High-activity Pt / GaCe-Al2O3 catalyst as well as preparation method and application thereof
By doping Ga and Ce in Al2O3 support and preparing Pt/GaCe-Al2O3 catalyst by ultrasonic impregnation, the problems of low activity and ease of inactivation in the existing catalyst are solved, and high-efficiency methylcyclohexane dehydrogenation and Production of high purity hydrogen.
Patent Information
- Application Number
- CN202411191846.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-28
AI Technical Summary
The existing Pt/Al2O3 catalysts have low catalytic activity in the dehydrogenation reaction of methylcyclohexane and are prone to inactivation, resulting in low purity of product hydrogen and short catalyst life.
Ga and Ce are doped into the Al2O3 support by hydrothermal method, and a high-active Pt/GaCe-Al2O3 catalyst was prepared, and the support of Pt was increased by ultrasonic impregnation to form a nanosheet-like structure to improve the adsorption performance and stability of the catalyst. .
The activity and stability of the catalyst are significantly improved, and the efficient dehydrogenation of methylcyclohexane is achieved, with a hydrogen purity of up to 99.9%, and the deactivation rate of the catalyst is reduced.
Smart Images

Figure CN118949980A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of catalyst preparation, and in particular to a high-activity Pt / GaCe-Al2O3 catalyst and a preparation method and application thereof. Background Art
[0002] Liquid organic hydrogen storage is based on the reversible reaction of hydrogenation and dehydrogenation of organic hydrides to store hydrogen. It has the characteristics of high hydrogen storage density, highly reversible hydrogenation-dehydrogenation, etc. It is very compatible with existing energy infrastructure and does not require large capital investment. Therefore, liquid organic hydrogen storage is considered to be an attractive hydrogen storage method. Methylcyclohexane (MCH) is considered to be an ideal liquid hydrogen storage material due to its low toxicity, high hydrogen cycle reversibility and theoretical hydrogen storage capacity (~6.1wt.%). The dehydrogenation of methylcyclohexane is a strongly endothermic reaction, which usually requires a high reaction temperature to achieve an efficient hydrogen release rate, and also leads to a short catalyst life. Therefore, it is particularly important to develop a catalyst with high hydrogen release rate and good stability to achieve convenient hydrogen utilization.
[0003] In terms of catalyst preparation, Pt metal is widely used in catalytic dehydrogenation due to its strong CH bond activation ability and low CC bond cracking ability. In addition to active metals, carriers are also an important component. γ-Al2O3 can effectively improve the metal-carrier interaction, enhance the dispersion of active ingredients, and maintain the unique properties of impregnated metals due to its good mechanical and chemical properties. Therefore, Pt / Al2O3 catalyst is the most commonly used dehydrogenation catalyst. However, the above catalyst has low catalytic dehydrogenation activity and is easily deactivated, resulting in low purity of the product hydrogen. Summary of the invention
[0004] One of the purposes of the present invention is to provide a method for preparing a highly active Pt / GaCe-Al2O3 catalyst, which enhances the dehydrogenation rate and stability of a single metal Pt / Al2O3 catalyst by using a promoter metal.
[0005] The second object of the present invention is to provide a high-activity Pt / GaCe-Al2O3 catalyst prepared by the above preparation method.
[0006] The third object of the present invention is to provide the application of the above-mentioned high-activity Pt / GaCe-Al2O3 catalyst in catalytic dehydrogenation.
[0007] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0008] One aspect of the present invention provides a method for preparing a high-activity Pt / GaCe-Al2O3 catalyst, comprising the following steps:
[0009] (1) mixing aluminum salt, urea, cerium salt and gallium salt in water, placing the obtained mixture in an autoclave for hydrothermal reaction; after cooling to room temperature, washing, drying and calcining the precipitate to obtain a GaCe-Al2O3 carrier;
[0010] (2) Add the GaCe-Al2O3 carrier prepared in step (1) to the impregnation solution containing the platinum precursor, mix by ultrasonication, and then vacuum impregnate for 12 hours. After the impregnation is completed, dry it and calcine it in an inert atmosphere to obtain a Pt / GaCe-Al2O3 catalyst.
