Oxygen carrier for preparing synthesis gas and hydrogen through chemical chain conversion of biogas as well as preparation method and application of oxygen carrier
The w% Ni/CeO2 oxygen carrier prepared by one pot method solves the problems of easy sintering of the oxygen carrier and low methane conversion rate, and achieves efficient methane conversion and H2 yield, simplifies the preparation process and reduces costs. Excellent cycle stability.
Patent Information
- Application Number
- CN202411024481.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-15
AI Technical Summary
The existing oxygen carriers are prone to sintering under high temperature conditions, resulting in low methane conversion, low H2 yield, and complex preparation methods and high cost.
W% Ni/CeO2 oxygen carrier was prepared by one pot method. Through drying, calcining, calcining and hydrogen reduction, oxygen carrier with small Ni nanoparticle size and high metal Ni dispersion were formed. Some Ni was occupied in doped form. CeO2 site forms Ce1-xNixO2 solid solution, inhibits sintering and increases oxygen vacancies concentration.
Achieve higher methane conversion and H2 yield, simplify the preparation process, reduce costs, and maintain high CH4 conversion, CO2 conversion and H2O cleavage activity after 20 cycle reactions, with excellent cycle stability .
Smart Images

Figure CN118950009A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of biogas chemical chain conversion to produce synthesis gas and hydrogen, and particularly relates to an oxygen carrier used for biogas chemical chain conversion to produce synthesis gas and hydrogen, and a preparation method and application thereof. Background Art
[0002] The burning of fossil fuels releases a large amount of greenhouse gases, exacerbating global warming. Therefore, the search for clean and sustainable energy has become a top priority. Hydrogen, as a clean energy carrier, can achieve zero carbon dioxide emissions and is expected to become an ideal choice for methanol production, metal and glass casting in the coming decades. However, the process of producing hydrogen from fossil fuels will cause a large amount of carbon dioxide emissions. Therefore, in the long run, low-carbon and sustainable hydrogen production methods have received increasing attention.
[0003] Biogas is mainly produced by anaerobic digestion of organic matter such as crop straw, urban garbage, food industry garbage and agricultural garbage. It is a renewable carbon-neutral energy source that can replace fossil fuels to produce hydrogen. Biogas mainly contains CH4 and CO2, with a ratio close to 2, and other gas components are relatively small. Chemical chain biogas conversion technology can achieve the co-production of hydrogen and synthesis gas by circulating oxygen carriers between reduction reactors and oxidation reactors. In the reduction reactor, biogas is catalyzed by oxygen carriers and reacts with its lattice oxygen to generate synthesis gas, mainly including two reactions: partial oxidation of methane (CH4+MeO→2H2+CO+Me) and dry reforming of methane (CH4+CO2→2CO+2H2). Subsequently, in the oxidation reactor, the reduced oxygen carrier is oxidized and regenerated by H2O, and high-purity hydrogen (Me+H2O→MeO+H2) is produced at the same time. Compared with traditional processes, high-purity hydrogen can be obtained without water-gas shift, pressure swing adsorption and amine absorption and other technical treatments, which greatly reduces the cost of hydrogen separation.
[0004] CeO2 is widely used in chemical looping technology due to its excellent oxygen storage and release capacity and high syngas selectivity. However, the activity of pure CeO2 is low, resulting in a low methane conversion rate. Active metal Ni has good methane activation ability and is often used as an active additive or dopant to promote the reaction between Ce-based oxygen carriers and methane. However, the Ni / CeO2 oxygen carrier prepared by the traditional impregnation method, Ni nanoparticles are easily sintered under high temperature conditions, resulting in a significant decrease in CH4 activation ability and low oxygen carrying capacity, which in turn limits its H2 production. The main application bottlenecks facing oxygen carriers at present are easy sintering, low methane conversion rate, and low H2 production. Summary of the invention
[0005] In order to overcome the problem of low methane conversion rate, the purpose of the present invention is to provide an oxygen carrier for biogas chemical chain conversion to produce synthesis gas and hydrogen, and its preparation method and application. The oxygen carrier has a smaller Ni nanoparticle size, a higher methane conversion rate, a high H2 yield, and a simple preparation method, easy to operate, and is suitable for industrial production.
[0006] To achieve the above object, the technical solution adopted by the present invention is:
[0007] An oxygen carrier used for biogas chemical chain conversion to produce synthesis gas and hydrogen, the chemical formula of the oxygen carrier is w% Ni / CeO2, wherein 1%≤w%≤10%.
[0008] Furthermore, w% is 1%, 3%, 5%, 7% or 10%.
[0009] A method for preparing an oxygen carrier for biogas chemical chain conversion to synthesis gas and hydrogen comprises drying, roasting, calcining, and then reducing with hydrogen to obtain an oxygen carrier for biogas chemical chain conversion to synthesis gas and hydrogen.
[0010] Furthermore, the Ce precursor is at least one of Ce(NO3)3·6H2O and CeCl3·6H2O.
[0011] Furthermore, the Ni precursor solution is an aqueous solution of Ni(NO3)2·6H2O and NiCl2·6H2O.
[0012] Furthermore, the ratio of the molar amount of glycine to the total molar amount of Ce and Ni is 1.5-2.5:1.
[0013] Further, the drying temperature is 40-60°C and the time is 0.5-1h;
[0014] The calcination process is: calcination at 400-600°C for 3-5 minutes, and then calcination at 700-900°C for 3-5 hours.
[0015] Furthermore, the reduction process is: reducing at 400-600° C. for 5-50 min under the condition of a mixed gas of H 2 and He.
