Micro-electrical disturbance bionic antifouling surface and preparation method thereof
Through the combination of hydrogel materials and conductive electrode materials, the microelectrolytic disturbed bionic antifouling surface is constructed using the electroosmotic flow effect, which solves the problem of broad-spectrum and long-term effectiveness of existing antifouling technologies, and achieves low energy consumption and high efficiency The marine biological anti-fouling effect is suitable for ships and marine equipment.
Patent Information
- Application Number
- CN202410871276.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-01
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-01
AI Technical Summary
The existing anti-fouling surface has problems such as broad-spectrum and long-term effectiveness in blocking marine biological pollution. Traditional toxic anti-fouling agents have been banned. Environmentally friendly anti-fouling technology has limited effect in actual application, and bionic form prevention The production cost of dirty surfaces is high and commercial application fails.
Use hydrogel materials and conductive electrode materials to build a microelectrometic biomiscible antifouling surface through electroosmotic flow effect, use electroosmotic flow to destroy the growth environment of microorganisms and drive away large-scale dirty organisms, and combine it with a low-surface energy antifouling layer to reduce the possibility of biological adhesion .
It effectively prevents marine organisms from adhesion at low voltages, reduces energy consumption, provides dynamic control and anti-fouling effect, is suitable for ships and marine equipment, and avoids the formation of biological pollution and ecological environment hazards.
Smart Images

Figure CN118950433A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of marine antifouling functional surfaces, belongs to a novel intelligent response surface, and specifically relates to a micro-electric perturbation bionic antifouling surface and a preparation method thereof. Background Art
[0002] Marine biofouling refers to the attachment and growth of fouling organisms (such as bacteria, algae, barnacles, etc.) on underwater surfaces. The problem of marine biofouling has been hindering the pace of human exploration of the ocean since ancient times. Today, with the prosperity of global shipping trade, the economic losses and environmental problems caused by the large-scale accumulation of marine organisms on the surfaces of marine equipment such as ships, docks, drilling platforms, and cross-sea bridges are becoming more and more serious. The main consequences are: ① Increase the weight and surface roughness of underwater equipment, significantly increase navigation resistance and fuel consumption, and bring about a substantial increase in operating costs. Studies have shown that even if there is mild biofouling in the form of mucus film on the surface of the ship, it will increase the shaft power required to overcome additional resistance and maintain operating speed by 11%. In contrast, if biofouling produces heavy calcium deposits, the power loss of the ship will be as high as 86%. ② Excessive fuel consumption increases the emission of greenhouse gases and harmful gases such as carbon dioxide, sulfur oxides and nitrogen oxides, which ultimately affects the climate environment and endangers human health. ③ Change the local microenvironment of the underwater surface, accelerate the surface corrosion rate, and affect the safety of underwater equipment. ④ Cause biological invasion. Fouling organisms travel around the world with ships. When they reach new waters without natural enemies, they are likely to cause biological invasion and endanger the local ecological environment.
[0003] The formation process of biofouling can usually be divided into four stages: ① Formation of conditional film: In the first few seconds after the material surface is immersed in seawater, inorganic and organic macromolecules (such as proteins) will be adsorbed through physical action. This stage will form the basic environment for the survival of microorganisms, which is the first step of biological adhesion. The duration of this stage depends on the physicochemical properties of the solid material surface, such as surface roughness, chemical composition, etc. ② Reversible adhesion and colonization stage of microorganisms: In the next few hours, bacteria, algae and other microorganisms migrate to the surface and secrete extracellular polymers (EPS) to promote adhesion and form biofilms. Bacteria and algae can detach from the surface under the action of external forces, so this process is reversible. ③ Irreversible adhesion and aggregation stage: In the next few days, multicellular organisms (such as large algae and protozoan spores) reach the surface, and then begin to grow and reproduce in large quantities, and secrete harmful substances, accelerating the corrosion rate of underwater surfaces. ④ Biofilm maturation and recolonization stage: In the next few weeks, the biofilm has been formed and stabilized, some animal larvae begin to gather (such as barnacles and mussels), and their impact on the facilities gradually reaches a peak. The above biofouling formation process is generally accepted by researchers, but it is also affected by the sea area, season, and type of fouling organisms. Some stages will overlap or occur in parallel. In general, interfering with the formation of bacterial biofilms is the key to blocking subsequent biofouling.
