Separator and electrochemical conversion cell comprising same

By stacking hydrophilic or hydrophobic porous structural layers on the surface of the ion exchange membrane, the problem of drying and deformation of the anion exchange membrane at room temperature is solved, the mechanical characteristics and performance of the electrochemical conversion battery is improved, and efficient carbon dioxide conversion and stable voltage are ensured. .

CN118946689APending Publication Date: 2024-11-12LG CHEM LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202380031255.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-04-18
Filing Date
2023-04-19
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The anion exchange membrane is prone to drying and deforming at room temperature, resulting in a decrease in the mechanical properties and processability of the electrochemical conversion battery, affecting the stability and efficiency of the equipment.

Method used

A separator is designed to stack a porous structural layer with hydrophilic or hydrophobic properties on the surface of the ion exchange membrane to ensure that the ion exchange membrane retains a certain amount of moisture at room temperature and improves mechanical properties and moisture wetting.

Benefits of technology

By maintaining moisture wettability, the service life of the separator is extended, the carbon dioxide conversion rate, carbon monoxide Faraday efficiency and voltage performance of the electrochemical conversion battery are improved, and the processability of assembly at room temperature is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118946689A_ABST
    Figure CN118946689A_ABST
Patent Text Reader

Abstract

The present invention relates to a separator comprising a base membrane and a hydrophilic porous structure layer or a hydrophobic porous structure layer stacked on at least one side of the base membrane wherein the base membrane is an anion exchange membrane, a cation exchange membrane or an amphoteric ion exchange membrane.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the benefit of priority to Korean Patent Application No. 10-2022-0049687, filed on April 21, 2022, and Korean Patent Application No. 10-2023-0050853, filed on April 18, 2023, which are hereby incorporated by reference in their entirety. Technical Field

[0004] The present invention relates to a separator and an electrochemical conversion cell comprising the same. Background Art

[0005] Carbon dioxide is a greenhouse gas that contributes to global warming and therefore needs to be reduced. Carbon dioxide can be reduced by capture, chemical conversion or electrochemical conversion. In particular, electrochemical conversion can precisely control the composition so that other synthesis gas can be produced and thus can provide better economic benefits than removing carbon dioxide alone.

[0006] The process of electrochemical decomposition of carbon dioxide is similar to water electrolysis technology, but because the activity of the electrochemical reaction is greater in a strong alkaline atmosphere, a KOH aqueous solution with a certain concentration is usually used as an electrolyte. When an electric current is applied while water is supplied to the anode, the water is decomposed into hydrogen ions and electrons, and oxygen is generated at the same time. The electrons move to the cathode through the external conductor, and the hydrogen ions move to the cathode through the ion selective separator. At this time, the transferred electrons react with the carbon dioxide and water supplied to the cathode, decomposing into carbon monoxide and hydroxide ions (OH - ), and the generated hydroxide ions react with the hydrogen ions (H + ) reacts to generate water, thereby becoming electrically neutral. The above process completes the electrochemical decomposition reaction of carbon dioxide. In this case, in addition to the reaction that generates carbon monoxide, the water supplied together with carbon dioxide is electrolyzed by reacting with the transferred electrons to generate both hydrogen and hydroxide ions. The reaction between water and electrons is in a competitive reaction relationship with the reaction that generates carbon monoxide. The above reaction is an electrochemical reaction, and therefore the amount of carbon monoxide generated and the ratio of hydrogen / carbon dioxide can be easily controlled by voltage regulation.

[0007] Meanwhile, when using anion exchange membrane as ion selective separator, the electrolysis reaction of carbon dioxide can show excellent carbon dioxide conversion. However, there is usually the risk of anion exchange membrane being easily dried and deformed at room temperature, and in order to prevent this risk, anion exchange membrane can be stored in an environment with sufficient moisture. However, when anion exchange membrane is exposed to room temperature to assemble electrochemical conversion cell or stack at room temperature, anion exchange membrane may dry out and rupture or damage in a short time, and such low mechanical properties cause the processability of assembly work to reduce.

[0008] (Patent Document 1) KR 10-2019-0125822A Summary of the invention

[0009] Technical issues

[0010] One aspect of the present invention provides improved mechanical properties at room temperature by ensuring that a certain amount of moisture is constantly present in the separator.

[0011] That is, the present invention provides a separator and an electrochemical conversion cell including the same, wherein the separator is formed to have a structure in which a porous structure layer having hydrophilic or hydrophobic properties is stacked on the surface of an ion exchange membrane, and the ion exchange membrane in turn continuously retains a certain amount of moisture, thereby maintaining the performance of the ion exchange membrane at the same level and improving the mechanical properties at room temperature.