[0016] An oxygen carrier is used in biogas chemical chain conversion to produce synthesis gas and hydrogen. The oxygen carrier is circulated between two interconnected fuel reactors and a regeneration reactor. In the fuel reactor, the oxygen carrier oxidizes biogas at 700-900°C to generate synthesis gas. In the regeneration reactor, the oxygen carrier is oxidized and regenerated in an oxidizing atmosphere at 700-900°C and then enters the fuel reactor.
[0017] Furthermore, the biogas in the fuel reactor is a mixture of CH4 and CO2 in a volume ratio of 1 to 3:1, CH4 and CO2 are mixed and fed together, the oxidizing atmosphere is water vapor, the temperature is 25 to 50°C, and the saturated vapor pressure is 3 to 14 kPa.
[0018] Compared with the prior art, the present invention has the following beneficial technical effects:
[0019] The oxygen carrier w% Ni / CeO2 (1%≤w%≤10%) of the present invention is an oxygen carrier prepared by a one-pot method. Compared with the oxygen carrier w% Ni / CeO2-IM prepared by a traditional impregnation method, the w% Ni / CeO2-OP prepared by the present invention has a smaller Ni nanoparticle size, a higher metal Ni dispersion and an active specific surface area, and part of the Ni in the w% Ni / CeO2-OP oxygen carrier occupies the Ce site of CeO2 in the form of doping to form Ce 1-x Ni x O2 solid solution, which not only inhibits the sintering of active Ni nanoparticles but also increases the oxygen vacancy concentration, which is beneficial to the activation of CH4 and the rapid migration of lattice oxygen.
[0020] The invention uses a Ce precursor, a Ni precursor solution, and glycine dissolved in water to form a precursor solution, which is dried, roasted, calcined, and then reduced with hydrogen to obtain an oxygen carrier for biogas chemical chain conversion to produce synthesis gas and hydrogen. The preparation method of the invention is simple, environmentally friendly, low in cost, and easy to industrialize.
[0021] When the oxygen carrier of the present invention is used in biogas chemical chain conversion to produce synthesis gas and hydrogen, in the reduction reactor, when the biogas chemical chain conversion generates synthesis gas, two reactions mainly occur: partial oxidation of methane (CH4+MeO→2H2+CO+Me) and dry reforming of methane (CH4+CO2→2CO+2H2). Subsequently, in the oxidation reactor, the reduced oxygen carrier is oxidized and regenerated by H2O, and high-purity hydrogen (Me+H2O→MeO+H2) is generated at the same time. Compared with hydrogen production by methane water cracking or traditional fossil fuel hydrogen production technology, chemical chain biogas conversion hydrogen production technology has many advantages: (1) No complex separation steps are required, and in-situ carbon-hydrogen separation can be achieved through simple water vapor condensation operation, which greatly improves the efficiency of pure hydrogen production; (2) Only one oxygen carrier is required instead of multiple solid catalysts, which simplifies the hydrogen production process; (3) Biogas is used instead of methane, and a mixture of methane and carbon dioxide is used, which reduces the cost of separation of methane and carbon dioxide, achieves good economic benefits, and also provides a new idea for biogas utilization and hydrogen production; (4) Synthesis gas is co-produced, which realizes the simultaneous production of hydrogen and synthesis gas, improves resource utilization efficiency and expands the product range. The oxygen carrier prepared by the present invention has excellent methane activation ability and cycle stability. After 20 redox cycles, the CH4 conversion rate of the sample prepared by the impregnation method decreased significantly, while the CH4 and CO2 conversion rates of the Ni / CeO2 oxygen carrier prepared by the one-pot method remained at 92% and 83%, the synthesis gas yield remained basically stable, and the H2 yield was 3.2mmol / g cat , CO yield was 2.43mmol / g cat In summary, the 5% Ni / CeO2-OP prepared by the one-pot method maintained high CH4 conversion, CO2 conversion, syngas yield and H2O cracking activity during 20 cycles, and had excellent cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is a comparison diagram of the X-ray powder diffraction spectra of the oxygen carrier in the fresh state of Comparative Example 1 and Example 1; wherein (a) is a comparison diagram of the X-ray powder diffraction spectra, and (b) is a partial enlarged diagram of Figure (a);
[0023] Figure 2 It is a comparison diagram of oxygen activity measured by H2 programmed temperature reduction of oxygen carriers of comparative example 1 and example 1;
[0024] Figure 3 It is a comparison diagram of the Raman spectrum test spectra of the oxygen carrier of Comparative Example 1 and Example 1;
[0025] Figure 4The transmission electron microscope element distribution diagrams of the oxygen carriers of Comparative Example 1, Example 1, Comparative Example 2 and Example 2 are compared, wherein (a) is the microscopic morphology diagram of Example 1, (b) is the element distribution diagram in Example 1, (c) is the Ce element distribution diagram in Example 1, (d) is the O element distribution diagram in Example 1, and (e) is the Ni element distribution diagram in Example 1; (f) is the microscopic morphology diagram of Comparative Example 1, (g) is the element distribution diagram in Comparative Example 1, (h) is the Ce element distribution diagram in Comparative Example 1, and (i) is the O element distribution diagram in Comparative Example 1. Element distribution diagram, (j) is the Ni element distribution diagram in comparative example 1; (k) is the microscopic morphology diagram of Example 2, (l) is the element distribution diagram in Example 2, (m) is the Ce element distribution diagram in Example 2, (n) is the O element distribution diagram in Example 2, and (o) is the Ni element distribution diagram in Example 2; (p) is the microscopic morphology diagram of comparative example 2, (q) is the element distribution diagram in comparative example 2, (r) is the Ce element distribution diagram in comparative example 2, (s) is the O element distribution diagram in comparative example 2, and (t) is the Ni element distribution diagram in comparative example 2;
[0026] Figure 5 A comparison diagram of the methane reaction activity kinetics of the oxygen carrier prepared in Example 2;
[0027] Figure 6 A comparison diagram of the methane reaction activity kinetics of the oxygen carrier prepared in Comparative Example 2;
[0028] Figure 7 This is a comparison chart of CH4 conversion rates of oxygen carriers prepared in Comparative Example 1 and Example 1 during 20 cycles of reaction;
[0029] Figure 8 This is a comparison chart of CO2 conversion rates of oxygen carriers prepared in Comparative Example 1 and Example 1 during 20 cycles of reaction;
[0030] Fig. 9 This is a comparison chart of the synthesis gas yields of the oxygen carriers prepared in Comparative Example 1 and Example 1 during 20 cycles of reaction;
[0031] Fig.10 This is a comparison chart of H2O decomposition activity of oxygen carriers prepared in Comparative Example 1 and Example 1 during 20 cycles of reaction;
[0032] Fig.11 The X-ray powder diffraction spectrum of the oxygen carrier prepared in Example 2; wherein (a) is the X-ray powder diffraction spectrum of the oxygen carrier in Example 2, and (b) is a partial enlarged view of part of Figure (a);
[0033] Fig.12 This is a comparison chart of the reaction activities of methane and carbon dioxide in two feeding methods in Example 1. DETAILED DESCRIPTION
[0034] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present invention are given in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thoroughly and comprehensively understood.
