Continuous process for oxidative leaching of nickel

By controlling the acid concentration and temperature in the tower reactor, the problems of inconvenience and high cost in nickel sulfate production are solved, and efficient and high-purity nickel sulfate production are achieved, and conversion rate and capacity are maximized.

CN118946676APending Publication Date: 2024-11-12UMICORE(BE)
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380024512.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-03
Filing Date
2023-03-02
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing nickel sulfate manufacturing methods have problems such as inconvenient operation, high cost and unreacted fine metal entrainment, making it difficult to achieve high purity and high efficiency nickel sulfate production.

Method used

The consumption and temperature of acid concentration are controlled in the tower reactor through the oxidation leaching method to ensure the maximum conversion rate of nickel to nickel sulfate. The continuous flow conditions and a constant composition process are used to optimize the feeding method of sulfuric acid and hydrogen peroxide. , the acid ratio and flow rate are controlled to improve conversion efficiency.

Benefits of technology

The efficient production of high-purity nickel sulfate is achieved, which maximizes the capacity and conversion rate of the tower, reduces the entrainment of unreacted substances, and improves the economics of the process and the convenience of operation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
Patent Text Reader

Abstract

The present invention provides a method for producing a nickel sulfate solution in a tower reactor in which metal particles containing nickel are reacted with an oxidizing leach solution comprising sulfuric acid and hydrogen peroxide in water, and in which the acid in the oxidizing leach solution is substantially consumed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing nickel sulfate. Background Art

[0002] Secondary lithium-ion batteries (LIBs) have found widespread use in portable devices and electric vehicles, as well as in specialized aerospace applications. Important properties of reusable batteries include charge / discharge efficiency, cycle durability, energy density, and safety. Much development has focused on improving the performance of the cathode of LIBs.

[0003] In addition to lithium cobalt oxide, lithium manganese oxide and lithium iron phosphate, lithium nickel manganese cobalt oxide ("NMC", LiNi x Mn y Co z O2) and lithium nickel cobalt aluminum oxide ("NCA", LiNi x Co y Al z O2) have received a lot of attention due to their excellent properties. They can be easily obtained by mixing a suitable mixed metal precursor with a suitable lithium compound and subsequently heat treating the mixture. Further processing steps are widely reported, for example for doping with additional elements, providing surface coatings, improving crystallite size, etc.

[0004] The growing demand for electric vehicles (EVs) has led to an increased demand for high-purity nickel, especially high-purity nickel sulfate. In fact, nickel refining for the preparation of high-purity nickel is considered to be extremely important for the supply of battery materials in the next decade. Such nickel refining will require the realization of high capacity and high efficiency of the process to produce the required nickel sulfate in the required amount and high purity. Therefore, new methods need to be developed and optimized. Among other methods, oxidative leaching of Ni from high-purity nickel metal is considered to be one of the more promising routes.

[0005] The process of leaching Ni metal in sulfuric acid in the presence of hydrogen peroxide is carried out according to the following reaction:

[0006] Ni + H2O2 + H2SO4 -> NiSO4 + 2 H2O

[0007] This method is also known as oxidative leaching of Ni metal, which is a highly exothermic (-423 kJ / mol) process.

[0008] WO 2021 / 105 365 describes a method for producing nickel sulfate by leaching metal particles containing nickel in an aqueous sulfuric acid solution, the method comprising the following steps: - introducing metal particles into an aqueous sulfuric acid solution; - introducing an aqueous hydrogen peroxide solution into an aqueous sulfuric acid solution containing metal particles, wherein the aqueous hydrogen peroxide solution is gradually introduced into the aqueous sulfuric acid solution containing metal particles. However, new methods are needed to provide new methods that allow easy operation, high throughput and optimized use of reactants. JP 2011 / 126757 describes a method for producing an aqueous nickel sulfate solution with a low content of free sulfuric acid. The method includes filling a metallic nickel block into a metal dissolving tower, feeding heated sulfuric acid from the upper part of the metal dissolving tower, and feeding air or oxygen from the lower part of the metal dissolving tower. However, such methods may suffer from entrainment of unreacted metal fines in the resulting process output. Summary of the invention

[0009] The present invention provides a solution to at least one of the above problems by providing a method for oxidative leaching of Ni according to claim 1. Preferably, the method is carried out in a tower reactor under continuous flow conditions, wherein the acid concentration in the oxidative leaching solution is substantially consumed. More specifically, the acid in the oxidative leaching solution is consumed to such an extent that the temperature of the resulting nickel sulfate solution increases to a temperature just below the boiling point of the solution. The inventors have found that under such conditions, the conversion of Ni to nickel sulfate is maximized, and therefore the capacity of the tower is also maximized. The method of the present invention is schematically shown in Figure 1 middle. BRIEF DESCRIPTION OF THE DRAWINGS

[0010] By way of further instruction, the accompanying drawings are included to better understand the teachings of the present invention. The drawings are intended to aid in describing the present invention and are not intended to be limitations of the presently disclosed invention.

