Forsterite particles and method for producing forsterite particles

By using molybdenum compounds as flux in magnesium compounds and silicon compounds to sinter forsterite particles, the problem of insufficient characteristics of forsterite particles in the prior art is solved, and low aggregation and controlled shape forsterite particles are achieved Production improves production efficiency and quality.

CN118946978APending Publication Date: 2024-11-12DIC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280094169.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2022-04-28
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the prior art, knowledge about forsterite particles and their production methods is limited, and there is room for research, so it is difficult to produce forsterite particles with excellent characteristics.

Method used

Molybdenum compounds are used as flux, and magnesium compounds and silicon or silicon compounds are sintered in the presence of molybdenum compounds to control the content and distribution of molybdenum, and to produce forsterite particles containing molybdenum to optimize their shape and aggregation degree.

Benefits of technology

Successfully produced forsterite particles with excellent properties, including particles with low aggregation and controlled shape, reducing impurity content and improving production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005059192660000261
    Figure BDA0005059192660000261
  • Figure BDA0005059192660000271
    Figure BDA0005059192660000271
  • Figure HDA0005059192670000011
    Figure HDA0005059192670000011
Patent Text Reader

Abstract

Relates to forsterite particles containing molybdenum. The invention also relates to a production method of the forsterite particles. The method includes firing a magnesium compound and silicon or a silicon compound in the presence of a molybdenum compound.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to forsterite particles and a method for producing the forsterite particles. Background Art

[0002] Forsterite is excellent in strength and is used as a thin thermal insulation material. Forsterite has high insulation resistance and is widely used as an electrical insulating material. In addition, forsterite is used in places where adhesion to metal is considered important, such as insulating parts for vacuum tubes and base members for metal film resistors, by utilizing its high thermal expansion coefficient.

[0003] Forsterite has a dielectric constant of 6.5 and can be used as a high-frequency insulating material because forsterite has a low dielectric loss tangent (tan δ) and low microwave loss, and is an inorganic material expected to be used for 5G transmission in the future.

[0004] PTL 1 discloses a method for producing forsterite fine particles. In this method, a solution containing a water-soluble magnesium salt and colloidal silica at a magnesium to silicon molar ratio (Mg / Si) of 2 is dried by spraying the solution in an atmosphere at a temperature of 50° C. to less than 300° C., and then sintered in an air atmosphere at a temperature of 800° C. to 1,000° C., thereby obtaining forsterite fine particles having a primary particle size in the range of 1 nm to 200 nm as observed by an electron microscope.

[0005] PTL 2 discloses a method for producing silane-treated forsterite particles and an organic solvent dispersion of the silane-treated forsterite particles. The method comprises (a) wet-pulverizing a particle having a specific surface area of ​​5 m2 in a dispersion medium containing an organic solvent by using a bead mill. 2 / g to 100m 2 / g of forsterite fine particles to obtain an organic solvent dispersion; and (b) by adding methyltrimethoxysilane, phenyltrimethoxysilane, methyltriethoxysilane, methacryloxypropyltrimethoxysilane and / or a hydrolyzate thereof to the organic solvent dispersion obtained in the step (a) so that the mass ratio of the organosilicon compound to the forsterite fine particles (organosilicon compound / forsterite fine particles) is 0.01 to 0.50, and a methyltrimethoxysilyl group, a phenyltrimethoxysilyl group, a methyltriethoxysilyl group or a methacryloxypropyltrimethoxysilyl group is bonded to the surface of the forsterite fine particles.

[0006] [Citation List]

[0007] [Patent Document]

[0008] [PTL 1]

[0009] Japanese Unexamined Patent Application Publication No. 2016-222517

[0010] [PTL 2]

[0011] Japanese Unexamined Patent Application Publication No. 2020-100561 Summary of the invention

[0012] Problem that the invention aims to solve

[0013] However, knowledge about conventional forsterite particles and their production methods is limited, and there is room for research.

[0014] The present invention has been made to solve such problems as described above and an object of the present invention is to provide forsterite particles having excellent characteristics and a method for producing forsterite particles.

[0015] Solutions for solving problems

[0016] The present inventors have conducted extensive research to solve the above-mentioned problems, and have therefore found that forsterite particles can be easily produced using a molybdenum compound as a flux, and that forsterite particles containing molybdenum can also be produced. This has led to the completion of the present invention. That is, the present invention includes the following embodiments.

[0017] (1) Forsterite particles containing molybdenum.

[0018] (2) In the forsterite particles specified in item (1), the content of molybdenum in the forsterite particles is 0.05 mass % to 35 mass % (Mo1) as MoO3 relative to 100 mass % of the forsterite particles as measured by XRF analysis of the forsterite particles.

[0019] (3) In the forsterite particles specified in item (1) or (2), the content of molybdenum in the surface layer of each forsterite particle is (Mo2) 0.05 mass % to 25 mass % relative to 100 mass % of the surface layer of the forsterite particle, as measured by XPS surface analysis of the forsterite particles.

[0020] (4) In the forsterite particles specified in any one of the items (1) to (3), the average size of primary particles of the forsterite particles is 0.1 μm to 100 μm.

[0021] (5) In the forsterite particles specified in any one of items (1) to (4), the forsterite particles have a specific surface area of ​​0.02 m 2 / g to 20m 2 / g.

[0022] (6) A method for producing forsterite particles as specified in any one of items (1) to (5), which comprises calcining a magnesium compound and silicon or a silicon compound in the presence of a molybdenum compound.

[0023] (7) In the method for producing forsterite particles as specified in item (6), the molybdenum compound is at least one selected from the group consisting of molybdenum trioxide, lithium molybdate, potassium molybdate and sodium molybdate.

[0024] (8) In the method for producing forsterite particles specified in item (6) or (7), the calcination temperature of the magnesium compound and silicon or the silicon compound is 800°C to 1,600°C.

[0025] (9) In the method for producing forsterite particles as specified in any one of items (6) to (8), the molar ratio of molybdenum to magnesium and silicon (Mo / (Mg+Si)) in the fired raw material is 0.001 to 5.

[0026] Effects of the Invention

[0027] According to the present invention, forsterite particles having excellent characteristics and a method for producing forsterite particles can be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] [ Figure 1 ]

[0029] Figure 1 is a SEM image of the forsterite particles of Example 1.

[0030] [ Figure 2 ]

[0031] Figure 2 is a SEM image of the forsterite particles of Example 2.

[0032] [ Figure 3 ]

[0033] Figure 3 is a SEM image of the forsterite particles of Example 3.

[0034] [ Figure 4 ]

[0035] Figure 4 is a SEM image of the forsterite particles of Example 4.

[0036] [ Figure 5 ]

[0037] Figure 5 is a SEM image of the forsterite particles of Example 5.

[0038] [ Figure 6 ]

[0039] Figure 6 is a SEM image of the forsterite particles of Example 6.

[0040] [ Figure 7 ]

[0041] Figure 7 is a SEM image of the forsterite particles of Example 7.

[0042] [ Figure 8 ]

[0043] Figure 8 is a SEM image of the forsterite particles of Example 8.

[0044] [ Fig. 9 ]

[0045] Fig. 9 is a SEM image of the forsterite particles of Example 9.

[0046] [ Fig.10 ]

[0047] Fig.10 is a SEM image of the forsterite particles of Comparative Example 1.

[0048] [ Fig.11 ]

[0049] Fig.11 This is a SEM image of the forsterite particles of Comparative Example 2.

[0050] [ Fig.12 ]

[0051] Fig.12 : is a graph showing X-ray diffraction (XRD) patterns of the forsterite particles of Examples 1 to 9 and Comparative Examples 1 and 2. DETAILED DESCRIPTION

[0052] The forsterite particles according to an embodiment of the present invention and a method for producing the forsterite particles according to an embodiment of the present invention are described below.

[0053] <<Forsterite Granules>>

[0054] The forsterite particles according to this embodiment are forsterite particles containing molybdenum. The forsterite particles according to this embodiment contain molybdenum and have excellent characteristics such as catalytic activity derived from molybdenum.

[0055] The forsterite particles according to this embodiment may have an excellent characteristic, ie, a controlled shape.

