Preparation method of efficient anthraquinone degradation product regeneration catalyst

The preparation of hollow alumina nanoparticles by reacting in aqueous ethanol solution and kneading with acid and additives, the problems of short service life and poor reactive properties of existing catalysts are solved, and high-efficiency and long-life regeneration of anthraquinone degradable substances are achieved Catalysts reduce production costs and environmental pollution.

CN118949964APending Publication Date: 2024-11-15GUANGXI RES INST OF CHEM IND CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410886488.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-03
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing alumina catalysts produced by hydrogen peroxide with anthraquinone method have short service life, poor living performance and complex processes, resulting in high production costs and serious environmental pollution.

Method used

The reaction of organic acid, organic alkali and aluminum sources in aqueous ethanol solution is used, template agent and metal salt are added, and hollow alumina sphere nanoparticles are prepared by stirring, drying and high-temperature roasting, and then kneading with acid and additives and extruding strips to form High-efficiency anthraquinone degradation catalyst.

Benefits of technology

The prepared catalyst has a high specific surface, strength and large pore size, and its activity reaches more than 7.4 g/L, and its service life exceeds 163 days. It significantly reduces the accumulation and production cost of anthraquinone degradants and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004926190730000111
    Figure BDA0004926190730000111
Patent Text Reader

Abstract

The invention discloses a preparation method of a high-efficiency anthraquinone degradation product regeneration catalyst, which comprises the following steps: (1) dissolving organic acid in a mixed solution of ethanol and water, adding organic alkali to adjust the pH value, then adding a template agent, an aluminum source and at least one IIA metal or salt containing the IIA metal, mixing and stirring until a full reaction, taking out gel, drying, and roasting at high temperature to obtain an anthraquinone degradation product regeneration catalyst; the aluminum oxide hollow sphere nano-particles are obtained; and (2) mixing and kneading the alumina hollow sphere nanoparticles obtained in the step (1) with acid and an auxiliary agent, performing extrusion molding, drying and performing high-temperature roasting to obtain the anthraquinone degradation product regeneration catalyst. The preparation process is simple and easy to control, and the prepared regenerated catalyst has the advantages of long service life and good regeneration activity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of producing hydrogen peroxide by an anthraquinone process, and particularly relates to a method for preparing a highly efficient anthraquinone degradation product regeneration catalyst. Background Art

[0002] The chemical formula of hydrogen peroxide is H2O2, commonly known as hydrogen peroxide. It is a colorless, transparent liquid and a strong oxidant. It is widely used in chemical, papermaking, printing and dyeing, medicine and other fields.

[0003] At present, hydrogen peroxide is widely used and in great demand, and has broad market prospects. Hydrogen peroxide synthesis methods include inorganic chemical reaction method, hydrolysis peroxide method, hydrocarbon self-oxidation method, isopropanol oxidation method, electrolysis method, anthraquinone method, direct synthesis method of hydrogen and oxygen, etc. Only the anthraquinone method and the direct synthesis method of hydrogen and oxygen are used for industrial production, among which H2O2 produced by the anthraquinone method accounts for about 95% of the global production and about 98% of the domestic production. However, the anthraquinone method uses traditional alumina regeneration agents to produce a large amount of waste, causing serious pollution to the environment, and the waste treatment consumes a lot of energy and has high costs. The above reasons require that the production process and waste treatment process of hydrogen peroxide produced by the anthraquinone method need to be continuously innovated and improved.

[0004] In the anthraquinone method, alkyl anthraquinone is converted into alkyl hydroanthraquinone through a hydrogenation reaction, and then reacts with oxygen or air to release hydrogen peroxide and realize the alkyl anthraquinone cycle. Degradation products will be produced in the above hydrogenation and oxidation processes. As the number of cycles increases, the anthraquinone degradation products will continue to increase, causing the efficiency of the anthraquinone working solution to gradually decrease and eventually fail, resulting in increased production costs. Therefore, in the hydrogen peroxide production process, the regeneration of anthraquinone degradation products into effective anthraquinone is the key to controlling production costs and reducing environmental pollution. In the regeneration process of anthraquinone degradation products, activated alumina exhibits good regeneration ability and has been used on a large scale. At present, there are a large number of methods for preparing activated alumina catalysts, such as:

[0005] The invention patent application CN102728338A discloses an anthraquinone degradation product regeneration catalyst and a preparation method thereof, which provides an anthraquinone degradation product regeneration catalyst which can be expressed as MeO / Al2O3, wherein MeO is any one or more of an alkaline earth metal oxide or ZnO. The catalytic regeneration efficiency is relatively high, but the preparation thereof requires the hydrotalcite precursor to be synthesized by a hydrothermal method, which is complex in process and the preparation cost of the catalyst is relatively high.

[0006] The invention patent application CN110102276A discloses a catalyst and a preparation method thereof and a regeneration method of anthraquinone degradation products, wherein a quick-degrading powder, an alkaline earth metal compound and an auxiliary agent are mixed, and an acid solvent is added to mix with a silicon source to form a liquid, and then kneaded, extruded, dried and roasted to obtain an anthraquinone degradation product regeneration catalyst. The catalyst can only regenerate anthraquinone degradation products to an effective anthraquinone of up to 5.7 g / L, and the regeneration effect is average.

[0007] The invention patent application of CN108187663A discloses a catalyst and a preparation method thereof and a use thereof in catalyzing the regeneration of anthraquinone degradation products into effective anthraquinone, wherein the catalyst adopts a liquid impregnation method to load metal elements, and alkali metals, alkaline earth metals and fourth period transition metal elements are loaded on alumina as active components. This method requires the loading of multiple metal elements, which easily causes the pores of alumina to be blocked, resulting in a decrease in regeneration activity, and the maximum increase in effective anthraquinone can only reach 5.1 g / L.