[0004] Existing antifouling surfaces are mainly divided into two categories: traditional toxic antifouling surfaces and new environmentally friendly antifouling surfaces.
[0005] (1) Traditional toxic antifouling surface
[0006] Humans have a long history of fighting against marine biofouling. In 700 BC, the Phoenicians began to use lead to cover the bottom of sailboats to inhibit fouling. Later, toxic substances such as mercury, arsenic, and cuprous oxide were used as antifouling agents to kill fouling organisms. In the 1950s, tributyltin (TBT) was discovered and widely used due to its excellent antifouling ability. Tributyltin has the characteristics of broad spectrum and long-term effect. However, due to its negative impact on the marine environment, the Marine Environment Protection Committee (MEPC) of the International Maritime Organization (IMO) has promulgated regulations in 2008 to prohibit the use of TBT-type surfaces on ship surfaces. Since then, environmentally friendly antifouling surfaces have become a research hotspot.
[0007] (2) Environmentally friendly anti-fouling technology
[0008] Environmentally friendly antifouling surfaces that have emerged in recent years can be roughly divided into the following categories: ① Antifouling surfaces containing natural products, which extract natural products with antifouling activity from marine organisms (mainly algae, seaweed, marine invertebrates and microorganisms) and terrestrial organisms (such as peppers), and compound them into other materials to obtain antifouling surfaces. However, biological antifouling strategies are usually diverse, and surfaces containing a single antifouling agent are difficult to achieve broad-spectrum and long-term antifouling properties, and are still limited in actual engineering applications. ② Fouling-release surfaces, fouling organisms have low adhesion on low surface energy surfaces and are easily desorbed from the surface under shear forces such as water flow, playing an antifouling role. However, this type of surface will only be effective under shear forces exceeding a certain hydrodynamic force, which means that the effect will only be significant when applied to high-speed ships, and it will not be very effective for ships in a moored state and facilities such as aquaculture. ③ Conductive antifouling surface: a conductive coating is applied to the surface of the ship, and an electric current is passed to electrolyze seawater to produce hypochlorite ions, thereby preventing the attachment of marine organisms such as bacteria, algae, and shellfish. Although conductive antifouling coatings have excellent potential, their practical application as antifouling technology needs to be further deepened. ④ Bionic morphology antifouling surface: by imitating typical biological surfaces (such as sharks, lotus leaves, etc.), advanced manufacturing technologies (such as reactive ion beam etching, plasma etching, laser processing, nanoimprint lithography, electrospinning, electrochemical deposition, etc.) are used to construct a single-level or multi-level topological bionic micro-nanostructure surface. The antifouling effect is excellent, but there are also certain defects. A typical example is the American Sharklet antifouling surface. Due to its high production cost, its commercial application in the field of ships has failed. Summary of the invention
[0009] In order to solve the above problems, inspired by the dynamic epidermal antifouling structure of typical cetacean skin, the present invention proposes a micro-electric perturbation bionic antifouling surface and a preparation method thereof.
[0010] The bionic antifouling surface of the present invention is composed of a hydrogel material, an electrode material on the surface of the hydrogel material, and an antifouling surface material on the surface of the electrode material; the hydrogel material has a porous three-dimensional network structure, can absorb and retain a large amount of water, and has strong softness and elasticity. The conductive electrode can drive the hydrogel to generate electroosmotic flow under the stimulation of an external electric field and cause the hydrogel material to undergo macroscopic deformation under the electroosmotic action, causing the antifouling surface material on the surface of the electrode material to produce microscopic fluid flow.
[0011] The preparation method of the micro-electric perturbation bionic antifouling surface in the present invention is as follows:
[0012] (1) Preparation of hydrogel materials
[0013] The hydrogel material is prepared by generating free radicals through an initiator under the action of heat, light or chemical substances, initiating a free radical polymerization reaction of hydrogel monomers, and then adding a crosslinking agent to form a hydrogel crosslinking network.
