Grain-oriented electrical steel sheet and method for forming insulating coating film

By forming a crystalline metal phosphate intermediate layer and a metal phosphate tension coating layer on the orientation electromagnetic steel plate, the problems of equipment limitation and poor workingability in the prior art are solved, and high adhesion, excellent magnetic characteristics and low cost are achieved Production improves the corrosion resistance and dissolution resistance of steel plates.

CN118946684APending Publication Date: 2024-11-12NIPPON STEEL CORPORATION
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202380030383.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-06
Filing Date
2023-04-06
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the prior art, when manufacturing an oriented electromagnetic steel plate without a forsterite film, there are problems of equipment limitation and poor workingability, and it is difficult to ensure excellent adhesion, tension and magnetic properties of the film, and at the same time, the cost is high.

Method used

An intermediate layer containing crystalline metal phosphate salt is formed on the surface of the oriented electromagnetic steel plate, and a tension coating layer of metal phosphate salt and silica is formed thereon. The dense film is ensured by specific processes such as pickling and surface adjustment. Combination and tension.

Benefits of technology

The production of an oriented electromagnetic steel plate without a forsterite film is realized, and it has excellent film adhesion, tension and magnetic properties, while reducing production costs and improving corrosion resistance and dissolution resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005059614390000201
    Figure BDA0005059614390000201
  • Figure BDA0005059614390000221
    Figure BDA0005059614390000221
  • Figure BDA0005059614390000251
    Figure BDA0005059614390000251
Patent Text Reader

Abstract

The grain-oriented electrical steel sheet has a base steel sheet and an insulating coating film formed on the surface of the base steel sheet, the insulating coating film has an intermediate layer formed on the base steel sheet side and containing a crystalline metal phosphate salt, and a tension coating film layer formed on the surface side of the insulating coating film, and the average thickness of the intermediate layer is 0.10-5.0 [mu] m. The coating area ratio of the intermediate layer with respect to the base steel sheet is 40-90%, the crystalline metal phosphate salt in the intermediate layer is one or more of zinc phosphate, manganese phosphate, iron phosphate, and zinc calcium phosphate, and the tension coating layer contains a metal phosphate salt and silica. The content of the silica in the tension coating layer is 20-60 mass%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a grain-oriented electrical steel sheet and a method for forming an insulating film.

[0002] This application claims priority based on Japanese Patent Application No. 2022-063398 filed in Japan on April 6, 2022, and the contents are incorporated herein by reference. Background Art

[0003] Grain-oriented electrical steel sheets are mainly used in transformers. Transformers are continuously excited for a long period of time from installation to disposal, and energy loss continues to occur. Therefore, the energy loss when magnetized with alternating current, that is, iron loss, becomes the main indicator for determining the performance of the transformer.

[0004] In order to reduce the iron loss of grain-oriented electrical steel sheets, various technologies have been developed from the following perspectives: (a) improving the {110} <001> (b) increasing the content of solid solution elements such as Si to increase the resistance of the steel sheet, or (c) reducing the thickness of the electromagnetic steel sheet.

[0005] In addition, applying tension to the steel sheet is effective in reducing iron loss. Forming a film of a material with a smaller thermal expansion coefficient than the steel sheet on the surface of the steel sheet at high temperature is an effective means for reducing iron loss. In the final annealing process of the electromagnetic steel sheet, the forsterite-based film (inorganic-based film) with excellent film adhesion generated by the reaction of the oxide on the surface of the steel sheet with the annealing separator is a film that can apply tension to the steel sheet.

[0006] For example, the method disclosed in Patent Document 1 of forming an insulating film by baking a coating liquid mainly composed of colloidal silica and phosphate onto the surface of a steel sheet is effective for reducing iron loss because it has a large effect of applying tension to the steel sheet. Therefore, it has become a common method for manufacturing grain-oriented electrical steel sheets to leave the forsterite-based film generated in the final annealing step and apply an insulating coating mainly composed of phosphate thereon.

[0007] However, in recent years, the demand for miniaturization and high performance of transformers has increased. In order to miniaturize the transformer, it is required that the oriented electromagnetic steel sheet has good iron loss even under high magnetic flux density, that is, excellent high magnetic field iron loss. At the same time, it has been clarified in recent years that forsterite-based films hinder the movement of magnetic domain walls and have an adverse effect on iron loss. In oriented electromagnetic steel sheets, the magnetic domain walls move and the magnetic domains change under an AC magnetic field. It is believed that the smooth and rapid movement of the magnetic domain walls is effective in reducing iron loss, but the forsterite-based film is a non-magnetic body and has a concave-convex structure at the steel plate / film interface. This concave-convex structure hinders the movement of the magnetic domain walls and thus has an adverse effect on iron loss.

[0008] Therefore, as a means of improving high magnetic field iron loss, the following technologies are being studied: a method of removing the inorganic film using mechanical means such as grinding or chemical means such as pickling, or a technology of preventing the formation of the inorganic film during high-temperature final annealing, thereby producing a oriented electromagnetic steel sheet without an inorganic film; a technology of making the surface of the steel sheet mirror-finished (in other words, a technology of magnetically smoothing the surface of the steel sheet).

[0009] As a technology for preventing the formation of inorganic coatings, for example, Patent Document 2 discloses the following technology: after the usual final annealing, pickling is performed to remove the surface formation, and then the surface of the steel sheet is made into a mirror state by chemical polishing or electrolytic polishing. It is found that by forming a tension-imparting insulating coating on the surface of the oriented electromagnetic steel sheet without an inorganic coating obtained by this known method, a better iron loss improvement effect can be obtained. In addition, depending on the difference in the tension-imparting insulating coating, in addition to improving the iron loss, various characteristics such as corrosion resistance, heat resistance, and sliding properties can be imparted.

[0010] However, the inorganic coating has the effect of exhibiting insulation and has the effect of serving as an intermediate layer to ensure adhesion when forming a tension coating (tension-imparting insulating coating). That is, since the inorganic coating is formed in a state of penetrating into the steel plate, it has excellent adhesion to the steel plate as a metal. Therefore, in the case where a tension-imparting coating (tension coating) having colloidal silica, phosphate, etc. as the main component is formed on the surface of the inorganic coating, the coating has excellent adhesion. On the other hand, generally, since it is difficult for metals to combine with oxides, it is difficult to ensure sufficient adhesion between the tension coating and the surface of the electromagnetic steel plate (parent steel plate) in the absence of an inorganic coating.

[0011] Therefore, when forming a tension coating on a grain-oriented electrical steel sheet having no inorganic coating, a study is underway to provide a layer that functions as an intermediate layer in place of the inorganic coating.

[0012] For example, Patent Document 3 discloses a technique in which a SiO2 layer is formed on the surface of a grain-oriented electrical steel sheet without an inorganic coating by annealing the sheet in a weakly reducing atmosphere, thereby selectively thermally oxidizing silicon that is necessarily contained in the silicon steel sheet, thereby forming a tension-imparting insulating coating. In addition, Patent Document 4 discloses a technique in which a SiO2 layer is formed on the surface of a grain-oriented electrical steel sheet without an inorganic coating by subjecting the sheet to an anodic electrolysis treatment in a silicate aqueous solution, thereby forming a tension-imparting insulating coating.

[0013] Furthermore, Patent Document 5 discloses a technique of ensuring the adhesion of a tension-applying insulating coating by applying a coating serving as an intermediate layer in advance when forming a tension-applying coating layer.

[0014] In addition, Patent Document 6 discloses a oriented electrical steel sheet comprising a base steel sheet and a tension-applying insulating coating, wherein the tension-applying insulating coating is present on the surface of the oriented electrical steel sheet, and an iron-based oxide layer having a thickness of 100 to 500 nm is present between the base steel sheet and the tension-applying insulating coating.