[0056] The forsterite particles according to this embodiment may have excellent characteristics in that the degree of aggregation is low or no aggregation occurs.

[0057] The forsterite particles according to this embodiment may contain molybdenum derived from the molybdenum compound used in the production method described below. Using the molybdenum compound in the production method described below can control the shape of the forsterite particles produced, reduce the content of impurities, and can easily produce forsterite particles with a low degree of aggregation.

[0058] There is no particular limitation on the state or amount of molybdenum contained in the forsterite particles according to this embodiment. Molybdenum may be contained in the forsterite particles in the form of metallic molybdenum, an oxide of molybdenum, or a partially reduced molybdenum compound. It is conceivable that molybdenum is contained in the forsterite particles in the form of MoO3. Molybdenum may be contained in the forsterite particles in the form of MoO2 or MoO instead of MoO3.

[0059] There is no particular limitation on the form of molybdenum contained. Molybdenum may be contained in a form in which molybdenum is attached to the surface of forsterite particles, in a form in which molybdenum is substituted into a part of the crystal structure of forsterite particles, or in an amorphous state. These may be combined.

[0060] In the present specification, controlling the shape of forsterite particles means that the shape of the produced forsterite particles is not irregular. In the present specification, forsterite particles having a controlled shape mean forsterite particles that are not irregular in shape.

[0061] The forsterite particles according to this embodiment may be those having a polyhedral shape. The forsterite particles according to this embodiment may be crystal shape controlled and may have an automorphic polyhedral shape. The crystal shape controlled forsterite particles may be produced by a method for producing forsterite particles according to the embodiment described below.

[0062] The cluster (powder) of forsterite particles may contain forsterite particles having a shape other than a polyhedral shape in any state. In terms of mass or quantity, the content of forsterite particles having a polyhedral shape is preferably 80% or more, more preferably 90% or more, and further more preferably 95% or more relative to the amount of the cluster (powder) of forsterite particles. The form of the forsterite particles can be confirmed using a scanning electron microscope (SEM).

[0063] The forsterite particles according to this embodiment allow the size or molybdenum content of the obtained forsterite particles to be controlled by controlling the amount or type of the molybdenum compound used as a raw material, or the firing temperature, etc. in the production method described below.

[0064] The average size of primary particles of the forsterite particles according to the embodiment may be 0.1 μm to 100 μm, 0.2 μm to 50 μm, or 0.3 μm to 40 μm.

[0065] The average size of the primary particles of the forsterite particles was calculated as a converted particle size based on the specific surface area described below, assuming that the particles were ideally spherical. The following conversion equation was used.

[0066] Primary particle size Dsa [nm] = 6,000 / (density [g / cm 3 ]×specific surface area [m 2 / g])

[0067] The median diameter D of the forsterite particles according to this embodiment calculated by the laser diffraction-scattering method is 50 It may be 0.1 μm to 100 μm, 0.2 μm to 50 μm, or 0.3 μm to 40 μm.

[0068] The median diameter D of the forsterite particles was calculated by laser diffraction-scattering method. 50 It can be determined as a particle diameter at which the cumulative volume percentage is 50% in a particle size distribution measured in a dry mode using a laser diffraction particle size distribution analyzer.

[0069] The forsterite particles according to this embodiment may have a specific surface area of ​​0.02 m 2 / g to 20m 2 / g, 0.04m 2 / g to 18m 2 / g or 0.05m 2 / g to 15m 2 / g.

[0070] The above-mentioned specific surface area is calculated in the following manner: the surface area per gram of the sample measured from nitrogen adsorption by the BET method (Brunauer-Emmett-Teller method) using a specific surface area analyzer (e.g., BELSORP-mini manufactured by MicrotracBEL Corporation) is regarded as the specific surface area (m 2 / g).

[0071] The forsterite particles according to this embodiment are forsterite particles containing forsterite.

[0072] The forsterite particles according to this embodiment preferably contain 65 mass% or more of Mg2SiO4, more preferably 65 mass% to 99.95 mass% of Mg2SiO4, further more preferably 70 mass% to 99.5 mass% of Mg2SiO4, and still further more preferably 75 mass% to 99 mass% of Mg2SiO4, relative to 100 mass% of the forsterite particles.

[0073] The content of magnesium contained in the forsterite particles can be measured by XRF analysis. The content of magnesium in the forsterite particles according to this embodiment is preferably 30% to 80% by mass, more preferably 35% to 70% by mass, and further more preferably 40% to 66% by mass, as measured by XRF analysis of the forsterite particles, relative to 100% by mass of the forsterite particles, in terms of MgO (Mg1).

[0074] The content of silicon contained in the forsterite particles can be measured by XRF analysis. The content of silicon in the forsterite particles according to this embodiment is preferably 10% to 60% by mass, more preferably 15% to 50% by mass, and further more preferably 20% to 45% by mass, relative to 100% by mass of the forsterite particles, as measured by XRF analysis of the forsterite particles, in terms of SiO2.

[0075] The forsterite particles according to this embodiment are forsterite particles containing molybdenum. The content of molybdenum contained in the forsterite particles can be measured by XRF analysis. By XRF analysis of the forsterite particles, the content of molybdenum in the forsterite particles according to this embodiment is preferably a content (Mo1) of 0.05% by mass or more in terms of MoO3, more preferably 0.05% by mass to 35% by mass, further more preferably 0.08% by mass to 30% by mass, and still further more preferably 0.09% by mass to 25% by mass, relative to 100% by mass of the forsterite particles.

[0076] In the forsterite particles according to this embodiment, the upper and lower limits of each of the above-exemplified content (Mg1), content (S1) and content (Mo1) can be freely combined. The content (Mg1), content (S1) and content (Mo1) can also be freely combined.

[0077] The forsterite particles according to this embodiment may be, for example, forsterite particles wherein the content (Mg1) is 30 to 80% by mass, the content (S1) is 10 to 60% by mass, and the content (Mo1) is 0.05 to 35% by mass, relative to 100% by mass of the forsterite particles, as determined by XRF analysis of the forsterite particles; forsterite particles wherein the content (Mg1) is 35 to 70% by mass, the content (S1) is 15 to 50% by mass, and the content (Mo1) is 0.08 to 30% by mass; or forsterite particles wherein the content (Mg1) is 40 to 66% by mass, the content (S1) is 20 to 45% by mass, and the content (Mo1) is 0.09 to 25% by mass.

[0078] For the above-mentioned XRF analysis, an X-ray fluorescence analyzer (such as Primus IV manufactured by Rigaku Corporation) can be used.

[0079] The content (Mg1) in terms of MgO is a value determined from the amount of MgO obtained by converting the content of magnesium measured by XRF analysis of forsterite particles using a calibration curve in terms of MgO.

[0080] The content (S1) in terms of SiO 2 is a value determined from the amount of SiO 2 obtained by converting the silicon content measured by XRF analysis of forsterite particles using a calibration curve in terms of SiO 2 .

[0081] The content (Mo1) in terms of MoO 3 is a value determined from the amount of MoO 3 obtained by converting the content of molybdenum measured by XRF analysis of forsterite particles using a calibration curve in terms of MoO 3 .

[0082] The content of magnesium contained in the surface layer of the forsterite particles can be measured by XPS (X-ray photoelectron spectroscopy) surface analysis. The content of magnesium in the surface layer of each forsterite particle according to this embodiment is preferably 1% by mass to 70% by mass, more preferably 3% by mass to 60% by mass, and further more preferably 5% by mass to 50% by mass, relative to 100% by mass of the surface layer of the forsterite particles, as determined by XPS surface analysis of the forsterite particles.

[0083] The content of silicon contained in the surface layer of the forsterite particles can be measured by XPS (X-ray photoelectron spectroscopy) surface analysis. The content of silicon in the surface layer of each forsterite particle according to this embodiment is preferably 1% by mass to 70% by mass, more preferably 3% by mass to 60% by mass, and further more preferably 5% by mass to 50% by mass, relative to 100% by mass of the surface layer of the forsterite particles, as determined by XPS surface analysis of the forsterite particles.

