Preparation method and application of activated peroxymonosulfate composite catalyst
By preparing barium iron titanate single atom catalyst, the problem of low efficiency in degrading pollutants in water in the prior art was solved, and efficient and flexible catalyst application was achieved, which significantly improved the pollutant degradation effect.
Patent Information
- Application Number
- CN202411115716.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-15
AI Technical Summary
The single-atom catalysts that activate persulfate to degrade contaminants in water in existing advanced oxidation processes are inefficient, and traditional methods require a large amount of energy input or lead to metal ion contamination.
A method of activating permonosulphate composite catalyst is used to prepare barium titanate by stirring and baking at room temperature, and then adding Fe3+ or Fe2+ to the water bath reaction to prepare barium titanate iron single atom catalyst for efficient degradation of water. Pollutants.
It improves the utilization rate of metal atoms and the flexibility of catalysts, significantly improves the activation efficiency of persulfate, and achieves efficient degradation of pollutants in water, avoids energy input and metal ion pollution.
Smart Images

Figure CN118950000A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of water pollution degradation, and particularly relates to a preparation method and application of an activated permonosulfate composite catalyst. Background Art
[0002] Barium titanate (BaTiO3) is the most common perovskite material. Barium titanate is usually a white powder ABO3 perovskite oxide. The molar mass is 234.233 g / mol and the density is 6.2 g / cm 3 ; Insoluble in water, dilute nitric acid and alkali, soluble in concentrated acid (hydrochloric acid, sulfuric acid and hydrofluoric acid); decomposed into titanium oxide and barium oxide under high temperature conditions. When the A and B positions of the ABO3 type are occupied by Ba ions and Ti ions respectively, BaTiO3 material is formed, which has a typical polycrystalline phase structure of perovskite materials and exhibits different crystal phase structures under different temperature conditions. When the temperature reaches above 120°C, the original cubic phase crystal shows stable behavior and is maintained to 1460°C. When this temperature is exceeded, it exhibits a hexagonal phase crystal.
[0003] There are many ways to activate persulfate. Heterogeneous activation using catalysts is the most common and practical way. The common activation of persulfate by light irradiation, electricity, heat, etc. requires a lot of energy input, which limits its application to a certain extent. Compared with the above activation methods, although persulfate activated by metal ions does not require additional energy input, metal ions are not easy to recover and are prone to secondary pollution of the water after the reaction, increasing the difficulty of subsequent treatment. Therefore, a new type of activator is urgently needed to solve these problems, among which SACs (single atom catalysts) are undoubtedly a good choice. Compared with traditional homogeneous and heterogeneous catalysts, SACs make up for their shortcomings and show higher performance in advanced oxidation, with stronger reactivity, higher catalytic efficiency, wider pH range and less metal ion leaching. Therefore, more and more scholars are trying to use SACs to activate persulfate to degrade organic pollutants.
[0004] SACs have the advantages of homogeneous catalysts and heterogeneous catalysts, becoming a bridge connecting homogeneous catalysts and heterogeneous catalysts. With nearly 100% atomic utilization and unique catalytic properties, they are widely used in electrocatalysis, photocatalysis and thermocatalysis. Compared with ordinary heterogeneous catalysts composed of various active centers, the most important structural feature of SACs is that their isolated single atoms dispersed on the carrier not only maximize the atomic efficiency of the metal, but also provide more uniform and clear active centers. Therefore, SACs have become a hot spot in catalyst research.
[0005] With the introduction of the concept of SACs, more and more studies have shown the potential and advantages of SACs in the field of heterogeneous catalysis. Most metals in traditional catalysts exist in the form of nanoparticles or atomic clusters, in which most metal atoms cannot be effectively utilized. The metal actives in SACs are mononuclear and isolated, so they have great metal utilization, excellent catalytic activity and structural stability. This structure not only maximizes the atomic utilization, but also makes SACs have catalytic behavior different from that of nanocatalysts. At the same time, SACs have also attracted great attention from scholars due to their unique structure and characteristics, especially in maximizing the utilization of atoms and improving catalytic activity. It has become an emerging branch in the environmental field and has been widely used to remove various difficult-to-degrade organic pollutants. Compared with nanoparticle catalysts, SACs also have superior persulfate activation and pollutant degradation performance. The activated persulfate can produce free radicals (SO4 − •, •OH, etc.) and non-free radicals ( 1 O2), used to treat sewage and wastewater. Since Xuning LI et al. first introduced SACs into the Fenton-like reaction of activated persulfate, more and more research has focused on the application of SACs in the activation of persulfate. Among a large number of SACs, Fe, Co, Mn and Cu are the four most studied metal single-atom catalysts for permonosulfate (PMS) activation. Summary of the invention
[0006] In view of the problem of low efficiency of single-atom catalysts for activating PMS to degrade pollutants in water in the current advanced oxidation process, the present invention provides a preparation method and application of an activated permonosulfate composite catalyst.