[0035] The present invention discloses a method for preparing an oxygen carrier for preparing synthesis gas and hydrogen by biogas chemical chain conversion, which adopts a one-pot method and specifically comprises the following steps:
[0036] A Ce precursor, a Ni precursor solution and glycine are dissolved in distilled water in proportion to form a precursor solution, which is subjected to low-temperature drying, solution roasting, grinding, calcination and hydrogen reduction to obtain an oxygen carrier for biogas chemical chain conversion to produce synthesis gas and hydrogen, denoted as w% Ni / CeO2 (1%≤w%≤10%), wherein the preferred w% is 1%, 3%, 5%, 7% or 10%, i.e., the mass content of Ni in the oxygen carrier for biogas chemical chain conversion to produce synthesis gas and hydrogen is w%.
[0037] Wherein, the Ce precursor is at least one of Ce(NO3)3·6H2O and CeCl3·6H2O;
[0038] The Ni precursor is at least one of Ni(NO3)2·6H2O and NiCl2·6H2O;
[0039] The molar ratio of glycine to total metal ions is 1.5-2.5:1.
[0040] The prepared oxygen carrier is marked as w% Ni / CeO2-OP.
[0041] Drying temperature: 40-60℃, drying time: 0.5-1h.
[0042] The calcination process is that the solution is directly placed in a muffle furnace preheated to 400-600°C and calcined for 3-5 minutes. The obtained particles are ground into powder and then heated to the target temperature for calcination. The target calcination temperature is 700-900°C and the calcination time is 3-5 hours.
[0043] The reduction process is: reduction is carried out at 400-600° C. for 5-50 minutes under the condition of 5-20% H2 / He. 5-20% H2 / He means that the volume percentage of H2 in the mixed gas of H2 and He is 5-20%.
[0044] The oxygen carrier as described above is used for the application of biogas chemical chain conversion to produce synthesis gas and hydrogen, specifically: the oxygen carrier circulates between two connected reactors (a fuel reactor and a regeneration reactor); in the fuel reactor, the oxygen carrier oxidizes the biogas at 700-900°C to produce synthesis gas; in the regeneration reactor, the oxygen carrier is oxidized and regenerated at 700-900°C in an oxidizing atmosphere, and then enters the fuel reactor.
[0045] Among them, the biogas in the fuel reactor is a mixture of CH4 and CO2, the volume of CH4 and CO2 in the biogas is 1 to 3:1, the oxidizing atmosphere is water vapor, and the water vapor is brought into the reactor by bubbling (the flow rate of He is 15 mL / min, the bubbler is placed in a water bath at 25 to 50°C, and the saturated vapor pressure is 3 to 14 kPa).
[0046] The oxygen carrier has a smaller Ni nanoparticle size (54.4-62.3nm), a higher metal Ni dispersion (2.8-3.3%) and an active specific surface area. After 20 oxidation cycles, the CH4 and CO2 conversion rates of the oxygen carrier remained at 92% and 83%, respectively. The syngas yield remained basically stable during the cycle, and the H2 yield of H2O cracking remained at 1.37mmol / g. Compared with the isovolumetric impregnation method, the Ni / CeO2 prepared by the one-pot method has higher CH4 activation ability, syngas yield and H2O cracking activity, and has excellent reaction activity and cycle stability, which highlights the superiority of the one-pot method for preparing Ni / CeO2 oxygen carriers.
[0047] Comparative Example 1
[0048] Preparation of 5% Ni / CeO2 by equal volume impregnation method.
[0049] Ce(NO3)3·6H2O and glycine (the molar ratio of glycine to total metal ions is 2.5:1) are dissolved in appropriate amount of water in proportion. The solution is then dried in a 60°C oven for 1 hour, followed by calcination in a muffle furnace (500°C) for 5 minutes, and marked as CeO2-500. Then, the diluted Ni solution is added to CeO2-500 in proportion (Ni to CeO2 mass fraction ratio is 5%), and stirred until it becomes a paste. Then, it is sealed with aluminum foil and allowed to stand at room temperature for 4 hours, then placed in a 60°C constant temperature drying oven for 12 hours, ground into powder, and finally calcined at 800°C for 4 hours to obtain the desired supported oxide, marked as 5% NiO / CeO2-IM. Subsequently, the supported oxide is reduced for 30 minutes under 10% H2 / He at 500°C, and marked as 5% Ni / CeO2-IM.