[0012] Technical Solution

[0013] The present invention provides a separator and an electrochemical conversion cell including the same.

[0014] (1) According to one aspect of the present invention, there is provided a separator comprising a base membrane and a hydrophilic porous structure layer or a hydrophobic porous structure layer stacked on at least one side of the base membrane, wherein the base membrane is an anion exchange membrane, a cation exchange membrane or a zwitterion exchange membrane.

[0015] (2) The present invention provides the separator according to (1) above, wherein the hydrophilic porous structure layer contains a hydrophilic polymer.

[0016] (3) The present invention provides the separator according to (1) or (2) above, wherein the hydrophilic porous structural layer is a polytetrafluoroethylene (PTFE) structural layer having a hydrophilically treated surface.

[0017] (4) The present invention provides the separator according to any one of (1) to (3) above, wherein the average pore diameter of the hydrophilic porous structure layer is 0.2 μm to 0.45 μm.

[0018] (5) The present invention provides the separator according to any one of (1) to (4) above, wherein the hydrophilic porous structure layer is stacked on either side of the base membrane.

[0019] (6) The present invention provides the separator according to any one of (1) to (5) above, wherein the separator does not contain a binder between the base membrane and the hydrophilic porous structure layer.

[0020] (7) The present invention provides a separator according to any one of (1) to (6) above, wherein the hydrophobic porous structure layer comprises at least one selected from the group consisting of PTFE, PVDF, nylon, cellulose acetate (CA) and polyethylene sulfide (PES).

[0021] (8) According to another aspect of the present invention, there is provided an electrochemical conversion cell comprising a cathode, an anode, an electrolyte, and a separator according to any one of (1) to (7) above, the separator being disposed between the cathode and the anode.

[0022] (9) The present invention provides the electrochemical conversion cell according to (8) above, wherein the electrochemical conversion cell converts carbon dioxide into carbon monoxide.

[0023] Beneficial Effects

[0024] The separator of the present invention forms a structure in which a porous structure layer having hydrophilic or hydrophobic properties is stacked on the surface of an ion exchange membrane and can maintain a certain level of moisture in the ion exchange membrane for a long time even at room temperature and can thus improve the mechanical properties of the exchange membrane.

[0025] Furthermore, according to the separator of the present invention, moisture wettability is maintained even at room temperature, thereby preventing the separator from drying out and being damaged or cracked, and thus, poor workability that may be caused by cracking when assembling a battery or a stack at room temperature can be improved.

[0026] In addition, the electrochemical conversion cell including the separator of the present invention includes a separator that can maintain moisture wettability even at room temperature and can thereby improve mechanical properties, and also has equivalent or higher levels in carbon monoxide Faraday efficiency, carbon dioxide conversion rate and voltage of the electrochemical conversion cell. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 A side view showing the structure of a separator according to the present invention;

[0028] Figure 2 This is an image showing the state of a typical anion exchange membrane after being exposed to room temperature atmosphere for 2 hours;

[0029] Figure 3 An image showing a state after the separator according to the present invention is exposed to the atmosphere at room temperature for 2 hours;

[0030] Figure 4 The carbon dioxide conversion rate, carbon monoxide Faraday efficiency and voltage of Examples 1 to 5 and Comparative Examples 1 and 2 are shown; and

[0031] Figure 5 : is a SEM image showing the shape of the porous structure layer according to the present invention. DETAILED DESCRIPTION

[0032] Hereinafter, the present invention will be described in detail to help understand the present invention. As used herein, it will be understood that the words or terms used in the specification and claims of the present invention should not be interpreted as limited to having the meanings defined in commonly used dictionaries. It should also be understood that the words or terms should be understood as having the meanings consistent with their meanings in the relevant art background and the technical concept of the present invention based on the inventors can appropriately define the meanings of the words or terms in order to best illustrate the principles of the present invention.

[0033] Separators

[0034] The separator of the present invention may include a base membrane and a hydrophilic porous structure layer or a hydrophobic porous structure layer stacked on at least one side of the base membrane, wherein the base membrane may be an anion exchange membrane, a cation exchange membrane or a zwitterion exchange membrane.

[0035] According to one embodiment of the present invention, the separator may include a base membrane and a porous structure layer, and the porous structure layer may be stacked on at least one side of the base membrane. The base membrane may be an ion selective exchange membrane, and the base membrane may include an anion exchange membrane, a cation exchange membrane or amphoteric ion exchange membrane. Specifically, the separator of the present invention may be an anion exchange membrane.