[0015] Prior art literature

[0016] Patent Literature

[0017] Patent Document 1: Japanese Patent Application Laid-Open No. 48-039338

[0018] Patent Document 2: Japanese Patent Application Laid-Open No. 49-96920

[0019] Patent Document 3: Japanese Patent Application Laid-Open No. 6-184762

[0020] Patent Document 4: Japanese Patent Application Laid-Open No. 11-209891

[0021] Patent Document 5: Japanese Patent Application Laid-Open No. 5-279747

[0022] Patent Document 6: Japanese Patent Application Publication No. 2020-111814 Summary of the invention

[0023] Problems to be solved by the invention

[0024] However, the technology disclosed in the above-mentioned Patent Document 3 requires annealing equipment capable of controlling the atmosphere in order to perform annealing in a weakly reducing atmosphere, which has a problem in terms of processing cost. In addition, in the technology disclosed in the above-mentioned Patent Document 4, in order to obtain a SiO2 layer having sufficient adhesion to the tension-imparting insulating film on the surface of the steel sheet by performing anodic electrolysis in a silicate aqueous solution, it is necessary to prepare a new electrolytic treatment equipment, which has a problem in terms of processing cost.

[0025] Furthermore, the technique disclosed in Patent Document 5 has a problem that a tension-applying insulating film having a large tension cannot be maintained with good adhesion.

[0026] Furthermore, the technology disclosed in Patent Document 6 adopts the following method to form an iron-based oxide layer: a grain-oriented electrical steel sheet that has been surface-treated at a steel sheet temperature of 700 to 900° C. for 5 to 60 seconds is subjected to a heat treatment in an atmosphere having an oxygen concentration of 1 to 21% by volume and a dew point of −20 to 30° C. Therefore, when a steel sheet having an inorganic coating is manufactured on the same production line, the atmosphere of the annealing furnace needs to be changed, which deteriorates the workability.

[0027] As described above, it is difficult to provide a grain-oriented electrical steel sheet having excellent film adhesion, high film tension, and excellent magnetic properties without forsterite-based film (inorganic film) under the premise of a method that does not deteriorate workability due to equipment limitations.

[0028] Therefore, the present invention aims to provide a grain-oriented electrical steel sheet which does not have a forsterite-based coating, has excellent coating adhesion, excellent coating tension, excellent magnetic properties, and has sufficient corrosion resistance and dissolution resistance. In addition, the present invention aims to provide a method for forming an insulating coating of such a grain-oriented electrical steel sheet.

[0029] Means used to solve problems

[0030] The present inventors have studied the above-mentioned problems and found that, in a grain-oriented electrical steel sheet having no forsterite-based film on the surface, an intermediate layer containing a crystalline metal phosphate is provided between a base steel sheet and a tension film, and the coverage area ratio of the intermediate layer relative to the base steel sheet is set within a predetermined range, thereby achieving sufficient corrosion resistance and dissolution resistance while improving film adhesion, film tension and magnetic properties.

[0031] The present invention is made based on the above-mentioned knowledge. The gist of the present invention is as follows.

[0032] [1] A grain-oriented electrical steel sheet according to one embodiment of the present invention comprises a base steel sheet and an insulating film formed on a surface of the base steel sheet, the insulating film comprising an intermediate layer formed on the base steel sheet side and comprising a crystalline metal phosphate, and a tension coating layer formed on the surface side of the insulating coating, the intermediate layer having an average thickness of 0.10 to 5.0 μm, a coverage area ratio of the intermediate layer relative to the base steel sheet of 40 to 90%, the crystalline metal phosphate in the intermediate layer being one or more of zinc phosphate, manganese phosphate, iron phosphate, and zinc calcium phosphate, the tension coating layer comprising a metal phosphate and silicon dioxide, and a content of the silicon dioxide in the tension coating layer being 20 to 60% by mass.

[0033] [2] A method for forming an insulating film according to another embodiment of the present invention is a method for forming the insulating film provided on the grain-oriented electrical steel sheet described in [1], the method comprising the following steps: a final annealing step, wherein an annealing separator containing 10 to 100 mass % of Al2O3 is applied to the steel sheet and dried, and then final annealing is performed; an annealing separator removal step, wherein the remaining annealing separator is removed from the steel sheet after the final annealing step; a light pickling step, wherein the steel sheet after the annealing separator removal step is pickled for 5 to 30 seconds with a mixed acid having a liquid temperature of 25 to 85°C, wherein the mixed acid is a mixture of one or more of sulfuric acid, phosphoric acid, and nitric acid, and has a concentration of 0.5 to 10 mass %; and a surface conditioning step, wherein the steel sheet after the light pickling step is treated with a titanium-based or zinc-based The steel sheet is immersed in a surface conditioning agent of a colloid or a microparticle emulsion of manganese phosphate at a liquid temperature of 25 to 50° C. for 10 to 60 seconds; an immersion step, wherein the steel sheet after the surface conditioning step is immersed in a treatment liquid containing 5 to 50% by mass of a metal phosphate at a liquid temperature of 20 to 85° C. for 5 to 50 seconds; a drying step, wherein the steel sheet after the immersion step is lifted from the treatment liquid, washed with water to remove the remaining treatment liquid, and then dried; and a tension coating layer forming step, wherein a coating liquid containing a metal phosphate and colloidal silica is applied to the steel sheet after the drying step and dried, and then maintained at a plate temperature of 700 to 950° C. for 10 to 50 seconds, the coating liquid containing the metal phosphate and the colloidal silica in an amount of 30 to 150 parts by mass relative to 100 parts by mass of the metal phosphate.

[0034] [3] According to the method for forming an insulating film described in [2], the annealing separator may further contain one or both of 5 to 90 mass % of MgO and 0.5 to 10.0 mass % of a chloride.

[0035] Effects of the Invention

[0036] According to the above aspect of the present invention, it is possible to provide a grain-oriented electrical steel sheet that does not have a forsterite-based coating, has excellent coating adhesion, excellent coating tension, and excellent magnetic properties. In addition, the grain-oriented electrical steel sheet has sufficient corrosion resistance and dissolution resistance. In addition, according to the present invention, it is possible to provide a method for forming an insulating coating of the grain-oriented electrical steel sheet. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 This is a diagram showing an example of a cross-sectional view of a grain-oriented electrical steel sheet according to the present embodiment. DETAILED DESCRIPTION

[0038] A grain-oriented electrical steel sheet according to one embodiment of the present invention (grain-oriented electrical steel sheet according to the present embodiment) and a method for manufacturing the grain-oriented electrical steel sheet according to the present embodiment including a method for forming an insulating film provided in the grain-oriented electrical steel sheet according to the present embodiment will be described.

[0039] First, the grain-oriented electrical steel sheet according to the present embodiment will be described.

[0040] The grain-oriented electrical steel sheet 100 of this embodiment is as follows Figure 1 As shown, there are a base steel plate 1 and an insulating film 2 formed on the surface of the base steel plate 1 , but there is no forsterite-based film on the surface of the base steel plate 1 .

[0041] The insulating film 2 includes a tension coating layer 22 formed on the surface side of the insulating film 2 (ie, the surface side of the grain-oriented electrical steel sheet 100 ), and an intermediate layer 21 formed on the base steel sheet 1 side and containing a crystalline metal phosphate. Figure 1 In the embodiment, the insulating film 2 is formed on both surfaces of the base steel plate 1, but may be formed on only one surface.