[0011] The drawings and symbols contained therein have meanings that are generally understood by a person of ordinary skill in the art to which the present invention belongs.

[0012] Figure 1 The process according to the invention is schematically shown in a column reactor.

[0013] Figure 2 The average acid concentration (x-axis, g / L sulfuric acid, calculated as C) at a constant volume flow rate through the column is shown. SA, i and C SA, o The dissolution rate of nickel in the oxidative leaching process according to the method of the present invention (Y-axis, kg / h) as a function of the average value of DETAILED DESCRIPTION

[0014] Unless otherwise defined, all terms (including technical and scientific terms) used to disclose the present invention have the meanings commonly understood by one of ordinary skill in the art to which the present invention belongs. By way of further guidance, term definitions are included to better understand the teachings of the present invention. As used herein, the following terms have the following meanings:

[0015] As used herein, "a", "an", and "the" refer to both singular and plural references unless the context clearly indicates otherwise. For example, "a compartment" refers to one or more than one compartment.

[0016] As used herein, "about" with respect to a measurable value (such as a parameter, amount, transient duration, etc.) is intended to encompass the specified value and variations of + / -20% or less, preferably + / -10% or less, more preferably + / -5% or less, even more preferably + / -1% or less, and still more preferably + / -0.1% or less from the specified value, as long as such variations are suitable for making in the disclosed invention. However, it is to be understood that the value to which the modifier "about" refers is itself also specifically disclosed.

[0017] As used herein, "comprising" and "consisting of" are synonymous with "including" or "containing", and are inclusive or open-ended terms that specify the presence of following materials, such as components, and do not exclude or preclude the presence of additional, unrecited components, features, elements, components, steps known in the art or disclosed herein.

[0018] Numerical ranges recited by endpoints include all values ​​and fractions contained within the range, as well as the recited endpoints. All percentages are understood to be weight percentages (abbreviated as "wt %") or volume percentages (abbreviated as "vol %"), unless otherwise defined or unless a different meaning is apparent to one skilled in the art from its use and in the context in which it is used.

[0019] In the context of the present invention, the term "continuous process" will be considered as such a process, wherein the solution produced has a substantially constant composition. Specifically, a continuous process is such a process, wherein the solution produced has a constant composition in the range considered to be normal process variations. In addition, it is envisioned that the liquid reagents fed into the reactor have a fixed composition under normal process conditions. More specifically, the solution produced has such a composition, wherein the concentration of each component is in the range of + / -20% or less, preferably + / -10% or less, more preferably + / -5% or less, even more preferably + / -3% or less of its average concentration. In a preferred embodiment, the invention provides a continuous process operating under steady state conditions.

[0020] Preferably, sulfuric acid and hydrogen peroxide are fed to the process according to the invention at substantially constant concentrations and flow rates. Ni metal may be fed to the process intermittently or gradually. Preferably, the invention provides a process, preferably a continuous process, wherein the bed volume of metal particles containing nickel is controlled in a tower reactor within the range of + / -20% or less, preferably + / -10% or less, more preferably + / -5% or less, even more preferably + / -3% or less of its average bed volume.

[0021] In the context of the present invention, the term "concentrated nickel sulfate solution" is considered to be synonymous with the term "nickel sulfate solution", which has a nickel content of at least 60g Ni / L, optionally containing additional contents, such as sulfuric acid in an amount of less than 30g / L H2SO4, preferably less than 20g / L, and more preferably less than 10g / L. Preferably, the nickel sulfate solution has a nickel content of at least 60g Ni / L, and preferably at least 80g Ni / L. The nickel sulfate solution preferably has a nickel sulfate content below the saturation point of nickel sulfate at processing temperature (i.e. at a temperature of about 90°C or about 95°C). Preferably, the Ni content of the nickel sulfate solution is between 80g Ni / L and 200g Ni / L, preferably between 90g Ni / L and 175g Ni / L, and more preferably between 100g Ni / L and 150g Ni / L. Preferably, the nickel sulfate solution obtained by the oxidative leaching reaction is a nickel sulfate solution having a nickel content between 110 g / L and 140 g / L, more preferably between 120 g / L and 140 g / L, and most preferably is a nickel sulfate solution having a nickel content of about 130 g / L.

[0022] In a first aspect, the present invention provides a method for preparing a nickel sulfate solution by oxidative leaching of metal particles containing nickel in a tower reactor. The tower reactor has a feed section located at the bottom of the reactor, an outflow or overflow section located at the upper or top end of the reactor, and a reaction section located between the feed section and the overflow section. The method comprises the following steps:

[0023] i. feeding nickel-containing metal particles into the reaction section of the tower reactor;

[0024] ii. feeding an oxidative leaching solution comprising sulfuric acid and hydrogen peroxide in water to the reaction section via the feed section, thereby contacting the oxidative leaching solution with the nickel-containing metal particles in the reaction section to obtain a residual amount of sulfuric acid (C SA,o ) nickel sulfate solution; and

[0025] iii. Discharging the nickel sulfate solution from the overflow section of the tower reactor.