[0008] The invention patent application CN110327907A discloses a catalyst for regeneration of anthraquinone degradation products, and provides a method for preparing anthraquinone regeneration catalyst in a high temperature and high pressure crystallization reactor with aluminum oxide as the main component and metal oxide or metal hydroxide as the active component. The reaction equipment of this method is relatively harsh and is not conducive to industrial production.

[0009] In conclusion, the activated alumina currently used in hydrogen peroxide production has some common defects, such as short service life, poor regeneration activity, and complex production process. Therefore, the development of a new anthraquinone degradation product regeneration catalyst that can avoid these defects and is more efficient and practical is still the key to controlling the production cost of hydrogen peroxide and increasing profits. Summary of the invention

[0010] The invention discloses a method for preparing a high-efficiency anthraquinone degradation product regeneration catalyst. The preparation process is simple and easy to control, and the prepared regeneration catalyst has the advantages of long service life and good regeneration activity.

[0011] To achieve the above object, the technical solution of the present invention is:

[0012] A method for preparing a highly efficient anthraquinone degradation product regeneration catalyst comprises the following steps:

[0013] (1) dissolving an organic acid in a mixed solution of ethanol and water, adding an organic base to adjust the pH to 6-10, then adding a template, an aluminum source, and at least one ⅡA metal or a salt containing ⅡA metal, mixing and stirring until the reaction is fully reacted, taking out the gel, drying it, and calcining it at high temperature to obtain hollow alumina sphere nanoparticles;

[0014] (2) The hollow alumina nanoparticles obtained in step (1) are mixed with an acid and an auxiliary agent, kneaded, extruded, dried and calcined at high temperature to obtain an anthraquinone degradation product regeneration catalyst.

[0015] Preferably, in step (1), the organic acid is one or a mixture of more than one of malonic acid, sebacic acid and dodecanedioic acid.

[0016] Preferably, in step (1), the organic base is one or a mixture of more than one of triethylamine, pyridine and diethylamine.

[0017] Preferably, in step (1), the aluminum source is one or a mixture of more than one of aluminum sulfate, aluminum nitrate, dihydroxyamino aluminum acetate, aluminum diisopropionate, basic aluminum carbonate, aluminum butyrate, aluminum acrylate, and triisobutyl aluminum.

[0018] Preferably, in step (1), the ⅡA metal is one or a mixture of more than one of magnesium, calcium, strontium and barium.

[0019] Preferably, in step (1), the stirring time is 6-20 hours.

[0020] Preferably, in step (1), the high temperature calcination temperature is 500-800° C. and the calcination time is 4-8 hours.

[0021] Preferably, in step (1), the molar ratio of the organic acid, the mixed solution of ethanol and water, the template, the aluminum source, and the IA metal or the salt containing the IA metal is 0.5-1:35-55:0.1-0.4:8-15:0.3-0.8.

[0022] Preferably, in step (1), the volume ratio of ethanol to water is 1-10:1.

[0023] Preferably, in step (1), the template is hexadecyltrimethylammonium bromide.

[0024] Step (2) is to extrude the alumina hollow sphere nanoparticles to make their crystal structure more stable and their mechanical strength higher, which is a common processing process. The present invention also further provides the preferred process parameters of step S2, the acid is one or a mixture of nitric acid, hydrochloric acid, sulfuric acid and acetic acid, the weight percentage is 15-25%, the auxiliary agent is one or a mixture of starch, sesbania powder and cellulose, the weight percentage is 3-10%, the rest is alumina hollow sphere nanoparticles, the high temperature roasting temperature is 500-700 ° C, and the roasting time is 2.5-5h.

[0025] The preparation method of the high-efficiency anthraquinone degradation product regeneration catalyst described above comprises the following steps: the hydrophilic and hydrophobic relationship of the added hexadecyltrimethylammonium bromide and the organic acid groups in the water / ethanol system forms expanded micelles, and then the aluminum salt and the ⅡA metal are hydrolyzed and fused with the expanded micelles under the catalytic action of the organic base to form giant self-organized vesicles, and the expanded micelles are removed after high-temperature calcination to obtain macroporous-mesoporous alumina hollow sphere nanoparticles with highly sponge-like characteristics; and then the particles are kneaded with mixed acid and an auxiliary agent, extruded into strips, dried and calcined to prepare a novel high-efficiency anthraquinone degradation product regeneration catalyst.

[0026] The regenerated catalyst prepared by the present invention has the following advantages:

[0027] (1) It has a high specific surface area, high strength, and large pore size. The regeneration activity can reach above 7.4 g / L, and the highest can reach 12.4 g / L, which significantly reduces the accumulation of anthraquinone degradation products in the working solution and improves industrial production efficiency.

[0028] (2) The service life is long, which can exceed 163 days and the longest can reach 210 days. It reduces the number of catalyst replacements and the amount of waste catalyst, thereby reducing production costs and the cost of handling waste catalysts, and has good economic and environmental benefits.

[0029] (3) The preparation method is simple, low-cost and suitable for industrial production. DETAILED DESCRIPTION

[0030] The technical solutions in the embodiments of the present invention will be described clearly and completely below. However, the following embodiments are only part of the embodiments of the present invention, not all of them.