[0014] The hydrogel monomer is a combination of one or more of N-isopropylacrylamide, hydroxyethyl acrylic acid, vinyl pyrrolidone, acrylic acid, 2-hydroxyethyl acrylic acid, methyl methacrylate, and acrylamide; the initiator is one of potassium persulfate, azobisisobutyronitrile, 2,2-dimethoxy-2-phenylacetophenone (DMPA), ammonium persulfate, tetrabutylammonium persulfate, and N-isopropylacrylamide. Different hydrogel monomers will affect the electroosmotic responsiveness, mechanical properties (strength, elasticity, and toughness, etc.), binding force with electrode materials, water absorption (porosity, pore size, swelling rate, etc.) and other properties of the hydrogel, thereby affecting the antifouling performance of the hydrogel.
[0015] The crosslinking agent is a combination of one or more of N,N'-methylenebisacrylamide, glutaraldehyde, trimethacrylate, diisocyanate, 1,4-butanediol dimethacrylate, diethylenetriamine, persulfate, disulfide, epoxy compound, formaldehyde, and ethylene glycol dimethacrylate.
[0016] (2) Preparation of conductive electrodes
[0017] The conductivity of the hydrogel material is >10 prepared by physical deposition, chemical deposition, conductive polymer coating, nanomaterial composite, deposition of metal film, self-assembled monolayer, 3D printing method. 3 S cm -1 Conductive electrodes;
[0018] The electrode materials are metals and their alloys (copper, silver, gold, aluminum, copper, nickel, platinum, palladium, etc.), carbon-based materials (graphite, graphene, carbon nanotubes, conductive carbon black, activated carbon, carbon fiber, etc.), MXenes (Ti 3 C 2 、Ti 2 C.V 2 C、Nb 2 C.Mo 2 C. Ti 4 N 3 、Ti 2 N, etc.), two-dimensional materials (transition metal sulfides, black phosphorus), conductive polymer materials (polyaniline, polypyrrole, polythiophene, etc.), conductive oxides (zinc oxide, iron oxide, indium tin oxide, etc.), polymer / inorganic composites (metal / carbon composites, conductive polymer composites), perovskite materials, conductive inks and adhesives, etc., and a combination of one or more of the following materials.
[0019] After the electrode material is prepared on the surface of the hydrogel material, applying a DC voltage to the electrode material will place the hydrogel as a whole in an electric field environment. The liquid (seawater) in the hydrogel pores will form a double layer, and the net charge in the double layer will move due to the Coulomb force of the electric field. At the same time, due to the solvation effect, the movement of the charge will drive the flow of the liquid around the charge, which will lead to the flow of liquid in the hydrogel pores to form electroosmotic flow. On a macro scale, the flow of liquid will cause the volume of the hydrogel to expand / contract, causing the gel to deform.
[0020] (3) Preparation of low surface energy antifouling layer
[0021] In order to further reduce the possibility of marine organisms adhering to the surface, it is also necessary to construct a low surface energy antifouling layer on the surface of the material. The low surface energy material is introduced into fluorine or silicon groups through coating, chemical grafting, plasma treatment, blending, physical adsorption, nanotechnology, 3D printing, etc. to form a low surface energy antifouling layer on the surface of the conductive electrode material. Among them, chemical grafting is free radical grafting, surface activation or photochemical grafting;
[0022] The low surface energy material is a combination of one or more of fluoropolymers, silicone polymers, polyethylene, polypropylene, polyepoxide, polystyrene, polyurethane, polyetheretherketone, polyvinyl alcohol, polyisobutylene, polymethyl methacrylate, polycarbonate and the like, and a combination of monomers or monomer derivatives of these substances.
[0023] The thickness of the micro-electric perturbation bionic anti-fouling surface finally prepared by the present invention is 10 μm to 5000 μm.