[0084] The content of molybdenum contained in the surface layer of the forsterite particles can be measured by XPS (X-ray photoelectron spectroscopy) surface analysis. The content of molybdenum in the surface layer of each forsterite particle according to this embodiment is preferably 0.05% by mass or more in terms of MoO3 (Mo2), more preferably 0.05% by mass to 25% by mass, further more preferably 0.08% by mass to 20% by mass, and still further more preferably 0.1% by mass to 15% by mass, as determined by XPS surface analysis of the forsterite particles, relative to 100% by mass of the surface layer of the forsterite particles.

[0085] In the forsterite particles according to this embodiment, the upper and lower limits of the content (Mg2), the content (S2) and the content (Mo2) exemplified above can be freely combined. The content (Mg2), the content (S2) and the content (Mo2) can also be freely combined.

[0086] The forsterite particles according to this embodiment may be, for example, forsterite particles wherein the content (Mg2) is 1 to 70 mass%, the content (S2) is 1 to 70 mass%, and the content (Mo2) is 0.05 to 25 mass%, relative to 100 mass% of the surface layer of each forsterite particle, as determined by XPS analysis of the forsterite particles; forsterite particles wherein the content (Mg2) is 3 to 60 mass%, the content (S2) is 3 to 60 mass%, and the content (Mo2) is 0.08 to 20 mass%; or forsterite particles wherein the content (Mg2) is 5 to 50 mass%, the content (S2) is 5 to 50 mass%, and the content (Mo2) is 0.1 to 15 mass%.

[0087] For the above-mentioned XPS analysis, a scanning X-ray photoelectron spectrometer (for example, QUANTERA SXM manufactured by Ulvac-Phi Inc.) may be used.

[0088] The content (Mg2) is a value of the MgO content relative to 100 mass % of the surface layer of the forsterite particles measured as follows: the forsterite particles are subjected to XPS surface analysis by an X-ray photoelectron spectrometer (XPS) to obtain the abundance (atomic %) of each element, and the magnesium content is converted into the oxide content.

[0089] The content (S2) is a value of SiO2 content relative to 100 mass % of the surface layer of the forsterite particles measured in the following manner: the forsterite particles are subjected to XPS surface analysis by an X-ray photoelectron spectrometer (XPS) to obtain the abundance (atomic %) of each element, and the silicon content is converted into the oxide content.

[0090] The content (Mo2) is a value of the MoO3 content relative to 100 mass % of the surface layer of the forsterite particles measured in the following manner: the forsterite particles are subjected to XPS surface analysis by an X-ray photoelectron spectrometer (XPS) to obtain the abundance (atomic %) of each element, and the molybdenum content is converted into the oxide content.

[0091] In the forsterite particles according to this embodiment, molybdenum is preferably unevenly distributed in the surface layer of each forsterite particle.

[0092] In this specification, the term "surface layer" refers to a portion within 10 nm from the surface of each forsterite particle according to the embodiment. In the examples, this distance corresponds to the depth detected by XPS for measurement.

[0093] Herein, the phrase “non-uniformly distributed in the surface layer” refers to a state in which the mass of molybdenum or the molybdenum compound per unit volume of the surface layer is greater than the mass of molybdenum or the molybdenum compound per unit volume of a portion other than the surface layer.

[0094] In the forsterite particles according to this embodiment, the fact that molybdenum is unevenly distributed in the surface layer of each forsterite particle can be confirmed by the fact that, as shown in the following examples, the content (Mo2) of molybdenum in terms of MoO3 relative to 100% by mass of the surface layer of the forsterite particles determined by XPS surface analysis of the forsterite particles is greater than the content (Mo1) of molybdenum in terms of MoO3 relative to 100% by mass of the forsterite particles determined by XRF (X-ray fluorescence) analysis of the forsterite particles.

[0095] In the forsterite particles according to the embodiment, as an indicator of the fact that molybdenum is unevenly distributed in the surface layer of each forsterite particle, the forsterite particles according to the embodiment may be such that the surface layer uneven distribution ratio (Mo2 / Mo1) of molybdenum (which is the ratio of the content (Mo2) calculated as MoO3 relative to 100 mass % of the surface layer of each forsterite particle to the content (Mo1) calculated as MoO3 relative to 100 mass % of the forsterite particles determined by XPS surface analysis of the forsterite particles) may be 1.1 or more or may be in the range of 1.1 to 10.

[0096] Compared with when molybdenum or a molybdenum compound is uniformly present both in the surface layer and in a portion other than the surface layer (inner layer), making molybdenum or a molybdenum compound unevenly distributed in the surface layer of each forsterite particle can effectively exhibit excellent properties such as catalytic activity.

[0097] The forsterite particles according to this embodiment may be provided in the form of clusters of forsterite particles. For the above-mentioned magnesium content, silicon content, and molybdenum content, values ​​measured using clusters as samples may be used.

[0098] The forsterite particles according to this embodiment may contain lithium, potassium, or sodium in addition to molybdenum.

[0099] <Method for producing forsterite particles>

[0100] A method for producing forsterite particles according to an embodiment includes firing a magnesium compound and silicon or a silicon compound in the presence of a molybdenum compound. More specifically, the production method according to this embodiment is a method for producing forsterite particles, and may include mixing a magnesium compound, silicon or a silicon compound, and a molybdenum compound into a mixture and firing the mixture.

[0101] Compared with when no molybdenum compound is used, firing the magnesium compound and silicon or the silicon compound in the presence of the molybdenum compound can improve the production reaction efficiency of forsterite particles. Therefore, high-quality forsterite particles with reduced impurity content can be efficiently produced. In addition, forsterite particles with a low degree of aggregation can be easily produced.

[0102] When a compound containing silicon and magnesium such as magnesium silicate is used, it is considered that a magnesium compound and a silicon compound are used. From the viewpoint that even the production reaction of a composite oxide such as forsterite (magnesium silicate) can be well performed using a molybdenum compound, the magnesium compound and the silicon compound as raw materials preferably do not include magnesium silicate.

[0103] When a compound containing molybdenum and magnesium such as magnesium molybdate is used, it is considered to be when a molybdenum compound and a magnesium compound are used.

[0104] When a compound containing silicon and molybdenum such as molybdenum silicide is used, it is considered to be when a silicon compound and a molybdenum compound are used.

[0105] According to the method for producing forsterite particles according to this embodiment, the forsterite particles according to the above-described embodiment can be produced.

[0106] A preferred method for producing forsterite particles includes a step of mixing a magnesium compound, silicon or a silicon compound, and a molybdenum compound into a mixture (mixing step) and a step of firing the mixture (firing step).

[0107] [Mixing Step]

[0108] The mixing step is a step of mixing a magnesium compound, silicon or a silicon compound, and a molybdenum compound into a mixture (mixing step). The components of the mixture are as follows.

[0109] (Magnesium compounds)

[0110] There is no particular limitation on the type of magnesium compound. Examples of magnesium compounds include magnesium hydroxide, magnesium oxide, magnesium carbonate, magnesium molybdate, magnesium silicate, magnesium acetate, magnesium chloride, magnesium nitrate and magnesium sulfate. Magnesium hydroxide or magnesium carbonate is preferred because of easy reaction. Magnesium hydroxide is more preferred from the viewpoint that the generated gas is water vapor.

[0111] The shape of the fired forsterite particles is hardly affected by the shape of the magnesium compound as a raw material. Therefore, the magnesium compound can be satisfactorily used in the form of, for example, spheres, irregularly shaped solids, shapes with high aspect ratios (wires, fibers, ribbons or tubes, etc.), or sheets.

[0112] (Silicon or silicon compound)

[0113] There is no particular restriction on the type of silicon or silicon compound. Not only silicon atoms but also known silicon compounds can be used. Examples of silicon and silicon compounds include artificially synthesized silicon compounds such as silicon dioxide (SiO2), magnesium silicate, molybdenum silicide, silicomolybdic acid, metallic silicon (silicon atoms), organosilane compounds, silicone resins, silicon dioxide particles, silica gel, mesoporous silica, SiC and mullite, and natural silicon compounds such as biogenic silica.

[0114] There is no particular limitation on the shape of silicon or silicon compounds. Silicon or silicon compounds can be satisfactorily used in the form of, for example, spheres, irregularly shaped solids, shapes with high aspect ratios (wires, fibers, ribbons or tubes, etc.), or sheets.