[0050] Comparative Example 2
[0051] Preparation of 5% Ni / CeO2-IM-20cycle
[0052] First, weigh 100 mg of the oxygen carrier in Comparative Example 1, place the sample between double layers of quartz wool, heat to 850°C at 10°C / min in a 20mL / min He atmosphere, then reduce the oxygen carrier in a simulated biogas atmosphere for 8 minutes, the mixed gas composition is 4% CH4 / 2% CO2 / He, the gas flow rate is 15mL / min; after reduction, purge with He for 6 minutes, the gas flow rate is 20mL / min; then use the bubbling method to bring water vapor into the reactor for oxidation, the oxidation time is 8 minutes, the He flow rate is 15mL / min, the bubbler is placed in a 30°C water bath, and the saturated vapor pressure of water is 4.1kPa. Repeat the above steps 20 times to obtain a catalyst, recorded as 5% Ni / CeO2-IM-20cycle.
[0053] Example 1
[0054] Preparation of 5% Ni / CeO2 by one-pot method.
[0055] First, the weighed Ni(NO3)2·6H2O was dissolved in 10mL of distilled water to obtain a Ni solution, and Ce(NO3)3·6H2O, Ni solution and glycine (the molar ratio of glycine / total metal ions was 2.5:1) were dissolved in 6mL of water in proportion (Ni to CeO2 mass fraction ratio was 5%). Then the solution was dried in a 60℃ oven at a constant temperature for 1h. Subsequently, the solution was directly placed in a muffle furnace preheated to 500℃ and calcined for 5min. Finally, the obtained powder was ground into powder and calcined at 800℃ for 4h to obtain a supported oxide. Subsequently, the supported oxide was reduced for 30min under 10% H2 / He at a temperature of 500℃ to obtain an oxygen carrier for biogas chemical chain conversion to produce synthesis gas and hydrogen, marked as 5% Ni / CeO2-OP.
[0056] Example 2
[0057] Preparation of 5% Ni / CeO2-OP-20cycle.
[0058] First, 100 mg of the oxygen carrier in Example 1 was weighed, and the sample was placed between double layers of quartz wool. The temperature was raised to 850° C. at 10° C. / min in a 20 mL / min He atmosphere. The oxygen carrier was then reduced in a simulated biogas atmosphere for 8 min, with a mixed gas composition of 4% CH4 / 2% CO2 / He and a gas flow rate of 15 mL / min. After reduction, He was purged for 6 min at a gas flow rate of 20 mL / min. Then, water vapor was brought into the reactor for oxidation using a bubbling method. The oxidation time was 8 min, the He flow rate was 15 mL / min, the bubbler was placed in a 30° C. water bath, and the saturated vapor pressure of water was 4.1 kPa%. The above steps were repeated 20 times to obtain a catalyst, recorded as 5% Ni / CeO2-OP-20cycle.
[0059] Example 3
[0060] The oxygen carriers prepared in Comparative Example 1 and Example 1 were subjected to XRD tests on a PANalytical X'Pert-Propowder X-ray powder diffractometer, and Cu Kα radiation with a wavelength of λ=0.15418 nm was used to obtain X-ray diffraction spectra (XRD). The X-ray diffraction test results are shown in FIG. Figure 1 As shown in (a) and (b), Figure 1 (a) is the X-ray powder diffraction spectrum of the fresh oxygen carrier. Figure 1 (b) is a partial enlarged view of Figure (a).
[0061] from Figure 1 It can be seen that the oxygen carrier prepared by the impregnation method is consistent with CeO2 (PDF#03-065-5923), while the oxygen carrier prepared by the one-pot method is offset to a higher angle. This indicates that part of the Ni (Ni 2+ :72pm) occupies the Ce site of CeO2 in the form of doping (Ce 4+ :92pm), forming Ce 1-x Ni x O2 solid solution.
[0062] Example 4
[0063] The oxygen carriers prepared in Comparative Example 1 and Example 1 were tested for oxygen activity of fresh oxygen carriers by H2-TPR using a Micromerics Autochem II 2920 device. 200 mg of the sample was placed in a quartz tube and heated to 900° C. at a heating rate of 10° C. / min in a 10% H2 / Ar mixture (50 mL / min). The H2-TPR test results are shown in Table 1. Figure 2 shown.
[0064] from Figure 2It can be seen that both oxygen carriers have three reduction peaks, marked as peaks α, β and γ. Peak α is mainly attributed to the reduction process of Ni species on the carrier surface that have weak interaction with CeO2, peak β is attributed to the reduction of Ni species that have strong interaction with CeO2, and peak γ is attributed to the reduction of CeO2. Compared with 5% NiO / CeO2-IM, the α reduction peak of 5% NiO / CeO2-OP has a higher reduction temperature, a smaller reduction peak intensity, and an enhanced β reduction peak intensity, indicating that the oxygen carrier prepared by the one-pot method has less free NiO on the surface and an increased content of Ni species that have strong interaction with CeO2. This is because part of Ni occupies the Ce sites of CeO2 in the form of doping, forming Ce 1-x Ni x O2 solid solution, which is consistent with the XRD results.
[0065] Example 5
[0066] The oxygen carriers prepared in Comparative Example 1 and Example 1 were tested for Raman spectra using a NanoWizard Raman spectrometer, using a 532nm wavelength laser as the incident light source. The test results are shown in Figure 2. Figure 3 shown.
[0067] from Figure 3 It can be seen that 460cm -1 The stronger peak at 555cm is due to the local symmetry vibration of the octahedron around the CeO2 lattice. -1 The obvious shoulder peak at is caused by the oxygen vacancies in CeO2. Figure 3 It can be found that 5% Ni / CeO2-OP has a higher peak at 555 cm than 5% Ni / CeO2-IM. -1 The larger integrated area at the bottom of the graphene indicates that the one-pot prepared oxygen carrier generates more oxygen vacancies, which may be due to the formation of Ce during the one-pot preparation process. 1-x Ni x O2 solid solution. The presence of oxygen vacancies facilitates the migration of lattice oxygen and the partial oxidation of methane.