[0036] Furthermore, the porous structure layer may have hydrophilic or hydrophobic properties.The porous structure layer may be stacked on at least one side of the base film, and may thus serve to retain a certain amount of moisture in the base film.

[0037] In addition, the porous structure layer has a porous structure, and the porous structure refers to a structure with a large number of pores (i.e., holes) on or inside the material. The hole can have an irregular shape, such as a spherical shape, an elliptical shape or a rod shape, and as will be described later, the average diameter of the hole can be 0.2 μm to 0.45 μm. As for the average diameter of the hole, the length of the main axis of the surface hole found in a random sampling range (a width of 10 μm or more and a length of 15 μm or more) in an image measured using a scanning electron microscope (FE-SEM) can be measured as the pore size. The porous structure layer of the present invention has a porous structure, and can therefore be lightweight and have excellent mechanical strength, and have low resistance to promote material transmission through the hole.

[0038] Meanwhile, generally, anion exchange membrane is usually used as a separator of an electrochemical conversion device. When anion exchange membrane is used as a separator of an electrochemical conversion device, it is shown as excellent according to the electrochemical conversion rate of the electrochemical conversion device, but the anion exchange membrane may be easily dried when exposed to room temperature, and when assembled to the battery or stack of the electrochemical conversion device at room temperature, the anion exchange membrane is easy to dry, and the water content cannot be maintained, and it may be broken or damaged. Specifically, the anion exchange membrane can be stored with water or a fluid that maintains sufficient moisture, but in view of the process of assembling the battery or stack at room temperature, the moisture in the anion exchange membrane is easily evaporated, and although the anion exchange membrane is stored in water with sufficient moisture, when the anion exchange membrane is exposed to room temperature, the anion exchange membrane may also be damaged. Therefore, due to such low mechanical properties at room temperature, typical anion exchange membranes may seriously affect workability. Therefore, in order to improve or maintain the mechanical properties and workability of the anion exchange membrane, a certain amount of moisture needs to be continuously present in the anion exchange membrane to maintain moisture wettability.

[0039] The separator of the present invention has the effect of improving low mechanical properties and low workability, which are limitations of typical separators, while maintaining performance equal to or greater than that of typical separators. Specifically, the separator of the present invention has a porous structure layer having hydrophilic or hydrophobic properties stacked on at least one surface of a base film, and can therefore maintain a certain amount of moisture in the separator for a long time even at room temperature, and can therefore improve low mechanical properties and low workability.

[0040] Figure 2 shows the state of a typical anion exchange membrane treated with a hydrophilic coating when exposed at room temperature for 2 hours, and Figure 3 Shown is the state when the separator of the present invention in which the hydrophilic porous structure layer is stacked on the surface of the anion exchange membrane is exposed to the same room temperature for 2 hours. Figure 3(a) is a state where PTFE treated to make the surface hydrophilic or hydrophobic is applied, and Figure 3 (b) is a state where PVDF subjected to surface hydrophilicity or hydrophobicity treatment is applied.

[0041] According to one embodiment of the present invention, when the separator is exposed at room temperature for 2 hours or more, the separator may not be deformed compared to an initial shape.

[0042] Specifically, refer to Figure 2 , when the separator of the present invention and the typical separator are similarly exposed to room temperature, the typical separator is cracked or mechanically warped after 1 to 2 hours due to evaporation of water.

[0043] On the other hand, refer to Figure 3 , the separator of the present invention can maintain the original shape without being broken or damaged even after 1 to 2 hours. The separator of the present invention has a structure in which a porous structure layer having hydrophilic or hydrophobic properties is stacked on the surface of a base film, and can therefore have a larger water content than a film subjected to a simple hydrophilic treatment, and maintain the water content for a long time.

[0044] Therefore, the separator can maintain its original shape without deformation due to moisture, and can thus improve the low mechanical properties and workability caused at room temperature. In addition, even when exposed at room temperature for 2 hours or more, the separator of the present invention can maintain a weight of 50% or more, 60% or more, 70% or more, 80% or more, or 90% or more relative to the initial weight. In addition, when the separator is exposed at room temperature for 2 hours or more, the shrinkage rate of the separator can be 15% or less, 13% or less, 11% or less, 9% or less, 7% or less, 5% or less, or 3% or less. The shrinkage rate can be calculated by (initial length of the separator - length of the separator after shrinking for 2 hours at 25°C) / (initial length of the separator)×100.