[0031] Example 1

[0032] (1) 0.7 mol of sebacic acid was added dropwise to 2200 ml of ethanol / water (volume ratio 10:1), and stirred at 40°C for 15 minutes; triethylamine was added to adjust the pH to 6, and stirred for 30 minutes; 0.2 mol of hexadecyltrimethylammonium bromide, 10 mol of aluminum diisopropionate, and 0.5 mol of magnesium chloride were added and stirred for 10 hours; after the reaction, the white gel was poured into a petri dish and dried at 65°C for 1 hour, and calcined in a muffle furnace at 550°C for 5 hours, with a ramp of 1°C / min.

[0033] (2) The alumina hollow sphere nanoparticles obtained in step (1) are weighed with a mixed solution of sulfuric acid and water (volume ratio of 1:4), a mixed solution of nitric acid and water (volume ratio of 1:4), and field sesbania powder in a mass ratio of 75:10:10:5, added to a kneader and mixed evenly, and then the mixture is put into an extruder and extruded and cut into 5 mm spheres, dried in an oven at 110° C., and calcined in a muffle furnace at 550° C. for 3 hours to obtain an anthraquinone degradation product regeneration catalyst.

[0034] The anthraquinone degradation product regeneration catalyst of this embodiment has a regeneration activity of 12.4 g / L for anthraquinone degradation products (50° C., 10 g catalyst, 100 ml working solution, reaction time 24 h); service life: 210 days.

[0035] Example 2

[0036] (1) 0.7 mol of sebacic acid was added dropwise to 2200 ml of ethanol / water (volume ratio 10:1), and stirred at 40°C for 15 minutes; triethylamine was added to adjust the pH to 8, and stirred for 30 minutes; 0.2 mol of hexadecyltrimethylammonium bromide, 10 mol of aluminum nitrate, and 0.5 mol of magnesium chloride were added and stirred for 10 hours; after the reaction, the white gel was poured into a petri dish and dried at 65°C for 1 hour, and calcined in a muffle furnace at 550°C for 5 hours, with a ramp of 1°C / min.

[0037] (2) The alumina hollow sphere nanoparticles obtained in step (1) are weighed with a mixed solution of sulfuric acid and water (volume ratio of 1:4), a mixed solution of nitric acid and water (volume ratio of 1:4), and field sesbania powder in a mass ratio of 75:10:10:5, added to a kneader and mixed evenly, and then the mixture is put into an extruder and extruded and cut into 5 mm spheres, dried in an oven at 110° C., and calcined in a muffle furnace at 550° C. for 3 hours to obtain an anthraquinone degradation product regeneration catalyst.

[0038] The anthraquinone degradation product regeneration catalyst of this embodiment has a regeneration activity of 9.7 g / L for anthraquinone degradation products (50° C., 10 g catalyst, 100 ml working solution, reaction time 24 h); service life: 185 days.

[0039] Example 3

[0040] (1) 0.6 mol of sebacic acid was added dropwise to 2200 ml of ethanol / water (volume ratio 8:1), and stirred at 40°C for 15 minutes; triethylamine was added to adjust the pH to 10, and stirred for 30 minutes; 0.2 mol of hexadecyltrimethylammonium bromide, 10 mol of basic aluminum carbonate, and 0.5 mol of magnesium chloride were added and stirred for 10 hours; after the reaction, the white gel was poured into a petri dish and dried at 65°C for 1 hour, and calcined in a muffle furnace at 550°C for 5 hours, with a ramp of 1°C / min.

[0041] (2) The alumina hollow sphere nanoparticles obtained in step (1) are weighed with a mixed solution of sulfuric acid and water (volume ratio of 1:4), a mixed solution of nitric acid and water (volume ratio of 1:4), and field sesbania powder in a mass ratio of 75:10:10:5, added to a kneader and mixed evenly, and then the mixture is put into an extruder and extruded and cut into 5 mm spheres, dried in an oven at 110° C., and calcined in a muffle furnace at 550° C. for 3 hours to obtain an anthraquinone degradation product regeneration catalyst.

[0042] The anthraquinone degradation product regeneration catalyst of this embodiment has a regeneration activity of 8.9 g / L for anthraquinone degradation products (50° C., 10 g catalyst, 100 ml working solution, reaction time 24 h); and a service life of 175 days.

[0043] Example 4

[0044] (1) 0.7 mol of malonic acid was added dropwise to 2200 ml of ethanol / water (volume ratio 10:1), and stirred at 40°C for 15 minutes; triethylamine was added to adjust the pH to 6, and stirred for 30 minutes; 0.2 mol of hexadecyltrimethylammonium bromide, 10 mol of aluminum butyrate, and 0.5 mol of magnesium chloride were added and stirred for 10 hours; after the reaction, the white gel was poured into a petri dish and dried at 65°C for 1 hour, and calcined in a muffle furnace at 550°C for 5 hours, with a ramp of 1°C / min.

[0045] (2) The alumina hollow sphere nanoparticles obtained in step (1) are weighed with a mixed solution of sulfuric acid and water (volume ratio of 1:4), a mixed solution of nitric acid and water (volume ratio of 1:4), and field sesbania powder in a mass ratio of 75:10:10:5, added to a kneader and mixed evenly, and then the mixture is put into an extruder and extruded and cut into 5 mm spheres, dried in an oven at 110° C., and calcined in a muffle furnace at 550° C. for 3 hours to obtain an anthraquinone degradation product regeneration catalyst.

[0046] The anthraquinone degradation product regeneration catalyst of this embodiment has a regeneration activity of 10.5 g / L for anthraquinone degradation products (50° C., 10 g catalyst, 100 ml working solution, reaction time 24 h); service life: 194 days.