[0011] Preferably, the temperature of the hydrothermal reaction in step (1) is 100° C. and the time is 48 h.
[0012] Preferably, in step (1), the drying temperature is 100° C. and the time is 12 h; and the calcination temperature is 750° C. and the time is 2 h.
[0013] Preferably, in step (1), the aluminum salt is aluminum nitrate, the cerium salt is cerium nitrate, and the gallium salt is gallium nitrate.
[0014] Preferably, the impregnation solution in step (2) is one of deionized water, ethanol and acetone.
[0015] Preferably, the calcination temperature in step (2) is 500° C. and the calcination time is 2 h.
[0016] Preferably, the platinum precursor in step (2) is chloroplatinic acid.
[0017] Another aspect of the present invention provides a high-activity Pt / GaCe-Al2O3 catalyst prepared by the above-mentioned preparation method.
[0018] Preferably, the loading amount of Pt in the catalyst is 0.5wt.%; the added amount of Ga is 1.5wt.%; and the added amount of Ce is 1.5wt.%.
[0019] The catalyst has a nano-sheet structure and has strong adsorption properties for methylcyclohexane.
[0020] Another aspect of the present invention also provides the use of the above-mentioned high-activity Pt / GaCe-Al2O3 catalyst in catalyzing the dehydrogenation of MCH.
[0021] The specific application steps include: the catalyst is tableted, crushed, and sieved into catalyst particles with a particle size of 40-60 mesh. 50 mg of the catalyst diluted with quartz sand (total amount: 0.55 g) is added to a reaction tube (inner diameter = 8 mm), and then the temperature is maintained at 300° C. and the pressure is maintained at 0.1 MPa. The flow rate of methylcyclohexane is controlled by an injection pump to be maintained at 30 μL / min and it is gasified at 180° C. The flow rate of the carrier gas (Ar) is adjusted to 10-50 mL / min by a mass flow controller, and the methylcyclohexane and Ar mixed gas are pumped into the reactor together. The product is analyzed online by a gas chromatograph equipped with a TCD and FID detector.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] (1) The non-precious metals Ga and Ce were doped into the Al2O3 carrier by a hydrothermal synthesis method to synthesize an excellent carrier GaCe-Al2O3 with a mesoporous nanosheet structure. This structure can ensure that the reactants can smoothly enter the pores and contact the active metals.
[0024] (2) The Pt / Ga1.5Ce1.5-Al2O3 catalyst was prepared by impregnating the GaCe-Al2O3 carrier with an ethanol-dissolved H2PtCl6·6H2O solution. It exhibited efficient methylcyclohexane adsorption and carbon deposition inhibition properties, improved catalyst activity, and maintained an extremely low deactivation rate (0.09% / min).