[0026] Preferably, the method according to the first aspect of the present invention is a continuous method. Preferably, the method according to the first aspect of the present invention is applied to the preparation of a concentrated nickel sulfate solution. The method is generally carried out in a tower reactor under continuous flow conditions, and the acid in the oxidative leaching solution is substantially consumed after passing through the tower reactor. Specifically, step ii. and step iii. are generally carried out under continuous flow conditions, while step i. may be carried out under continuous flow conditions or may be carried out gradually or intermittently. More specifically, the acid in the oxidative leaching solution is consumed to the extent that the temperature of the obtained nickel sulfate solution is raised to a temperature just below the boiling point of the solution, and it is ensured that the capacity of the tower is maximized for the target acid concentration in the nickel sulfate solution at the top of the reactor. The inventors have found that under such conditions, the conversion of Ni to nickel sulfate is maximized, and therefore the capacity of the tower is also maximized.

[0027] The sulfuric acid concentration (C SA,o ) and the sulfuric acid concentration (C SA,i The consumption of sulfuric acid on the tower reactor is represented by the ratio of sulphuric acid to sulfuric acid. Within the scope of the present invention, the inventors propose to keep the ratio between 0.90 and 0.01, preferably between 0.80 and 0.01, and more preferably between 0.70 and 0.02. In the context of the present invention, this ratio is called the "acid ratio".

[0028] Figure 1 The process according to the invention is schematically shown in a column reactor.

[0029] The present inventors have found that the desired (ie sufficiently low) acid ratio can be controlled by maintaining a sufficiently low flow rate of the oxidizing leaching solution through the tower reactor.

[0030] The inventors have found that it is easier to control the process in the tower reactor at a lower flow rate of the oxidizing leaching solution through the tower reactor. Maintaining a sufficiently low flow rate of the oxidizing leaching solution results in consumption of sulfuric acid at the top of the tower reactor. Moreover, a sufficiently low flow rate of the oxidizing leaching solution to the tower reactor allows the leaching reaction to be controlled so that the temperature of the nickel sulfate solution at the top of the tower reactor remains below the boiling point of the solution, while the inlet temperature can be kept at a medium to low temperature. A sufficiently low flow rate allows the progress of the leaching reaction to be controlled to ensure complete consumption of the oxidant, and is preferably managed to cause the temperature at the top of the tower to be just below the boiling point of the solution. Importantly, the inventors recognize that operating the method in a tower reactor at a sufficiently low flow rate results in a higher average acid concentration in the tower reactor, and therefore Ni metal is converted to NiSO4 more quickly.

[0031] Figure 2 The average acid concentration (x-axis, g / L sulfuric acid, calculated as C) at a constant volume flow rate through the column is shown. SA, i and C SA, o The dissolution rate of nickel in the oxidative leaching process according to the method of the invention (Y axis, kg / h) as a function of the average value of the column. The results show that the nickel dissolution rate increases with the average acid concentration in the column. The maximum capacity of the continuous process can be obtained at the maximum consumption of acid in the column, provided that the temperature at the top of the column reactor is controlled to a temperature below the boiling point of the nickel sulfate solution.

[0032] On the other hand, processes operating with a higher ratio of the sulfuric acid concentration of the nickel sulfate solution obtained in step ii. to the sulfuric acid concentration of the oxidative leaching solution, such as a ratio between 0.95 and 1.0, operate at higher flow rates, which inevitably results in lower average acid concentrations in the reaction zone. As a result, such processes experience slower conversion of Ni metal to NiSO4, and lower capacity.

[0033] In a preferred embodiment, the present invention provides a method according to the first aspect, wherein on a macroscopic scale a ID flow profile is maintained throughout the column.

[0034] In a preferred embodiment, the present invention provides a method according to the first aspect, wherein the acid ratio, i.e. the sulfuric acid concentration (C SA,o ) and the sulfuric acid concentration (C SA,i ) is lower than 0.70, lower than 0.65, lower than 0.60, lower than 0.55 or even lower than 0.50. Preferably, the ratio is between 0.5 and 0.1. Preferably, the ratio is lower than 0.45 and even lower than 0.40. Preferably, the ratio is higher than 0.05. Most preferably, the ratio is about 0.10, about 0.15, about 0.20, about 0.25, 0.30, about 0.35 or any value therebetween.

[0035] In a preferred embodiment, the present invention provides a method according to the first aspect, wherein the acid concentration C SA, i and C SA, o The difference Δ ac is at least 5 g / L sulfuric acid and at most 80 g / L sulfuric acid, preferably at least 10 g / L sulfuric acid and at most 70 g / L sulfuric acid. Preferably, the difference in acid concentration Δ ac is at least 15 g / L or more preferably at least 20 g / L. Preferably, the difference in acid concentration Δ ac is at most 60 g / L or at most 50 g / L and more preferably at most 45 g / L. Most preferably, the difference in acid concentration Δ acAbout 15 g / L, 20 g / L, 25 g / L, 30 g / L, 35 g / L, 40 g / L or 45 g / L or any value therebetween.

