Calcium carbonate transparent coating as well as preparation method and application thereof

By growing a transparent film of calcium carbonate on the base surface of the oil-water separation material, the orderly accumulation of 20-50nm calcite calcium carbonate particles is solved, and the existing material pollution and durability are achieved is achieved efficient oil-water separation and transparency, which is suitable for Oil and water separation field.

CN118950435AInactive Publication Date: 2024-11-15JIANGHAN UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411019519.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing oil-water separation materials are easily contaminated by oil pollution during long-term use, reducing separation efficiency, and multi-scale nanostructures make the material opaque, difficult to apply in underwater optical equipment, or have poor mechanical properties, low durability, and preparation process Complex, the modification layer has little bonding power to the substrate.

Method used

Using a transparent calcium carbonate coating, the calcium carbonate particles of 20-50nm are accumulated in an orderly manner. Calcium carbonate film is grown on the substrate surface by spin coating method of glacial acetic acid to form nanocalcium calcium carbonate transparent The membrane is combined with a transparent calcium carbonate film to modify the substrate to achieve superhydrophilicity and superoleophobicity.

Benefits of technology

It achieves super hydrophilicity in the air and super oleophobicity underwater, has high transparency, excellent anti-oil and mechanical properties, is low-cost, simple preparation method, and is suitable for oil-water separation field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118950435A_ABST
    Figure CN118950435A_ABST
Patent Text Reader

Abstract

The invention discloses a calcium carbonate transparent coating as well as a preparation method and application thereof, and belongs to the technical field of composite material synthesis, the underwater super-oleophobic calcium carbonate transparent coating is formed by orderly stacking calcite particles with the particle size of 30-50nm, the preparation method comprises the following steps: pre-treating a substrate, spin-coating a chitosan solution, and drying to obtain the underwater super-oleophobic calcium carbonate transparent coating. Preparing a mineralization solution A of calcium chloride, magnesium chloride and PAA and a mineralization solution B of sodium carbonate, placing the substrate at the bottom of the solution A, strictly controlling the dripping speed of the solution by virtue of a peristaltic pump, slowly dripping the solution B into the mixed solution A, taking out the substrate with a calcium carbonate transparent coating growing on the surface after the reaction is finished, washing with deionized water, and airing. According to the method, the calcium carbonate transparent coating grows on the surface of the substrate in a mineralization mode, the substrate modified by the calcium carbonate transparent coating shows super-hydrophilicity in the air and shows super-oleophobicity underwater, the preparation method is simple, cost is low, and large-scale production and application are easy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of composite material synthesis, and particularly relates to a calcium carbonate transparent coating and a preparation method and application thereof. Background Art

[0002] Since the 21st century, with the rapid development of industry, the demand for oil in countries around the world has increased, the scale of oil field exploitation has continued to expand, and the oily wastewater generated by industrial production and people's lives has also continued to increase. Oil-water separation has become a problem closely related to people's lives, economic development and environmental protection. On the one hand, a large amount of industrial oily wastewater is generated in food processing, metal smelting, petrochemicals, textiles and other fields, which will cause very serious pollution to the environment; on the other hand, with the exploitation of submarine oil, oil leakage has become more and more serious, which will also cause greater pollution to the marine environment. Therefore, how to achieve efficient separation of oil and water has become a problem that needs to be solved in today's society, and the oil-water separation network with special wettability has gradually attracted people's attention.

[0003] The essence of oil-water separation is to design and change the wettability of the material surface to prepare superoleophobic or superhydrophobic separation materials. Underwater superoleophobic materials have attracted much attention due to their potential applications in anti-fouling, self-cleaning and oil-water separation. Traditional oil-water separation materials are mostly oleophilic and hydrophobic materials, such as fluorine-containing materials, polytetrafluoroethylene, polydimethylsiloxane, carbon materials, etc. These materials are easily contaminated by oil during long-term use, causing pore blockage, reducing separation efficiency and increasing separation costs. In order to achieve underwater superoleophobic properties of materials, conventional methods are to design multi-scale nano-micro structures or use high surface energy materials. However, due to the scattering effect of light, these multi-scale nano-micro structures will reduce the transmittance of the material and become opaque, which hinders its application in underwater optical equipment.