[0025] (3) The above catalyst is applied to the dehydrogenation reaction of methylcyclohexane, and the reaction is carried out in a continuous fixed bed reactor. The selectivity of toluene is extremely high (~99.9%), and the resulting hydrogen has high purity, and there is no need to separate the gas product. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 It is the XRD diagram of the catalysts with different additive addition amounts prepared in Example 1 of the present invention and Comparative Examples 1-4;
[0027] Figure 2 is a SEM image of the Pt / Ga1.5Ce1.5-Al2O3 catalyst prepared in Example 1 of the present invention;
[0028] Figure 3 is a TEM image of the Pt / Ga1.5Ce1.5-Al2O3 catalyst prepared in Example 1 of the present invention;
[0029] Figure 4 It is the MCH-TPD graph of the catalysts with different additive addition amounts prepared in Example 1 of the present invention and Comparative Examples 1-4;
[0030] Figure 5is the effect of Ce addition on the dehydrogenation of methylcyclohexane;
[0031] Figure 6 is the effect of Ga addition on the dehydrogenation of methylcyclohexane;
[0032] Figure 7 is the effect of different impregnation solutions on the dehydrogenation of methylcyclohexane;
[0033] Figure 8 The effect of carrier gas flow rate on the dehydrogenation of methylcyclohexane. DETAILED DESCRIPTION
[0034] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0035] Example 1: Preparation of catalyst Pt / Ga1.5Ce1.5-Al2O3
[0036] 1. Preparation of Ga1.5Ce1.5-Al2O3 Support by Hydrothermal Synthesis
[0037] 6.44g Al(NO3)3·9H2O, 9.28g CO(NH2)2, 41.34mg Ce(NO3)3·6H2O and 48.60mg Ga(NO3)3·xH2O were dissolved in 100mL deionized water. The obtained mixture was placed in a 200mL Teflon-lined stainless steel autoclave and kept at 100℃ for 48h. After cooling to room temperature, the precipitate was washed and filtered with deionized water several times, then dried at 100℃ for 12h, and finally calcined at 750℃ for 2h in a muffle furnace at a heating rate of 2℃ / min to obtain Ga1.5Ce1.5-Al2O3.
[0038] 2. Synthesis of Pt / Ga1.5Ce1.5-Al2O3 Catalyst by Impregnation Method
[0039] 0.5 g of the carrier prepared above was added to an ethanol solution containing 6.67 mg of H2PtCl6·6H2O and ultrasonicated for 20 min; the mixed solution was then impregnated in a vacuum drying oven for 12 h, dried after impregnation, and calcined at 500°C for 2 h in an inert atmosphere to obtain a Pt / Ga1.5Ce1.5-Al2O3 catalyst.
[0040] Comparative Example 1: Preparation of Pt / Al2O3 Catalyst
[0041] The above-mentioned hydrothermal synthesis method was used for treatment (the steps are the same as those in Example 1), and 6.44 g Al(NO3)3·9H2O and 9.28 g CO(NH2)2 were added in the first step of dissolution; Pt / Al2O3 was synthesized by the traditional impregnation method (the steps are the same as those in Example 1).
[0042] Comparative Example 2: Preparation of Pt / Ce-Al2O3 Catalysts Doped with Different Ce
[0043] The above-mentioned hydrothermal synthesis method was used for treatment (with the same steps as in Example 1). In the first step of dissolution, 6.44 g Al(NO3)3·9H2O, 9.28 g CO(NH2)2 and 13.78 mg, 41.34 mg, 82.68 mg and 275.60 mg of Ce(NO3)3·6H2O were added respectively; Pt / Ce0.5-Al2O3, Pt / Ce1.5-Al2O3, Pt / Ce3-Al2O3 and Pt / Ce10-Al2O3 were synthesized by the conventional impregnation method (with the same steps as in Example 1).
[0044] Comparative Example 3: Preparation of Pt / Ga1.5-Al2O3 Catalyst
[0045] The above-mentioned hydrothermal synthesis method was used for treatment (with the same steps as in Example 1), and 6.44 g Al(NO3)3·9H2O, 9.28 g CO(NH2)2 and 48.60 mg Ga(NO3)3·xH2O were added in the first step of dissolution; Pt / Ga1.5-Al2O3 was synthesized by the conventional impregnation method (with the same steps as in Example 1).
[0046] Comparative Example 4: Preparation of Pt / GaCe1.5-Al2O3 Catalysts with Different Ga Doping
[0047] The above-mentioned hydrothermal synthesis method was used for treatment (with the same steps as in Example 1). In the first step of dissolution, 6.44 g Al(NO3)3·9H2O, 41.34 mg Ce(NO3)3·6H2O, 9.28 g CO(NH2)2 and 16.2 mg and 97.20 mg Ga(NO3)3·xH2O were added respectively; Pt / Ga0.5Ce1.5-Al2O3 and Pt / Ga3Ce1.5-Al2O3 were synthesized by the conventional impregnation method (with the same steps as in Example 1).