[0042] <Base Steel Plate>

[0043] (Chemical Composition)

[0044] A major feature of the grain-oriented electromagnetic steel sheet 100 of the present embodiment is the structure of the insulating film 2 formed on the surface of the base steel sheet 1. The base steel sheet 1 of the grain-oriented electromagnetic steel sheet 100 is not limited in its chemical composition and can be within the range of known grain-oriented electromagnetic steel sheets. For example, in order to obtain the characteristics generally required as a grain-oriented electromagnetic steel sheet, it is preferable to contain the following elements as chemical components. In the present embodiment, the % of the chemical component is mass % unless otherwise stated.

[0045] C: 0.010% or less

[0046] C (carbon) is an element that is effective in controlling the structure of the steel sheet in the process until the decarburization annealing process in the manufacturing process is completed. However, when the C content of the parent steel sheet of the finally obtained oriented electromagnetic steel sheet is greater than 0.010%, the magnetic properties of the oriented electromagnetic steel sheet are reduced. Therefore, in the parent steel sheet of the oriented electromagnetic steel sheet of the present embodiment, the C content is preferably set to 0.010% or less. The C content is more preferably 0.005% or less. The lower the C content, the more preferred it is, but even if the C content is reduced to less than 0.0001%, the effect of the structure control is saturated, which increases the manufacturing cost. Therefore, the C content can be set to 0.0001% or more.

[0047] Si: 2.50~4.00%

[0048] Si (silicon) is an element that increases the electrical resistance of oriented electrical steel sheets and improves iron loss characteristics. When the Si content is less than 2.50%, sufficient eddy current loss reduction effect cannot be obtained. Therefore, the Si content is preferably set to 2.50% or more. The Si content is more preferably 2.70% or more, and further preferably 3.00% or more.

[0049] On the other hand, when the Si content is greater than 4.00%, the grain-oriented electrical steel sheet becomes brittle and the passability is significantly deteriorated. In addition, the workability of the grain-oriented electrical steel sheet decreases, and the steel sheet breaks during rolling. Therefore, the Si content is preferably set to 4.00% or less. The Si content is more preferably 3.80% or less, and further preferably 3.70% or less.

[0050] Mn: 0.01~0.50%

[0051] Mn (manganese) is an element that combines with S to form MnS during the manufacturing process. This precipitate functions as an inhibitor (an inhibitor of normal grain growth), and secondary recrystallization occurs in the steel. Mn is an element that also improves the hot workability of steel. When the Mn content is less than 0.01%, the above-mentioned effect cannot be fully obtained. Therefore, the Mn content is preferably set to 0.01% or more. The Mn content is more preferably 0.02% or more.

[0052] On the other hand, when the Mn content exceeds 0.50%, secondary recrystallization does not occur, and the magnetic properties of the steel are reduced. Therefore, in the base steel sheet of the grain-oriented electrical steel sheet of the present embodiment, the Mn content is preferably set to 0.50% or less. The Mn content is more preferably 0.20% or less, and even more preferably 0.10% or less.

[0053] N: 0.010% or less

[0054] N (nitrogen) is an element that combines with Al in the manufacturing process to form AlN that functions as an inhibitor. However, when the N content is greater than 0.010%, an excessive amount of inhibitor will remain in the grain-oriented electrical steel sheet. In this case, the magnetic properties are reduced. Therefore, in the base steel sheet of the grain-oriented electrical steel sheet of the present embodiment, the N content is preferably set to 0.010% or less. The N content is more preferably 0.008% or less.

[0055] On the other hand, the lower limit of the N content is not particularly specified, but even if it is reduced to less than 0.001%, the manufacturing cost will increase unnecessarily. Therefore, the N content can be set to 0.001% or more.

[0056] sol.Al: 0.020% or less

[0057] Sol.Al (acid-soluble aluminum) is an element that combines with N to form AlN that functions as an inhibitor during the manufacturing process of the grain-oriented electrical steel sheet. However, when the sol.Al content of the base steel sheet is greater than 0.020%, the acid will leave an excessive amount of inhibitor in the base steel sheet. In this case, the magnetic properties are reduced. Therefore, in the base steel sheet of the grain-oriented electrical steel sheet of the present embodiment, the sol.Al content is preferably set to less than 0.020%. The sol.Al content is more preferably less than 0.010%, and further preferably less than 0.001%. The lower limit of the sol.Al content is not specifically specified, but even if it is reduced to less than 0.0001%, the manufacturing cost is increased unnecessarily. Therefore, the sol.Al content can be set to more than 0.0001%.

[0058] S: 0.010% or less

[0059] S (sulfur) is an element that combines with Mn in the manufacturing process to form MnS that functions as an inhibitor. However, when the S content is greater than 0.010%, the magnetic properties are reduced due to the residual inhibitor. Therefore, in the parent steel plate of the oriented electromagnetic steel sheet of the present embodiment, the S content is preferably set to 0.010% or less. The S content in the oriented electromagnetic steel sheet is more preferably as low as possible. For example, less than 0.001%. However, even if the S content in the oriented electromagnetic steel sheet is reduced to less than 0.0001%, the manufacturing cost is increased in vain. Therefore, the S content in the oriented electromagnetic steel sheet can be greater than 0.0001%.

[0060] Balance: Fe and impurities

[0061] The chemical composition of the base steel sheet of the grain-oriented electrical steel sheet of the present embodiment contains the above-mentioned elements, and the balance may be Fe and impurities. However, for the purpose of improving magnetic properties, Sn, Cu, Se, and Sb may be further contained within the ranges shown below. In addition, as elements other than these, for example, even if any one or two or more of W, Nb, Ti, Ni, Co, V, Cr, and Mo are contained in a total amount of 1.0% or less, it does not hinder the effect of the grain-oriented electrical steel sheet of the present embodiment.

[0062] Here, “impurities” refer to elements mixed from raw material ores, scraps, or the manufacturing environment when the base steel sheet is industrially manufactured, and refer to elements that are allowed to be contained in a content that does not adversely affect the function of the grain-oriented electrical steel sheet of the present embodiment.

[0063] Sn: 0~0.50%

[0064] Sn (tin) is an element that helps improve magnetic properties by controlling the primary recrystallization structure. To obtain the effect of improving magnetic properties, the Sn content is preferably set to 0.01% or more. The Sn content is more preferably 0.02% or more, and even more preferably 0.03% or more.

[0065] On the other hand, when the Sn content exceeds 0.50%, secondary recrystallization becomes unstable and magnetic properties deteriorate. Therefore, the Sn content is preferably set to 0.50% or less. The Sn content is more preferably set to 0.30% or less, and further preferably set to 0.10% or less.

[0066] Cu: 0~0.50%

[0067] Cu (copper) is an element that contributes to increasing the Goss orientation occupancy of the secondary recrystallization structure. To obtain the above effect, the Cu content is preferably set to 0.01% or more. The Cu content is more preferably 0.02% or more, and even more preferably 0.03% or more.

[0068] On the other hand, when the Cu content exceeds 0.50%, the steel sheet becomes brittle during hot rolling. Therefore, the Cu content of the base steel sheet of the grain-oriented electrical steel sheet of the present embodiment is preferably set to 0.50% or less. The Cu content is more preferably 0.30% or less, and even more preferably 0.10% or less.

[0069] Se: 0~0.020%

[0070] Se (selenium) is an element that has the effect of improving magnetic properties. When Se is contained, in order to exert the effect of improving magnetic properties well, the Se content is preferably set to 0.001% or more. The Se content is more preferably 0.003% or more, and further preferably 0.006% or more.

[0071] On the other hand, when the Se content exceeds 0.020%, the adhesion of the film deteriorates. Therefore, the Se content is preferably set to 0.020% or less. The Se content is more preferably set to 0.015% or less, and further preferably set to 0.010% or less.