[0045] In addition, the process of preparing the separator of the present invention can be simply carried out in a less complicated manner than the hydrophilic treatment process of a membrane. Specifically, the process of coating a separator with a hydrophilic material can be carried out at a high temperature of 100°C or higher, and in this case, the separator may deform and thus shrink or melt. In addition, due to the moisture present in the separator, the coating cannot be carried out well, and is only applicable when a water-based adhesive is used or a dry environment is provided. Therefore, in terms of process conditions, the process of hydrophilic treatment or coating of the surface of a typical separator may be complicated and time-consuming. In addition, in the case of using water as a solvent for coating, due to the high viscosity and surface tension of water, it is difficult to achieve uniform coating of the internal pores, and the hydrophilic coating material dissolves in water and separates from the separator, resulting in loss of hydrophilicity. In addition, when a binder is used, the separator has a larger thickness, thereby reducing efficiency such as reduced energy density and increased manufacturing costs.

[0046] According to one embodiment of the present invention, the separator may not include a binder between the base membrane and the hydrophilic porous structure layer. Specifically, the separator of the present invention is prepared by stacking a porous structure layer having hydrophilic properties without using a binder, and therefore, the separator can be prepared to have a smaller thickness. In addition, during the preparation process of the separator of the present invention, the stacked porous structure layer has greater adhesion due to the moisture present in the ion selective exchange membrane, and the porous structure layer can therefore be directly fixed to the ion selective exchange membrane. Therefore, when preparing a separator according to the present invention, the preparation time can be reduced compared to the time used to prepare a typical separator by hydrophilic treatment.

[0047] According to one embodiment of the present invention, the hydrophilic porous structure layer may include at least one selected from the group consisting of a hydrophilic polymer, a hydrophilic metal, a ceramic, and cellulose.

[0048] The hydrophilic porous structure layer included in the separator of the present invention may include a hydrophilic polymer. Specifically, the hydrophilic polymer may be a polymer prepared by polymerizing a monomer containing at least one hydrophilic group selected from the following: a hydroxyl functional group (-OH), a carboxylic acid functional group (-COOH), an alkylene oxide functional group (-RO-) and an amine functional group (-NH2). In addition, the hydrophilic polymer may include at least one selected from polypyrrolidone, polyethylene glycol and polyvinyl alcohol. In addition, the hydrophilic polymer may be a polymer in which at least one hydrophobic polymer selected from the following is treated hydrophilically: polyethylene (PE), polypropylene (PP), polycarbonate (PC), polyimide, polyetherimide (PEI), polysulfone (PSF), polyethersulfone (PES), polyvinylidene fluoride (PVDF) and polytetrafluoroethylene (PTFE). More specifically, the hydrophilic polymer that can be used for the hydrophilic porous structure layer of the present invention may be polytetrafluoroethylene (PTFE) that has been subjected to a hydrophilic treatment.

[0049] In addition, the hydrophilic porous structure layer may contain a hydrophilic metal, and most metals and metal oxides have high surface energy and may therefore have hydrophilic properties. A hydrophilic metal may refer to a metal or metal oxide whose surface is completely wetted by water and has a contact angle of less than 90° relative to water. The metal may include at least one selected from the following: Ni, Cu, Al, Fe, stainless steel, an alloy based on Fe-Ni, an alloy based on Fe-Ni-Cr, and an alloy based on Fe-Ni-SiC, and the metal oxide is a hydrophilic metal oxide, and may include, for example, at least one selected from titanium butoxide, zirconium butoxide, MgO, hydrophilic zeolite A, and a porous material based on ETS.

[0050] Furthermore, the hydrophilic porous structure layer may contain ceramics therein, and the ceramics may include at least one selected from the group consisting of ZrO 2 , Al 2 O 3 , and SiO 2 .

[0051] Furthermore, the hydrophilic porous structure layer may contain cellulose, and the cellulose may include cellulose acetate and cellulose nitrate.

[0052] According to one embodiment of the present invention, the hydrophilic porous structure layer may be a polytetrafluoroethylene (PTFE) structure layer having a hydrophilic treated surface.

[0053] Polytetrafluoroethylene (PTFE) is a polymer compound composed of carbon and fluorine, and is a crystalline material having excellent electrical resistance, high thermal stability, acid resistance, chemical resistance, melting point, and dimensional stability. At the same time, polytetrafluoroethylene exhibits excellent sliding properties and non-stick properties, and is a high molecular compound composed only of carbon and fluorine, and is therefore inherently hydrophobic.