[0024] Beneficial effects of the present invention:
[0025] 1. The micro-electric perturbation bionic antifouling surface is constructed based on the electroosmotic effect. Electroosmosis (electroosmotic flow) is a liquid movement phenomenon caused by an electric field. When the solid surface in the solution is charged due to the dissociation of surface groups or the selective adsorption of certain ions from the solution, due to the requirement of electrical neutrality, there must be excess counterions in the liquid near the charged surface with the same number of charges as the solid surface but opposite signs, forming the so-called double layer. When an electric field is applied to such a system, the net charge in the double layer moves under the action of the Coulomb force, causing the liquid to flow. This flow is electroosmotic flow. Under the action of external electrical stimulation, the bionic antifouling surface exhibits reversible macroscopic mechanical deformation and microscopic fluid flow similar to that of cetacean skin. Based on this principle, the present invention provides a new antifouling solution.
[0026] 2. The microscopic fluid flow on the micro-electric perturbation bionic anti-fouling surface can effectively destroy the stable microenvironment for the growth and reproduction of microorganisms, prevent the adhesion of microorganisms on the surface of the material, and can play an efficient anti-fouling role in components such as ships, seawater pipelines, marine detection equipment and high-performance marine sports equipment.
[0027] 3. The macroscopic fluid disturbance of the micro-electric perturbation bionic anti-fouling surface can effectively drive away large fouling organisms and prevent them from adhering to the surface.
[0028] 4. The low surface energy antifouling surface greatly reduces the possibility of marine organisms forming biofilms on it by creating an extremely smooth and unfavorable surface for microbial attachment at the microscopic level.
[0029] 5. The micro-electric perturbation bionic antifouling surface is constructed based on the electroosmotic effect, which can achieve excellent material deformation properties and electroosmotic flow at low voltage (<3V). When a low voltage is applied, these structures are able to generate tiny electric fields that induce electroosmotic effects on the surface of the material, resulting in microflows. This flow helps to push away liquids and suspended particles on the surface, including dirt and microorganisms, thereby preventing them from accumulating on the surface. The electroosmotic effect is not only very effective in preventing the attachment of organisms, but also because the voltage used is very low, the energy consumption is extremely low, and it has little effect on the overall energy efficiency of the device.
[0030] 6. This electroosmotic-driven antifouling mechanism allows for dynamic control of the antifouling effect. By adjusting the applied voltage and current, the intensity of the electroosmotic flow can be adjusted as needed, thereby optimizing the antifouling performance under different environmental conditions.
[0031] 7. It can resist various biological fouling in a purely physical way, such as the attachment of bacteria, algae and other organisms, and is an environmentally friendly anti-fouling technology. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 This is a schematic diagram of the structure of the micro-electric perturbation bionic anti-fouling surface;
[0033] Figure 2 This is an electron micrograph of a porous hydrogel;
[0034] Figure 3 The actual picture is before and after the hydrogel surface is covered with metal electrodes;
[0035] Figure 4 This is a real picture of the deformation of the micro-electric perturbation bionic anti-fouling surface under a voltage of 3V;
[0036] Figure 5 This is a physical picture of the electroosmotic effect of the micro-electric perturbation bionic anti-fouling surface at a voltage of 3V;
[0037] Figure 6 This is a comparison between the actual sea hanging board test of the micro-electric perturbation bionic anti-fouling surface and the PU anti-fouling coating. DETAILED DESCRIPTION
[0038] In order to further understand the present invention, the preparation method and application of the bionic antifouling surface provided by the present invention are described below in conjunction with embodiments. The protection scope of the present invention is not limited by the following embodiments.
[0039] Example 1
[0040] 1. Preparation of Hydrogel
[0041] First, 12mmol of methyl methacrylate (MMA) and 3mmol of acrylamide (AAm) were dissolved in 15mL of deionized water. Then, ethylene glycol dimethacrylate (200μL) and 2,2-dimethoxy-2-phenylacetophenone (30mg) dissolved in 300μL of dimethyl sulfoxide were added to the aqueous solution of methyl methacrylate and acrylamide as crosslinkers and initiators. The prepared solution was placed in a polyethylene terephthalate (PET) mold and sandwiched between glass sheets (thickness 50 to 2000 microns). The solution was cured by ultraviolet irradiation for 30 minutes to obtain a hydrogel film.