[0068] Example 6
[0069] The oxygen carriers prepared in Comparative Example 1, Example 1, Comparative Example 2 and Example 2 were subjected to H2 pulse chemical adsorption test, and the particle size, dispersion and active specific surface area of the metal nanoparticles on the surface of the samples were determined using the AutoChemⅡ2920 chemical adsorption instrument produced by Micromeritics. 100 mg of the sample was weighed in a U-shaped tube and heated at 30 mL min -1The temperature was raised to 500°C at a rate of 10°C / min in pure H2 atmosphere and maintained for 1 h, then switched to Ar atmosphere for 30 min, and then dropped to 50°C in Ar atmosphere. After the temperature and baseline were stable, H2 pulse test (10% H2 / Ar) was started. The test results are summarized in Table 1.
[0070] Table 1 Structural properties of oxygen carriers
[0071]
[0072] a The Ni crystallite size was estimated based on the Scherrer formula based on the Ni(111) crystal plane in the XRD spectrum.
[0073] b The Ni particle size, Ni dispersion and Ni active metal specific surface area were estimated based on the chemically adsorbed H2 pulse.
[0074] According to Table 1, the Ni particle sizes of 5% Ni / CeO2-OP and 5% Ni / CeO2-IM are 21.9-30.6 nm and 39.4-53.0 nm, respectively. After 20 redox cycles, the Ni nanoparticle size of 5% Ni / CeO2-OP-20cycle only slightly increases to 27.8-35.7 nm, while the Ni nanoparticle size of 5% Ni / CeO2-IM-20cycle grows sharply to 54.4-62.3 nm; compared with the traditional impregnation method (metal dispersion is 1.6-1.9%), the Ni-based oxygen carrier prepared by the one-pot method has a higher metal dispersion (2.8-3.3%), and the specific surface area is almost twice that of the oxygen carrier prepared by the traditional impregnation method. Even after 20 cycles, it still has a high Ni dispersion and specific surface area. It can be seen that the Ni-based oxygen carrier prepared by the one-pot method has smaller particles, better dispersion, and larger specific surface area, which is conducive to contact and activation with CH4.
[0075] Example 7
[0076] For the oxygen carriers prepared in Comparative Example 1, Example 1, Comparative Example 2 and Example 2, element distribution maps (EDS-mapping) of the samples were obtained by transmission electron microscopy (JEOL JEM-2100F TEM) equipped with an energy dispersive X-ray spectrometer (EDS). The EDS-mapping characterization results are shown in FIG. Figure 4As shown. Wherein, (a)-(e): Example 1, fresh oxygen carrier prepared by one-pot method, denoted as 5% Ni / CeO2-OP. (f)-(j): Comparative Example 1, fresh oxygen carrier prepared by equal volume impregnation method, denoted as 5% Ni / CeO2-IM. (k)-(o): Example 2, oxygen carrier after 20 cycles prepared by one-pot method, denoted as 5% Ni / CeO2-OP-20cycle. (p)-(t): Comparative Example 2, oxygen carrier after 20 cycles prepared by equal volume impregnation method. denoted as 5% Ni / CeO2-IM-20cycle.
[0077] from Figure 4 It can be seen that the fresh and 20-cycle oxygen carrier particles are composed of three elements: Ce, O and Ni. The Ce and O elements are evenly distributed. Compared with the fresh 5% Ni / CeO2-IM oxygen carrier prepared by the equal volume impregnation method, the Ni nanoparticles of 5% Ni / CeO2-OP are smaller and more evenly distributed. After 20 redox cycles, the Ni nanoparticles in the sample prepared by the impregnation method grew significantly after 20 cycles. No obvious particle aggregation and growth was observed in 5% Ni / CeO2-OP-20cycle, which is consistent with the above-mentioned H2 pulse chemical adsorption test results.
[0078] Example 8
[0079] The oxygen carriers prepared in Comparative Example 2 and Example 2 were evaluated for methane reactivity. The oxygen carrier mass was 100 mg, and was treated with 5% CH4 / He (30 mL / min). The temperature was increased from 20°C to 850°C at a heating rate of 10°C / min. The reaction outlet gas was analyzed using a mass spectrometer (IPI GAM 200). The reaction results are shown in Figure 2. Figure 5 and Figure 6 shown.
[0080] from Figure 5 It can be seen that for 5% Ni / CeO2-OP-20cycle, the signals of H2 and CO were detected at 355℃ and 510℃, respectively, which correspond to the CH bond breaking of CH4 (CH4→*C+2H2) and the selective oxidation of C atoms in CH4 by lattice oxygen (*C+OL→CO+[O vac. ]).
[0081] from Figure 6 It can be seen that the starting temperature of the 5% Ni / CeO2-IM-20cycle syngas significantly increased to 537°C for H2 and 550°C for CO. In addition, the signal intensity of the syngas also decreased significantly. These indicate that the oxygen carrier prepared by the one-pot method has higher methane reactivity and syngas yield after 20 cycles than the oxygen carrier prepared by the equal volume impregnation method.
[0082] Example 10
[0083] For the oxygen carriers of Comparative Example 1 and Example 1, a fixed bed reactor was used to evaluate the cyclic stability of the oxygen carrier biogas chemical chain conversion to produce synthesis gas and hydrogen. The mass of the oxygen carrier is 100 mg, the fuel reaction gas is simulated biogas (CH4 / CO2=4% / 2%), the flow rate is 15 mL / min, the reaction temperature is 850°C, and the reaction time is 8 min. He was purged for 6 min (20 mL / min), and then water vapor was brought into the reactor by bubbling (the flow rate of He was 15 mL / min, and the bubbler was placed in a 30°C water bath, and the saturated vapor pressure of water at this temperature was 4.1 kPa), and the oxidation time was 8 min. The above steps were repeated 20 times to test the stability of the oxygen carrier. The reaction outlet gas was analyzed online using a mass spectrometer (IPI GAM 200). The stability evaluation results are shown in the figure. Figure 7 , Figure 8 , Fig. 9 and Fig.10 shown.