[0054] Therefore, the polytetrafluoroethylene that can be used in the hydrophilic porous structure layer of the present invention is a typical polytetrafluoroethylene that has been subjected to a hydrophilic treatment, and the hydrophilic treated polytetrafluoroethylene can maintain mechanical strength and dimensional stability equal to or greater than that of the typical polytetrafluoroethylene, and can also have improved adhesion and hydrophilicity. Therefore, the hydrophilic porous structure layer containing the hydrophilic treated polytetrafluoroethylene has improved adhesion to the anion exchange membrane, and can therefore be stacked and then fixed without a separate binder.

[0055] In contrast, hydrocarbon-based polymer materials such as polyethylene have low mechanical strength, become brittle when dry, and swell when wet, resulting in low dimensional stability. In addition, the porous structure layer containing polyethylene has weak adhesion to the anion exchange membrane, and therefore requires a separate binder, and therefore, the separator as a whole has a greater thickness, resulting in poor energy density and resistance.

[0056] The method of hydrophilic treatment of polytetrafluoroethylene aims to reduce the contact angle of water on the surface of the polymer material to ensure hydrophilicity, and methods such as high-voltage corona discharge and DC plasma discharge can be used to change the contact angle.

[0057] According to one embodiment of the present invention, the average pore diameter of the hydrophilic porous structure layer is 0.2 μm to 0.45 μm. More specifically, the average pore diameter of the hydrophilic porous structure layer can be 0.2 μm or more, 0.22 μm or more, 0.24 μm or more, 0.26 μm or more, or 0.28 μm or more, and can also be 0.45 μm or less, 0.43 μm or less, or 0.41 μm or less, 0.4 μm or less, or 0.37 μm or less. When the average pore diameter of the hydrophilic porous structure layer of the present invention satisfies the above range, the hydrophilic porous structure layer has a reduced resistance, and can therefore have improved electrolyte permeability and also have excellent mechanical strength.

[0058] Figure 5 is a SEM image of the porous structure layer containing PTFE of the present invention. As for the average diameter of the pores, the sample surface is magnified 2,500 times using a scanning electron microscope (FE-SEM) (Hitachi S-4800 scanning electron microscope) and then measured, after which the length of the main axis of the surface pores found within a random sampling range (width of 10 μm or more and length of 15 μm or more) in the measured image can be measured as the pore size. The number of measurements is at least 10 times, and the average value and maximum value of the pore size obtained after the measurement can be determined.

[0059] According to one embodiment of the present invention, the hydrophilic porous structure layer can be stacked on either side of the base membrane. The hydrophilic porous structure layer can be stacked on at least one side of the base membrane, and more specifically, the hydrophilic porous structure layer can be stacked only on one side of the base membrane. Even for a separator in which the hydrophilic porous structure layer is stacked only on one side of the base membrane, the separator can also maintain a water content equivalent to the water content of the separator in which the hydrophilic porous structure layer is stacked on both sides of the base membrane, and sufficient mechanical strength and workability for assembling a battery or a stack can therefore be obtained. In addition, the separator of the present invention in which the hydrophilic porous structure layer is stacked only on one side of the base membrane has a reduced thickness as a whole to have a high ionic conductivity, and has a reduced resistance to obtain high performance and conversion rate.

[0060] Meanwhile, in the case of a structure in which an anion exchange membrane or an ion conductive polymer material is impregnated in a hydrophilically treated porous structure layer, the porous structure layer cannot retain moisture in the exchange membrane, and therefore, moisture wettability may be significantly reduced compared to a separator having a stacked structure.

[0061] In addition, in the separator with an impregnation structure, the entire area of ​​the anion exchange membrane is not in the form of a single layer, and each pore of the porous structure layer is impregnated with the anion exchange membrane, and therefore the transport of ions is not carried out uniformly over the entire area of ​​the anion exchange membrane, resulting in a decrease in the carbon monoxide Faraday efficiency.

[0062] According to one embodiment of the present invention, the separator of the present invention may include a base membrane and a hydrophobic porous structure layer on at least one side of the base membrane.

[0063] The hydrophobic porous structure layer can be used to prevent the residual water from evaporating or escaping to the outside when the ion selective exchange membrane is stored by the hydrophobic property. The material that can be used as the material for the hydrophobic porous structure layer may include at least one selected from polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), nylon, cellulose acetate (CA) and polyethylene sulfide (PES), and specifically, the hydrophobic porous structure layer of the present invention may include PVDF.

[0064] Electrochemical conversion cell

[0065] The electrochemical conversion cell of the present invention may include an anode, a cathode, an electrolyte, and a separator disposed between the cathode and the anode. The separator includes the above-mentioned separator according to the present invention.