[0042] 2. Synthesis of Au Nanoparticles
[0043] First, tetraoctylammonium bromide (concentration of 20 mmol / L) dissolved in 80 mL of toluene and tetrachloroauric acid trihydrate (concentration of 30 mmol / L) dissolved in deionized water (30 mL) were stirred for more than 30 min, and the toluene phase was separated. Then, sodium borohydride (concentration of 400 mmol / L) dissolved in 25 mL of deionized water was added to the separated toluene phase and stirred to obtain a toluene solution of Au nanoparticles. After the reduction reaction for 3 hours, the Au nanoparticles were precipitated with H 2 SO 4 The Au nanoparticle solution was washed with NaOH (0.1 M), NaOH (0.1 M), and deionized water for several times to obtain a toluene solution of Au nanoparticles.
[0044] 3. Preparation of biomimetic antifouling surfaces
[0045] First, PAA-co-PAAm hydrogel was prepared in a polyethyleneimine (PEI) aqueous solution (1 to 30 mg mL -1 ) for more than 24 hours. Since PEI will penetrate into the hydrogel matrix, the hydrogel film will swell to varying degrees depending on the concentration of the PEI solution. Then, the swollen hydrogel is immersed in a toluene solution containing Au nanoparticles. As the deposition time of the Au nanoparticles increases, the adsorbed Au nanoparticles are converted into porous Au nanofilms through capillary-assisted in situ nanoparticle assembly. Subsequently, additional deswelling treatment of the hydrogel coated with the gold nanofilm electrode in air (3 hours) or toluene (3 days) can produce biomimetic antifouling surfaces with different relative surface ratios.
[0046] 4. Preparation of low surface energy antifouling surfaces
[0047] By a simple dip-coating method, PDMS containing imine groups was uniformly coated on the micro-electrically perturbed biomimetic antifouling surface using bis(3-aminopropyl)-terminated PDMS and benzene-1,3,5-tricarboxaldehyde solution to form a PDMS layer of about 10 μm on the biomimetic antifouling surface ( Figure S21 ).
[0048] Example 2
[0049] 1. Preparation of Hydrogel
[0050] Acrylamide (monomer), potassium persulfate (initiator), N,N-methylenebisacrylamide (cross-linking agent), NaHCO 3 (porogen) was dissolved in water at a mass ratio of 1000:10:30:5 (where the mass ratio of acrylamide to water was 150:1000), and stirred until uniform. The prepared solution was placed in a polyethylene terephthalate (PET) mold and sandwiched between glass sheets (thickness 50 μm to 2000 μm). Then, it was heated at 80 °C for 1 h to solidify into a gel, and then immersed in a hydrochloric acid solution with a pH of 5 to remove NaHCO 3 A hydrogel film was obtained.
[0051] 2. Preparation of Conductive Electrodes
[0052] A total of 5 g of polydimethylsiloxane (PDMS) precursor and 0.5 g of cross-linking agent were dispersed in 20 g of ethyl acetate solution and stirred at room temperature until completely dissolved. Multi-walled carbon nanotubes with relative masses of 13%, 15% and 17% were added to the above mixture, stirred at room temperature for 1 hour, and then left to stand for 0.5 hours by ultrasonic oscillation to obtain a conductive solution. Subsequently, the conductive solution was first sprayed on the hydrogel film, paying attention to controlling the spraying distance and number of times, and operating the entire process in a protective cover. After spraying, the composite film was left to stand for 10 minutes to avoid rapid evaporation of the organic solvent due to temperature changes. The film was then cured in an oven at 60°C for 2 hours and aged at 100°C for 2 hours. Finally, a conductive hydrogel film was successfully obtained using a sputtering current of 30 mA and a sputtering time of 200 seconds.
