness: 1.0 mm to 1.2 mm, manufactured by Matsunami Glass Co., Ltd.) to prepare test pieces. It should be noted that when attaching the adhesive sheet, a manual roller was used to avoid dirt such as fingerprints on the surface and to prevent foreign matter and air bubbles from entering.
[0479] The L of the test piece was measured using a simple spectrophotometer (trade name "DOT-3C", manufactured by Murakami Color Research Laboratory Co., Ltd.). * Value, b * Value and a * It should be noted that the measurement was performed by irradiating the adhesive sheet surface of the test piece with light.
[0480] L * Value, b * Value and a * The values are based on JIS Z8781-4 (2013).
[0481] About b after thermal shock test *After the test piece prepared as described above was subjected to the above-mentioned heat shock test, it was placed in an environment with a temperature of 23°C and a relative humidity of 50% for more than 2 hours, and measured using a simple spectrophotometer (trade name "DOT-3C", manufactured by Murakami Color Research Laboratory Co., Ltd.). * Subtract b before thermal shock test * The difference is taken as b after the thermal shock test. * The difference (Δb * ).
[0482] (10) Adhesion and peeling charge to acrylic sheet
[0483] [Measurement method of adhesive strength to acrylic sheet]
[0484] As the adherend, an acrylic plate with a width of 70 mm and a length of 100 mm (manufactured by Mitsubishi Rayon Co., Ltd., trade name "ACRYLITE", thickness: 1 mm) was prepared. The adhesive sheet obtained in each embodiment and comparative example was cut into a size of 25 mm wide and 100 mm long, and its adhesive surface was crimped to the above-mentioned acrylic plate at a pressure of 0.25 MPa and a speed of 0.3 m / min. After it was attached and placed for 30 minutes under an environment of 23°C and 50% RH, a universal tensile testing machine was used under the same environment to peel off the adhesive sheet from the above-mentioned acrylic plate at a peeling speed of 300 mm / min and a peeling angle of 180°, and the adhesive force [N / 25mm] at this time was measured.
[0485] [Measurement method of peeling charge]
[0486] The adhesive sheet obtained in each example and comparative example was cut into a size of 25 mm in width and 80 mm in length, and after peeling off the release liner, it was attached to an acrylic plate (manufactured by Mitsubishi Rayon Co., Ltd., trade name "ACRYLITE", thickness: 1 mm, width: 25 mm, length: 70 mm) that had been previously destaticized, and one end of the adhesive sheet was made to protrude 10 mm from the end of the acrylic plate, and was crimped with a hand roller.
[0487] After the sample was placed in an environment of 23°C / 50%RH for 1 day, it was set at a position of a sample fixing table with a height of 20mm. The end of the adhesive sheet protruding 10mm from the acrylic plate was fixed to an automatic winder and peeled at a peeling angle of 150° and a peeling speed of 5m / min. For the potential on the surface of the adherend (acrylic plate) generated at this time, the peeling voltage was measured by a potential meter (manufactured by Kasuga Electric Co., Ltd., model "KSD-0103") fixed at a height of 100mm from the center of the acrylic plate. The measurement was carried out in an environment of 23°C and 50%RH.
[0488] (11) Evaluation of adhesion to adherends (adhesion difference absorption)
[0489] For the adhesive sheets obtained in each embodiment and comparative example, the adhesion (height difference absorption) was investigated using so-called printed glass. On the surface of the printed glass used, a printed layer with a printing height difference of 15 μm relative to the glass surface was patterned, and the adhesive sheet was attached to the printed pattern-forming surface of such printed glass using a manual roller at room temperature. Then, in the adhesive sheet attached to the printed glass, if no ridge with a width of more than 1 mm was generated along the edge of the printed pattern on the glass surface (the portion with printed height difference), it was evaluated as good adhesion (○), and if such a ridge with a width of more than 1 mm was generated, it was evaluated as poor adhesion (×).
[0490] (12) Evaluation of voids after thermal shock test
[0491] In the same manner as the above-mentioned evaluation of adhesion, a test piece was prepared by attaching the adhesive sheet to the printed glass with a manual roller. After the prepared test piece was subjected to the above-mentioned heat shock test, it was placed in an environment of a temperature of 23°C and a relative humidity of 50% for more than 2 hours, and visually confirmed whether there were gaps in the printed height difference portion. In the adhesive sheet attached to the printed glass, if no ridge with a width of more than 1 mm was generated along the edge of the printed pattern on the glass surface (the portion with printed height difference), it was evaluated as good adhesion (○), and if such a ridge with a width of more than 1 mm was generated, it was evaluated as poor adhesion (×).
[0492]
[0493] Modifications of the present invention will be described below.
[0494] [Supplementary Note 1] An optical adhesive sheet, wherein the optical adhesive sheet has a laminated structure in which a substrate and an adhesive layer are laminated, the substrate has a first surface and a second surface, the adhesive layer is laminated on the first surface of the substrate, characterized in that the adhesive layer contains a liquid antistatic agent, and the surface resistance value of the adhesive layer is less than 10 10 Ω, and the haze of the optical pressure-sensitive adhesive sheet after the following heat shock test is 1% or less.