[0047] Example 5

[0048] (1) 0.7 mol of dodecanedioic acid was added dropwise to 2200 ml of ethanol / water (volume ratio 10:1), stirred at 40°C for 15 minutes; triethylamine was added to adjust the pH to 6, stirred for 30 minutes; then 0.2 mol of hexadecyltrimethylammonium bromide, 10 mol of aluminum acrylate, and 0.5 mol of magnesium chloride were added and stirred for 10 hours. After the reaction, the white gel was poured into a petri dish and dried at 55°C for 1.5 hours, and calcined in a muffle furnace at 550°C for 5 hours, with a ramp of 1°C / min.

[0049] (2) The alumina hollow sphere nanoparticles obtained in step (1) are weighed with a mixed solution of sulfuric acid and water (volume ratio of 1:4), a mixed solution of nitric acid and water (volume ratio of 1:4), and field sesbania powder in a mass ratio of 75:10:10:5, added to a kneader and mixed evenly, and then the mixture is put into an extruder and extruded and cut into 5 mm spheres, dried in an oven at 110° C., and calcined in a muffle furnace at 550° C. for 3 hours to obtain an anthraquinone degradation product regeneration catalyst.

[0050] The anthraquinone degradation product regeneration catalyst of this embodiment has a regeneration activity of 11.6 g / L for anthraquinone degradation products (50° C., 10 g catalyst, 100 ml working solution, reaction time 24 h); and a service life of 206 days.

[0051] Example 6

[0052] (1) 0.7 mol of sebacic acid was added dropwise to 2200 ml of ethanol / water (volume ratio 10:1), stirred at 40°C for 15 minutes; diethylamine was added to adjust the pH to 6, stirred for 30 minutes; then 0.2 mol of hexadecyltrimethylammonium bromide, 8 mol of aluminum diisopropionate, and 0.6 mol of magnesium chloride were added and stirred for 10 hours. After the reaction, the white gel was poured into a petri dish and dried at 65°C for 1 hour, and calcined in a muffle furnace at 600°C for 4.5 hours, with a ramp of 1°C / min.

[0053] (2) The alumina hollow sphere nanoparticles obtained in step (1) are weighed with a mixed solution of sulfuric acid and water (volume ratio of 1:4), a mixed solution of nitric acid and water (volume ratio of 1:4), and field sesbania powder in a mass ratio of 75:10:10:5, added to a kneader and mixed evenly, and then the mixture is put into an extruder and extruded and cut into 5 mm spheres, dried in an oven at 110° C., and calcined in a muffle furnace at 550° C. for 3 hours to obtain an anthraquinone degradation product regeneration catalyst.

[0054] The anthraquinone degradation product regeneration catalyst of this embodiment has a regeneration activity of 7.4 g / L for anthraquinone degradation products (50° C., 10 g catalyst, 100 ml working solution, reaction time 24 h); and a service life of 163 days.

[0055] Example 7

[0056] (1) 0.7 mol of sebacic acid was added dropwise to 2200 ml of ethanol / water (volume ratio 10:1), and stirred at 40°C for 15 minutes; pyridine was added to adjust the pH to 6, and stirred for 30 minutes; 0.2 mol of hexadecyltrimethylammonium bromide, 10 mol of aluminum diisopropionate, and 0.5 mol of magnesium chloride were added, and stirring was continued for 10 hours; after the reaction was completed, the white gel was poured into a culture dish and dried at 65°C for 1 hour, and calcined in a muffle furnace at 550°C for 5 hours, with a ramp of 1°C / min.

[0057] (2) The alumina hollow sphere nanoparticles obtained in step (1) are weighed with a mixed solution of sulfuric acid and water (volume ratio of 1:4), a mixed solution of nitric acid and water (volume ratio of 1:4), and field sesbania powder in a mass ratio of 75:10:10:5, added to a kneader and mixed evenly, and then the mixture is put into an extruder and extruded and cut into 5 mm spheres, dried in an oven at 110° C., and calcined in a muffle furnace at 550° C. for 3 hours to obtain an anthraquinone degradation product regeneration catalyst.

[0058] The anthraquinone degradation product regeneration catalyst of this embodiment has a regeneration activity of 9.2 g / L for anthraquinone degradation products (50° C., 10 g catalyst, 100 ml working solution, reaction time 24 h); and a service life of 165 days.

[0059] Example 8

[0060] (1) 0.7 mol of sebacic acid was added dropwise to 2200 ml of ethanol / water (volume ratio 10:1), and stirred at 40°C for 15 minutes; triethylamine was added to adjust the pH to 6, and stirred for 30 minutes; 0.2 mol of hexadecyltrimethylammonium bromide, 10 mol of aluminum diisopropionate, and 0.5 mol of magnesium nitrate were added and stirred for 10 hours; after the reaction, the white gel was poured into a culture dish and dried at 65°C for 1 hour, and calcined in a muffle furnace at 550°C for 5 hours, with a ramp of 1°C / min.

[0061] (2) The alumina hollow sphere nanoparticles obtained in step (1) are weighed with a mixed solution of sulfuric acid and water (volume ratio of 1:4), a mixed solution of nitric acid and water (volume ratio of 1:4), and field sesbania powder in a mass ratio of 75:10:10:5, added to a kneader and mixed evenly, and then the mixture is put into an extruder and extruded and cut into 5 mm spheres, dried in an oven at 110° C., and calcined in a muffle furnace at 550° C. for 3 hours to obtain an anthraquinone degradation product regeneration catalyst.