[0036] In a preferred embodiment, the oxidative leaching process (i.e., the tower reactor) is controlled to ensure that the nickel sulfate solution obtained from the tower reactor has a residual sulfuric acid content (C 20) between 1 g / L and 20 g / L. SA,o ). Leaching to a lower residual sulfuric acid content ensures that sulfuric acid is used economically in the process. Preferably, the residual amount of sulfuric acid in the nickel sulfate solution is between 2 g / L and 15 g / L, more preferably between 2 g / L and 10 g / L, and most preferably the residual amount of sulfuric acid is about 2 g / L, 4 g / L, 6 g / L, 8 g / L or 10 g / L or any value therebetween.

[0037] In a preferred embodiment, the present invention provides a method according to the first aspect, wherein the oxidative leaching solution is fed to the reactor (i.e., the tower reactor) at a temperature above 20°C, preferably above 30°C, preferably above 40°C, and more preferably above 50°C. Specifically, the oxidative leaching solution is fed to the reactor at a temperature of 50°C to 85°C, preferably at a temperature between 65°C and 85°C, more preferably at a temperature of about 75°C. It is advantageous to provide a cooler oxidative leaching solution to the tower to allow a higher concentration of acid. This higher concentration of acid will allow a higher Ni conversion and therefore a higher process capacity. However, the inventors recognize that it is appropriate to maintain a sufficiently high temperature of the oxidative leaching solution entering the tower to ensure sufficiently fast reaction kinetics of the oxidative leaching reaction. The required temperature (e.g., 60°C) can be achieved by mixing sulfuric acid and / or hydrogen peroxide with a partially cooled fraction of the tower effluent at room temperature. In addition, maintaining a sufficiently high temperature allows an effective cooling operation of the effluent fraction. Feeding the oxidizing leaching solution at a lower temperature also ensures that decomposition of hydrogen peroxide in the feed solution is suppressed.

[0038] In a preferred embodiment, the present invention provides a method according to the first aspect, wherein the nickel sulfate solution is removed from the reactor at a temperature below the boiling temperature of the nickel sulfate solution, preferably at a temperature of 90° C. to 105° C., more preferably at a temperature between 95° C. and 100° C. Preferably, the nickel sulfate solution discharged from the reactor has a temperature of 95° C. to 99° C., such as 96° C., 97° C., 98° C. or 99° C.

[0039] In a preferred embodiment, the present invention provides a method according to the first aspect, wherein the first fraction φ1 of the nickel sulfate solution is cooled from a temperature above 90°C to a temperature below 85°C, and wherein the fraction φ1 is mixed with sulfuric acid and hydrogen peroxide in water to form an oxidizing leaching solution, which is then fed into the reactor. Preferably, the first fraction 1 is cooled from a temperature above 95°C to a temperature below 85°C, preferably to a temperature below 80°C, more preferably to a temperature below 75°C, and even more preferably to a temperature below 70°C, more preferably from a temperature above 97°C to a temperature below 85°C. Advantageously, the first fraction φ1 is cooled to a temperature above 50°C, preferably above 60°C, more preferably above 70°C.

[0040] The cooling can be carried out in a heat exchanger such as a plate heat exchanger, a shell and tube heat exchanger, or in a reactor with a cooling device. Preferably, the heat exchanger consists of a reactor with a cooling device. Such a reactor additionally allows buffering of a certain volume of the first fraction φ1. Alternatively, sulfuric acid and / or hydrogen peroxide can be preheated with heat recovered from the heat exchanger. Advantageously, the process conditions according to the process of the invention ensure that a constant nickel sulfate solution temperature is achieved at the top of the tower reactor, which allows a direct cooling process.

[0041] In a preferred embodiment, the present invention provides a method according to the first aspect, wherein the first fraction φ1 of the nickel sulfate solution is mixed with sulfuric acid and / or hydrogen peroxide to form an oxidative leaching solution, which is then fed into the reactor. In a preferred embodiment, the volume ratio of the first fraction φ1 to the total volume of the nickel sulfate solution is between 0.70 and 0.98, preferably between 0.75 and 0.95, more preferably between 0.80 and 0.93, and most preferably equal to 0.80, 0.82, 0.84, 0.86, 0.88, 0.90, 0.92 or any value therebetween.

[0042] In a preferred embodiment, the present invention provides a method according to the first aspect, wherein the heat recovered from the cooling step of the first fraction φ1 is at least partly used to heat the oxidative leaching solution and / or the contents of the reactor. Preferably, the heat is used to heat the oxidative leaching solution and / or the contents of the reactor to a temperature between 55°C and 85°C, preferably to a temperature between 60°C and 85°C, more preferably to a temperature between 65°C and 80°C, most preferably to a temperature of about 65°C.