[0004] Although some polymer materials with high surface energy have high transparency and can achieve underwater superoleophobic properties, they have poor mechanical properties and are therefore not very durable in underwater optical equipment applications. They are easily scratched and seriously affect transmittance. Although the new separation membranes reported recently have good separation effects, they all have disadvantages such as complex preparation processes, weak bonding between the modified layer and the substrate, and the use of fluorinated compounds.

[0005] There are some special biological structures in nature, such as shells and fish scales, which have high transparency, show super hydrophilicity in air, and show super oleophobicity underwater. Research has found that this is closely related to the surface of shells and fish scales, which are multi-level nano-micro structures composed of orderly calcium carbonate nanoparticles. This unique surface can keep shells and fish clean in polluted water. This provides inspiration for the design of new oil-water separation materials. Summary of the invention

[0006] The purpose of the present invention is to provide a calcium carbonate transparent coating and a preparation method and use thereof. The calcium carbonate transparent film is mineralized and grown on the surface of a substrate. The calcium carbonate film is formed by dense accumulation of nano-calcite calcium carbonate particles. The substrate modified by the calcium carbonate transparent film exhibits superhydrophilicity in the air and superoleophobicity underwater, and is suitable for the field of oil-water separation.

[0007] To achieve the above object, the present invention provides a method for preparing a transparent calcium carbonate coating, wherein the transparent calcium carbonate coating is formed by orderly stacking calcite particles with a particle size of 20-50 nm, comprising the following steps:

[0008] S1, cutting and pre-processing the substrate;

[0009] S2. Prepare chitosan solution using glacial acetic acid.

[0010] S3, using a spin coater to evenly spin-coat the chitosan solution onto the substrate surface;

[0011] S4. Prepare 50-100 ml of mineralization solution A at room temperature and stir for 10-20 minutes until it is fully dissolved;

[0012] S5. Prepare 50-100 ml of mineralization solution B at room temperature and stir for 10-20 minutes until fully dissolved;

[0013] S6, slowly adding the mineralization solution B to the mineralization solution A, and placing the substrate spin-coated with the chitosan solution at the bottom of the beaker containing the mineralization solution A;

[0014] S7. After the addition of the mineralization solution B is completed, the substrate with the calcium carbonate film grown on the surface is taken out, cleaned with deionized water, and dried.

[0015] Preferably, in step S1, the substrate to be treated is selected from a polyethylene plastic net, a polyethylene plastic sheet or a glass sheet, the cutting size of the substrate to be treated is 2cm×2cm-5cm×5cm, the glass sheet is pretreated by hydrophilizing with piranha solution and then washing with deionized water, and the polyethylene plastic net and the polyethylene plastic sheet are pretreated by ultrasonic treatment with anhydrous ethanol and then washing with deionized water.

[0016] Preferably, in step S2, the concentration of the chitosan solution is 1.0-2.5 wt %.

[0017] Preferably, in step S4, the raw materials in the mineralization solution A include calcium chloride, magnesium chloride and PAA, and the concentrations of calcium chloride, magnesium chloride and PAA in the mineralization solution A are 5.4-10.8 mM, 1.2-1.8 mM and 1-4 wt %, respectively.

[0018] Preferably, in step S5, the raw material sodium carbonate in the mineralization solution B has a concentration of sodium carbonate in the mineralization solution B of 3.24-6.48 mM.

[0019] Preferably, in step S6, a peristaltic pump is used to control the dripping rate of the mineralization solution B, and the dripping rate of the peristaltic pump is 2.0-5.0 ml / h.

[0020] Preferably, in step S4, Ca in the mineralization solution A 2+ Mg 2+ The molar ratio between them is 6.25:9.

[0021] Preferably, the temperature of the piranha solution is 90° C., and the volume ratio of concentrated sulfuric acid to hydrogen peroxide in the piranha solution is 3:1.

[0022] The invention also discloses a calcium carbonate transparent coating prepared by the preparation method of the calcium carbonate transparent coating.

[0023] The invention also discloses a calcium carbonate transparent coating applied in the technical field of oil-water separation.