[0066] According to another embodiment of the present invention, the electrochemical conversion cell can be used in all electrochemical conversion devices, and the electrochemical conversion device can include a device such as a fuel cell or water electrolysis that can produce useful chemicals by electrochemical conversion, and a device that can reduce and convert carbon dioxide and NOx. Specifically, the electrochemical conversion cell can be an electrochemical conversion cell included in an electrolysis device that converts carbon dioxide into carbon monoxide.

[0067] According to one embodiment of the present invention, the electrochemical conversion cell can be a cell for converting carbon dioxide into carbon monoxide, and can include an anode, a cathode, an electrolyte and a separator. Electrolysis means that a material is decomposed via an oxidation-reduction reaction by applying a DC voltage for a decomposition reaction that does not occur spontaneously. The anode as an oxidation electrode oxidizes water to produce oxygen, and in this case, hydrogen ions are produced. The hydrogen ions produced at the anode are transferred to the cathode through the electrolyte, and the cathode is a reduction electrode, and the reactant injected into the cathode can react with the electrons and hydrogen ions transferred from the anode to produce a product. In addition, a separator can be set between the anode and the cathode. The separator can be composed of an inert material that does not participate in the electrochemical reaction itself, but can provide a path for ions to move between the anode and the cathode, and is used to separate the physical contact between the anode and the cathode.

[0068] In addition, the anode and cathode of the electrochemical conversion cell of the present invention may each include a catalyst layer. In addition, the water vapor supplied together with carbon dioxide in the cathode region produces a reduction product by an electroreduction reaction on the cathode surface. Therefore, the cathode may include a gas diffusion layer to uniformly supply humidified carbon dioxide gas to the cathode region. When the cathode includes a hydrophobic gas diffusion layer, the supplied carbon dioxide can be well diffused, distributed and supplied to the catalyst layer of the cathode. In addition, the hydrophobic gas diffusion layer effectively prevents the condensation of moisture, so that carbon dioxide is continuously and uniformly supplied, and the electrolysis reaction is well performed. In addition, the catalyst layer may have a surface with a porous structure, etc., so that the gas permeability characteristics are well exerted on the surface.

[0069] According to one embodiment of the present invention, the anode may contain a catalyst active in the electrolysis of water, and the catalyst layer of the anode may contain at least one selected from the following: Pt, Au, Pd, Ir, Ag, Rh, Ru, Ni, Al, Mo, Cr, Cu, Ti, W, alloys thereof or mixed metal oxides, such as Ta2O5, IrO2, etc., for oxygen generation reaction. Specifically, the anode in the carbon dioxide electrolysis device of the present invention may contain nickel (Ni) coated with ruthenium oxide (RuO2) and cerium oxide (CeO2).

[0070] In addition, since the carbon dioxide reduction reaction occurring at the cathode competes with the hydrogen generation reaction, a catalyst having a high voltage required for the hydrogen generation reaction and showing activity in the carbon dioxide reduction reaction may be included. The catalyst layer of the cathode may include at least one selected from the following: Sn, Sn alloy, Al, Au, Ag, C, Cd, Co, Cr, Cu, Cu alloy, Ga, Hg, In, Mo, Nb, Ni, NiCo2O4, Ni alloy, Ni-Fe alloy, Pb, Rh, Ti, V, W, Zn and mixtures thereof for hydrogen generation reaction. Specifically, the cathode in the carbon dioxide electrolysis device of the present invention may include silver (Ag).

[0071] In addition, as the separator, a cation exchange membrane (CEM) or an anion exchange membrane (AEM) may be included.

[0072] In addition, the electrolyte can be selected from KHCO3, K2CO3, KOH, KCl, KClO4, K2SiO3, Na2SO4, NaNO3, NaCl, NaF, NaClO4, CaCl2, guanidinium cations, H + Cations, alkali metal cations, ammonium cations, alkylammonium cations, halide ions, alkylamines, borates, carbonates, guanidinium derivatives, nitrites, nitrates, phosphates, condensed phosphates, perchlorates, silicates, sulfates, tetraalkylammonium salts, or aqueous solutions containing mixtures thereof are used, and the electrolyte of the carbon dioxide electrolysis device of the present invention may contain KOH.

[0073] In addition, as the gas diffusion layer, a porous material using a carbon material, such as carbon fiber cloth, carbon fiber felt and carbon fiber paper, or a porous metal material formed by a thin metal plate with a mesh structure, such as mesh iron and metal mesh, can be used, and in the carbon dioxide electrolysis device of the present invention, carbon fiber cloth can be used as the gas diffusion layer.

[0074] Hereinafter, embodiments of the present invention will be described in detail in such a manner that a person skilled in the art can easily carry out the present invention. However, the present invention can be embodied in many different forms and is not limited to the embodiments set forth herein.