[0084] from Figure 7 It can be seen that the initial CH4 conversion rates of 5% Ni / CeO2-OP and 5% Ni / CeO2-IM are similar. After 20 cycles, the methane conversion rate of 5% Ni / CeO2-IM drops significantly to 78%, while the methane conversion rate of 5% Ni / CeO2-OP can still be maintained at 92%.
[0085] from Figure 8 It can be seen that the initial CO2 conversion rates of 5% Ni / CeO2-OP and 5% Ni / CeO2-IM were similar at the beginning of the reaction. After 20 redox cycles, the CO2 conversion rate of 5% Ni / CeO2-IM decreased to 75%, but the CO2 conversion rate of 5% Ni / CeO2-OP increased to 83%.
[0086] from Fig. 9 It can be seen that during the biogas reduction reaction, the H2 yield and CO yield of 5% Ni / CeO2-IM decreased, while the synthesis gas of 5% Ni / CeO2-OP remained basically stable, among which the H2 yield remained stable at 3.2mmol / g cat , CO yield remained stable at 2.43mmol / g cat .
[0087] from Fig.10It can be seen that in the process of H2O cracking to produce hydrogen, the initial H2 yield of 5% Ni / CeO2-OP and 5% Ni / CeO2-IM is close to 1.47mmol / g. After 20 cycles of reaction, 5% Ni / CeO2-IM drops to 1.21mmol / g, while 5% Ni / CeO2-OP can still be maintained at 1.37mmol / g.
[0088] It can be seen that compared with the 5% Ni / CeO2-IM prepared by the isovolumetric impregnation method, the 5% Ni / CeO2-OP prepared by the one-pot method still maintains high CH4 conversion (92%), CO2 conversion (83%), and syngas yield (H2 yield of 3.2 mmol / g) after 20 redox cycles. cat , CO yield was 2.43mmol / g cat ) and H2O splitting activity (H2 yield remained at 1.37 mmol / g), and had excellent cyclic stability.
[0089] Embodiment 11
[0090] The oxygen carrier prepared in Example 2 was subjected to XRD test on a PANalytical X'Pert-Propowder X-ray powder diffractometer, and Cu Kα radiation with a wavelength of λ=0.15418nm was used to obtain an X-ray diffraction spectrum (XRD). The X-ray diffraction test results are shown in FIG. Fig.11 As shown, Fig.11 (a) is the X-ray powder diffraction spectrum of the oxygen carrier of Example 2, Fig.11 (b) is a partial enlarged view of part of Figure (a).
[0091] from Fig.11 It can be seen that the oxygen carrier prepared by the one-pot method shifts to a higher angle after 20 cycles. This indicates that the Ce formed in the oxygen carrier prepared by the one-pot method 1-x Ni x The O2 solid solution was still maintained after 20 redox cycles.
[0092] Example 12
[0093] In the biogas chemical looping process for producing synthesis gas in Example 10, CH4 0 The active sites are activated and dissociated to generate H2 and activated carbon species (CH4→*C+2H2), and then the lattice oxygen (*C+O L →CO+[O vac. ]) and CO2 oxidize C atoms (CO2+C→2CO) to generate CO. By analyzing the contents of CH4, CO2, and products, the partial oxidation of methane (OL ) and the ratio of methane dry reforming (CO2), the calculation results are shown in Table 2.
[0094] Table 2 CH4 conversion pathways of fresh and recycled 5% Ni / CeO2-X oxygen carriers
[0095]
[0096] As can be seen from Table 2, during the first redox cycle, the methane dry reforming conversion rates (39%) of 5% Ni / CeO2-OP and 5% Ni / CeO2-IM were the same, and there was no significant change after 20 redox cycles (39%→38-40%), that is, the oxygen carriers prepared by different methods had little effect on the methane dry reforming performance. However, the methane partial oxidation conversion rate of 5% Ni / CeO2-IM was as high as 57% during the first cycle, which was significantly reduced to 40% after 20 redox cycles. This indicates that the oxidation ability of lattice oxygen to carbon species gradually weakens, that is, with the cyclic reaction, the lattice oxygen migration ability of the oxygen carrier prepared by the impregnation method gradually decreases. However, the oxygen carrier prepared by the one-pot method still maintained a high methane partial oxidation conversion rate (52%) after 20 redox cycles, proving that the oxygen carrier prepared by the one-pot method has a higher lattice oxygen mobility during the methane partial oxidation process.
[0097] Embodiment 13
[0098] For Example 1, a fixed bed reactor was used to test the activity of the oxygen carrier biogas chemical chain conversion to produce synthesis gas and hydrogen (the biogas feeding method was separate feeding and mixed feeding). First, 100 mg of the oxygen carrier in Example 1 was weighed, and the sample was placed between double layers of quartz wool. The temperature was raised to 850°C at 10°C / min under a 20mL / min He atmosphere, and then the oxygen carrier was reduced in a reducing atmosphere for 8min, with a gas flow rate of 15mL / min. He was purged for 6min (20mL / min), and then the oxygen carrier was oxidized in an oxidizing atmosphere for 8min. The reaction outlet gas was analyzed online using a mass spectrometer (IPI GAM 200). Among them, the mixed feed: the reducing atmosphere was a mixed gas of 4% CH4 / 2% CO2 / He, and the oxidizing atmosphere was water vapor (the water vapor was brought into the reactor using a bubbling method, the flow rate of He was 15mL / min, and the bubbler was placed in a 30°C water bath, and the saturated vapor pressure of water at this temperature was 4.1kPa). Feed separately: reducing atmosphere is 4% CH4 / He mixed gas, oxidizing atmosphere is 2% CO2 / He mixed gas. Test results are as follows Fig.12 shown.