[0115] (Molybdenum compounds)

[0116] Examples of the molybdenum compound include molybdenum oxide, molybdic acid, molybdenum sulfide, molybdenum silicide, silicomolybdic acid, magnesium molybdate, and molybdate compounds. Molybdenum oxide or molybdate compounds are preferred.

[0117] Examples of molybdenum oxides include molybdenum dioxide (MoO2) and molybdenum trioxide (MoO3). Molybdenum trioxide is preferred.

[0118] The molybdate compound is not particularly limited and may be a salt of a molybdenum oxyanion, such as MoO4 2- 、Mo2O7 2- 、Mo3O 10 2- 、Mo4O 13 2- 、Mo5O 16 2- 、Mo6O 19 2- 、Mo7O 24 6- or Mo8O 26 4- The molybdate compound may be an alkali metal salt, an alkaline earth metal salt or an ammonium salt of a molybdenum oxyanion.

[0119] The molybdate compound is preferably an alkali metal salt of a molybdenum oxyanion; more preferably lithium molybdate, potassium molybdate or sodium molybdate; further more preferably potassium molybdate or sodium molybdate; particularly preferably sodium molybdate.

[0120] In the method for producing forsterite particles according to this embodiment, the molybdate compound may be a hydrate.

[0121] The molybdenum compound is preferably at least one selected from the group consisting of molybdenum trioxide, lithium molybdate, potassium molybdate and sodium molybdate; more preferably at least one selected from the group consisting of molybdenum trioxide, potassium molybdate and sodium molybdate; further more preferably molybdenum trioxide and / or sodium molybdate.

[0122] In the method for producing forsterite particles according to this embodiment, use of a molybdate compound tends to reduce the ratio of the molybdenum content of the produced forsterite particles, and is preferred from the viewpoint of increasing the crystallinity of forsterite.

[0123] The method for producing forsterite particles according to the embodiment may include a step of calcining a magnesium compound and silicon or a silicon compound in the presence of a molybdenum compound, a sodium compound, and / or a potassium compound.

[0124] The method for producing forsterite particles according to this embodiment may include a step of mixing a magnesium compound, silicon or a silicon compound, a molybdenum compound, a sodium compound and / or a potassium compound into a mixture before the calcining step (mixing step), and may include a step of calcining the mixture (calcining step).

[0125] In the production method according to this embodiment, the use of the sodium compound and / or the potassium compound allows the size of the produced forsterite particles to be easily adjusted, and forsterite particles with a low degree of aggregation or no aggregation can be easily produced.

[0126] Herein, a compound containing molybdenum and sodium such as sodium molybdate may be used to replace at least a portion of the molybdenum compound and the sodium compound. Similarly, a compound containing molybdenum and potassium such as potassium molybdate may be used to replace at least a portion of the molybdenum compound and the potassium compound.

[0127] Therefore, the step of mixing a magnesium compound, silicon or a silicon compound, and a compound containing molybdenum and potassium and / or sodium into a mixture is considered to be a step of mixing a magnesium compound, silicon or a silicon compound, a molybdenum compound, a potassium compound and / or a sodium compound into a mixture.

[0128] Compounds containing molybdenum and sodium suitable as fluxes can be produced in the firing process using, for example, relatively cheap and readily available molybdenum compounds and sodium compounds as raw materials. In this document, both when molybdenum compounds and sodium compounds are used as fluxes and when compounds containing molybdenum and sodium are used as fluxes are considered to be when molybdenum compounds and sodium compounds are used as fluxes, i.e., when molybdenum compounds and sodium compounds are present.

[0129] Compounds containing molybdenum and potassium suitable as fluxes can be produced in the firing process using, for example, relatively cheap and readily available molybdenum compounds and potassium compounds as raw materials. In this document, both when molybdenum compounds and potassium compounds are used as fluxes and when compounds containing molybdenum and potassium are used as fluxes are considered to be when molybdenum compounds and potassium compounds are used as fluxes, i.e., when molybdenum compounds and potassium compounds are present.

[0130] The above-mentioned molybdenum compounds may be used alone or in combination of one or more molybdenum compounds.

[0131] Sodium molybdate (Na2Mo n O 3n+1 , wherein n is 1 to 3) contains sodium and can therefore be used as the sodium compound described below.

[0132] Potassium molybdate (K2Mo n O 3n+1 , wherein n is 1 to 3) contains potassium and can therefore be used as the potassium compound described below.

[0133] (Sodium compounds)

[0134] There is no particular limitation on the sodium compound. Examples of the sodium compound include sodium carbonate, sodium molybdate, sodium oxide, sodium sulfate, sodium hydroxide, sodium nitrate, sodium chloride, and metallic sodium. Among them, sodium carbonate, sodium molybdate, sodium oxide, or sodium sulfate is preferably used from the viewpoint of industrial availability and operability.

[0135] The above-mentioned sodium compounds may be used alone or in combination of one or more sodium compounds.

[0136] Similar to the above, sodium molybdate contains molybdenum and thus can be used as the above-mentioned molybdenum compound.

[0137] (Potassium compounds)

[0138] There is no particular limitation on the potassium compound. Examples of the potassium compound include potassium chloride, potassium chlorite, potassium chlorate, potassium sulfate, potassium hydrogen sulfate, potassium sulfite, potassium hydrogen sulfite, potassium nitrate, potassium carbonate, potassium hydrogen carbonate, potassium acetate, potassium oxide, potassium bromide, potassium bromate, potassium hydroxide, potassium silicate, potassium phosphate, potassium hydrogen phosphate, potassium sulfide, potassium hydrogen sulfide, potassium molybdate, and potassium tungstate. In this case, the potassium compound and the molybdenum compound include isomers. Among them, potassium carbonate, potassium hydrogen carbonate, potassium oxide, potassium hydroxide, potassium chloride, potassium sulfate, or potassium molybdate is preferably used, and potassium carbonate, potassium hydrogen carbonate, potassium chloride, potassium sulfate, or potassium molybdate is more preferably used.

[0139] The above potassium compounds may be used alone or in combination of one or more potassium compounds.

[0140] Similar to the above, potassium molybdate contains molybdenum and thus can be used as the above-mentioned molybdenum compound.

[0141] In the method for producing forsterite particles according to this embodiment, the use of magnesium hydroxide, silicon dioxide, and molybdenum trioxide can be exemplified as a preferred raw material combination.

[0142] Similarly, in the method for producing forsterite particles according to this embodiment, the use of magnesium hydroxide, silicon dioxide, and sodium molybdate or a hydrate thereof can be exemplified as a preferred raw material combination.

[0143] Similarly, in the production method of forsterite particles according to this embodiment, the use of magnesium hydroxide, silicon dioxide, molybdenum trioxide, and sodium molybdate or a hydrate thereof can be exemplified as a preferred raw material combination.

[0144] Sintering magnesium compounds and silicon or silicon compounds in the presence of sodium compounds and sodium compounds or in the presence of molybdenum compounds and potassium compounds makes it easy to adjust the size of the produced forsterite particles, and can easily produce forsterite particles with a low degree of aggregation or no aggregation. Although the reason is unclear, the following reasons can be imagined. For example, because K2MoO4 and Na2MoO4 are stable compounds and are unlikely to volatilize during the sintering step, K2MoO4 and Na2MoO4 are unlikely to cause severe reactions during the volatilization process, and are likely to control the growth of forsterite particles. Molten K2MoO4 and Na2MoO4 exhibit solvent-like functions, and it is conceivable that the size of the particles can be increased by increasing, for example, the reaction time. Because molten K2MoO4 and Na2MoO4 exhibit such solvent-like functions, it is conceivable that the forsterite particles are dispersed and are unlikely to aggregate.

[0145] In the production method of forsterite particles according to this embodiment, a molybdenum compound is used as a flux. In this specification, the production method in which the molybdenum compound is used as a flux is referred to as a "flux method" in some cases. It is conceivable that after the magnesium compound, silicon or silicon compound and the oxide of molybdenum react at high temperature to form magnesium molybdate and silicomolybdic acid due to this firing, when the magnesium molybdate decomposes into magnesium oxide and molybdenum oxide and silicomolybdic acid decomposes into silicon oxide and molybdenum oxide at a higher temperature, a portion of the molybdenum oxide is incorporated into the forsterite particles. Most of the molybdenum oxide evaporates and is removed outside the system. When the molybdenum compound used is sodium molybdate or potassium molybdate, the molybdenum oxide is likely to react with the alkali metal compound to form molybdate again, which is hardly discharged outside the system and remains in the system.