[0048] Table 1 Physical structure properties of catalysts
[0049]
[0050] a The specific surface area was calculated according to the BET method.
[0051] b The total pore volume is calculated at a relative pressure of P / P0 = 0.99
[0052] c The average pore size is calculated according to the BJH method.
[0053] As shown in Table 1, the specific surface area, pore volume and pore diameter of the carrier Al2O3 are 161m 2 / g, 0.77cm 3 / g and 8.05nm. After loading metal Pt, the specific surface area and pore volume of the catalyst Pt / Al2O3 are relatively reduced, which can be attributed to the collapse of some mesopores after re-calcination and the blocking of some small pores by particles formed by metal clusters. In addition, all catalysts have mesoporous structures with pore sizes distributed between 6.70-8.15nm, which is significantly larger than the dynamic pore size (0.70nm) of toluene and MCH molecules. Therefore, the mesoporous structure of the catalyst helps to promote the diffusion of reactant molecules.
[0054] Figure 1 is the XRD diagram of different catalysts prepared in Example 1 and Comparative Examples 1-4; Figure 1 It can be seen that all samples have clear characteristic diffraction peaks corresponding to γ-Al2O3 at 31.9°, 37.4°, 39.4°, 45.8° and 66.9°. A small diffraction peak related to the (111) plane of CeO2 cubic fluorite structure appears at 28.6° in Pt / Ga1.5Ce1.5-Al2O3, indicating that Ga 3+ The ions enter the CeO2 lattice to form a solid solution structure, which causes the lattice to shrink slightly and increases the 2θ value of the (111) peak. The diffraction peak of Pt is not detected, which may be due to its low content and high dispersion on the support.
[0055] Figure 2 is a SEM image of the catalyst prepared in Example 1; Figure 2 It can be seen that the catalysts all present a nanosheet morphology.
[0056] Figure 3 This is a TEM image of the catalyst prepared in Example 1; when Ga or Ce is added, spherical particles of 5-10 nm in size are observed and are evenly distributed on the catalyst surface.
[0057] Figure 4 It is the MCH-TPD diagram of different catalysts prepared in Example 1 and Comparative Examples 1-4; the Pt / Ga1.5Ce1.5-Al2O3 catalyst exhibits higher adsorption capacity due to its largest desorption peak. In addition, the order of change of MCH desorption peak temperature is: Pt / Ga1.5Ce1.5-Al2O3 (120°C)>Pt / Ce1.5-Al2O3 (109°C)>Pt / Ga1.5-Al2O3 (91°C)>Pt / Al2O3 (87°C). This shows that the addition of the auxiliary metals Ga and Ce significantly enhances the adsorption performance of the catalyst for MCH, thereby promoting the dehydrogenation reaction of MCH.
[0058] Example 2: Application of Pt / GaCe-Al2O3 catalyst to dehydrogenation of methylcyclohexane
[0059] All catalytic reactions were carried out in a micro fixed bed.
[0060] All catalysts are processed by tableting, crushing and sieving into catalyst particles with a particle size of 40-60 mesh.
[0061] In a typical experiment, 50 mg of catalyst diluted with quartz sand (total amount: 0.55 g) was added to the reaction tube (inner diameter = 8 mm), and then the bed temperature was maintained at 300°C and the pressure was maintained at 0.1 MPa. The MCH flow rate was controlled by a syringe pump to be maintained at 30 μL / min and vaporized at 180°C. The carrier gas (Ar) was adjusted to a flow rate of 30 mL / min by a mass flow controller, and the MCH and Ar mixed gas were pumped into the reactor together. The product was analyzed online by a gas chromatograph equipped with TCD and FID detectors. The hydrogen release rate is an important value for the dehydrogenation efficiency of the catalyst, and the first-order deactivation rate is an important value for the stability of the catalyst, which are calculated according to formulas 1-1 and 1-2 respectively:
[0062] Hydrogen release rate
[0063] μ is the feed rate of MCH, μL / min;
[0064] ρ is the density of MCH, g / mL;
[0065] X is the MCH rate, %;
[0066] m is the mass of the catalyst, g;
[0067] M is the relative molecular mass of MCH, g / mol;
[0068] W is the loading amount of platinum, %;
[0069] k d is the first-order inactivation rate;
[0070] t is the reaction time, min.