[0072] Sb: 0~0.50%

[0073] Sb (antimony) is an element having an effect of improving magnetic properties. When Sb is contained, in order to exert the effect of improving magnetic properties well, the Sb content is preferably set to 0.005% or more. The Sb content is more preferably 0.01% or more, and further preferably 0.02% or more.

[0074] On the other hand, when the Sb content exceeds 0.50%, the adhesion of the film deteriorates significantly. Therefore, the Sb content is preferably set to 0.50% or less. The Sb content is more preferably set to 0.30% or less, and further preferably set to 0.10% or less.

[0075] As described above, the present embodiment exemplifies that the chemical composition of the base material steel sheet of the grain-oriented electrical steel sheet contains the above-mentioned elements, and the balance includes Fe and impurities.

[0076] The chemical composition of the parent steel plate of the oriented electromagnetic steel plate of the present embodiment can be measured using the well-known ICP emission spectrometry. However, when measuring, if an insulating film is formed on the surface, it is peeled off before measuring. As a stripping method, stripping can be performed by immersing in a high-concentration alkali solution (for example, a 30% sodium hydroxide solution heated to 85°C) for more than 20 minutes. Whether stripping has occurred can be determined visually. In the case of a small sample, stripping can be performed by surface grinding.

[0077] <Insulation coating>

[0078] The grain-oriented electrical steel sheet 100 of the present embodiment has an insulating film 2 formed on the surface of a base steel sheet 1. More specifically, since the grain-oriented electrical steel sheet 100 of the present embodiment does not have a forsterite-based film, the insulating film 2 is formed in contact with the base steel sheet 1.

[0079] The insulating coating 2 is formed of an intermediate layer 21 and a tension coating layer 22 in this order from the base steel plate 1 side.

[0080] (Middle layer)

[0081] The intermediate layer 21 contains a crystalline metal phosphate and is a layer (film) having an average thickness of 0.10 to 5.0 μm.

[0082] As described above, a grain-oriented electrical steel sheet generally has a forsterite-based film formed in the final annealing process and an insulating film (tension insulating film) formed thereon. However, in recent years, it has been found that the forsterite-based film hinders the movement of the magnetic domain wall and has an adverse effect on the iron loss. In order to further improve the magnetic properties, grain-oriented electrical steel sheets without a forsterite-based film are being studied. However, in the absence of a forsterite-based film, it is difficult to ensure sufficient adhesion between the tension film and the base steel sheet.

[0083] In the grain-oriented electrical steel sheet 100 of the present embodiment, the intermediate layer 21 including crystalline metal phosphate is formed between the base steel sheet 1 and the tension coating, so that the intermediate layer 21 improves the adhesion between the base steel sheet 1 and the tension coating layer 22 .

[0084] This is because, if the intermediate layer 21 contains a crystalline metal phosphate, the tension film formed thereon (which becomes the tension film layer 22 after formation) also contains the metal phosphate, and therefore the affinity is high, and the adhesion between the intermediate layer and the tension film layer is excellent. In addition, when the intermediate layer is formed by immersion in a treatment liquid containing a metal phosphate as described later, it can be formed on the surface of the base steel plate 1 by chemical reaction, and the adhesion between the intermediate layer 21 and the base steel plate 1 can also be ensured.

[0085] The above effect cannot be obtained when the intermediate layer 21 does not contain a crystalline metal phosphate. The ratio of the crystalline metal phosphate in the intermediate layer is preferably 80% by mass or more, and may be 100% by mass. As the metal phosphate, one or more of zinc phosphate, manganese phosphate, iron phosphate, and zinc calcium phosphate are used in terms of adhesion.

[0086] The intermediate layer may contain oxides and elements such as Fe and Si diffused from the base steel sheet as the balance of the metal phosphate.

[0087] When the average thickness of the intermediate layer 21 is less than 0.10 μm, the intermediate layer does not sufficiently improve the adhesion between the base steel sheet and the insulating film. On the other hand, when the average thickness of the intermediate layer exceeds 5.0 μm, the magnetic properties deteriorate significantly.

[0088] However, if the coverage area ratio of the intermediate layer to the base steel plate is less than 40%, a sufficient effect cannot be obtained. Therefore, the coverage area ratio is set to 40% or more.

[0089] On the other hand, if the intermediate layer is formed uniformly, the coverage area ratio may be 100%. In the case of a conventional formation method based on immersion, if the coverage area ratio exceeds 90%, the metal phosphate constituting the intermediate layer is locally stacked, and the intermediate layer becomes locally thick, which may deteriorate the magnetic properties of the obtained grain-oriented electrical steel sheet. Therefore, the coverage area ratio is set to 90% or less. Preferably, it is 85% or less.

[0090] (Tension film layer)

[0091] The grain-oriented electrical steel sheet 100 of the present embodiment has the tension coating layer 22 on the surface side of the insulating coating 2 by forming the tension coating on the surface of the intermediate layer 21 .

[0092] The tension coating layer 22 is not particularly limited as long as it can be used as an insulating coating of the grain-oriented electrical steel sheet, but from the viewpoint of adhesion with the intermediate layer 21 (adhesion with the base steel sheet 1 via the intermediate layer 21), the tension coating layer 22 contains a metal phosphate and silicon dioxide (colloidal silicon dioxide derived from the coating liquid) so that the silicon dioxide content is 20% by mass or more. On the other hand, if the silicon dioxide content of the tension coating layer 22 exceeds 60% by mass, it causes powdering, so it is set to 60% by mass or less.

[0093] The tension coating layer 22 preferably contains 70% by mass or more of the metal phosphate and silicon dioxide in total. The balance other than the metal phosphate and silicon dioxide may contain ceramic fine particles such as alumina and silicon nitride.

[0094] The thickness of the tension film layer 22 is not limited, but when the average thickness of the intermediate layer 21 is within the above range, the average thickness of the insulating film 2 (intermediate layer 21 + tension film layer 22) is preferably set to 2.0 to 10.0 μm. When the average thickness of the insulating film 2 is less than 2.0 μm, sufficient film tension cannot be obtained. In addition, the dissolution of phosphoric acid increases. In this case, it may cause stickiness and reduced corrosion resistance, and may sometimes cause film peeling. In addition, when the thickness of the insulating film 2 is greater than 10.0 μm, the space factor may sometimes decrease, causing the magnetic properties to deteriorate, or the adhesion may decrease due to cracks, or the corrosion resistance may decrease.

[0095] The thickness of the intermediate layer 21, the thickness of the tension coating layer 22, and the thickness of the insulating coating 2 are determined by the following method.

[0096] The average thickness is determined by observing the cross section of the sample with a scanning electron microscope and measuring the thickness at five or more points. During the measurement, the base steel plate 1 and the insulating film 2 can be distinguished by the reflection of the electron beam of the scanning electron microscope. In addition, the intermediate layer 21 and the tension film layer 22 in the insulating film 2 can be distinguished by the presence or absence of silicon derived from silicon dioxide (the tension film layer contains silicon dioxide as described above, but the intermediate layer does not substantially contain silicon dioxide).

[0097] Furthermore, the average thickness of the insulating film 2 can be obtained by adding the average thickness of the intermediate layer 21 and the average thickness of the tension film layer 22 .

[0098] The mass ratio of the metal phosphate and the type of the metal phosphate in the intermediate layer 21 and the tension coating layer 22 can be determined by the following method.

[0099] Similar to the method of measuring the thickness of the intermediate layer 21 and the tension coating layer 22 , the mass ratio of the metal phosphate and the type of the metal phosphate can be determined by using a scanning electron microscope and an energy dispersive element analyzer.