[0146] As for the formation mechanism of the molybdenum compound contained in the forsterite particles, it can be thought that, more specifically, Mo-O-Mg and Mo-O-Si are formed in the forsterite particles by the reaction of Mg atoms and Si atoms, most of Mo is eliminated by high-temperature sintering, and a part of the molybdenum forms Mo-O-Mg and Mo-O-Si and remains in the forsterite particles.

[0147] The molybdenum oxide not incorporated into the forsterite particles can be collected by sublimation and reused. This enables the amount of molybdenum oxide adhering to the surface of the forsterite particles to be reduced and the inherent properties of the forsterite particles to be presented to the maximum extent.

[0148] On the other hand, the alkali metal salt of the molybdenum oxyanion does not volatilize within the firing temperature range and can be easily collected by washing after firing. Therefore, the amount of molybdenum compound released to the outside of the firing furnace is reduced, thereby significantly reducing production costs.

[0149] It is conceivable that when, for example, a molybdenum compound and a sodium compound are used in combination in a flux method, the molybdenum compound and the sodium compound react to form sodium molybdate. At the same time, it is conceivable that the molybdenum compound reacts with a magnesium compound and a silicon compound to form magnesium molybdate and silicomolybdic acid, and that the magnesium molybdate and silicomolybdic acid are decomposed by further high-temperature sintering to form forsterite. It is conceivable that the evaporation of the above-mentioned flux (sublimation of MoO3) is suppressed in such a manner that magnesium molybdate and silicomolybdic acid decompose in a liquid phase in the presence of, for example, sodium molybdate to form forsterite and then grow crystals, and forsterite particles with a low degree of aggregation or no aggregation can be easily obtained.

[0150] (Metal Compounds)

[0151] The metal compound may be used in the firing as needed. The method for producing forsterite particles according to this embodiment may include a step of mixing a magnesium compound, silicon or a silicon compound, a molybdenum compound, a sodium compound and / or a potassium compound with a metal compound as a mixture before the firing step (mixing step), and may include a step of firing the mixture (firing step).

[0152] The metal compound is not particularly limited, and preferably includes at least one selected from the group consisting of Group II metal compounds and Group III metal compounds.

[0153] Examples of the Group 2 metal compound include calcium compounds, strontium compounds, and barium compounds.

[0154] Examples of the Group III metal compound include scandium compounds, yttrium compounds, lanthanum compounds, and cerium compounds.

[0155] The above-mentioned metal compound means an oxide, hydroxide, oxycarbide or chloride of a metal element. Examples of yttrium compounds include yttrium oxide (Y2O3), yttrium hydroxide and yttrium oxycarbide. Among them, the metal compound is preferably an oxide of a metal element. These metal compounds include isomers.

[0156] Among them, metal compounds of the third period elements, metal compounds of the fourth period elements, metal compounds of the fifth period elements, and metal compounds of the sixth period elements are preferred; metal compounds of the fourth period elements and metal compounds of the fifth period elements are more preferred; and metal compounds of the fifth period elements are further preferred. In particular, calcium compounds, yttrium compounds, or lanthanum compounds are preferably used; calcium compounds or yttrium compounds are more preferably used; and yttrium compounds are particularly preferably used.

[0157] The metal compound is preferably used in a proportion of, for example, 0 mass % to 1.2 mass % (eg, 0 mol % to 1 mol %) relative to the amount of the magnesium compound used in the mixing step.

[0158] In the method for producing forsterite particles according to this embodiment, there is no particular limitation on the blending amount of the magnesium compound, silicon or silicon compound, and molybdenum compound used. In the raw material, for example, in the mixture, 1 to 500 parts by mass or 5 to 200 parts by mass of the molybdenum compound may be blended with 100 parts by mass of the total blending amount of the magnesium compound and silicon or silicon compound.

[0159] In the method for producing forsterite particles according to this embodiment, the molar ratio of magnesium to silicon (Mg / Si) in the raw material (e.g., in the mixture) is substantially 2. Since MgO that may be excessively produced can be easily removed, Mg / Si may be 2 or more, 2 to 3, or 2 to 2.5.

[0160] In the method for producing forsterite particles according to this embodiment, the molar ratio of molybdenum in the molybdenum compound to magnesium and silicon in the magnesium compound and silicon compound in the raw material (for example, in a mixture) (molybdenum / (magnesium+silicon)) is preferably 0.001 or more, more preferably 0.01 or more, further more preferably 0.02 or more, and particularly preferably 0.04 or more.

[0161] The upper limit of the molar ratio of molybdenum in the molybdenum compound to magnesium and silicon in the magnesium compound and silicon compound in the raw material (e.g., in the mixture) can be appropriately determined. From the viewpoint of reducing the amount of molybdenum compound used and increasing production efficiency, for example, the molar ratio (molybdenum / (magnesium+silicon)) can be 5 or less, 3 or less, 1 or less, or 0.5 or less.

[0162] As examples of numerical ranges for the molar ratio (molybdenum / (magnesium+silicon)) in the raw materials (eg, in a mixture), for example, the value of molybdenum / (magnesium+silicon) may be 0.001 to 5, 0.01 to 3, 0.02 to 1, or 0.04 to 0.5.

[0163] As the amount of molybdenum used relative to magnesium and silicon increases, as shown in Table 2 in the following Examples, forsterite particles having larger sizes shown in the above particle size distribution tend to be obtained.

[0164] Use of various compounds within the above range allows the amount of the molybdenum compound contained in the obtained forsterite particles to be sufficient, and allows forsterite particles having a controlled shape and size to be easily obtained.

[0165] [Firing steps]

[0166] The firing step is a step of firing the mixture. The forsterite particles according to this embodiment are obtained by firing the mixture. The production method is called a flux method as described above.

[0167] The flux method is classified as a solution method. More specifically, the flux method is a method for growing crystals using the fact that the crystal-flux binary phase diagram shows eutectic. It is inferred that the mechanism of the flux method is as follows. That is, heating a mixture of a melt and a flux causes the melt and the flux to become a liquid phase. Because the flux is a fusing agent, that is, because the melt-flux binary phase diagram shows eutectic, the melt melts at a temperature below its melting point to form a liquid phase. The evaporation of the flux in this state causes the flux concentration to decrease, that is, the effect of reducing the melting point of the melt by the flux is weakened, so that the evaporation of the flux serves as a driving force for inducing the crystal growth of the melt (flux evaporation method). The melt and the flux can induce the crystal growth of the melt by cooling the liquid phase (slow cooling method).

[0168] The flux method has the following advantages: crystals can be grown at temperatures well below the melting point, the crystal structure can be precisely controlled, and self-shaped crystals can be formed.

[0169] Although the mechanism of producing forsterite particles by the flux method using a molybdenum compound as a flux is not clear, the mechanism is presumed to be as follows, for example. That is, magnesium compounds and silicon compounds are fired in the presence of molybdenum compounds so that magnesium molybdate and silicomolybdic acid are formed. In this case, magnesium molybdate and silicomolybdic acid grow forsterite crystals at a temperature lower than the melting point of forsterite, as understood from the above description. Evaporation, for example, decomposes magnesium molybdate and silicomolybdic acid, and forsterite particles can be obtained by crystal growth. That is, the molybdenum compound is used as a flux, and forsterite particles are produced from an intermediate of magnesium molybdate and silicomolybdic acid.

[0170] Forsterite particles containing molybdenum and in which the molybdenum is unevenly distributed in the surface layer of each forsterite particle can be produced by a flux method.

[0171] The firing method is not particularly limited, and may be a known common method. It is conceivable that the magnesium compound, silicon or a silicon compound, and the molybdenum compound react to form magnesium molybdate and silicomolybdic acid during firing. In addition, it is conceivable that when the firing temperature reaches 700° C. or more, magnesium molybdate and silicomolybdic acid decompose to form forsterite particles. In the forsterite particles, it is conceivable that magnesium molybdate and silicomolybdic acid decompose into magnesium oxide, silicon dioxide, and molybdenum oxides, and then when forsterite is formed, the molybdenum compound is incorporated into the forsterite particles.