[0495] Thermal shock test
[0496] The optical pressure-sensitive adhesive sheet was subjected to 200 cycles of exposure to an atmosphere of −40° C. for 30 minutes and then to an atmosphere of 80° C. for 30 minutes using a heat shock tester.
[0497] [Supplementary Note 2] The optical pressure-sensitive adhesive sheet according to Supplementary Note 1, wherein the antistatic agent is an ionic liquid.
[0498] [Supplementary Note 3] The optical pressure-sensitive adhesive sheet according to Supplementary Note 2, wherein the ionic liquid contains an anion portion having 10 or less fluorine atoms.
[0499] [Appendix 4] An optical adhesive sheet as described in any one of Appendices 1 to 3, wherein the difference in haze of the optical adhesive sheet before and after the heat shock test (haze of the optical adhesive sheet after the heat shock test - haze of the optical adhesive sheet before the heat shock test) is 2% or less.
[0500] [Supplementary Note 5] The optical adhesive sheet according to any one of Supplementary Notes 1 to 4, wherein the absolute value of the difference in surface resistance value of the adhesive layer represented by the following formula before and after the heat shock test is 1 logΩ or less,
[0501] |Log 10 B-Log 10 A|
[0502] A: Surface resistance value before thermal shock test
[0503] B: Surface resistance value after thermal shock test.
[0504] [Appendix 6] The optical pressure-sensitive adhesive sheet according to any one of Appendices 1 to 5, wherein the second surface of the substrate is subjected to an anti-reflection treatment and / or an anti-glare treatment.
[0505] [Appendix 7] The optical pressure-sensitive adhesive sheet according to any one of Appendices 1 to 6, wherein the pressure-sensitive adhesive layer is an acrylic pressure-sensitive adhesive layer containing an acrylic polymer.
[0506] [Supplementary Note 8] An image display device, comprising laminating the optical pressure-sensitive adhesive sheet according to any one of Supplementary Notes 1 to 7 and an image display panel.
[0507] [Supplement 9] A spliced display, wherein the spliced display is formed by arranging a plurality of image display devices as described in Supplement 8.
[0508] Description of symbols
[0509] 10A, 10B Optical Adhesive Sheet
[0510] 1. Substrate
[0511] 1a The first side of the substrate
[0512] 1b The second side of the substrate
[0513] 2 adhesive layers
[0514] 3. Anti-reflection treatment and / or anti-glare treatment
[0515] 20 Image display device
[0516] 4 Image display panel
[0517] 30 splicing display
[0518] 31 Support substrate
Claims
1. An optical adhesive sheet, wherein: The optical adhesive sheet has a laminated structure in which a substrate and an adhesive layer are laminated, the substrate has a first surface and a second surface, and the adhesive layer is laminated on the first surface of the substrate, characterized in that: The adhesive layer contains a liquid antistatic agent, The surface resistance of the adhesive layer is less than 10 10 Ω, The haze of the optical pressure-sensitive adhesive sheet after the following heat shock test is 1% or less, Thermal shock test: The optical pressure-sensitive adhesive sheet was subjected to 200 cycles of exposure to an atmosphere of −40° C. for 30 minutes and then to an atmosphere of 80° C. for 30 minutes using a heat shock tester.
2. The optical pressure-sensitive adhesive sheet according to claim 1, wherein The antistatic agent is an ionic liquid.
3. The optical adhesive sheet according to claim 2, wherein The ionic liquid includes an anion portion having 10 or less fluorine atoms.
4. The optical pressure-sensitive adhesive sheet according to any one of claims 1 to 3, wherein The difference in haze of the optical pressure-sensitive adhesive sheet before and after the heat shock test (haze of the optical pressure-sensitive adhesive sheet after the heat shock test−haze of the optical pressure-sensitive adhesive sheet before the heat shock test) is 2% or less.
5. The optical pressure-sensitive adhesive sheet according to any one of claims 1 to 4, wherein The absolute value of the difference in surface resistance of the adhesive layer before and after the heat shock test represented by the following formula is 1 logΩ or less. |Log 10 B-Log 10 A| A: Surface resistance value before thermal shock test B: Surface resistance value after thermal shock test.
6. The optical pressure-sensitive adhesive sheet according to any one of claims 1 to 5, wherein The second surface of the substrate is subjected to anti-reflection treatment and / or anti-glare treatment.
7. The optical pressure-sensitive adhesive sheet according to any one of claims 1 to 6, wherein The adhesive layer is an acrylic adhesive layer containing an acrylic polymer.
8. An image display device, wherein: The image display device is formed by laminating the optical pressure-sensitive adhesive sheet according to any one of claims 1 to 7 and an image display panel.
9. A spliced display, wherein: The spliced display is formed by arranging a plurality of the image display devices according to claim 8 .