[0100] In addition, whether the metal phosphate of the intermediate layer 21 is a crystalline metal phosphate can be determined by X-ray crystal structure analysis. For example, by using an X-ray diffraction measurement device "SmartLab" manufactured by RIGAKU CORPORATION under the conditions of a Cu vacuum tube, a voltage of 40 kV, a current of 40 mA, and a 2θ of 5 to 90°, a crystalline metal phosphate can be identified.

[0101] The silica content of the tension coating layer 22 can be measured using a scanning electron microscope and an energy dispersive element analyzer.

[0102] The coverage area ratio of the intermediate layer is measured by the following method.

[0103] Before forming the surface tension film layer, or even after forming it, when it can be peeled off by mechanical grinding to expose the intermediate layer, the surface of the steel plate (the surface of the intermediate layer) is observed using an electron microscope, for example, at a magnification of 1000 times in an area of ​​100×100 μm or more, and the Si concentration is measured using EDS. The area ratio of the metal phosphate layer that does not contain silicon dioxide (Si concentration is 3 mass % or less) is measured, and the coating area ratio is calculated.

[0104] On the other hand, when a tension coating layer is formed and it is difficult to expose the intermediate layer, the surface of the base steel plate in a length range of 20 μm or more is observed with an electron microscope at a magnification of, for example, 5000 times for a cross section in the plate thickness direction of the surface layer portion of the grain-oriented electrical steel sheet, and the metal phosphate layer that does not contain silicon dioxide and is in contact with the metal surface (the surface of the base steel plate) is regarded as the intermediate layer. The length of the intermediate layer per unit measurement length is measured to calculate the coverage area ratio.

[0105] In any case, the coverage area ratio was calculated for five viewing fields and the average value was taken as the coverage area ratio.

[0106] <Manufacturing method>

[0107] The grain-oriented electromagnetic steel sheet of the present embodiment can be suitably manufactured by a manufacturing method that satisfies the manufacturing conditions described below. However, it is a matter of course that the grain-oriented electromagnetic steel sheet of the present embodiment is not limited to the manufacturing method. That is, the grain-oriented electromagnetic steel sheet having the above-mentioned structure is regarded as the grain-oriented electromagnetic steel sheet of the present embodiment regardless of its manufacturing conditions.

[0108] The grain-oriented electrical steel sheet of the present embodiment can be produced by a production method including the following steps:

[0109] (I) a hot rolling step, in which a steel slab having a predetermined chemical composition is hot rolled to obtain a hot-rolled sheet;

[0110] (II) a hot-rolled sheet annealing step, wherein the hot-rolled sheet is annealed;

[0111] (III) a cold rolling step, wherein the hot rolled sheet after annealing is cold rolled to obtain a steel sheet (cold rolled sheet);

[0112] (IV) a decarburization annealing step, wherein the steel sheet is subjected to decarburization annealing;

[0113] (V) a final annealing step, wherein the steel sheet after the decarburization annealing step is coated with an annealing separator containing 10 to 100 mass % of Al2O3 and dried, and then subjected to final annealing;

[0114] (VI) an annealing separator removal step, wherein the remaining annealing separator is removed from the steel sheet after the final annealing step;

[0115] (VII) a light pickling step, wherein the steel sheet after the annealing separator removal step is pickled for 5 to 30 seconds using a mixed acid having a liquid temperature of 25 to 85° C., wherein the mixed acid is a mixture of one or more of sulfuric acid, phosphoric acid, and nitric acid, and has a concentration of 0.5 to 10 mass %;

[0116] (VIII) a surface conditioning step, wherein the steel sheet after the light pickling step is immersed in a surface conditioning agent containing a titanium-based or zinc-based colloid or a fine-particle emulsion of manganese phosphate at a liquid temperature of 25 to 50° C. for 10 to 60 seconds;

[0117] (IX) an immersion step, wherein the steel sheet after the surface conditioning step is immersed in a treatment liquid containing 5 to 50% by mass of a metal phosphate at a liquid temperature of 20 to 85° C. for 5 to 50 seconds;

[0118] (X) a drying step, wherein the steel sheet after the immersion step is lifted out of the treatment liquid, washed with water to remove the remaining treatment liquid, and then dried; and

[0119] (XI) A tension coating layer forming step, wherein a coating liquid comprising a metal phosphate and colloidal silica is applied to the steel plate after the drying step and dried, and then maintained at a plate temperature of 700 to 950° C. for 10 to 50 seconds, wherein the coating liquid comprises 30 to 150 parts by mass of the colloidal silica relative to 100 parts by mass of the metal phosphate.

[0120] Furthermore, the method for producing a grain-oriented electrical steel sheet according to the present embodiment may further include any one or both of the following steps:

[0121] (XII) a nitriding treatment step, wherein the cold-rolled sheet is subjected to a nitriding treatment between the decarburization annealing step and the final annealing step; and

[0122] (XIII) A magnetic domain subdividing step of controlling the magnetic domains of the steel sheet after the tension coating layer forming step.

[0123] Among them, the production of the grain-oriented electrical steel sheet of the present embodiment is characterized by (V) final annealing step to (XI) tension coating layer forming step mainly related to the formation of the insulating coating, and other steps or conditions not described can adopt known conditions.

[0124] These steps are described below.

[0125] <Hot rolling process>

[0126] The hot rolling step heats a steel slab or other steel billet having a predetermined chemical composition and then hot-rolls the steel slab to obtain a hot-rolled sheet. The heating temperature of the steel billet is preferably set within a range of 1100 to 1450° C. The heating temperature is more preferably 1300 to 1400° C.

[0127] The chemical composition of the steel billet can be changed according to the chemical composition of the grain-oriented electrical steel sheet to be finally obtained. For example, the following chemical composition can be illustrated, which contains the following elements in mass %: C: 0.01-0.20%, Si: 2.50-4.00%, sol.Al: 0.010-0.040%, Mn: 0.01-0.50%, N: 0.020% or less, S: 0.005-0.040%, Cu: 0-0.50%, Sn: 0-0.50%, Se: 0-0.020%, Sb: 0-0.50%, and the balance includes Fe and impurities.

[0128] The hot rolling conditions are not particularly limited and may be appropriately set based on the required properties. The thickness of the hot-rolled sheet is preferably within a range of 2.0 mm to 3.0 mm, for example.

[0129] <Hot-rolled sheet annealing process>

[0130] The hot-rolled sheet annealing step is to anneal the hot-rolled sheet produced by the hot-rolling step. Such annealing treatment is preferred because it causes recrystallization in the steel sheet structure and enables good magnetic properties to be achieved.

[0131] When hot-rolled sheet annealing is performed, the hot-rolled sheet manufactured by the hot rolling process can be annealed according to a known method. During annealing, there is no particular limitation on the means of heating the hot-rolled sheet, and a known heating method can be used. In addition, there is no particular limitation on the annealing conditions. For example, the hot-rolled sheet can be annealed in a temperature range of 900 to 1200° C. for 10 seconds to 5 minutes.

[0132] <Cold rolling process>

[0133] The cold rolling process is to cold-roll the hot-rolled sheet after the hot-rolled sheet annealing process to obtain a steel sheet (cold-rolled sheet). The cold rolling may be a single cold rolling (a series of cold rolling without intermediate annealing), or the cold rolling may be interrupted before the final pass of the cold rolling process and intermediate annealing may be performed at least once or twice to perform multiple cold rollings with intermediate annealing.