[0172] There is no particular limitation on the state of the magnesium compound, silicon or silicon compound, and molybdenum compound during firing. The magnesium compound, silicon or silicon compound, and molybdenum compound may be present in the same space where the molybdenum compound can act on the magnesium compound and silicon or silicon compound. In particular, the powder of the molybdenum compound, the powder of the magnesium compound, and the powder of the silicon or silicon compound may be simply mixed, may be mechanically mixed using a crusher or the like, may be mixed using a mortar or the like, or may be mixed in a dry or wet state.

[0173] The firing temperature conditions are not particularly limited and may be appropriately determined in consideration of the size of the target forsterite particles, the formation of the molybdenum compound in the forsterite particles, or the shape of the forsterite particles, etc. The firing temperature may be 700° C. or higher, which is close to the decomposition temperature of magnesium molybdate and silicomolybdic acid; may be 800° C. or higher; may be 900° C. or higher; may be 950° C. or higher; or may be 1,000° C. or higher.

[0174] As the firing temperature increases, forsterite particles having a controlled shape and a larger size tend to be obtained. From the viewpoint of efficiently producing such forsterite particles, the firing temperature is preferably 950°C or higher, more preferably 1,000°C or higher, further preferably 1,100°C or higher, and particularly preferably 1,200°C or higher.

[0175] Generally, in order to control the shape of forsterite particles obtained after firing, firing needs to be performed at a high temperature exceeding 1,800° C. (close to the melting point of forsterite). This is significantly problematic for industrial use from the viewpoint of the load on the firing furnace and fuel cost.

[0176] According to one embodiment of the present invention, forsterite particles can be efficiently formed at low cost even if the maximum firing temperature for firing the magnesium compound and silicon or the silicon compound is 1,800° C. or less, for example. This contributes to reducing energy costs and reducing environmental load.

[0177] According to the method for producing forsterite particles according to this embodiment, even if the firing temperature is 1,600° C. or less, which is much lower than the melting point of forsterite, automorphic forsterite particles can be formed regardless of the shape of the precursor. From this viewpoint, the firing temperature is preferably 1,500° C. or less, more preferably 1,400° C. or less, and further preferably 1,300° C. or less.

[0178] The calcination temperature of the magnesium compound and silicon or the silicon compound in the calcination step may have a numerical range of, for example, 800°C to 1,600°C, 900°C to 1,500°C, 950°C to 1,400°C, or 1,000°C to 1,300°C.

[0179] From the viewpoint of production efficiency, the heating rate may be 20° C. / h to 600° C. / h, 40° C. / h to 500° C. / h, or 80° C. / h to 400° C. / h.

[0180] Regarding the firing time, heating to a predetermined firing temperature is preferably performed in the range of 15 minutes to 10 hours. The holding time at the firing temperature may be 5 minutes or more, preferably in the range of 5 minutes to 1,000 hours, and more preferably in the range of 1 hour to 30 hours. In order to effectively form forsterite particles, the firing temperature holding time is more preferably 2 hours or more, and particularly preferably 2 hours to 24 hours.

[0181] Selecting conditions including, for example, a firing temperature of 800° C. to 1,600° C. and a firing temperature holding time of 2 hours to 24 hours makes it easy to obtain the molybdenum-containing forsterite particles according to this embodiment.

[0182] If the effects of the present invention are obtained, there is no particular limitation on the firing atmosphere; preferably, it is an oxygen-containing atmosphere such as air or oxygen; or an inert atmosphere such as nitrogen, argon or carbon dioxide; when cost is considered, air atmosphere is more preferred.

[0183] The firing device does not need to be limited, and may be a so-called firing furnace. The firing furnace is preferably made of a material that does not react with the sublimated molybdenum oxide. In addition, it is preferred to use a firing furnace with high airtightness so that the molybdenum oxide is effectively used.

[0184] [Cooling Step]

[0185] The method for producing forsterite particles may include a cooling step. The cooling step is a step of cooling the forsterite particles crystal-grown in the firing step.

[0186] There is no particular limitation on the cooling rate. The cooling rate is preferably 1°C / h to 1,000°C / h, more preferably 5°C / h to 500°C / h, and further more preferably 50°C / h to 100°C / h. The cooling rate is preferably 1°C / h or more because the production time can be reduced. On the other hand, the cooling rate is preferably 1,000°C / h or less because the firing container is hardly broken due to thermal shock and can be used for a long time.

[0187] There is no particular limitation on the cooling method, and natural cooling may be used. In the cooling method, a cooling device may be used.

[0188] [Molybdenum removal step]

[0189] The method for producing forsterite particles according to this embodiment may further include a molybdenum removing step of removing at least a portion of the molybdenum after the calcining step, as necessary.

[0190] Examples of methods for removing molybdenum include washing and high temperature treatment. These may be performed in combination.

[0191] Since molybdenum sublimes during firing as described above, controlling the firing time or firing temperature, etc. can control the content of molybdenum present in the surface layer of each forsterite particle, and can control the content or state of molybdenum present in the portion (inner layer) other than the surface layer of the forsterite particle.

[0192] Molybdenum may adhere to the surface of forsterite particles. Molybdenum may be removed by washing with water, an aqueous ammonia solution, an aqueous sodium hydroxide solution, or the like instead of sublimation.

[0193] In this operation, the molybdenum content in the forsterite particles can be controlled by appropriately changing the amount of water used, the concentration or amount of the ammonia solution or the sodium hydroxide solution used, the washed portion and the washing time, etc.

[0194] An example of the high-temperature treatment method is a method in which a mixture of forsterite particles and a molybdenum compound is heated to a temperature higher than or equal to the sublimation point or boiling point of the molybdenum compound.

[0195] [Crushing Step]

[0196] Because the forsterite particles aggregate, the fired product obtained by the firing step does not satisfy the preferred particle size range for the application considered in some cases. Therefore, the forsterite particles may be pulverized as needed to satisfy the preferred particle size range.

[0197] There is no particular limitation on the method for pulverizing the fired product. Conventionally known pulverizers such as a ball mill, a jaw crusher, a jet mill, a disc mill, a spectro mill, a grinder, and a mixer mill can be used.

[0198] [Grading steps]

[0199] In order to adjust the particle size range, the fired product containing forsterite particles obtained by the firing step may be appropriately subjected to classification treatment. The term "classification treatment" refers to an operation of grouping particles according to particle size.

[0200] Classification can be carried out in wet or dry form. From the viewpoint of productivity, dry classification is preferred. Examples of dry classification include classification by screening and pneumatic classification by the difference between centrifugal force and fluid resistance. From the viewpoint of classification accuracy, pneumatic classification is preferred, and can be carried out using a classifier such as an air classifier, a spiral air classifier, a forced vortex centrifugal classifier or a quasi-free vortex centrifugal classifier that utilizes the Coanda effect.

[0201] The above-mentioned pulverization step or classification step may be performed at a necessary stage. For example, the average size of the obtained forsterite particles can be adjusted by whether to perform pulverization and classification or by selecting the conditions thereof.

[0202] The forsterite particles according to one embodiment or the forsterite particles obtained by the production method according to one embodiment have a low degree of aggregation or do not aggregate. Therefore, the forsterite particles are likely to exhibit inherent properties, the handleability is more excellent, and from the viewpoint that the dispersibility of the forsterite particles is more excellent when the forsterite particles are dispersed in a dispersion medium and used, it is preferred.

[0203] According to the method for producing forsterite particles according to the above-mentioned embodiment, forsterite particles with low or no aggregation can be easily produced. Therefore, the method has the following excellent advantages: even without performing a pulverization step or a classification step, forsterite particles with excellent target properties can be produced with high productivity.

[0204] According to the method for producing forsterite particles according to the above-described embodiment, high-quality forsterite particles containing molybdenum and having a controlled shape can be efficiently produced.

[0205] [Example]

[0206] The present invention is described in further detail below with reference to Examples. The present invention is not limited to the following Examples.