[0007] In order to achieve the above object, the present invention adopts the following technical solutions: A method for preparing an activated permonosulfate composite catalyst comprises the following steps: Step 1, under stirring at room temperature, firstly slowly drop tetrabutyl titanate into ethanolamine to obtain a mixture 1; Step 2, adding sodium hydroxide and barium chloride dihydrate dropwise to the mixture 1 in sequence to form a suspension; Step 3, sealing the suspension in a polytetrafluoroethylene-lined stainless steel autoclave and baking it to produce a white precipitate; Step 4, centrifuging the white precipitate, then repeatedly washing with ethanol and deionized water to remove the residual reactants, and vacuum drying to obtain BaTiO3; Step 5, add BaTiO3 to the mixture 2 of water and ethylene glycol, and then add Fe 3+ or Fe 2+ The activated permonosulfate composite catalyst is obtained by carrying out a water bath reaction.
[0008] Furthermore, the volume ratio of tetrabutyl titanate to ethanolamine is 1:5.88.
[0009] Further, the molar ratio of sodium hydroxide and barium chloride dihydrate to the mixture is 5:1.
[0010] Furthermore, the baking temperature in step 3 is 180° C. and the baking time is 24 hours.
[0011] Furthermore, the vacuum drying temperature in step 4 is 60°C.
[0012] Furthermore, in step 5, the usage ratio of BaTiO3, water and ethylene glycol is 0.2g:27mL:3mL.
[0013] Furthermore, the temperature of the water bath reaction is 60°C and the reaction time is 10h.
[0014] Further, the Fe 3+ is FeCl3·6H2O, wherein the Fe 2+ It is FeCl2·4H2O.
[0015] Further, the Fe 3+ or Fe 2+ The amount added was 4wt% of the mixture.
[0016] The application of barium iron titanate single-atom catalyst in the degradation of organic pollutants includes the following steps: (1) Pour 1 mL of 200 mg / L sulfamethoxazole solution (SIZ) and 99 mL of ultrapure water into a 100 mL beaker; (2) Add a certain amount of 4 wt% Fe 3+ BTO catalyst and PMS were added to the mixed solution and magnetically stirred at room temperature for 20 minutes; (3) The initial pH was adjusted with 0.1 M HCl or NaOH; 1 mL of liquid sample was collected from the beaker at regular intervals and filtered through a membrane with a pore size of 0.22 μm. The sample was placed in a liquid phase vial, and the concentration of SIZ was subsequently measured using ultra-high performance liquid chromatography tandem mass spectrometry (UPLC-MS / MS) equipped with a Waters ACQUITY liquid chromatograph and a Xevo TQ-S triple quadrupole mass spectrometer (Waters Co., Milford, MA, USA).
[0017] Compared with the prior art, the present invention has the following advantages: The composite catalyst preparation method of the present invention is simple, and iron is successfully attached to barium titanate to prepare an activated permonosulfate composite catalyst, which can effectively improve the utilization rate of metal atoms; The single-atom catalyst preparation method of the present invention is simple, the metal loading and proportion of iron are adjustable, and the catalyst has high flexibility. The present invention has extremely high activation efficiency of PMS, thereby efficiently degrading pollutants in water. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 This is a 200nm TEM image of FeCl3·6H2O with 4% content added; Figure 2 This is a 50nm TEM image with 4% FeCl3·6H2O added; Figure 3 Schematic diagram of the degradation efficiency of barium iron titanate single-atom catalyst for the degradation of organic pollutants; Figure 4 For different proportions of Fe 3+ Schematic diagram of the degradation efficiency of single-atom catalysts. DETAILED DESCRIPTION
[0019] In order to gain a deeper understanding of the present invention, we will provide a comprehensive and detailed description of the present invention. However, the present invention has multiple implementations and is not limited to the specific examples listed herein. The presentation of these examples is intended to deepen the comprehensive understanding of the disclosure of the present invention.
[0020] Example 1
[0021] A method for preparing an activated permonosulfate composite catalyst comprises the following steps: Step 1, under stirring at room temperature, 2.5 mmol of tetrabutyl titanate was slowly dropped into 5 mL of ethanolamine (EA) to obtain a mixture 1; Step 2, NaOH (4.8 M, 12.5 mL) and BaCl2·2H2O (1.0 M, 2.5 mL) were added dropwise to the mixture 1 to form a suspension; Step 3, the suspension was sealed in a 50 mL polytetrafluoroethylene-lined stainless steel autoclave and baked at 180° C. for 24 hours to produce a white precipitate; Step 4, centrifuging the white precipitate, then repeatedly washing with ethanol and deionized water to remove the residual reactants, and vacuum drying at 60° C. to obtain BaTiO3; Step 5, 0.2 g BaTiO3 was added to a mixture 2 of 27 mL water and 3 mL ethylene glycol, and then 4 wt% FeCl3·6H2O was added, and the mixture was reacted in a water bath at 60°C for 10 h to obtain an activated permonosulfate composite catalyst. Its TEM images are shown in Figure (1) and Figure (2).