[0062] The anthraquinone degradation product regeneration catalyst of this embodiment has a regeneration activity of 11.7 g / L for anthraquinone degradation products (50° C., 10 g catalyst, 100 ml working solution, reaction time 24 h); service life: 201 days.

[0063] Example 9

[0064] (1) 0.7 mol of sebacic acid was added dropwise to 2200 ml of ethanol / water (volume ratio 10:1), and stirred at 40°C for 15 minutes; triethylamine was added to adjust the pH to 6, and stirred for 30 minutes; 0.2 mol of hexadecyltrimethylammonium bromide, 10 mol of aluminum diisopropionate, and 0.5 mol of calcium chloride were added and stirred for 10 hours; after the reaction, the white gel was poured into a petri dish and dried at 65°C for 1 hour, and calcined in a muffle furnace at 550°C for 5 hours, with a ramp of 1°C / min.

[0065] (2) The alumina hollow sphere nanoparticles obtained in step (1) are weighed with a mixed solution of sulfuric acid and water (volume ratio of 1:4), a mixed solution of nitric acid and water (volume ratio of 1:4), and field sesbania powder in a mass ratio of 75:10:10:5, added to a kneader and mixed evenly, and then the mixture is put into an extruder and extruded and cut into 5 mm spheres, dried in an oven at 110° C., and calcined in a muffle furnace at 550° C. for 3 hours to obtain an anthraquinone degradation product regeneration catalyst.

[0066] The anthraquinone degradation product regeneration catalyst of this embodiment has a regeneration activity of 9.0 g / L for anthraquinone degradation products (50° C., 10 g catalyst, 100 ml working solution, reaction time 24 h); and a service life of 173 days.

[0067] Example 10

[0068] (1) 0.7 mol of sebacic acid was added dropwise to 2200 ml of ethanol / water (volume ratio 7:1), and stirred at 40°C for 15 minutes; triethylamine was added to adjust the pH to 6, and stirred for 30 minutes; 0.2 mol of hexadecyltrimethylammonium bromide, 10 mol of aluminum diisopropionate, and 0.8 mol of strontium chloride were added, and stirring was continued for 10 hours; after the reaction was completed, the white gel was poured into a petri dish and dried at 65°C for 1 hour, and calcined in a muffle furnace at 550°C for 7 hours, with a ramp of 1°C / min.

[0069] (2) The alumina hollow sphere nanoparticles obtained in step (1) are weighed with a mixed solution of sulfuric acid and water (volume ratio of 1:4), a mixed solution of nitric acid and water (volume ratio of 1:4), and field sesbania powder in a mass ratio of 75:10:10:5, added to a kneader and mixed evenly, and then the mixture is put into an extruder and extruded and cut into 5 mm spheres, dried in an oven at 110° C., and calcined in a muffle furnace at 550° C. for 3 hours to obtain an anthraquinone degradation product regeneration catalyst.

[0070] The anthraquinone degradation product regeneration catalyst of this embodiment has a regeneration activity of 8.4 g / L for anthraquinone degradation products (50° C., 10 g catalyst, 100 ml working solution, reaction time 24 h); service life: 185 days.

[0071] Embodiment 11

[0072] (1) 0.7 mol of sebacic acid was added dropwise to 2200 ml of ethanol / water (volume ratio 10:1), and stirred at 40°C for 15 minutes; triethylamine was added to adjust the pH to 6, and stirred for 30 minutes; 0.2 mol of hexadecyltrimethylammonium bromide, 13 mol of aluminum diisopropionate, and 0.5 mol of barium chloride were added, and stirring was continued for 10 hours; after the reaction was completed, the white gel was poured into a petri dish and dried at 65°C for 1 hour, and calcined in a muffle furnace at 600°C for 5 hours, with a ramp of 1°C / min.

[0073] (2) The alumina hollow sphere nanoparticles obtained in step (1) are weighed with a mixed solution of sulfuric acid and water (volume ratio of 1:4), a mixed solution of nitric acid and water (volume ratio of 1:4), and field sesbania powder in a mass ratio of 75:10:10:5, added to a kneader and mixed evenly, and then the mixture is put into an extruder and extruded and cut into 5 mm spheres, dried in an oven at 110° C., and calcined in a muffle furnace at 550° C. for 3 hours to obtain an anthraquinone degradation product regeneration catalyst.

[0074] The anthraquinone degradation product regeneration catalyst of this embodiment has a regeneration activity of 8.0 g / L for anthraquinone degradation products (50° C., 10 g catalyst, 100 ml working solution, reaction time 24 h); and a service life of 181 days.

[0075] Example 12

[0076] (1) 0.7 mol of sebacic acid was added dropwise to 2200 ml of ethanol / water (volume ratio 10:1), and stirred at 40°C for 15 minutes; triethylamine was added to adjust the pH to 6, and stirred for 30 minutes; 0.2 mol of hexadecyltrimethylammonium bromide, 10 mol of aluminum diisopropionate, 0.25 mol of magnesium chloride and 0.25 mol of calcium chlorate were added, and stirring was continued for 10 hours; after the reaction was completed, the white gel was poured into a petri dish and dried at 65°C for 1 hour, and calcined in a muffle furnace at 550°C for 5 hours, with a ramp of 1°C / min.

[0077] (2) The alumina hollow sphere nanoparticles obtained in step (1) are weighed with a mixed solution of sulfuric acid and water (volume ratio of 1:4), a mixed solution of nitric acid and water (volume ratio of 1:4), and field sesbania powder in a mass ratio of 75:10:10:5, added to a kneader and mixed evenly, and then the mixture is put into an extruder and extruded and cut into 5 mm spheres, dried in an oven at 110° C., and calcined in a muffle furnace at 550° C. for 3 hours to obtain an anthraquinone degradation product regeneration catalyst.