[0134] When intermediate annealing is performed, it is preferably maintained at a temperature of 1000 to 1200° C. for 5 to 180 seconds. The annealing atmosphere is not particularly limited. In consideration of the manufacturing cost, the number of intermediate annealing is preferably within 3 times.

[0135] Furthermore, before the cold rolling step, the surface of the hot-rolled sheet may be pickled.

[0136] The cold rolling process of this embodiment is to cold roll the hot rolled sheet after the hot rolled sheet annealing process according to a known method to produce a cold rolled sheet. For example, the final reduction ratio can be set within the range of 80 to 95%. When the final reduction ratio is 80% or more, {110} <001> On the other hand, when the final reduction ratio exceeds 95%, the possibility of secondary recrystallization becoming unstable in the final annealing step to be performed later increases, which is not preferred.

[0137] The final reduction ratio refers to the cumulative reduction ratio of cold rolling, and when intermediate annealing is performed, it refers to the cumulative reduction ratio of cold rolling after the final intermediate annealing.

[0138] <Decarburization annealing process>

[0139] The decarburization annealing step decarburizes the obtained cold-rolled sheet. If the decarburization annealing can cause the cold-rolled sheet to undergo primary recrystallization and remove C from the steel sheet that has an adverse effect on the magnetic properties, the decarburization annealing conditions are not limited. For example, the oxidation degree (PH2O / PH2) in the annealing atmosphere (furnace atmosphere) is set to 0.3 to 0.6, and the annealing temperature is maintained at 800 to 900°C for 10 to 600 seconds.

[0140] <Nitriding treatment process>

[0141] A nitriding treatment may be performed between the decarburization annealing step and the final annealing step described later.

[0142] In the nitriding process, for example, the steel plate after the decarburization annealing process is maintained at about 700 to 850°C in a nitriding atmosphere (an atmosphere containing gases with nitriding potential such as hydrogen, nitrogen and ammonia). In the case of effectively utilizing AlN as an inhibitor, the nitrogen concentration of the steel plate treated by nitriding is preferably set to 40 ppm or more. On the other hand, in the case where the nitrogen concentration of the steel plate is greater than 1000 ppm, excessive AlN will also exist in the steel plate after the secondary recrystallization is completed in the final annealing. This AlN will cause iron loss degradation. Therefore, the nitrogen concentration of the steel plate after the nitriding process is preferably set to less than 1000 ppm.

[0143] <Final annealing process>

[0144] In the final annealing step, the steel sheet (cold-rolled sheet) that has undergone the decarburization annealing step or further undergone the nitriding treatment is coated with an annealing separator containing 10 to 100 mass % of Al2O3 and dried, and then the final annealing is performed.

[0145] In the conventional method for producing a grain-oriented electrical steel sheet, a forsterite-based film is formed on the surface of a steel sheet (cold-rolled sheet) by applying an annealing separator mainly composed of MgO and performing final annealing. In contrast, the method for producing a grain-oriented electrical steel sheet according to the present embodiment uses an annealing separator containing Al2O3 in order not to form a forsterite-based film.

[0146] On the other hand, the ratio of Al2O3 may be 100% by mass, but from the perspective of preventing Al2O3 from being baked to the surface of the steel sheet, in the method for manufacturing the grain-oriented electromagnetic steel sheet of this embodiment, MgO is preferably included in the annealing separator. MgO may be 0%, and in the case of obtaining the above-mentioned effect, the ratio of MgO is preferably set to 5% by mass or more. In the case of including MgO, in order to ensure 10% by mass or more of Al2O3, the ratio of MgO is set to 90% by mass or less. The ratio of MgO is preferably 50% by mass or less.

[0147] In addition, in the method for manufacturing the grain-oriented electrical steel sheet of the present embodiment, the annealing separator may further contain a chloride. By making the annealing separator contain a chloride, the effect of being less likely to form a forsterite-based film can be obtained. The content of the chloride is not particularly limited and may be 0%. In the case of obtaining the above-mentioned effect, it is preferably 0.5 to 10% by mass. As the chloride, for example, bismuth chloride, calcium chloride, cobalt chloride, iron chloride, nickel chloride, etc. are effective.

[0148] The final annealing conditions are not limited, and for example, a condition of maintaining the temperature at 1150 to 1250° C. for 10 to 60 hours may be adopted.

[0149] <Annealing separator removal step>

[0150] In the annealing separator removal step, the steel sheet after the final annealing step is washed with water to remove the remaining annealing separator.

[0151] <Light pickling process>

[0152] In the light pickling process, the steel sheet after the annealing separator removal process is pickled with a mixed acid obtained by mixing one or more of sulfuric acid, phosphoric acid, and nitric acid. During pickling, the concentration of the mixed acid is 0.5 to 10% by mass, the liquid temperature is 25 to 85°C, and the pickling time is 5 to 30 seconds. In this way, unnecessary substances on the surface of the steel sheet are removed and the surface is made active.

[0153] <Surface Conditioning Process>

[0154] In the surface conditioning step, the steel sheet after the light pickling step is immersed in a surface conditioning agent containing a titanium or zinc colloid or a microparticle emulsion of manganese phosphate at 25 to 50° C. for 10 to 60 seconds. This reduces the particle size of the crystalline metal phosphate and forms a dense intermediate layer, thereby increasing the coverage area ratio of the intermediate layer.

[0155] If the surface conditioner does not contain titanium or zinc colloids or manganese phosphate microparticle emulsion, the particle size of the crystalline metal phosphate may become coarse, the coverage area ratio of the intermediate layer may become small, and the adhesion of the film may be reduced. In addition, when the temperature of the surface conditioner is lower than 25°C, the adhesion may be deteriorated. In addition, when the temperature of the surface conditioner is higher than 50°C, the adhesion of the intermediate layer may be uneven.

[0156] If the immersion time is less than 10 seconds, the adhesion may be deteriorated, and if the immersion time is more than 60 seconds, the crystalline metal phosphate may grow in the thickness direction of the intermediate layer, making the intermediate layer too thick, or the coating area ratio may be too large, or the adhesion of the intermediate layer may be uneven.

[0157] <Immersion process>

[0158] <Drying process>

[0159] In the immersion process, the steel sheet after the surface conditioning process is immersed in a treatment liquid containing 5 to 50% by mass of a predetermined phosphate metal salt at a liquid temperature of 40 to 85°C for 5 to 25 seconds. Then, in the drying process, the steel sheet is lifted out of the treatment liquid, washed with water to remove the remaining treatment liquid, and then dried. Thus, an intermediate layer containing a crystalline phosphate metal salt is formed on the surface of the steel sheet (parent steel sheet).

[0160] When the liquid temperature is lower than 20°C or the immersion time is shorter than 5 seconds, an intermediate layer of sufficient thickness cannot be obtained. On the other hand, when the liquid temperature is higher than 85°C or the immersion time is longer than 50 seconds, the coverage area ratio becomes too large.

[0161] In addition, when the metal phosphate in the treatment solution is less than 5% by mass, the formation of the intermediate layer slows down, and the industrial cost increases. On the other hand, when the metal phosphate is greater than 50% by mass, the crystal grains become coarse, which sometimes causes the decrease in adhesion. As the metal phosphate contained in the treatment solution, one or more of zinc phosphate, manganese phosphate, and zinc calcium phosphate can be used.

[0162] <Tension film layer forming step>

[0163] In the tension film layer forming step, a coating liquid containing a phosphate metal salt and colloidal silica is applied to the steel plate after the drying step (a steel plate having an intermediate layer formed on a base steel plate), and after drying, the coating liquid is maintained at a plate temperature of 700 to 950° C. for 10 to 50 seconds to form a tension film. The layer formed by the tension film (tension film layer) and the intermediate layer constitute an insulating film.