[0022] Example 2
[0023] This embodiment provides a barium iron titanate single-atom catalyst for degrading organic pollutants. The specific steps are as follows: (1) Pour 1 mL of SIZ (200 mg / L) solution and 99 mL of ultrapure water into a 100 mL beaker; (2) Add a certain amount of 4wt%Fe 3+ BTO catalyst and PMS were added to the mixed solution and magnetically stirred at room temperature for 20 minutes; (3) Adjust the initial pH with 0.1 M HCl or NaOH. At regular intervals, collect 1 mL of liquid sample from the beaker and filter it with a membrane with a pore size of 0.22 μm. The degradation efficiency is shown in Figure (3).
[0024] Example 3
[0025] This example provides different proportions of Fe 3+ The degradation efficiency of the single atom catalyst was changed compared with Example 1. 3+ The content of FeCl3·6H2O is 2wt%, 6wt%, 8wt% and 10wt% respectively. Figure 4 shown.
[0026] Example 4
[0027] This embodiment provides Fe 2+ The method for preparing the single-atom catalyst is different from that in Example 1 except that 4% FeCl2·4H2O is added.
[0028] The contents not described in detail in the specification of the present invention belong to the prior art known to the professional and technical personnel in the field. Although the illustrative specific embodiments of the present invention are described above to facilitate the understanding of the present invention by the technical personnel in the field, it should be clear that the present invention is not limited to the scope of the specific embodiments. For the ordinary technical personnel in the field, as long as various changes are within the spirit and scope of the present invention defined and determined by the attached claims, these changes are obvious, and all inventions and creations using the concept of the present invention are protected.
Claims
1. A method for preparing an activated permonosulfate composite catalyst, characterized in that: The following steps are involved: Step 1, under stirring at room temperature, firstly slowly drop tetrabutyl titanate into ethanolamine to obtain a mixture 1; Step 2, adding sodium hydroxide and barium chloride dihydrate dropwise to the mixture 1 in sequence to form a suspension; Step 3, sealing the suspension in a polytetrafluoroethylene-lined stainless steel autoclave and baking it to produce a white precipitate; Step 4, centrifuging the white precipitate, then repeatedly washing with ethanol and deionized water to remove the residual reactants, and vacuum drying to obtain BaTiO3; Step 5, add BaTiO3 to the mixture 2 of water and ethylene glycol, and then add Fe 3+ or Fe 2+ The activated permonosulfate composite catalyst is obtained by carrying out a water bath reaction.
2. The method for preparing an activated permonosulfate composite catalyst according to claim 1, characterized in that: The volume ratio of tetrabutyl titanate to ethanolamine is 1:5.
88.
3. The method for preparing an activated permonosulfate composite catalyst according to claim 1, characterized in that: The molar ratio of sodium hydroxide and barium chloride dihydrate to the mixture is 5:
1.
4. The method for preparing an activated permonosulfate composite catalyst according to claim 1, characterized in that: The baking temperature in step 3 is 180° C. and the baking time is 24 hours.
5. The method for preparing an activated permonosulfate composite catalyst according to claim 1, characterized in that: The vacuum drying temperature in step 4 is 60°C.
6. The method for preparing an activated permonosulfate composite catalyst according to claim 1, characterized in that: In the step 5, the usage ratio of BaTiO3, water and ethylene glycol is 0.2g:27mL:3mL.
7. The method for preparing an activated permonosulfate composite catalyst according to claim 1, characterized in that: The temperature of the water bath reaction was 60°C and the reaction time was 10 h.
8. The method for preparing an activated permonosulfate composite catalyst according to claim 1, characterized in that: The Fe 3+ is FeCl3·6H2O, wherein the Fe 2+ It is FeCl2·4H2O.
9. The method for preparing an activated permonosulfate composite catalyst according to claim 1, characterized in that: The Fe 3+ or Fe 2+ The amount added was 4wt% of the mixture.
10. Use of the barium iron titanate single-atom catalyst according to any one of claims 1 to 9 in the degradation of organic pollutants, characterized in that: The following steps are involved: (1) Pour 1 mL of 200 mg / L sulfamethoxazole solution and 99 mL of ultrapure water into a 100 mL beaker; (2) Add a certain amount of 4 wt% Fe 3+ BTO catalyst and PMS were added to the mixed solution and magnetically stirred at room temperature for 20 minutes; (3) The initial pH was adjusted with 0.1 M HCl or NaOH. At regular time intervals, 1 mL of liquid sample was collected from the beaker, filtered through a membrane with a pore size of 0.22 μm, and placed in a liquid vial. The concentration of SIZ was then measured using ultra-high performance liquid chromatography-tandem mass spectrometry equipped with a Waters ACQUITY liquid chromatograph and a Xevo TQ-S triple quadrupole mass spectrometer.