[0024] Therefore, the present invention adopts the above-mentioned calcium carbonate transparent coating and its preparation method and use, and its beneficial effects are:

[0025] (1) The preparation method of the calcium carbonate transparent coating of the present invention is simple, low-cost, mild in reaction, has no special requirements on the substrate, is universal, and is easy to scale up for production;

[0026] (2) The calcium carbonate transparent coating prepared by the preparation method of the present invention is firmly bonded to the substrate, has excellent mechanical properties, high optical transmittance, and excellent anti-oil performance. The substrate modified with the calcium carbonate transparent coating exhibits superhydrophilicity in the air and superoleophobicity underwater, and has a very broad application prospect in the field of oil-water separation.

[0027] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The light transmittance pictures of the calcium carbonate transparent coating prepared in the present invention, wherein a is the light transmittance picture of the sample prepared in Example 1, and b is the light transmittance picture of the sample prepared in Example 2;

[0029] Figure 2 This is a polarized light micrograph of the transparent calcium carbonate coating prepared in Example 1 of the present invention;

[0030] Figure 3 A scanning electron micrograph of the calcium carbonate transparent coating prepared in Example 1 of the present invention;

[0031] Figure 4 This is a contact angle picture of the calcium carbonate transparent coating prepared in Example 1 of the present invention in air;

[0032] Figure 5 This is a picture of the underwater contact angle of the calcium carbonate transparent coating prepared in Example 1 of the present invention;

[0033] Figure 6 The transmittance test data of the calcium carbonate transparent coating prepared in Example 2 of the present invention;

[0034] Figure 7 XRD spectrum of the calcium carbonate transparent coating prepared in Example 2 of the present invention;

[0035] Figure 8 The mechanical properties data of the calcium carbonate transparent coating prepared in Example 2 of the present invention;

[0036] Fig. 9 This is an electronic scanning photograph of the plastic mesh substrate without modified calcium carbonate film in Example 3 of the present invention;

[0037] Fig.10 This is an electronic scanning photograph of a plastic mesh substrate modified with a calcium carbonate film in Example 3 of the present invention;

[0038] Fig.11 This is an energy spectrum photograph of a modified calcium carbonate film plastic mesh substrate in Example 3 of the present invention;

[0039] Fig.12 This is a photo of oil-water separation of a plastic mesh substrate modified with a calcium carbonate film according to Example 3 of the present invention. DETAILED DESCRIPTION

[0040] The technical solution of the present invention is further described below through the accompanying drawings and embodiments.

[0041] Unless otherwise defined, technical or scientific terms used in the present invention shall have the common meanings understood by one having ordinary skills in the field to which the present invention belongs.

[0042] In addition, it should be understood that although this specification is described according to the implementation modes, not every implementation mode includes only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment can also be appropriately combined to form other implementation modes that can be understood by those skilled in the art. These other implementation modes are also covered within the protection scope of the present invention.

[0043] The preparation method of the underwater super oleophobic calcium carbonate transparent coating is specifically described below in conjunction with the accompanying drawings and examples, but it should be understood that these examples are only used to illustrate the present invention and do not limit the scope of protection of the present invention in any way.

[0044] Example 1

[0045] S1. Soak a glass sheet (2 cm × 2 cm, 1 mm thick) in 90°C piranha solution (concentrated sulfuric acid: hydrogen peroxide = 3:1, volume ratio) for 2 hours for hydrophilic treatment. After treatment, take it out, clean it with deionized water, and dry it.

[0046] S2. Weigh 0.1 g of chitosan powder and add it to 50 ml of deionized water. Add a few drops of glacial acetic acid until the chitosan powder is completely dissolved to obtain a 1 wt% chitosan solution.

[0047] S3. Spin-coat the prepared chitosan solution onto the surface of the glass slide at a rotation speed of 3000 rpm for 30 seconds.

[0048] S4. Prepare 50 ml of mineralization solution A containing 6.25 mM calcium chloride, 9 mM magnesium chloride and 1 wt% PAA at room temperature, and stir for 10-20 min until fully dissolved.

[0049] S5. Prepare 50 ml of 6.25 mM sodium carbonate mineralization solution B at room temperature and stir for 10-20 minutes until fully dissolved.