[0164] When the plate temperature is less than 700°C, the tension becomes low and the magnetic properties deteriorate. Therefore, the plate temperature is preferably set to 700°C or higher. On the other hand, when the plate temperature is greater than 950°C, the rigidity of the steel plate decreases and it becomes easy to deform. In this case, the steel plate may be deformed due to transportation, etc., and the magnetic properties may deteriorate. Therefore, the plate temperature is preferably set to 950°C or lower.

[0165] In addition, when the holding time is less than 10 seconds, the dissolution resistance deteriorates. Therefore, the holding time is set to be more than 10 seconds. On the other hand, when the holding time is more than 50 seconds, the adhesion of the tension film layer deteriorates. Therefore, the holding time is preferably less than 50 seconds.

[0166] The coating liquid contains metal phosphate and colloidal silica in an amount of 30 to 150 parts by mass of colloidal silica relative to 100 parts by mass of the metal phosphate. As the metal phosphate, for example, one or a mixture of two or more selected from aluminum phosphate, zinc phosphate, manganese phosphate, magnesium phosphate, nickel phosphate, copper phosphate, lithium phosphate, cobalt phosphate, molybdenum phosphate, etc. can be used.

[0167] The coating liquid may contain vanadium, tungsten, molybdenum, zirconium or the like as an additional element.

[0168] Colloidal silica can be S-type or C-type. S-type colloidal silica refers to colloidal silica in which the silica solution is alkaline, and C-type colloidal silica refers to colloidal silica in which the surface of the silica particles is treated with aluminum and the silica solution is alkaline to neutral. S-type colloidal silica is generally widely used and is relatively cheap, but there is a risk of aggregation and precipitation when mixed with an acidic metal phosphate solution, so it is necessary to pay attention. C-type colloidal silica is stable even when mixed with a metal phosphate solution and there is no risk of precipitation, but the processing time is long and it is correspondingly more expensive. It is preferably used according to the stability of the coating solution to be prepared.

[0169] <Magnetic Domain Subdivision Process>

[0170] The method for producing a grain-oriented electrical steel sheet according to the present embodiment may further include a magnetic domain refining step of refining the magnetic domains of the steel sheet.

[0171] By performing the magnetic domain refining treatment, the iron loss of the grain-oriented electrical steel sheet can be further reduced.

[0172] As methods for magnetic domain subdivision, there are the following methods: a method of narrowing the width of the 180° magnetic domain (subdividing the 180° magnetic domain) by forming linear or dot-shaped grooves extending in a direction intersecting the rolling direction at prescribed intervals in the rolling direction; and a method of narrowing the width of the 180° magnetic domain (subdividing the 180° magnetic domain) by forming linear or dot-shaped stress strain portions and grooves extending in a direction intersecting the rolling direction at prescribed intervals in the rolling direction when the method is performed after the insulating film layer formation step.

[0173] When forming the stress strain portion, laser beam irradiation, electron beam irradiation, etc. can be applied. In addition, when forming the groove portion, a mechanical groove forming method based on gears, etc., a chemical groove forming method by electrolytic etching, and a thermal groove forming method based on laser irradiation can be applied.

[0174] When the insulating film is damaged due to the formation of the stress strain portion or the groove portion and the properties such as the insulating property are deteriorated, the insulating film can be formed again to repair the damage.

[0175] Example

[0176] A slab containing, by mass%, 0.08% C, 3.31% Si, 0.028% sol.Al, 0.008% N, 0.15% Mn, 0.007% S, and the balance being Fe and impurities was cast.

[0177] The slab was heated to 1350°C and then hot-rolled to produce a hot-rolled plate with a thickness of 2.2 mm.

[0178] The hot-rolled sheet was annealed at 1100° C. for 10 seconds (hot-rolled sheet annealing), and then cold-rolled until the sheet thickness became 0.22 mm to obtain a cold-rolled sheet.

[0179] The cold-rolled sheet was subjected to decarburization annealing at 830° C. for 90 seconds in an atmosphere with a (PH2O / PH2) ratio of 0.4.

[0180] Next, an annealing separator containing 50 mass % of Al 2 O 3 , 45 mass % of MgO and 5 mass % of bismuth chloride was applied to the cold-rolled sheet and dried, and then final annealing was performed at 1200° C. for 20 hours.

[0181] The steel sheet after the final annealing step was washed with water to remove the remaining annealing separator, and it was found that no forsterite-based film was formed on the surface of the steel sheet.

[0182] After removing the annealing separator, light pickling was performed under the conditions in Table 1.

[0183] After light pickling, the surfaces were adjusted by immersing the samples except for a part thereof in any one of the following adjusting agents 1 to 3 as shown in Table 1.

[0184] Adjuster 1: Liquid containing titanium colloid

[0185] Adjuster 2: Manganese phosphate microparticle emulsion

[0186] Regulator 3: Liquid containing zinc colloid

[0187] The steel sheet after surface conditioning (light pickling if no surface conditioning was performed) was immersed in a phosphate treatment solution containing a metal phosphate shown in Table 1, and then heated and dried to form an intermediate layer. The intermediate layer is shown in Table 1. The thickness of the intermediate layer was the average of the results of 10 measurements.

[0188] The results of X-ray crystal structure analysis showed that the metal phosphate salts of the intermediate layers of Intermediate Nos. 1 to 11 were all crystalline metal phosphate salts. The metal phosphate salt (magnesium phosphate) of Intermediate No. 12 was not a crystalline metal phosphate salt.

[0189]

[0190] The steel plates (intermediate No. 1 to 12) formed with the intermediate layer are cut into a plurality of pieces as required, and a coating liquid containing a phosphate metal salt and colloidal silica shown in Table 2 is applied to each steel plate, and baked in a drying furnace for the time shown in Table 2 in such a manner as to reach the plate temperature in Table 2, thereby forming a tension film layer on the surface. When vanadium, tungsten, molybdenum, and zirconium are contained in the coating liquid, they are added in the form of an oxygen-containing acid (V2O4, WO3, MoO3, ZrO2) at the molar ratio shown in Table 2. When forming, the thickness of the tension film layer is changed by changing the coating amount of the coating liquid. Alumina or silicon nitride is contained in a part of the coating liquid as the remainder.

[0191] In this way, steel sheets (grain-oriented electromagnetic steel sheets) Nos. 101 to 122 were manufactured.

[0192] For these steel sheets, the silica content and metal phosphate content of the tension coating layer and the thickness (average thickness) of the insulation coating were determined by the above-mentioned method. The thickness of the insulation coating was determined by averaging the results of 10 measurements.

[0193] The results are shown in Table 2.

[0194] Furthermore, the chemical composition of the base steel plate was investigated and found to be 3.30% Si, 0.001% C, less than 0.001% sol.Al, 0.001% N, 0.001% Mn, less than 0.0005% S, and the balance Fe and impurities.

[0195]

[0196] In addition, the adhesion of the insulating film, the film tension, the corrosion resistance, the dissolution resistance, and the magnetic properties of these steel sheets were determined by the methods described below.

[0197] [Adhesion]

[0198] Regarding the adhesion of the film, a sample with a width of 30 mm and a length of 300 mm was taken from the steel plate, and the sample was subjected to stress relief annealing at 800°C for 2 hours in a nitrogen flow, then wound around a 10 mmφ cylinder, unwound, and the degree of peeling (area ratio) of the film after a bending adhesion test was evaluated.

[0199] The following evaluation criteria were used, and in the case of ◎ or ○, it was determined that the film adhesion was excellent.