[0099] from Fig.12It can be concluded that the CH4 conversion rate is maintained at about 98% by using both co-feeding and separate feeding of CH4 and CO2. However, the CO2 conversion rate of separate feeding is only 76%, and the conversion rate of co-feeding CO2 is higher at 85%. This is because the CO2 in the co-feed can provide oxygen for CH4 oxidation, thereby inhibiting methane cracking and carbon deposition, thereby greatly improving the CO2 conversion rate. In addition, biogas is a mixed gas of methane and carbon dioxide. Co-feeding also reduces the separation cost of methane and carbon dioxide. Therefore, directly using biogas as a raw material to prepare synthesis gas by co-feeding, coupled chemical chain hydrogen production has excellent economic benefits.
[0100] Embodiment 14
[0101] Preparation of 1% Ni / CeO2-OP
[0102] First, the weighed NiCl2·6H2O was dissolved in 10mL of distilled water to obtain a Ni solution, and CeCl3·6H2O, Ni solution and glycine (the molar ratio of glycine / total metal ions was 1.5:1) were dissolved in 3mL of water in proportion. The solution was then dried in a 40°C oven at a constant temperature for 1h. Subsequently, the solution was directly placed in a muffle furnace preheated to 400°C and calcined for 5min. Finally, the obtained powder was crushed into powder and calcined at 900°C for 3h to obtain the final desired supported oxide, marked as 1% NiO / CeO2-OP. Subsequently, the supported oxide was reduced for 50min under 5% H2 / He at a temperature of 500°C to obtain an oxygen carrier for biogas chemical chain conversion to produce synthesis gas and hydrogen, marked as 1% Ni / CeO2.
[0103] Embodiment 15
[0104] Preparation of 3% Ni / CeO2-OP
[0105] First, the weighed NiCl2·6H2O was dissolved in 10mL of distilled water to obtain a Ni solution, and CeCl3·6H2O, Ni solution and glycine (the molar ratio of glycine / total metal ions was 2.5:1) were dissolved in 5mL of water in proportion. The solution was then dried in a 60°C oven at a constant temperature for 0.5h. Subsequently, the solution was directly placed in a muffle furnace preheated to 600°C and calcined for 3min. Finally, the obtained powder was crushed into powder and calcined at 800°C for 5h to obtain the final desired supported oxide, marked as 3% NiO / CeO2-OP. Subsequently, at a temperature of 600°C, the supported oxide was reduced under 20% H2 / He for 5min to obtain an oxygen carrier for biogas chemical chain conversion to produce synthesis gas and hydrogen, marked as 3% Ni / CeO2.
[0106] Example 16
[0107] Preparation of 7% Ni / CeO2-OP
[0108] First, the weighed NiCl2·6H2O was dissolved in 10mL of distilled water to obtain a Ni solution, and CeCl3·6H2O, Ni solution and glycine (the molar ratio of glycine / total metal ions was 2.5:1) were dissolved in 11mL of water in proportion (Ni to CeO2 mass fraction ratio was 7%). Then the solution was dried in a 50℃ oven at a constant temperature for 0.5h. Subsequently, the solution was directly placed in a muffle furnace preheated to 600℃ and calcined for 3min. Finally, the obtained powder was crushed into powder and calcined at 700℃ for 5h to obtain the final desired supported oxide, marked as 7% NiO / CeO2-OP. Subsequently, the supported oxide was reduced for 25min under 15% H2 / He at a temperature of 400℃ to obtain an oxygen carrier for biogas chemical chain conversion to produce synthesis gas and hydrogen, marked as 7% Ni / CeO2.
[0109] Embodiment 17
[0110] Preparation of 10% Ni / CeO2-OP
[0111] First, the weighed NiCl2·6H2O was dissolved in 10mL of distilled water to obtain a Ni solution, and CeCl3·6H2O, Ni solution and glycine (the molar ratio of glycine to total metal ions was 1.5) were dissolved in 13mL of water in proportion (the mass fraction ratio of Ni to CeO2 was 10%). Then the solution was dried in a 50°C oven at a constant temperature for 0.5h. Subsequently, the solution was directly placed in a muffle furnace preheated to 600°C and roasted for 3min. Finally, the obtained powder was crushed into powder and calcined at 700°C for 5h to obtain the final desired supported oxide, marked as 10% NiO / CeO2-OP. Subsequently, at a temperature of 400°C, the supported oxide was reduced under the condition of 10% H2 / He for 25min to obtain an oxygen carrier for biogas chemical chain conversion to produce synthesis gas and hydrogen, marked as 10% Ni / CeO2.
[0112] Embodiment 18
[0113] An oxygen carrier for biogas chemical chain conversion to produce synthesis gas and hydrogen is used in the biogas chemical chain conversion to produce hydrogen and synthesis gas. The oxygen carrier is circulated between two connected fuel reactors and a regeneration reactor; in the fuel reactor, the oxygen carrier generates synthesis gas by oxidizing biogas at 700°C; in the regeneration reactor, the oxygen carrier is oxidized and regenerated at 700°C in an oxidizing atmosphere, and then enters the fuel reactor.
[0114] The biogas in the fuel reactor is a mixture of CH4 and CO2, and the volume ratio of CH4 to CO2 is 3:1.
[0115] In the regeneration reactor, the oxidizing atmosphere is 35°C water vapor, and the saturated vapor pressure of water is 5 kPa.