[0050] S6. Place the glass slide spin-coated with the chitosan film at the bottom of the beaker containing the mineralization solution A. Use a peristaltic pump to slowly drop the mineralization solution B into the mineralization solution A at a rate of 2.8 ml / h.

[0051] S7. Take out the glass piece after mineralization, rinse it with deionized water, and dry it, and a transparent calcium carbonate coating will grow on the surface of the glass piece.

[0052] The calcium carbonate film prepared on the glass substrate showed extremely high transparency ( Figure 1 a), a mesoscopic crystal formed by highly ordered assembly of nanoparticles, so the calcium carbonate film shows a mosaic pattern of light and dark under a polarizing microscope ( Figure 2 , Figure 3 The calcium carbonate film exhibits superhydrophilicity in air ( Figure 4 ), showing underwater superoleophobicity in water ( Figure 5 ).

[0053] Example 2

[0054] S1. Ultrasonicate a polyethylene plastic sheet (PE) (2 cm × 2 cm, 1 mm thick) with anhydrous ethanol for 5 min to remove the oil on the surface. Take it out and clean it with deionized water and dry it.

[0055] S2. Weigh 0.1 g of chitosan powder and add it to 50 ml of deionized water. Add a few drops of glacial acetic acid until the chitosan powder is completely dissolved to obtain a 1 wt% chitosan solution.

[0056] S3. Spin-coat the prepared chitosan solution onto the surface of the plastic sheet at a rotation speed of 3000 rpm for 30 seconds.

[0057] S4. Prepare 50 ml of mineralization solution A containing 6.25 mM calcium chloride, 9 mM magnesium chloride and 1 wt% PAA at room temperature, and stir for 10-20 min until fully dissolved.

[0058] S5. Prepare 50 ml of 6.25 mM sodium carbonate mineralization solution B at room temperature and stir for 10-20 minutes until fully dissolved.

[0059] S6. Place the plastic sheet spin-coated with the chitosan film at the bottom of the beaker containing the mineralization solution A. Use a peristaltic pump to slowly drop the mineralization solution B into the mixed solution A at a rate of 2.8 ml / h.

[0060] S7. Take out the glass sheet after mineralization, rinse it with deionized water, and dry it, and a transparent calcium carbonate coating will grow on the surface of the plastic sheet.

[0061] The calcium carbonate film prepared on the polyethylene plastic sheet shows extremely high transparency ( Figure 1 b), the transmittance of the prepared calcium carbonate film is close to 90% ( Figure 6 ), XRD data show that the phase of calcium carbonate film is calcite ( Figure 7 ), nanoindentation test shows that calcium carbonate film exhibits excellent mechanical properties, with a hardness of 1GPa and a Young's modulus of 35GPa ( Figure 8 ).

[0062] Example 3

[0063] S1. Cut a 300-mesh polyethylene plastic mesh into pieces of 3 cm × 3 cm. Ultrasonicate the plastic mesh with anhydrous ethanol for 5 minutes to remove the oil on the surface. After the ultrasonication, clean it with deionized water and dry it.

[0064] S2. Weigh 0.1 g of chitosan powder and add it to 50 ml of deionized water. Add a few drops of glacial acetic acid until the chitosan powder is completely dissolved to obtain a 1 wt% chitosan solution.

[0065] S3. Spin-coat the prepared chitosan solution onto the plastic mesh at a rotation speed of 2000 rpm for 30 seconds.

[0066] S4. Prepare 50 ml of mineralization solution A containing 6.25 mM calcium chloride, 9 mM magnesium chloride and 1 wt% PAA at room temperature and stir for 10 min until fully dissolved.

[0067] S5. Prepare 50 ml of 6.25 mM sodium carbonate mineralization solution B at room temperature and stir for 10-20 minutes until fully dissolved.

[0068] S6. Place the plastic mesh spin-coated with chitosan film at the bottom of the beaker containing mineralization solution A. Use a peristaltic pump to slowly drip mineralization solution B into mineralization solution A at a drip rate of 2.8 ml / h.

[0069] S7. Take out the plastic mesh after mineralization, rinse it with deionized water, and dry it, and a transparent calcium carbonate coating will grow on the surface of the plastic mesh.