[0078] The anthraquinone degradation product regeneration catalyst of this embodiment has a regeneration activity of 10.0 g / L for anthraquinone degradation products (50° C., 10 g catalyst, 100 ml working solution, reaction time 24 h); service life: 191 days.

[0079] Embodiment 13

[0080] (1) 0.7 mol of sebacic acid was added dropwise to 2200 ml of ethanol / water (volume ratio 10:1), and stirred at 40°C for 15 minutes; triethylamine was added to adjust the pH to 6, and stirred for 30 minutes; 0.2 mol of hexadecyltrimethylammonium bromide, 10 mol of aluminum diisopropionate, 0.25 mol of magnesium chloride and 0.25 mol of strontium chloride were added, and stirring was continued for 10 hours; after the reaction was completed, the white gel was poured into a petri dish and dried at 65°C for 1 hour, and calcined in a muffle furnace at 550°C for 5 hours, with a ramp of 1°C / min.

[0081] (2) The alumina hollow sphere nanoparticles obtained in step (1) are weighed with a mixed solution of sulfuric acid and water (volume ratio of 1:4), a mixed solution of nitric acid and water (volume ratio of 1:4), and field sesbania powder in a mass ratio of 75:10:10:5, added to a kneader and mixed evenly, and then the mixture is put into an extruder and extruded and cut into 5 mm spheres, dried in an oven at 110° C., and calcined in a muffle furnace at 550° C. for 3 hours to obtain an anthraquinone degradation product regeneration catalyst.

[0082] The anthraquinone degradation product regeneration catalyst of this embodiment has a regeneration activity of 9.4 g / L for anthraquinone degradation products (50° C., 10 g catalyst, 100 ml working solution, reaction time 24 h); and a service life of 179 days.

[0083] Embodiment 14

[0084] (1) 0.7 mol of sebacic acid was added dropwise to 2200 ml of ethanol / water (volume ratio 10:1), and stirred at 40°C for 15 minutes; triethylamine was added to adjust the pH to 6, and stirred for 30 minutes; 0.2 mol of hexadecyltrimethylammonium bromide, 10 mol of aluminum diisopropionate, 0.25 mol of magnesium chloride and 0.25 mol of barium chloride were added, and stirring was continued for 10 hours; after the reaction was completed, the white gel was poured into a petri dish and dried at 65°C for 1 hour, and calcined in a muffle furnace at 550°C for 5 hours, with a ramp of 1°C / min.

[0085] (2) The alumina hollow sphere nanoparticles obtained in step (1) are weighed with a mixed solution of sulfuric acid and water (volume ratio of 1:4), a mixed solution of nitric acid and water (volume ratio of 1:4), and field sesbania powder in a mass ratio of 75:10:10:5, added to a kneader and mixed evenly, and then the mixture is put into an extruder and extruded and cut into 5 mm spheres, dried in an oven at 110° C., and calcined in a muffle furnace at 550° C. for 3 hours to obtain an anthraquinone degradation product regeneration catalyst.

[0086] The anthraquinone degradation product regeneration catalyst of this embodiment has a regeneration activity of 8.7 g / L for anthraquinone degradation products (50° C., 10 g catalyst, 100 ml working solution, reaction time 24 h); service life: 174 days.

[0087] Embodiment 15

[0088] (1) 0.35 mol of malonic acid and 0.35 mol of sebacic acid were added dropwise to 2200 ml of ethanol / water (volume ratio 10:1), stirred at 40°C for 15 minutes; triethylamine was added to adjust the pH to 6, stirred for 30 minutes; 0.2 mol of hexadecyltrimethylammonium bromide, 10 mol of aluminum diisopropionate, and 0.5 mol of magnesium chloride were added and stirred for 10 hours. After the reaction, the white gel was poured into a petri dish and dried at 65°C for 1 hour, and calcined in a muffle furnace at 550°C for 5 hours, with a ramp of 1°C / min.

[0089] (2) The alumina hollow sphere nanoparticles obtained in step (1) are weighed with a mixed solution of sulfuric acid and water (volume ratio of 1:4), a mixed solution of nitric acid and water (volume ratio of 1:4), and field sesbania powder in a mass ratio of 75:10:10:5, added to a kneader and mixed evenly, and then the mixture is put into an extruder and extruded and cut into 5 mm spheres, dried in an oven at 110° C., and calcined in a muffle furnace at 550° C. for 3 hours to obtain an anthraquinone degradation product regeneration catalyst.

[0090] The anthraquinone degradation product regeneration catalyst of this embodiment has a regeneration activity of 11.5 g / L for anthraquinone degradation products (50° C., 10 g catalyst, 100 ml working solution, reaction time 24 h); service life: 193 days.

[0091] Example 16

[0092] (1) 0.35 mol of sebacic acid and 0.35 mol of dodecanedioic acid were added dropwise to 2420 ml of ethanol / water (volume ratio 10:1), and stirred at 40°C for 15 minutes; triethylamine was added to adjust the pH to 6, and stirred for 30 minutes; 0.2 mol of hexadecyltrimethylammonium bromide, 10 mol of aluminum diisopropionate, and 0.5 mol of magnesium chloride were added and stirred for 10 hours; after the reaction, the white gel was poured into a petri dish and dried at 60°C for 2 hours, and calcined in a muffle furnace at 550°C for 5 hours, with a ramp of 1°C / min.