[0053] 3. Preparation of low surface energy antifouling surfaces
[0054] By a simple dip coating method, bis(3-aminopropyl)-terminated PDMS and benzene-1,3,5-tricarboxaldehyde solution were used to uniformly coat the PDMS containing imine groups on the micro-electrical perturbation biomimetic antifouling surface to form a PDMS layer of about 10 μm on the biomimetic antifouling surface.
[0055] In the process of preparing the hydrogel material of the present invention, the water absorption rate and swelling behavior, mechanical properties, pore structure and pore size distribution, chemical stability, network structure and crosslinking density, and responsiveness of the hydrogel can be regulated by changing one or more combinations of reaction conditions such as temperature, pressure, pH value, type and concentration of initiator, type and concentration of crosslinking agent, post-treatment of the hydrogel, or by adding specific chemical substances.
[0056] During the preparation of the conductive electrode, by adjusting one or more combinations of parameters such as temperature, pressure, humidity, chemical environment, preparation time, etc. during the preparation process, a surface electrode with good conductivity, flexibility, mechanical properties and strong bonding strength with the hydrogel matrix is obtained.
[0057] Effect verification:
[0058] like Figure 1 The diagram shows the structure of the micro-electric perturbation bionic anti-fouling surface; Figure 4 As shown in the figure, after applying 3V direct current to the electrodes on both sides, the liquid (seawater) in the hydrogel pores will form a double layer, and the net charge in the double layer will move due to the Coulomb force of the electric field. At the same time, due to the solvation effect, the movement of the charge will drive the flow of the liquid around the charge, which will lead to the flow of liquid in the hydrogel pores to form electroosmotic flow. On a macro scale, the flow of liquid will cause the volume of the hydrogel to expand / contract, thereby causing the gel to deform. Figure 5 This is a physical picture of the reversible electroosmosis effect of the micro-electric perturbation bionic anti-fouling surface at a voltage of 3 V. The before and after comparison shows that the surface has undergone obvious shape changes.
[0059] Figure 6 The figure is a comparison between the real sea hanging board test of the micro-electric perturbation bionic antifouling surface and the PU antifouling coating. Among them, PU-0d, PU-30d and PU-60d are the experimental result photos of the PU antifouling coating after 0, 30 or 60 days of testing, respectively, and Sample-0d, Sample-30d and Sample-60d are the experimental result photos of the micro-electric perturbation bionic antifouling surface of the present invention after 0, 30 or 60 days of testing, respectively. It can be seen that the PU antifouling coating has already had fouling organisms attached, while the micro-electric perturbation bionic antifouling surface samples have almost no fouling organisms attached.
Claims
1. A micro-electric perturbation bionic anti-fouling surface, It is characterized in that The antifouling surface is composed of a hydrogel material, an electrode material on the surface of the hydrogel material, and an antifouling surface layer material on the surface of the electrode material; the hydrogel material has a porous three-dimensional network structure, can absorb and retain a large amount of water, and has strong softness and elasticity; the conductive electrode can drive the hydrogel to generate electroosmotic flow under the stimulation of an external electric field and cause the hydrogel material to undergo macroscopic deformation under the action of electroosmosis; The hydrogel material is prepared by generating free radicals by an initiator under the action of heat, light or chemical substances, initiating a free radical polymerization reaction of hydrogel monomers, and adding a crosslinking agent to form a hydrogel crosslinking network; the hydrogel monomers are a combination of one or more of N-isopropyl acrylamide, hydroxyethyl acrylic acid, vinyl pyrrolidone, acrylic acid, 2-hydroxyethyl acrylic acid, methyl methacrylate and acrylamide; The conductivity of the electrode material is>10 3 S cm -1 ; The antifouling surface material is a low surface energy polymer material.
2. The micro-electric perturbation bionic anti-fouling surface according to claim 1, It is characterized in that The electrode material is a combination of one or more of metal or its alloy, carbon-based material, MXene, transition metal sulfide two-dimensional material, black phosphorus, conductive polymer material, conductive oxide, perovskite material, and conductive ink. The metal material is one of copper, silver, gold, aluminum, copper, nickel, platinum and palladium; The carbon-based material is one of graphite, graphene, carbon nanotubes, conductive carbon black, activated carbon, and carbon fiber; The MXene is Ti 3 C 2 、Ti 2 C.V 2 C、Nb 2 C.Mo 2 C. Ti 4 N 3 、Ti 2 One of N; The conductive polymer material is polyaniline, polypyrrole or polythiophene; The conductive oxide is zinc oxide, iron oxide or indium tin oxide.