[0207] <Production of forsterite particles>

[0208] [Example 1]

[0209] 5.8 g of magnesium hydroxide ( 5, produced by Kyowa Chemical Industry Co., Ltd.), 3.0 g of silicon dioxide (VN3, produced by Tosoh Silica Corporation), 8.8 g of sodium molybdate dihydrate (a reagent produced by Kanto Chemical Co., Inc.), 30 g of ion exchange water and 120 g of Zirconia beads were then mixed and crushed for 120 minutes using a paint stirrer to obtain a mixture. The obtained mixture was transferred to a metal bucket and dried in an oven at 120°C, followed by crushing the dry matter with a mixer (manufactured by Osaka Chemical Co., Ltd.). The crushed raw materials were placed in a crucible and fired at 1,500°C for 10 hours in a ceramic electric furnace. Heating was performed at 2°C / min. After cooling, the crucible was taken out and a white powder was obtained.

[0210] Subsequently, the obtained white powder was transferred to a beaker, and 200 g of ion exchange water was added to the beaker, followed by stirring for 3 hours, thereby dissolving sodium molybdate in the ion exchange water. Next, 5C filter paper was used for filtration by suction filtration, and the obtained particles were dried at 120° C., thereby obtaining 6.8 g of white powder of Example 1.

[0211] [Example 2]

[0212] 5.8 g of magnesium hydroxide ( 5, produced by Kyowa Chemical Industry Co., Ltd.), 3.0 g of silicon dioxide (VN3, produced by Tosoh Silica Corporation), 0.88 g of molybdenum trioxide (produced by Nippon Inorganic Colour & Chemical Co., Ltd.) and 100 g of Zirconia beads were then mixed and pulverized at 200 rpm for 60 minutes using a planetary grinder (P-5, manufactured by Fritsch GmbH), thereby obtaining a mixture. The obtained mixture was put into a crucible and fired at 1,300° C. for 10 hours in a ceramic electric furnace. Heating was performed at 2° C. / min. After cooling, the crucible was taken out and a white powder was obtained.

[0213] Subsequently, the obtained white powder was transferred to a beaker, and 200 g of 0.5% ammonia water was added to the beaker, followed by stirring for 3 hours, thereby dissolving the remaining molybdenum trioxide in the ammonia water. Next, 5C filter paper was used to filter by suction filtration, and the obtained particles were dried at 120° C., thereby obtaining 6.8 g of white powder of Example 2.

[0214] [Example 3]

[0215] A white powder of Example 3 was obtained in the same manner as used in Example 1, except that the firing temperature was 1,000° C. and the heating rate was 5° C. / min.

[0216] [Example 4]

[0217] A white powder of Example 4 was obtained in the same manner as used in Example 1, except that the firing temperature was 1,300° C. and the heating rate was 5° C. / min.

[0218] [Example 5]

[0219] A white powder of Example 5 was obtained in the same manner as used in Example 2, except that the firing temperature was 1,100° C. and the heating rate was 5° C. / min.

[0220] [Example 6]

[0221] 8.28 g of magnesium hydroxide ( 5, produced by Kyowa Chemical Industry Co., Ltd.), 4.29 g of silicon dioxide (VN3, produced by Tosoh Silica Corporation), 6.96 g of sodium molybdate dihydrate (a reagent produced by Kanto Chemical Co., Inc.), 4.11 g of molybdenum trioxide (produced by Nippon Inorganic Colour & Chemical Co., Ltd.), 30 g of ion exchange water and 120 g of Zirconia beads were then mixed and crushed for 120 minutes using a paint stirrer to obtain a mixture. The obtained mixture was transferred to a metal bucket and dried in an oven at 120°C, followed by crushing the dry matter with a mixer (manufactured by Osaka Chemical Co., Ltd.). The crushed raw materials were placed in a crucible and fired at 900°C for 10 hours in a ceramic electric furnace. Heating was performed at 5°C / min. After cooling, the crucible was taken out and a white powder was obtained.

[0222] Subsequently, the obtained white powder was transferred to a beaker, and 200 g of ion exchange water was added to the beaker, followed by stirring for 3 hours, thereby dissolving sodium molybdate in the ion exchange water. Next, 5C filter paper was used to filter by suction filtration, and the obtained particles were dried at 120° C., thereby obtaining 10.2 g of white powder of Example 6.

[0223] [Example 7]

[0224] A white powder of Example 7 was obtained in the same manner as used in Example 6 except that the calcination temperature was 1,100°C.

[0225] [Example 8]

[0226] A white powder of Example 8 was obtained in the same manner as used in Example 6 except that the calcination temperature was 1,300°C.

[0227] [Example 9]

[0228] A white powder of Example 9 was obtained in the same manner as used in Example 6, except that the firing temperature was 1,500° C. and the heating rate was 2° C. / min.

[0229] [Examples 10 to 13]

[0230] White powders of Examples 10 to 13 were obtained in the same manner as used in Example 4 except that the amount of sodium molybdate dihydrate used was changed to the mass shown in Table 2.

[0231] [Comparative Example 1]

[0232] 5.8 g of magnesium hydroxide ( 5, produced by Kyowa Chemical Industry Co., Ltd.), 3.0 g of silicon dioxide (VN3, produced by Tosoh Silica Corporation), and 100 g of Zirconia beads were then mixed and pulverized using a planetary grinder (P-5, manufactured by Fritsch GmbH) for 60 minutes to obtain a mixture. The obtained mixture was placed in a crucible and fired in a ceramic electric furnace at 1,100°C for 10 hours. Heating was performed at 5°C / min. After cooling, the crucible was taken out and a white powder of Comparative Example 1 was obtained.

[0233] [Comparative Example 2]

[0234] A white powder of Comparative Example 2 was obtained in the same manner as used in Comparative Example 1 except that the calcination temperature was 1,300°C.

[0235] <Evaluation>

[0236] Sample powders were taken out from the powders obtained in each of Examples and Comparative Examples and evaluated as described below.

[0237] [Crystal structure analysis: X-ray diffraction (XRD) method]

[0238] The sample powder was filled into a 0.5 mm deep holder for measuring samples, the holder was set on a wide-angle X-ray diffraction (XRD) instrument (Ultima IV, manufactured by Rigaku Corporation), and the sample powder was measured under conditions including Cu Kα radiation, 40 kV / 40 mA, a scanning speed of 2° / min, and a scanning range of 10° to 70°.

[0239] [Measurement of specific surface area of ​​forsterite particles]

[0240] The specific surface area of ​​the forsterite particles was measured using a specific surface area analyzer (BELSORP-mini, manufactured by MicrotracBEL Corporation). The surface area per gram of the sample measured from nitrogen adsorption by the BET method was calculated as the specific surface area (m 2 / g).

[0241] [Primary particle size]

[0242] The primary particle size of the forsterite particles was calculated as a converted particle size based on the above specific surface area, assuming that the particles were perfectly spherical. The following conversion equation was used.

[0243] Primary particle size Dsa [nm] = 6,000 / (density [g / cm 3 ]×specific surface area [m 2 / g])

[0244] In the embodiment, the density of the forsterite particles is calculated to be 3.0 g / cm 3 .

[0245] [Measurement of size distribution]

[0246] The particle size distribution of the sample powder was measured in a dry method using a laser diffraction particle size distribution analyzer (HELOS (H3355) & RODOS, manufactured by Japan Laser Corporation) under conditions including a dispersion pressure of 3 bar and a suction pressure of 90 mbar. The particle size at the point where the cumulative volume distribution curve intersects the horizontal axis at 50% was determined as D 50 .

[0247] [X-ray fluorescence (XRF) analysis]

[0248] About 70 mg of the sample powder was put on filter paper, covered with a PP film, and subjected to X-ray fluorescence (XRF) analysis using an X-ray fluorescence analyzer Primus IV (manufactured by Rigaku Corporation) under the following conditions.

[0249] Measurement conditions

[0250] EZ Scan Mode

[0251] Measuring elements: F to U

[0252] Measuring time: Standard

[0253] Measuring diameter: 10mm

[0254] Residue (remaining component): None

[0255] The magnesium content, silicon content and molybdenum content of the forsterite particles measured by XRF analysis were converted into oxide contents, thereby obtaining the results of the MgO content (Mg1) relative to 100% by mass of the forsterite particles, the SiO2 content (S1) relative to 100% by mass of the forsterite particles, and the MoO3 content (Mo1) relative to 100% by mass of the forsterite particles.