[0043] In a preferred embodiment, the present invention provides a method according to the first aspect, wherein the second fraction φ2 of the nickel sulfate solution is subjected to a purification step to reduce the concentration of one or more impurities in the second fraction φ2, wherein the impurities comprise one or more selected from the list comprising Cu, Zn, Co, Mn, Fe, Al, F, C, Ca, Si, P, As, Cd, Sb and Mg. In a preferred embodiment, before subjecting the second fraction to a further purification step, a base is added to the second fraction φ2 of the nickel sulfate solution to react with the residual amount of sulfuric acid present in the nickel sulfate solution, wherein the base is selected from the group consisting of potassium hydroxide, potassium carbonate, nickel hydroxide, nickel carbonate, cobalt hydroxide, cobalt carbonate, manganese hydroxide, manganese carbonate, calcium hydroxide, calcium carbonate, sodium hydroxide, sodium carbonate, lithium hydroxide, lithium carbonate, magnesium oxide, magnesium hydroxide, magnesium carbonate, or a combination of two or more of the foregoing. Preferably, the base is added until the pH of the nickel sulfate solution is between 2 and 5, preferably between 2.5 and 4.5, more preferably between 3.0 and 4.0.

[0044] In a preferred embodiment, the present invention provides a method according to the first aspect, wherein the nickel-containing metal particles contain nickel in an amount of at least 97% by weight, preferably at least 98% by weight, more preferably at least 99% by weight, relative to the total weight of the metal particles. The metal particles may also contain up to 1% by weight of Co. Preferably, the metal particles contain Ni in an amount of at least 99.5% by weight. In the context of the present invention, the Ni metal feed preferably comprises high-purity Ni metal having a purity of typically 99.97+%, 99.98+% or even 99.99+%. The Ni metal may be fed into the reactor in the form of Ni cut cathode metal (chopped or cut full plate cathode metal obtained from an electrowinning process) of typically 1"×1", 2"×2" or 4"×4" in size; Ni metal rings; or Ni pellets, balls having a diameter of about 0.5 cm. The hydrogen peroxide used in the process is typically a 30 to 60 wt % solution in water, such as 50 wt %, and the sulfuric acid has a concentration of 78 to 98 wt % in water, preferably 98 wt % in water. Any water used in the process may be high purity water, such as demineralized water or reverse osmosis water.

[0045] In a preferred embodiment, the present invention provides a method according to the first aspect, wherein the oxidizing leaching solution comprises sulfuric acid in an amount of 10 g / L to 150 g / L, preferably in an amount of 15 g / L to 100 g / L. Preferably, the oxidizing leaching solution comprises sulfuric acid in an amount of 20 g / L to 80 g / L, more preferably in an amount of 20 g / L to 60 g / L.

[0046] In a preferred embodiment, the invention provides a method according to the first aspect, wherein the oxidizing leaching solution comprises hydrogen peroxide in an amount of 1 g / L to 50 g / L, preferably 1 g / L to 30 g / L, more preferably 5 g / L to 30 g / L. More preferably, the oxidizing leaching solution comprises hydrogen peroxide in an amount of 5 g / L to 20 g / L, more preferably in an amount of about 5 g / L to 12 g / L, even more preferably in an amount of about 7 g / L to 10 g / L.

[0047] In a first preferred embodiment, the present invention provides a method according to the first aspect, wherein hydrogen peroxide is present in the oxidizing leaching solution in a substoichiometric amount relative to the amount of sulfuric acid present in the oxidizing leaching solution fed to the tower reactor. For example, the oxidizing leaching solution may comprise 0.4 mol / L hydrogen peroxide and 0.5 mol / L sulfuric acid. Preferably, the molar ratio of hydrogen peroxide to sulfuric acid in the oxidizing leaching solution fed to the tower reactor is between 0.6 and 1.0, preferably between 0.8 and 1.0, and more preferably about 0.9. The method according to the present invention allows operation with substoichiometric amounts of hydrogen peroxide, wherein residual amounts of sulfuric acid are allowed in the nickel sulfate solution formed. In a second alternative embodiment, the present invention provides a method according to the first aspect, wherein sulfuric acid and hydrogen peroxide are present in the oxidizing leaching solution in stoichiometric amounts. Preferably, the molar ratio of sulfuric acid to hydrogen peroxide is between 1:1 and 1:1.2, more preferably between 1.0:1.0 and 1:1.1. Excess hydrogen peroxide supports further consumption of sulfuric acid. The excess hydrogen peroxide ensures that hydrogen peroxide is not the rate limiting factor of the process. The excess hydrogen peroxide can be recovered from the tower reactor effluent.

[0048] In a preferred embodiment, the present invention provides a method according to the first aspect, wherein the gas atmosphere in the overflow section of the tower reactor is circulated through a scrubber. Preferably, the scrubber is cooled. Preferably, the scrubber and the circulation reactor are integrated in a single unit. Preferably, the circulation reactor is maintained at a temperature between 50° C. and 90° C., preferably at a temperature of about 65° C. or about 85° C., more preferably at a temperature of about 75° C. Lower temperatures are beneficial to the efficiency of the scrubbing operation.