3. The micro-electric perturbation bionic anti-fouling surface according to claim 1, It is characterized in that The low surface energy polymer material is a combination of one or more of fluoropolymer, silicon polymer, polyethylene, polypropylene, polyepoxide, polystyrene, polyurethane, polyetheretherketone, polyvinyl alcohol, polyisobutylene, polymethyl methacrylate, and polycarbonate.
4. The method for preparing the micro-electric perturbation bionic antifouling surface according to claim 1, It is characterized in that The specific steps of this method are as follows: (1) Preparation of hydrogel materials The hydrogel material is prepared by generating free radicals through an initiator under the action of heat, light or chemical substances, initiating a free radical polymerization reaction of hydrogel monomers, and then adding a crosslinking agent to form a hydrogel crosslinking network. The hydrogel monomer is a combination of one or more of N-isopropyl acrylamide, hydroxyethyl acrylic acid, vinyl pyrrolidone, acrylic acid, 2-hydroxyethyl acrylic acid, methyl methacrylate, and acrylamide; The initiator is a combination of one or more of potassium persulfate, azobisisobutyronitrile, 2,2-dimethoxy-2-phenylacetophenone, ammonium persulfate, tetrabutylammonium persulfate, and N-isopropylacrylamide. The crosslinking agent is a combination of one or more of N,N'-methylenebisacrylamide, glutaraldehyde, trimethacrylate, diisocyanate, 1,4-butanediol dimethacrylate, diethylenetriamine, persulfate, disulfide, epoxy compound, formaldehyde, and ethylene glycol dimethacrylate. (2) Preparation of electrodes The conductivity of the hydrogel material is >10 prepared by physical deposition, chemical deposition, conductive polymer coating, nanomaterial composite, deposition of metal film, self-assembled monolayer, 3D printing method. 3 S cm -1 Conductive electrodes; (3) Preparation of antifouling surface materials The low surface energy material is introduced into the surface of the conductive electrode material through a coating method, chemical grafting, plasma treatment, fluorine or silicon groups, blending method, physical adsorption, nanotechnology, 3D printing method to form a low surface energy antifouling layer. Among them, the chemical grafting is free radical grafting, surface activation or photochemical grafting.
5. The method for preparing the micro-electric perturbation bionic antifouling surface according to claim 4, It is characterized in that In step (1), the initiator is a combination of one or more of potassium persulfate, azobisisobutyronitrile, 2,2-dimethoxy-2-phenylacetophenone, ammonium persulfate, tetrabutylammonium persulfate, and N-isopropylacrylamide.
6. The method for preparing the micro-electric perturbation bionic antifouling surface according to claim 4, It is characterized in that The crosslinking agent described in step (1) is a combination of one or more of N,N'-methylenebisacrylamide, glutaraldehyde, trimethacrylate, diisocyanate, 1,4-butanediol dimethacrylate, diethylenetriamine, persulfate, disulfide, epoxy compound, formaldehyde, and ethylene glycol dimethacrylate.
7. The method for preparing the micro-electric perturbation bionic antifouling surface according to claim 4, It is characterized in that The thickness of the bionic antifouling surface is 10 μm to 5000 μm.
Citation Information
Patent Citations
Cationic type antifouling and anti-drag composite functional paint and coating
CN105062248A
System for reducing biological attachment on underwater surface of solid-phase object
CN107311319A
Hydrogel biomimetic fish based on electrosensitive driving
CN109131798A
Piezoelectric / electromagnetic hybrid drive antifouling coating material and preparation method thereof
CN110157258A
Intelligent bionic antifouling material with controllable surface texture
CN110452536A
Cited By
Underwater suspension data center server cabinet heat dissipation module based on bionic gill