[0256] [XPS surface analysis]

[0257] Surface element analysis of the sample powder was performed by X-ray photoelectron spectroscopy (XPS) using Quantera SXM manufactured by Ulvac-Phi Inc. and monochromatic Al Kα radiation as an X-ray source. In the measurement of a 1,000 μm square area, an average value of n=3 measurements in atomic % was obtained for each element.

[0258] The magnesium and silicon contents of the surface layer of each forsterite particle measured by XPS analysis and the molybdenum content of the surface layer are converted into oxide contents, thereby determining the MgO content (Mg2) (mass %) relative to 100 mass % of the surface layer of the forsterite particle, the SiO2 content (S2) (mass %) relative to 100 mass % of the surface layer of the forsterite particle, and the MoO3 content (Mo2) (mass %) relative to 100 mass % of the surface layer of the forsterite particle.

[0259] <Results>

[0260] The values ​​obtained by the above evaluation are shown in Tables 1 to 2. In addition, "ND" is an abbreviation for "Not Detected" and means not detectable.

[0261] [Table 1]

[0262]

[0263] [Table 2]

[0264]

[0265] The SEM images of the powders of the examples and comparative examples taken with a scanning electron microscope (SEM) are shown in Figures 1 to 11 In each of the powders of Examples 1 to 9, a large number of beautiful polyhedral particles were observed, indicating that the crystal shape of the particles was controlled during the production process. On the other hand, in each of the powders of Comparative Examples 1 and 2, irregular shaped particles without a specific shape were observed.

[0266] The results of XRD analysis are shown in Fig.12 In the samples of Examples and Comparative Examples, a peak (unlabeled peak) derived from forsterite (Mg2SiO4) was found.

[0267] From the results of the above-mentioned SEM observation and XRD analysis, it was confirmed that the powder obtained in each of the examples and comparative examples was composed of forsterite particles containing forsterite.

[0268] In the sample powders of Examples 1 to 9, almost no peaks derived from impurities were observed ( Fig.12, "-" in the impurity detection in Table 1). On the other hand, in the sample powders of Comparative Examples 1 and 2, peaks derived from impurities such as enstatite (MgSiO3) were clearly detected ( Fig.12 (peaks marked with ● in Table 1) (“+” in the impurity detection in Table 1). This indicates that in the sample powders of Comparative Examples 1 and 2, the production reaction of forsterite was not completed and unreacted reactants remained.

[0269] This shows that, in each of the examples in which the magnesium compound and the silicon compound are fired in the presence of the molybdenum compound, the production reaction of forsterite proceeds well even at a relatively low firing temperature of 900° C. to 1,500° C., and high-quality forsterite particles having a reduced impurity content and a controlled shape can be efficiently produced.

[0270] After the forsterite particles were dispersed in ethanol, the forsterite particles were observed with TEM and the aggregation degree of the forsterite particles was evaluated according to the following criteria.

[0271] +: Aggregation of particles was observed.

[0272] -: No obvious particle aggregation was found.

[0273] Although significant aggregation or fusion of the forsterite particles of Comparative Examples 1 and 2 was found (aggregation degree: +), significant aggregation of the forsterite particles of Examples 1 to 9 was not found (aggregation degree: -).

[0274] This shows that, in each of the Examples in which the magnesium compound and the silicon compound were fired in the presence of the molybdenum compound, the reaction during firing proceeded well, and forsterite particles with a low degree of aggregation or no aggregation could be easily produced.

[0275] In a comparison between Examples 2 and 4 at the same firing temperature, the aggregation degree of the forsterite particles obtained in Example 4, in which the raw material used was Na2MoO4.2H2O, remained lower than that of the forsterite particles obtained in Example 2.

[0276] This shows that calcining a magnesium compound and a silicon compound in the presence of a molybdenum compound allows forsterite particles with a low degree of aggregation to be easily obtained.

[0277] In the examples (referring to, for example, Examples 1, 3 and 4), as the firing temperature is higher, forsterite particles having larger sizes tend to be obtained.

[0278] As described above, controlling the firing temperature enables the size of the forsterite particles to be controlled, and enables forsterite particles having a desired size to be produced.

[0279] The values ​​of the above-mentioned MgO content (Mg1), SiO2 content (S1), MoO3 content (Mo1), MgO content (Mg2), SiO2 content (S2) and MoO3 content (Mo2) are shown in Table 1.

[0280] From the results of the MoO3 content (Mo1), it was confirmed that forsterite particles containing molybdenum were obtained.

[0281] From the results of the MoO3 content (Mo2), the forsterite particles of Examples 1 to 9 have a surface layer containing molybdenum and can be expected to exhibit various effects such as catalytic activity due to molybdenum.

[0282] The calculation results of the surface layer uneven distribution ratio (Mo2 / Mo1) of MoO3 content (Mo2) to MoO3 content (Mo1) are shown in Table 1.

[0283] As is clear from the results of the surface layer uneven distribution ratio (Mo2 / Mo1), in the forsterite particles of Examples 1, 4, and 8, the molybdenum content of the surface layer of each forsterite particle measured by XPS surface analysis is greater than the molybdenum content measured by XRF analysis. It is thus confirmed that molybdenum is unevenly distributed in the surface layer of the forsterite particles, and various effects due to molybdenum can be expected to be effectively exhibited.

[0284] The forsterite particles obtained in Examples 2 and 5, in which the raw material used was MoO3, had a higher MoO3 content (Mo1) than the forsterite particles obtained in other Examples, although the (magnesium compound + silicon compound) / molybdenum compound ratio of the raw material was 10 / 1. In Examples 6 to 9, in which the raw material used was MoO3, the MoO3 content (Mo1) tended to be high.

[0285] As described above, controlling the amount or type of the molybdenum compound used enables control of the amount of molybdenum contained in the forsterite particles, and enables production of forsterite particles containing a desired amount of molybdenum.

[0286] Referring to Table 2, as the molar ratio of molybdenum to magnesium and silicon (Mo / (Mg+Si)) in the raw material is higher, forsterite particles with larger sizes tend to be obtained.

[0287] As described above, controlling the amount of the molybdenum compound used enables the size of the forsterite particles to be controlled, and enables the production of forsterite particles having a desired size.

[0288] The components and combinations thereof in the embodiments are examples. Components may be added, omitted, substituted and modified without departing from the spirit of the invention. The present invention is not limited to the embodiments and is only limited to the scope of the appended claims.

Claims

1. A forsterite particle containing molybdenum.

2. The forsterite particles according to claim 1, wherein the content of molybdenum in the forsterite particles is 0.05% by mass to 35% by mass (Mo1) calculated as MoO3 relative to 100% by mass of the forsterite particles as measured by XRF analysis of the forsterite particles.

3. The forsterite particles according to claim 1 or 2, wherein the content of molybdenum in the surface layer of each of the forsterite particles is a content (Mo2) of 0.05% by mass to 25% by mass in terms of MoO3 relative to 100% by mass of the surface layer of the forsterite particles as determined by XPS surface analysis of the forsterite particles. 4 . The forsterite particles according to claim 1 , wherein an average size of primary particles of the forsterite particles is 0.1 μm to 100 μm.

5. The forsterite particles according to any one of claims 1 to 4, wherein the specific surface area of ​​the forsterite particles measured by the BET method is 0.02 m 2 / g to 20m 2 / g.

6. A method for producing forsterite particles according to any one of claims 1 to 5, comprising calcining a magnesium compound and silicon or a silicon compound in the presence of a molybdenum compound. 7 . The method for producing forsterite particles according to claim 6 , wherein the molybdenum compound is at least one selected from the group consisting of molybdenum trioxide, lithium molybdate, potassium molybdate, and sodium molybdate.

8. The method for producing forsterite particles according to claim 6 or 7, wherein the magnesium compound and silicon or the silicon compound are fired at a temperature of 800°C to 1,600°C.

9. The method for producing forsterite particles according to any one of claims 6 to 8, wherein a molar ratio of molybdenum to magnesium and silicon (Mo / (Mg+Si)) in the fired raw material is 0.001 to 5.