[0093] (2) The alumina hollow sphere nanoparticles obtained in step (1) are weighed with a mixed solution of sulfuric acid and water (volume ratio of 1:4), a mixed solution of nitric acid and water (volume ratio of 1:4), and field sesbania powder in a mass ratio of 75:10:10:5, added to a kneader and mixed evenly, and then the mixture is put into an extruder and extruded and cut into 5 mm spheres, dried in an oven at 110° C., and calcined in a muffle furnace at 550° C. for 3 hours to obtain an anthraquinone degradation product regeneration catalyst.

[0094] The anthraquinone degradation product regeneration catalyst of this embodiment has a regeneration activity of 11.4 g / L for anthraquinone degradation products (50° C., 10 g catalyst, 100 ml working solution, reaction time 24 h); service life: 190 days.

[0095] Embodiment 17

[0096] (1) 0.7 mol of sebacic acid was added dropwise to 2090 ml of ethanol / water (volume ratio 10:1), and stirred at 40°C for 15 minutes; triethylamine was added to adjust the pH to 6, and stirred for 30 minutes; 0.2 mol of hexadecyltrimethylammonium bromide, 5 mol of aluminum diisopropionate and 5 mol of triisobutylaluminum, and 0.8 mol of magnesium chloride were added, and stirring was continued for 10 hours; after the reaction was completed, the white gel was poured into a petri dish and dried at 65°C for 0.9 hours, and calcined in a muffle furnace at 550°C for 5 hours, with a ramp of 1°C / min.

[0097] (2) The alumina hollow sphere nanoparticles obtained in step (1) are weighed with a mixed solution of sulfuric acid and water (volume ratio of 1:4), a mixed solution of nitric acid and water (volume ratio of 1:4), and field sesbania powder in a mass ratio of 75:10:10:5, added to a kneader and mixed evenly, and then the mixture is put into an extruder and extruded and cut into 5 mm spheres, dried in an oven at 110° C., and calcined in a muffle furnace at 550° C. for 3 hours to obtain an anthraquinone degradation product regeneration catalyst.

[0098] The anthraquinone degradation product regeneration catalyst of this embodiment has a regeneration activity of 9.1 g / L for anthraquinone degradation products (50° C., 10 g catalyst, 100 ml working solution, reaction time 24 h); service life: 184 days.

[0099] Comparative Example 1

[0100] The conventional anthraquinone degradation product regeneration catalyst currently available on the market was used, and the evaluation conditions were the same as those in Example 1-17. Its anthraquinone degradation product regeneration activity was 2.8 g / L (50° C., 10 g catalyst, 100 ml working solution, reaction time 24 h); service life: 60 days.

[0101] Comparative Example 2

[0102] (1) 0.7 mol hydrochloric acid was added dropwise to 2200 ml ethanol / water (volume ratio 10:1), and stirred at 40°C for 15 minutes; triethylamine was added to adjust the pH to 6, and stirred for 30 minutes; 0.2 mol hexadecyltrimethylammonium bromide, 5 mol aluminum diisopropionate and 5 mol triisobutylaluminum, and 0.5 mol magnesium chloride were added, and stirring was continued for 10 hours; after the reaction was completed, the white gel was poured into a petri dish and dried at 65°C for 1 hour, and calcined in a muffle furnace at 550°C for 5 hours, with a ramp of 1°C / min.

[0103] (2) The alumina hollow sphere nanoparticles obtained in step (1) are weighed with a mixed solution of sulfuric acid and water (volume ratio of 1:4), a mixed solution of nitric acid and water (volume ratio of 1:4), and field sesbania powder in a mass ratio of 75:10:10:5, added to a kneader and mixed evenly, and then the mixture is put into an extruder and extruded and cut into 5 mm spheres, dried in an oven at 110° C., and calcined in a muffle furnace at 550° C. for 3 hours to obtain an anthraquinone degradation product regeneration catalyst.

[0104] The anthraquinone degradation product regeneration catalyst of this comparative example has an anthraquinone degradation product regeneration activity of 5.2 g / L (50° C., 10 g catalyst, 100 ml working solution, reaction time 24 h); service life: 75 days.

[0105] Comparative Example 3

[0106] (1) 0.7 mol of sebacic acid was added dropwise to 2200 ml of ethanol / water (volume ratio 10:1), and stirred at 40°C for 15 minutes; sodium hydroxide was added to adjust the pH to 6, and stirred for 30 minutes; 0.2 mol of hexadecyltrimethylammonium bromide, 5 mol of aluminum diisopropionate and 5 mol of triisobutylaluminum, and 0.5 mol of magnesium chloride were added, and stirring was continued for 10 hours; after the reaction was completed, the white gel was poured into a culture dish and dried at 65°C for 1 hour, and calcined in a muffle furnace at 550°C for 5 hours, with a ramp of 1°C / min.

[0107] (2) The alumina hollow sphere nanoparticles obtained in step (1) are weighed with a mixed solution of sulfuric acid and water (volume ratio of 1:4), a mixed solution of nitric acid and water (volume ratio of 1:4), and field sesbania powder in a mass ratio of 75:10:10:5, added to a kneader and mixed evenly, and then the mixture is put into an extruder and extruded and cut into 5 mm spheres, dried in an oven at 110° C., and calcined in a muffle furnace at 550° C. for 3 hours to obtain an anthraquinone degradation product regeneration catalyst.

[0108] The anthraquinone degradation product regeneration catalyst of this comparative example has a regeneration activity of 4.1 g / L for anthraquinone degradation products (50° C., 10 g catalyst, 100 ml working solution, reaction time 24 h); service life: 79 days.