[0049] In a preferred embodiment, the present invention provides a method according to the first aspect, wherein the oxidizing leaching solution is contacted with the metal particles at atmospheric pressure (i.e. 1 bar) or at a reduced pressure of less than 0.5 bar, preferably less than 0.2 bar, more preferably less than 0.1 bar. Preferably, the oxidizing leaching solution is contacted with the metal particles under an atmosphere of oxygen, air or oxygen-enriched air. In another preferred embodiment, the gas atmosphere in the overflow section is flushed with an inert gas (such as N2). This allows the direct removal of hydrogen gas in the case of its formation in the tower reactor.

[0050] In another preferred embodiment, the present invention provides a process according to the first aspect, wherein the gaseous atmosphere in the overflow section is treated in a scrubber to remove water and any hydrogen that may have formed.

[0051] In a preferred embodiment, the present invention provides a process according to the first aspect, wherein the bed volume consisting of the metal particles in the tower reactor has a diameter D b and height H b , where the ratio H of the height to the diameter b :D b Between 0.8 and 5, preferably between 1 and 5. Preferably, the height and diameter of the bed volume remain substantially constant throughout the process.

[0052] The process of the present invention is carried out in a tower. In the context of the present invention, the term "column" is considered to be equivalent to the term "column reactor", "packed bed" or "packed bed reactor", "tower" or "tower reactor", and refers to a tower reactor of substantially cylindrical form having an inner diameter D and a height H. The tower reactor consists of a vertically arranged cylindrical tower and is arranged to operate without mechanical stirring, preferably in an upflow mode, i.e., the fluid flows from the bottom to the top of the tower. The tower reactor is also characterized by (i) a feed section located at the bottom of the cylindrical reactor, which is used to feed liquid reagents, such as an aqueous solution containing sulfuric acid and hydrogen peroxide; (ii) a top section or overflow section at the upper or top end of the tower reactor, on the opposite side of the feed section, characterized by being used to collect the effluent of the overflowing nickel sulfate solution; (iii) an intermediate section or a reaction section in the middle of the cylindrical reactor, where the leaching reaction is carried out. Metal particles containing nickel are preferably fed at the top of the reactor and can be dosed gradually or intermittently to form a bed of metal particles on the support in the tower reactor. The tower reactor preferably includes a support located above the feed section, which is used to load solid reagents such as Ni metal. The support consists of a carrier mesh for loading Ni metal. In addition, the tower reactor is preferably equipped with a device for feeding solid reagents (such as Ni metal) to the reaction zone of the tower reactor. In addition, the tower reactor is preferably also equipped with a device for radially and uniformly distributing the oxidizing leaching solution in the feed section of the tower reactor. Solid reagents can be dosed to the support by introducing Ni metal at the top of the reactor or at any position above the support. The overflow zone is equipped with an outlet to receive nickel sulfate solution via an overflow mechanism.

[0053] In a preferred embodiment, the present invention provides a method according to the first aspect of the invention, wherein the liquid volume consisting of the oxidative leaching solution in the tower reactor has a diameter D L and height H L , where the ratio H of the height to the diameter L :D L Between 1.0 and 10.0, preferably between 1.5 and 8.0, more preferably between 2.0 and 5.0, and most preferably about 2.0, 2.5, 3.0, 3.5, 4.0, 4.5 or 5.0 or any value therebetween. Suitable geometry of the liquid volume in the Taschini reactor, in particular a sufficiently high ratio H L :D LEnsure that 1-dimensional flow can be obtained throughout the tower; and that small metal particles produced by the reacting metal feed particles are not entrained upwards by the nickel sulfate solution produced by the oxidative leaching reaction, thereby entraining unreacted metal particles and thereby contaminating the resulting nickel sulfate solution and reducing the efficiency of the process.

[0054] In a preferred embodiment, the tower reactor is cylindrical in shape and has an inner diameter D and a height H, wherein the ratio of the height H to the diameter D is significantly higher than 1, such as between 1.0 and 10.0, preferably between 1.5 and 8.0, more preferably between 2.0 and 5.0, and most preferably about 2.0, 2.5, 3.0, 3.5, 4.0, 4.5 or 5.0 or any value therebetween. An appropriate geometry of the tower reactor, in particular a sufficiently high ratio H:D ensures that a 1-dimensional flow can be obtained throughout the tower.

[0055] In a preferred embodiment, the present invention provides a method according to the first aspect of the invention, wherein in step ii. the oxidative leaching solution comprising sulfuric acid and hydrogen peroxide in water is fed to the reaction section via the bottom section of the tower reactor, and wherein in step iii. the nickel sulfate solution is discharged from the reaction section via the top section of the tower reactor. Preferably, the metal particles are fed into the reaction zone via the top section of the tower reactor. The metal particles may be fed continuously or intermittently, preferably intermittently.

[0056] In a preferred embodiment, the reaction zone can also include a mechanical impeller, i.e., an impeller attached to a motor by means of a rod, for the purpose of mixing only liquid reagents. Alternatively, a static mixer is used. In a preferred embodiment, the reaction zone includes a plurality of vertical baffles, which are placed relative to each other in diameter and placed at a certain position between the inlet nozzle and the impeller, so that at least one baffle is placed on the end of the reactor wall that is opposite in diameter. In this embodiment, the impeller and the vertical baffle contribute to the microscopic horizontal mixing of the reactants. The impeller improves the reactor dynamics. The vertical baffles contribute to the maximum mixing of the reactants in the reaction zone. The placement of the vertical baffles ensures that the reaction is confined in the reaction zone and does not extend to the region above the reaction zone.