[0071] Depend on Figure 5 It can be seen that under the same reaction conditions, the initial conversion rate of the Pt / Al2O3 catalyst is 52%, and the hydrogen release rate is 963 mol / g Pt / min, the deactivation rate is 0.20% / min, and the toluene selectivity is ~99.6%. The initial conversion rate of Pt / Ce1.5-Al2O3 catalyst is 65%, and the hydrogen release rate is 1561 mol / g Pt / min, and the deactivation rate is 0.15% / min. In contrast, when the Ce addition amount is 1.5wt.%, the catalyst has the best hydrogen release rate and stability.
[0072] Depend on Figure 6 It can be seen that when the additive metal Ga is further added, Pt / Ce1.5Ga1.5-Al2O3 exhibits the highest initial conversion rate (73%) and hydrogen release rate (1914 mol / g Pt / min), and the toluene selectivity is ~99.9%. With the increase of Ga addition, the deactivation rate shows an obvious V-shaped change, among which Pt / Ce1.5Ga1.5-Al2O3 shows the lowest deactivation rate (0.09% / min). The results show that when 1.5wt.% of Ga as the auxiliary metal is further added, the catalyst shows excellent dehydrogenation activity and stability. This may be because the incorporation of Ga ions into the CeO2 lattice improves the adsorption performance of the catalyst for MCH and promotes the dehydrogenation reaction of methylcyclohexane, and the auxiliary metal weakens the accumulation of coke formation, thereby more effectively exposing the active sites and improving the stability of the catalyst.
[0073] In summary, when the addition amounts of Ga and Ce are both 1.5wt.%, the hydrogen release rate of the catalyst is outstanding and the catalytic effect is better.
[0074] Example 3: Effect of different impregnation solutions on dehydrogenation of methylcyclohexane
[0075] The above-mentioned hydrothermal synthesis method was used for treatment (the steps are the same as those in Example 1), and the traditional impregnation method was adopted, using an impregnation solution of deionized water, ethanol and acetone (the steps are the same as those in Example 1) to synthesize Pt / Ga1.5Ce1.5-Al2O3-deionized water, Pt / Ga1.5Ce1.5-Al2O3-ethanol, and Pt / Ga1.5Ce1.5-Al2O3-acetone.
[0076] Depend on Figure 7 It can be seen that under the same reaction conditions, although the dehydrogenation activities of the catalysts prepared with different impregnation solvents are similar, the stability of the catalysts is significantly different. When ethanol and benzophenone are used as impregnation solvents, the catalyst shows a lower deactivation rate, which is 0.09% / min and 0.10% / min respectively. When deionized water is used as the impregnation liquid, the deactivation rate of the catalyst is as high as 0.13% / min. This may be because ethanol and acetone have lower boiling points and have stronger diffusivity during the impregnation process, making the active components more evenly distributed. However, compared with ketones, ethanol is non-toxic and cheap, so ethanol is the best impregnation liquid.
[0077] Example 4: Effect of carrier gas flow rate on dehydrogenation of methylcyclohexane
[0078] Reaction conditions: 50 mg catalyst, methylcyclohexane = 30 μL / min, 300 °C, 0.1 MPa
[0079] The carrier gas flow rate has an important influence on the dehydrogenation reaction. The carrier gas flow rate determines the concentration and time of the MCH reaction, which in turn affects the conversion rate of methylcyclohexane. Figure 8 It can be seen that when the carrier gas flow rate increases from 10mL / min to 50mL / min, the conversion rate of methylcyclohexane decreases with the increase of carrier gas flow rate. This is because the relative concentration of methylcyclohexane and the reduction of reaction residence time reduce the contact between methylcyclohexane and the catalyst, so the conversion rate of methylcyclohexane decreases significantly with the increase of carrier gas flow rate.