[0075] Example 1

[0076] like Figure 1 As shown in , a separator including an anion exchange membrane and a hydrophilic porous structure layer stacked on one side of the anion exchange membrane was prepared. The process of preparing the separator is as follows.

[0077] An anion exchange membrane (Sustainion X37, Dioxide Materials) was prepared as a base membrane, and a surface hydrophilic treated polytetrafluoroethylene (PTFE) (Hyundai Micro) with a pore size of 0.2 μm was prepared as a porous structure layer. The surface of the surface hydrophilic treated PTFE porous structure layer was fully wetted with deionized water, stacked on the anion exchange membrane, and then fully bonded to the interface under constant pressure.

[0078] Example 2

[0079] A separator having a stacked structure was prepared in the same manner as in Example 1, except that a hydrophilically treated PVDF (Hyundai Micro) porous structure layer was used instead of a hydrophilically treated PTFE (Hyundai Micro) porous structure layer.

[0080] Example 3

[0081] A separator was prepared in the same manner as in Example 1, except that only the surface-hydrophilicized PTFE porous structure layer was used without the anion exchange membrane.

[0082] Example 4

[0083] A separator having a stacked structure was prepared in the same manner as in Example 1, except that a surface-hydrophilic treated PTFE porous structure layer having a pore size of 0.4 μm was used.

[0084] Example 5

[0085] A separator having a stacked structure was prepared in the same manner as in Example 1, except that a porous structure layer containing cellulose acetate was used instead of the hydrophilic-treated PTFE (Hyundai Micro).

[0086] Example 6

[0087] A separator having a stacked structure was prepared in the same manner as in Example 1, except that a porous structure layer containing polyethylene sulfide was used instead of the hydrophilically treated PTFE (Hyundai Micro).

[0088] Comparative Example 1

[0089] A separator was prepared in the same manner as in Example 1, except that the porous structure layer was not included and only the anion exchange membrane was included.

[0090] Comparative Example 2

[0091] A separator having a stacked structure was prepared in the same manner as in Example 1, except that a porous structure layer containing polyethylene (PE) was used.

[0092] Comparative Example 3

[0093] As a porous structure layer, a polytetrafluoroethylene (PTFE) (Hyundai Micro) with a pore size of 0.2 μm and treated with surface hydrophilicity is prepared. The polytetrafluoroethylene is fixed to a 10 cm × 10 cm frame, and the PTFE frame is fully immersed in a deionized water bath and kept at 60 ° C for 12 hours. An aqueous solution containing 30 wt % ethanolamine (sigma-aldrich>98%) is prepared, and then the PTFE frame is added thereto and stirred at 80 ° C for one day to react. Thereafter, the PTFE frame is washed several times with distilled water to remove residual ethanolamine, and vacuum dried at room temperature for one day. On an anion exchange membrane (SustainionX37, Dioxide Materials), a PTFE with ionic functional groups replaced on its surface and inside the pores fixed to the frame is placed, and left for 1 hour to impregnate the anion exchange membrane, thereby preparing a separator.

[0094] Experimental Example 1

[0095] The separators prepared in Examples and Comparative Examples were exposed to the external atmosphere at room temperature for 2 hours to observe a moisture evaporation phenomenon and the state of the separators, and the results of the state of the separators are shown in Table 1 below.

[0096] [Table 1]

[0097]

[0098] *○: Good condition

[0099] *△: The separator is cracked and partially damaged

[0100] *X: The separator is broken and the whole is damaged

[0101] Experimental Example 2

[0102] Carbon dioxide electrolysis was performed by adjusting the operating conditions of the carbon dioxide electrolysis device including the separators prepared in Examples and Comparative Examples as follows.

[0103] Reaction current density: 100mA / cm 2 (Constant current operation)

[0104] Reaction voltage: 3V to 3.5V

[0105] Reaction temperature: 40℃

[0106] Reaction pressure: 1 atmosphere (normal pressure)

[0107] Anode catalyst: RuO2+CeO2 on Ni mesh

[0108] Cathode catalyst: Ag powder

[0109] Electrode area: 25cm 2

[0110] Gas diffusion layer: Sigracet 39BB

[0111] Anolyte: 0.5M KHCO3 (25ml / min)

[0112] Cathode reactant: 40℃ humidified CO2 gas (25ccm)

[0113] During the electrolysis, the carbon dioxide conversion rate (%), carbon monoxide Faraday efficiency (CO Faraday efficiency, %) and voltage were measured, and the obtained values ​​are shown in the following Table 2, and the obtained values ​​are shown in Figure 4 .