[0057] Preferably, the reactor has a calming zone above the reaction zone. The calming zone has a tubular structure having a constant cross section, preferably equal to the cross section of the reaction zone, or having a widened cross section, wherein the diameter of the cross section of the tubular structure is greater than the diameter of the cross section of the reaction zone. The calming zone is in fluid communication with the reaction zone, and has a reaction zone at its distal end, and an overflow zone at its proximal end. The function of the calming zone is to achieve non-turbulent liquid flow, wherein unreacted metal particles adapt to non-fluidized conditions. This allows unreacted or insufficiently reacted metal particles to return to the reaction zone. The calming zone may include a plurality of horizontal baffles placed in the center, proximal and distal portions of the calming zone. In this embodiment, at least two of the provided horizontal baffles may be downward baffles having a central flow hole suitable for slowing down the speed of the reactant mixture. In yet another embodiment, the central horizontal baffle provided is a conical baffle with annular flow. In this embodiment, the placement of the horizontal baffles creates a tortuous flow path that allows large sized particles to settle while allowing the upward flowing mixture to travel smoothly into the overflow area.

[0058] In a preferred embodiment, the overflow zone has a tubular structure having a cross section equal to that of the calm zone and the reaction zone and is placed at the proximal end of the reactor. The overflow zone is equipped with an outlet to receive the formed nickel sulfate solution.

[0059] Example

[0060] The following examples are intended to further illustrate the present invention but are not intended to limit the scope of the present invention.

[0061] Example 1

[0062] Figure 1 The process according to the invention is schematically shown in a column reactor.

[0063] The oxidative leaching solution is prepared by mixing an aqueous sulfuric acid solution A with a hydrogen peroxide solution P in water. Subsequently, the mixture is heated to about T by mixing with fraction φ1 of the effluent of the tower reactor. i = 60°C. The tower reactor has an inner diameter D and a height H, wherein the ratio H:D is about 2.35. The fraction φ1 is cooled from a temperature of about 98°C to a temperature of about 65°C before being mixed with sulfuric acid and hydrogen peroxide. The oxidizing leaching solution thus prepared has a temperature of about 60°C and has a sulfuric acid content of about 45 g / L, and is fed into the reaction zone of the tower reactor via the feed section.

[0064] The reaction zone includes a Ni metal cut cathode with a size of about 50 mm x 50 mm and a nickel content of 99.97%. Metal particles containing nickel are intermittently fed onto a carrier plate above the reactor feed section; Figure 1 The metal particle feed is omitted. Ni metal is provided in a bed having a bed volume characterized by a height and a diameter, wherein the ratio of the height to the diameter is about 3. Upon contact with sulfuric acid and hydrogen peroxide, a nickel sulfate solution N is formed having a residual amount of sulfuric acid C of about 7 g / L. SA, o The ratio of the concentration of sulfuric acid in the effluent to the concentration of sulfuric acid in the feed solution is about 0.15. Due to the exothermic nature of the reaction, the temperature of the nickel sulfate solution N at the top of the column is T o It is about 98°C.

[0065] The first fraction φ1 of the nickel sulfate solution N is cooled from a temperature of about 98° C. to a temperature of about 65° C. and subsequently mixed with a mixture of sulfuric acid A and hydrogen peroxide P in water. The second fraction φ2 of the nickel sulfate solution N is further treated to a pH of about 3.5 and subsequently treated to remove impurities. Gases that may have formed in the atmosphere at the top of the tower reactor are treated in a scrubbing unit.

[0066] Example 2

[0067] The oxidative leaching solution is prepared by mixing an aqueous sulfuric acid solution A with a hydrogen peroxide solution P in water. Subsequently, the mixture is heated to about T by mixing with fraction φ1 of the effluent of the tower reactor. i = 75°C. The tower reactor has an inner diameter D and a height H, wherein the ratio H:D is about 2.6. The fraction φ1 is cooled from a temperature of about 98°C to a temperature of about 75°C before being mixed with sulfuric acid and hydrogen peroxide. The oxidizing leaching solution thus prepared has a temperature of about 75°C and a sulfuric acid content of about 31 g / L, and is fed into the reaction zone of the tower reactor via the feed section.

[0068] The reaction zone includes a Ni metal cut cathode with a size of about 50 mm x 50 mm, a thickness of 13 mm and a nickel content of 99.97%. Metal particles containing nickel are intermittently fed onto a carrier plate above the reactor feed section; Figure 1 The metal particle feed is omitted. Ni metal is provided in a bed having a bed volume characterized by a height and a diameter, wherein the ratio of the height to the diameter is about 5. Upon contact with sulfuric acid and hydrogen peroxide, a nickel sulfate solution N is formed having a residual amount of sulfuric acid C of about 10 g / L. SA, o The ratio of the concentration of sulfuric acid in the effluent to the concentration of sulfuric acid in the feed solution is about 0.32. Due to the exothermic nature of the reaction, the temperature of the nickel sulfate solution N at the top of the column is T o It is about 98°C.