Claims
1. A method for preparing a highly active Pt / GaCe-Al2O3 catalyst, characterized in that: The steps include: (1) mixing aluminum salt, urea, cerium salt and gallium salt in water, placing the obtained mixture in an autoclave for hydrothermal reaction; after cooling to room temperature, washing, drying and calcining the precipitate to obtain a GaCe-Al2O3 carrier; (2) Add the GaCe-Al2O3 carrier prepared in step (1) to the impregnation solution containing the platinum precursor, mix by ultrasonication, and then vacuum impregnate for 12 hours. After the impregnation is completed, dry it and calcine it in an inert atmosphere to obtain a Pt / GaCe-Al2O3 catalyst.
2. The method for preparing the highly active Pt / GaCe-Al2O3 catalyst according to claim 1, characterized in that: The temperature of the hydrothermal reaction in step (1) is 100° C. and the time is 48 h.
3. The method for preparing the highly active Pt / GaCe-Al2O3 catalyst according to claim 1, characterized in that: In step (1), the drying temperature is 100° C. and the time is 12 h; the calcination temperature is 750° C. and the time is 2 h.
4. The method for preparing a highly active Pt / GaCe-Al2O3 catalyst according to claim 1, characterized in that: In step (1), the aluminum salt is aluminum nitrate, the cerium salt is cerium nitrate, and the gallium salt is gallium nitrate.
5. The method for preparing the high-activity Pt / GaCe-Al2O3 catalyst according to claim 1, characterized in that: In step (2), the platinum precursor is chloroplatinic acid, and the impregnation solution is one of deionized water, ethanol and acetone.
6. The method for preparing a highly active Pt / GaCe-Al2O3 catalyst according to claim 1, characterized in that: The calcination temperature in step (2) is 500° C. and the calcination time is 2 h.
7. A highly active Pt / GaCe-Al2O3 catalyst, characterized in that: The method is prepared according to any one of claims 1 to 6.
8. A highly active Pt / GaCe-Al2O3 catalyst according to claim 7, characterized in that: The loading amount of Pt in the catalyst is 0.5 wt. %; the addition amount of Ga is 1.5 wt. %; and the addition amount of Ce is 1.5 wt. %.
9. Use of the high-activity Pt / GaCe-Al2O3 catalyst according to claim 7 or 8 in catalyzing the dehydrogenation of methylcyclohexane.
10. The use according to claim 9, characterized in that: The specific application steps include: Catalyst particles with a particle size of 40-60 mesh diluted with quartz sand are added to a reaction tube, and then the temperature is maintained at 300° C. and the pressure is maintained at 0.1 MPa; the flow rate of methylcyclohexane is controlled to be maintained at 30 μL / min and it is gasified at 180° C., the flow rate of the carrier gas is adjusted to 10-50 mL / min, and the mixed gas of methylcyclohexane and the carrier gas is pumped into the reactor together to obtain toluene and hydrogen.
Citation Information
Patent Citations
Supported platinum based three-way catalyst and preparing method and use
CN101164690A
Platinum-gallium catalyst loaded on double-oxide composite carrier as well as preparation method and application of platinum-gallium catalyst
CN104525196A
Pt-based dehydrogenation catalyst and preparation method thereof
CN108786801A
Platinum-based catalyst for efficiently and stably catalyzing dehydrogenation of liquid organic hydrogen carrier and preparation method of platinum-based catalyst
CN116809059A
Cited By
Electric internal heating Pt / CeO2 / Foam monolithic catalyst, preparation method thereof and methyl cyclohexane dehydrogenation method
CN122124787A