[0116] Embodiment 19
[0117] An oxygen carrier for biogas chemical chain conversion to produce hydrogen is used in the biogas chemical chain conversion to produce synthesis gas and hydrogen. The oxygen carrier is circulated between two connected fuel reactors and a regeneration reactor; in the fuel reactor, the oxygen carrier generates synthesis gas by oxidizing biogas at 900°C; in the regeneration reactor, the oxygen carrier is oxidized and regenerated at 900°C in an oxidizing atmosphere, and then enters the fuel reactor.
[0118] The biogas in the fuel reactor is a mixture of CH4 and CO2, and the volume ratio of CH4 to CO2 is 1:1.
[0119] The oxidizing atmosphere is water vapor. The oxidizing atmosphere is 50°C water vapor, and the saturated vapor pressure of water is 14 kPa.
[0120] Embodiment 20
[0121] An oxygen carrier for biogas chemical chain conversion to produce synthesis gas and hydrogen is used in the biogas chemical chain conversion to produce hydrogen and synthesis gas. The oxygen carrier is circulated between two connected fuel reactors and a regeneration reactor; in the fuel reactor, the oxygen carrier generates synthesis gas by oxidizing biogas at 800°C; in the regeneration reactor, the oxygen carrier is oxidized and regenerated at 800°C in an oxidizing atmosphere, and then enters the fuel reactor.
[0122] The biogas in the fuel reactor is a mixture of CH4 and CO2, and the volume ratio of CH4 to CO2 is 2:1.
[0123] In the regeneration reactor, the oxidizing atmosphere is 25°C water vapor, and the saturated vapor pressure of water is 3 kPa.
[0124] Embodiment 21
[0125] An oxygen carrier for biogas chemical chain conversion to produce synthesis gas and hydrogen is used in the biogas chemical chain conversion to produce hydrogen and synthesis gas. The oxygen carrier is circulated between two connected fuel reactors and a regeneration reactor; in the fuel reactor, the oxygen carrier generates synthesis gas by oxidizing biogas at 700-900°C; in the regeneration reactor, the oxygen carrier is oxidized and regenerated at 700-900°C in an oxidizing atmosphere, and then enters the fuel reactor.
[0126] The biogas in the fuel reactor is a mixture of CH4 and CO2, and the volume ratio of CH4 to CO2 is 1:1.
[0127] In the regeneration reactor, the oxidizing atmosphere is 40°C water vapor, and the saturated vapor pressure of water is 11 kPa.
[0128] The above description is only for the best embodiment of the present invention, but it should not be understood as limiting the claims. The present invention is not limited to the above embodiments, and its specific structure is allowed to be changed. However, all changes made within the protection scope of the independent claims of the present invention are within the protection scope of the present invention.
[0129] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
Claims
1. An oxygen carrier for biogas chemical chain conversion to produce synthesis gas and hydrogen, It is characterized in that The chemical formula of the oxygen carrier is w%Ni / CeO 2 , where 1%≤w%≤10%.
2. The oxygen carrier for biogas chemical chain conversion to produce synthesis gas and hydrogen according to claim 1, It is characterized in that w% is 1%, 3%, 5%, 7% or 10%.
3. A method for preparing an oxygen carrier for biogas chemical chain conversion to produce synthesis gas and hydrogen, It is characterized in that The precursor solution containing Ce precursor, Ni precursor solution and glycine is dried, roasted, calcined and then reduced with hydrogen to obtain an oxygen carrier for biogas chemical chain conversion to produce synthesis gas and hydrogen.
4. The method for preparing an oxygen carrier for biogas chemical chain conversion to produce synthesis gas and hydrogen according to claim 3, It is characterized in that The Ce precursor is Ce(NO 3 ) 3 6H 2 O and CeCl 3 6H 2 At least one of O.
5. The method for preparing an oxygen carrier for biogas chemical chain conversion to produce synthesis gas and hydrogen according to claim 3, It is characterized in that The Ni precursor solution is Ni(NO 3 ) 2 6H 2 O and NiCl 2 6H 2 O in an aqueous solution.
6. The method for preparing an oxygen carrier for biogas chemical chain conversion to produce synthesis gas and hydrogen according to claim 3, It is characterized in that The ratio of the molar amount of glycine to the total molar amount of Ce and Ni is 1.5-2.5:
1.
7. The method for preparing an oxygen carrier for biogas chemical chain conversion to produce synthesis gas and hydrogen according to claim 3, It is characterized in that The drying temperature is 40-60°C and the drying time is 0.5-1h; The calcination process is: calcination at 400-600°C for 3-5 minutes, and then calcination at 700-900°C for 3-5 hours.
8. The method for preparing an oxygen carrier for biogas chemical chain conversion to produce synthesis gas and hydrogen according to claim 3, It is characterized in that The reduction process is: 2 Under the condition of mixed gas with He, reduction is carried out at 400-600°C for 5-50min.
9. Use of the oxygen carrier as claimed in claim 1 or 2 in biogas chemical chain conversion to produce synthesis gas and hydrogen, It is characterized in that The oxygen carrier is circulated between two interconnected fuel reactors and a regeneration reactor; in the fuel reactor, the oxygen carrier oxidizes the biogas at 700-900°C to generate synthesis gas; in the regeneration reactor, the oxygen carrier is oxidized and regenerated in an oxidizing atmosphere at 700-900°C, and then enters the fuel reactor.
10. Use of the oxygen carrier for biogas chemical chain conversion to produce synthesis gas and hydrogen according to claim 9, It is characterized in that The biogas in the fuel reactor is CH 4 and CO 2 Mixed gas, CH 4 and CO 2 A mixed common feed is adopted, the oxidizing atmosphere is water vapor, the temperature is 25-50°C, and the saturated vapor pressure is 3-14 kPa.
Citation Information
Patent Citations
Cerium-cobalt composite oxygen carrier as well as preparation method and application thereof
CN115888737A
In-situ packaging catalyst and application thereof