[0069] The first fraction φ1 of the nickel sulfate solution N is cooled from a temperature of about 98° C. to a temperature of about 75° C. and subsequently mixed with a mixture of sulfuric acid A and hydrogen peroxide P in water. The second fraction φ2 of the nickel sulfate solution N is further treated to remove impurities. Gases that may have formed in the atmosphere at the top of the tower reactor are treated in a scrubbing unit.

Claims

1. A method for preparing a nickel sulfate solution (N) by oxidative leaching of metal particles containing nickel in a tower reactor (R), the method The following steps are involved: i. feeding nickel-containing metal particles into the reaction section of the tower reactor; ii. feeding an oxidative leaching solution comprising sulfuric acid and hydrogen peroxide in water to the reaction section via a feed section, thereby contacting the oxidative leaching solution with the nickel-containing metal particles in the reaction section to obtain a residual amount of sulfuric acid (C SA,o ) nickel sulfate solution; and iii. discharging the nickel sulfate solution from the tower reactor, The sulfuric acid concentration (C SA,o ) and the sulfuric acid concentration of the oxidative leaching solution (C SA,i ) is between 0.90 and 0.

01.

2. The process according to claim 1, wherein in step ii. the oxidative leaching solution comprising sulfuric acid and hydrogen peroxide in water is fed to the reaction section via the bottom section of the tower reactor, and wherein in step iii. the nickel sulfate solution is discharged from the reaction section via the top section of the tower reactor.

3. The method according to claim 1 or 2, wherein the sulfuric acid concentration (C SA,o ) and the sulfuric acid concentration of the oxidative leaching solution (C SA,i ) ratio is between 0.70 and 0.

02.

4. The process according to any one of claims 1 to 3, wherein the liquid volume consisting of the oxidative leaching solution in the tower reactor has a diameter D L and height H L , where the ratio H of the height to the diameter L :D L Between 1.0 and 10.0, preferably between 1.5 and 8.

0.

5. The process according to any one of claims 1 to 4, wherein the oxidizing leaching solution is fed into the reactor at a temperature of 50 to 85°C.

6. The process according to any one of claims 1 to 5, wherein the nickel sulfate solution is removed from the reactor at a temperature of 90°C to 100°C.

7. The method according to any one of claims 1 to 6, wherein the first fraction of the nickel sulfate solution is 1 from a temperature above 90°C to a temperature below 85°C, and wherein the fraction φ 1 Mixed with sulfuric acid and / or hydrogen peroxide to form an oxidizing leaching solution which is then fed into the reactor.

8. The method according to any one of claims 1 to 7, wherein the first fraction of the nickel sulfate solution is 1 mixed with sulfuric acid and / or hydrogen peroxide to form an oxidative leaching solution which is then fed into the reactor wherein the first fraction φ 1 The volume ratio to the total volume of the nickel sulfate solution is between 0.70 and 0.

95.

9. The method according to claim 7 or 8, wherein the first fraction φ 1 The heat recovered from the cooling step is at least partly used to heat the oxidative leaching solution and / or the contents of the reactor.

10. The method according to any one of claims 1 to 9, wherein the second fraction of the nickel sulfate solution is 2 The second fraction was subjected to a purification step to reduce φ 2 The concentration of one or more impurities in the mixture, wherein the impurities include one or more selected from the list consisting of Cu, Zn, Co, Mn, Fe, Al, F, C, Ca, Si, P, As, Cd, Sb and Mg.

11. The method according to any one of claims 1 to 10, wherein the nickel-containing metal particles comprise nickel in an amount of at least 96% by weight relative to the total weight of the metal particles.

12. The method of any one of claims 1 to 11, wherein the oxidizing leaching solution comprises sulfuric acid in an amount of 20 g / L to 100 g / L.

13. The method of any one of claims 1 to 12, wherein the oxidizing leaching solution comprises hydrogen peroxide in an amount of 1.5 g / L to 30 g / L.

14. A process according to any one of claims 1 to 13, wherein hydrogen peroxide is present in the oxidative leaching solution in a substoichiometric amount relative to the amount of sulphuric acid present in the oxidative leaching solution fed to the tower reactor.

15. The process according to any one of claims 1 to 14, wherein the gas atmosphere in the overflow section of the tower reactor is circulated through a scrubber.

16. The method of any one of claims 1 to 15, wherein the oxidizing leaching solution is contacted with the metal particles at atmospheric pressure or at a reduced pressure of less than 0.2 atmospheres.

17. The process according to any one of claims 1 to 16, wherein the tower reactor is controlled to ensure that the nickel sulfate solution obtained from the tower reactor has a residual sulfuric acid content (C 20) between 1 g / L and 20 g / L. SA,o ).