[0109] The catalyst performance test summary is shown in Table 1:

[0110] Table 1 Catalyst performance test table

[0111]

[0112] Note: The effective anthraquinone in Table 1 is the total increase of 2-ethylanthraquinone and tetrahydro-2-ethylanthraquinone.

[0113] It can be seen from the performance test results (Table 1) that the specific surface area, strength, effective anthraquinone regeneration amount and service life of the catalysts of this embodiment (Examples 1-17) have been significantly improved, wherein the regeneration activity can reach more than 7.4 g / L, significantly reducing the accumulation of anthraquinone degradation products in the working solution and improving industrial production efficiency; the service life can exceed 163 days, reducing the number of catalyst replacements and the amount of waste catalysts, thereby reducing production costs and the cost of treating waste catalysts, with good economic and environmental benefits. In addition, it is further preferred that the organic acid is sebacic acid, the organic base is triethylamine, the pH is 6, the aluminum source is aluminum diisopropionate, and the ⅡA metal is magnesium. Under this condition, aluminum salt and metal magnesium can be better hydrolyzed and fused under base catalysis. Under the new template, the aluminum-magnesium nanoparticles formed after calcination have better performance than the commercially available catalyst (Comparison of Example 1 with Comparative Example 1). The acid used in Comparative Example 2 is an inorganic acid, which has no hydrophobic group and cannot react with hexadecyltrimethylammonium bromide to form expanded micelles, while the base used in Comparative Example 3 is an inorganic base, which has a strong alkalinity and easily causes the formed expanded micelles to disperse. This shows that both inorganic acids and inorganic bases cannot form new templates, and the pore size and specific surface area of ​​the generated alumina particles are small, so that the performance of the anthraquinone degradation product regeneration catalyst prepared subsequently is not as good as the effect of forming the template.

[0114] In summary, the present invention overcomes the shortcomings of the prior art, optimizes the performance of anthraquinone degradation product regeneration catalyst, and provides a novel and efficient anthraquinone degradation product regeneration catalyst and a preparation method thereof. The method has simple process, mild conditions, low catalyst preparation cost, and excellent catalyst performance. The method is applied to the hydrogen peroxide production industry, can effectively save production costs and reduce the cost of subsequent treatment, and is suitable for industrial production.

Claims

1. A method for preparing a highly efficient anthraquinone degradation product regeneration catalyst, characterized in that The following steps are involved: (1) dissolving an organic acid in a mixed solution of ethanol and water, adding an organic base to adjust the pH to 6-10, then adding a template, an aluminum source, and at least one ⅡA metal or a salt containing ⅡA metal, mixing and stirring until the reaction is fully reacted, taking out the gel, drying it, and calcining it at high temperature to obtain hollow alumina sphere nanoparticles; (2) The hollow alumina nanoparticles obtained in step (1) are mixed with an acid and an auxiliary agent, kneaded, extruded, dried and calcined at high temperature to obtain an anthraquinone degradation product regeneration catalyst.

2. The method for preparing a highly efficient anthraquinone degradation product regeneration catalyst according to claim 1, characterized in that: In step (1), the organic acid is one or a mixture of more than one of malonic acid, sebacic acid and dodecanedioic acid.

3. The method for preparing a highly efficient anthraquinone degradation product regeneration catalyst according to claim 1, characterized in that: In step (1), the organic base is one or a mixture of more than one of triethylamine, pyridine and diethylamine.

4. The method for preparing a highly efficient anthraquinone degradation product regeneration catalyst according to claim 1, characterized in that: In step (1), the aluminum source is one of aluminum sulfate, aluminum nitrate, dihydroxyamino aluminum acetate, aluminum diisopropionate, basic aluminum carbonate, aluminum butyrate, aluminum acrylate, triisobutyl aluminum, or a mixture of more than one of them.

5. The method for preparing a highly efficient anthraquinone degradation product regeneration catalyst according to claim 1, characterized in that: In step (1), the ⅡA metal is one or a mixture of more than one of magnesium, calcium, strontium and barium.

6. The method for preparing a highly efficient anthraquinone degradation product regeneration catalyst according to claim 1, characterized in that: In step (1), the stirring time is 6-20 hours.

7. The method for preparing a highly efficient anthraquinone degradation product regeneration catalyst according to claim 1, characterized in that: In step (1), the high temperature calcination temperature is 500-800°C and the calcination time is 4-8h.

8. The method for preparing a highly efficient anthraquinone degradation product regeneration catalyst according to claim 1, characterized in that: In step (1), the molar ratio of the organic acid, the mixed solution of ethanol and water, the template, the aluminum source, and the IA metal or the salt containing the IA metal is 0.5-1:35-55:0.1-0.4:8-15:0.3-0.

8.

9. The method for preparing a highly efficient anthraquinone degradation product regeneration catalyst according to any one of claim 1, characterized in that: In step (1), the volume ratio of ethanol to water is 1-10:

1.

10. The method for preparing a highly efficient anthraquinone degradation product regeneration catalyst according to claims 1 to 9, characterized in that: In step (1), the template agent is hexadecyltrimethylammonium bromide.

Citation Information

Patent Citations

  • Anthraquinone degradation product regeneration catalyst and preparation method thereof

    CN102728338A

  • Novel efficient long-life anthraquinone degradation product regeneration catalyst and preparation method thereof

    CN106179427A

  • Preparation method of alumina supporter with large porosity and high mechanical strength

    CN108855024A

  • Catalyst and preparation method thereof and regeneration method of anthraquinone degradation product

    CN110102276A