[0200] ◎: Peeling area ratio 0~0.5%

[0201] ○: The peeling area ratio is greater than 0.5% and less than 5.0%

[0202] △: The peeling area ratio is greater than 5.0% and less than 20%

[0203] ×: The peeling area ratio is greater than 20% and less than 50%

[0204] ××: The peeling area ratio is greater than 50%

[0205] [Film tension]

[0206] The film tension was calculated by back-calculating the sample from the steel plate based on the bending state after peeling off the insulating film on one side of the sample.

[0207] When the obtained film tension was 4.0 MPa or more, it was determined that the film tension was excellent.

[0208] [Corrosion resistance]

[0209] According to the salt spray test of JIS Z2371:2015, a 5% NaCl aqueous solution is naturally dropped on a sample in an atmosphere at 35°C for 7 hours.

[0210] Then, the rust area was evaluated using 10 points.

[0211] According to the following evaluation criteria, a score of 5 or more (5 to 10) was judged to be excellent in corrosion resistance.

[0212] 10: No rust

[0213] 9: Very little rust (area ratio less than 0.10%)

[0214] 8: The rust area ratio is greater than 0.10% and less than 0.25%

[0215] 7: The rust area ratio is greater than 0.25% and less than 0.50%

[0216] 6: The rust area ratio is greater than 0.50% and less than 1.0%

[0217] 5: The rust area ratio is greater than 1.0% and less than 2.5%

[0218] 4: The rust area ratio is greater than 2.5% and less than 5.0%

[0219] 3: The rust area ratio is greater than 5.0% and less than 10%

[0220] 2: The rust area ratio is greater than 10% and less than 25%

[0221] 1: The rust area ratio is greater than 25% and less than 50%

[0222] [Dissolution resistance]

[0223] A sample was taken from the obtained steel sheet, and the sample was boiled in boiling pure water for 10 minutes, and the amount of phosphoric acid eluted into the pure water was measured. The amount of phosphoric acid eluted was divided by the area of ​​the insulating film of the boiled grain-oriented electrical steel sheet to calculate the elution amount per unit area (mg / m 2 ), and the dissolution resistance was evaluated.

[0224] The amount of phosphoric acid eluted into pure water was determined by cooling the pure water (solution) in which phosphoric acid was eluted and then measuring the phosphoric acid concentration of a sample obtained by diluting the cooled solution with pure water by ICP-AES.

[0225] The dissolution amount per unit area is less than 40 mg / m 2 , it was judged that the dissolution resistance was excellent.

[0226] [Magnetic properties]

[0227] As magnetic properties, iron loss was evaluated. Specifically, the obtained steel sheets were subjected to irradiation at UA (irradiation energy density) of 2.0 mJ / mm 2 The magnetic domain was subdivided by irradiating a laser beam under the conditions of , and as magnetic properties, B8 (magnetic flux density at a magnetization intensity of 800 A / m) (not shown in the table) and W17 / 50 (magnetic flux density amplitude 1.7T, iron loss per unit mass at 50Hz) were measured. These characteristic values ​​were measured by the single sheet magnetic property measurement method (Single Sheet Tester: SST) based on JIS C2556:2015.

[0228] When the iron loss is 0.70 W / kg or less, it is judged that the magnetic properties are excellent.

[0229] [Table 3]

[0230]

[0231] As shown in Tables 1 to 3, No. 101 to 113 as inventive examples have a base steel plate and an insulating film formed on the surface of the base steel plate, and the insulating film has a predetermined intermediate layer and a tension film layer. As a result, the film adhesion, film tension, magnetic properties, corrosion resistance, and dissolution resistance are excellent.

[0232] On the other hand, No. 114 to 122 as comparative examples have poor coating adhesion, coating tension, magnetic properties, corrosion resistance, and dissolution resistance in at least one of the following: because the thickness or coverage of the intermediate layer is outside the scope of the present invention, the intermediate layer does not contain crystalline metal phosphate, or the silica content of the tension coating layer is outside the scope of the present invention.

[0233] Industrial Applicability

[0234] According to the present invention, a grain-oriented electrical steel sheet having no forsterite-based film, excellent film adhesion, excellent film tension, and excellent magnetic properties, and a method for forming an insulating film possessed by the grain-oriented electrical steel sheet can be provided. The grain-oriented electrical steel sheet has high industrial applicability because it has no forsterite-based film, excellent film adhesion, excellent film tension, and excellent magnetic properties, and also has sufficient corrosion resistance and dissolution resistance.

[0235] Explanation of symbols

[0236] 1. Base steel plate

[0237] 2Insulation film

[0238] 21 Middle Layer

[0239] 22 tension film layer

[0240] 100 Grain-Oriented Magnetic Steel Sheet

Claims

1. A grain-oriented electromagnetic steel sheet, characterized in that: It has: Base steel plate, and The insulating film formed on the surface of the base steel plate, The insulating film has: an intermediate layer formed on the base steel plate side and containing a crystalline metal phosphate, and A tension coating layer is formed on the surface side of the insulating coating, The average thickness of the intermediate layer is 0.10 to 5.0 μm. The coverage area ratio of the intermediate layer to the base steel plate is 40 to 90%. The crystalline metal phosphate of the intermediate layer is one or more of zinc phosphate, manganese phosphate, iron phosphate, and zinc calcium phosphate. The tension coating layer includes a metal phosphate and silicon dioxide, and a content of the silicon dioxide in the tension coating layer is 20 to 60% by mass.

2. A method for forming an insulating film, characterized in that: This is a method for forming the insulating film provided in the grain-oriented electrical steel sheet according to claim 1, The method comprises the following steps: A final annealing step, wherein the steel sheet is coated with an annealing separator containing 10 to 100 mass % of Al2O3 and dried, and then the final annealing is performed; an annealing separator removal step, wherein, for the steel sheet after the final annealing step, the remaining annealing separator is removed; A light pickling step, wherein the steel plate after the annealing separator removal step is pickled for 5 to 30 seconds with a mixed acid having a liquid temperature of 25 to 85° C., wherein the mixed acid is a mixture of one or more of sulfuric acid, phosphoric acid, and nitric acid, and has a concentration of 0.5 to 10 mass %; A surface conditioning step, wherein the steel sheet after the light pickling step is immersed in a surface conditioning agent containing a titanium-based or zinc-based colloid or a microparticle emulsion of manganese phosphate at a liquid temperature of 25 to 50° C. for 10 to 60 seconds; an immersion step, wherein the steel sheet after the surface conditioning step is immersed in a treatment liquid containing 5 to 50 mass % of a phosphate metal salt at a liquid temperature of 20 to 85° C. for 5 to 50 seconds; a drying step, wherein the steel sheet after the immersion step is lifted out of the treatment liquid, washed with water to remove the remaining treatment liquid, and then dried; and A tension coating layer forming step, wherein a coating liquid comprising a metal phosphate and colloidal silica is applied to the steel plate after the drying step and dried, and then maintained at a plate temperature of 700 to 950° C. for 10 to 50 seconds, wherein the coating liquid comprises the metal phosphate and colloidal silica in an amount of 30 to 150 parts by mass relative to 100 parts by mass of the metal phosphate.

3. The method for forming an insulating film according to claim 2, wherein: The annealing separator further includes one or two of 5 to 90 mass % of MgO and 0.5 to 10.0 mass % of chloride.

Citation Information

Patent Citations

  • Formation of insulating film on grain oriented electrical steel sheet

    JP1993279747A

  • Formation of insulated film on grain-oriented silicon steel sheet

    JP1994184762A

  • Formation of insulated film on silicon steel sheet

    JP1999209891A

  • Grain oriented electromagnetic steel sheet and method for manufacturing the same

    JP2020111814A