[0114] *Measurement method

[0115] (1) Carbon monoxide conversion rate (%)

[0116] The conversion rate (%) was calculated as the ratio of the amount of carbon monoxide (CO) produced per hour to the amount of carbon dioxide (CO2) gas introduced.

[0117] (2) Carbon monoxide Faraday efficiency (%)

[0118] In the exhaust line, the gas composition was measured by gas chromatography (GC) analysis. In addition, the Faraday efficiency was calculated by the following equation.

[0119] [Equation 1]

[0120]

[0121] In Equation 1, Q represents the flow rate in the exhaust line, F represents the Faraday constant, p represents the pressure, T represents the measured temperature, and R represents the ideal gas constant. 总 ) is the total current applied over a period of time, and the product current (i 产物 ) is the gas volume (V 产物 ) calculated value.

[0122] (3) Voltage (V)

[0123] The current was applied and the voltage was measured by a VSP potentiostat from BioLogic. An 80A booster was installed to apply the current corresponding to a large area. The current was applied in stages at 100 mA / cm 2 , 200mA / cm 2 and 300mA / cm 2 The current was applied and maintained for a predetermined period of time, and the voltage was then recorded after 10 minutes. In this case, gas chromatography (GC) analysis was also performed.

[0124] [Table 2]

[0125]

[0126] With reference to Tables 1 and 2 above, it was determined that Examples 1 to 6 using a separator including a porous structure layer according to the present invention were in good condition even when exposed to the external atmosphere for 2 hours at room temperature, the state of the separator did not change, and this was because the moisture wettability of the separator was maintained by the porous structure layer, and thus the separator contained a certain level of moisture. On the other hand, it was determined that in Comparative Example 1 using only an anion exchange membrane without a porous structure layer, the entire separator was damaged and cracked when exposed to the external atmosphere for 2 hours at room temperature.

[0127] In addition, it was determined that Examples 1 to 6 maintained water wettability, resulting in improved workability, and also had excellent effects in terms of carbon dioxide conversion rate, CO Faraday efficiency, and overvoltage. At the same time, it was determined that Comparative Example 2 using a separator including a porous structure layer containing polyethylene (PE) maintained water wettability, but when assembled into an electrochemical conversion cell and used, an overvoltage of 6V or more occurred, and very poor effects were shown in terms of carbon dioxide conversion rate and CO Faraday efficiency.

[0128] In addition, Comparative Example 3 has a structure in which the anion exchange membrane is impregnated in the porous structure layer, and in Comparative Example 3, the anion exchange membrane having ion conductivity is not in the form of a single layer, but is impregnated and unevenly arranged in each hole, and therefore the porous structure layer cannot maintain moisture wettability, and the separator is broken after 1 to 2 hours. In addition, it was determined that in the separator of Comparative Example 3, the movement of ions cannot be uniformly performed over the entire area of ​​the anion exchange membrane, and therefore the carbon monoxide Faraday efficiency is reduced.

[0129] 100: Anion exchange membrane

[0130] 200: Porous structure layer

Claims

1. A separator, comprising: Basic membrane; and a hydrophilic porous structure layer or a hydrophobic porous structure layer stacked on at least one side of the base membrane, The base membrane is an anion exchange membrane, a cation exchange membrane or a zwitterion exchange membrane. The separator according to claim 1 , wherein the hydrophilic porous structure layer comprises a hydrophilic polymer. 3 . The separator according to claim 1 , wherein the hydrophilic porous structural layer is a polytetrafluoroethylene (PTFE) structural layer having a hydrophilically treated surface. 4 . The separator according to claim 1 , wherein the hydrophilic porous structure layer has an average pore diameter of 0.2 μm to 0.45 μm. The separator according to claim 1 , wherein the hydrophilic porous structure layer is stacked on either side of the base membrane. The separator according to claim 1 , wherein the separator does not include a binder between the base film and the hydrophilic porous structure layer. 7 . The separator according to claim 1 , wherein the hydrophobic porous structure layer comprises at least one selected from the group consisting of PTFE, PVDF, nylon, cellulose acetate (CA), and polyethylene sulfide (PES).

8. An electrochemical conversion cell comprising: cathode; an anode; an electrolyte; and The separator according to any one of claims 1 to 7, wherein the separator is provided between the cathode and the anode.

9. The electrochemical conversion cell according to claim 8, wherein the electrochemical conversion cell converts carbon dioxide into carbon monoxide.

Citation Information

Cited By

  • Sodium ion battery using PTFE / PE asymmetric composite diaphragm

    CN120497419A