[0070] The surface of the polyethylene plastic mesh without modified calcium carbonate film is very smooth ( Fig. 9 After modification, a thin film composed of nanoparticles grows on the surface of the plastic mesh. The small particles of about 10 nm in the same arrangement direction are first assembled into bundles, and then different bundles are closely arranged to form a calcium carbonate film ( Fig.10 ). SEM-EDS results show that the elements of calcium carbonate film include Ca, Mg, O, and C, and are evenly distributed in the film ( Fig.11 The plastic net modified with calcium carbonate film was placed in the middle of the device to assemble into an oil-water separation device. Sudan red was used to dye cyclohexane red, and methylene blue was used to dye deionized water blue. The experimental results showed that the plastic net modified with calcium carbonate film could block cyclohexane, while water could pass through the plastic net smoothly, showing excellent oil-water separation performance ( Fig.12 ).

[0071] Therefore, the present invention provides a calcium carbonate transparent coating and a preparation method and use thereof. The calcium carbonate transparent film is mineralized and grown on the surface of a substrate. The calcium carbonate film is formed by densely stacked nano-calcite calcium carbonate particles. The substrate modified with the calcium carbonate transparent film exhibits superhydrophilicity in the air and superoleophobicity underwater, and is suitable for the field of oil-water separation.

[0072] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.

Claims

1. A method for preparing a calcium carbonate transparent coating, characterized in that: The transparent calcium carbonate transparent coating is formed by orderly stacking of calcite particles with a particle size of 20-50 nm, and comprises the following steps: S1, cutting and pre-processing the substrate; S2. Prepare chitosan solution using glacial acetic acid. S3, using a spin coater to evenly spin-coat the chitosan solution onto the substrate surface; S4. Prepare 50-100 ml of mineralization solution A at room temperature and stir for 10-20 minutes until it is fully dissolved; S5. Prepare 50-100 ml of mineralization solution B at room temperature and stir for 10-20 minutes until fully dissolved; S6, slowly adding the mineralization solution B to the mineralization solution A, and placing the substrate spin-coated with the chitosan solution at the bottom of the beaker containing the mineralization solution A; S7. After the addition of the mineralization solution B is completed, the substrate with the calcium carbonate film grown on the surface is taken out, cleaned with deionized water, and dried.

2. The method for preparing a calcium carbonate transparent coating according to claim 1, characterized in that: In step S1, the substrate to be treated is selected from a polyethylene plastic net, a polyethylene plastic sheet or a glass sheet, and the cutting size of the substrate to be treated is 2cm×2cm-5cm×5cm. The glass sheet is pretreated by hydrophilizing with piranha solution and then washing with deionized water. The polyethylene plastic net and the polyethylene plastic sheet are pretreated by ultrasonic treatment with anhydrous ethanol and then washing with deionized water.

3. The method for preparing a calcium carbonate transparent coating according to claim 1, characterized in that: In step S2, the concentration of the chitosan solution is 1.0-2.5 wt%.

4. The method for preparing a calcium carbonate transparent coating according to claim 1, characterized in that: In step S4, the raw materials in the mineralization solution A include calcium chloride, magnesium chloride and PAA, and the concentrations of calcium chloride, magnesium chloride and PAA in the mineralization solution A are 5.4-10.8 mM, 1.2-1.8 mM and 1-4 wt %, respectively.

5. The method for preparing a calcium carbonate transparent coating according to claim 1, characterized in that: In step S5, the raw material sodium carbonate in the mineralization solution B has a concentration of sodium carbonate in the mineralization solution B of 3.24-6.48 mM.

6. The method for preparing a calcium carbonate transparent coating according to claim 1, characterized in that: In step S6, a peristaltic pump is used to control the dripping rate of the mineralization solution B, and the dripping rate of the peristaltic pump is 2.0-5.0 ml / h.

7. The method for preparing a calcium carbonate transparent coating according to claim 4, characterized in that: In step S4, Ca in the mineralization solution A 2+ Mg 2+ The molar ratio between them is 6.25:

9.

8. The method for preparing a calcium carbonate transparent coating according to claim 2, characterized in that: The temperature of the piranha solution is 90°C, and the volume ratio of concentrated sulfuric acid to hydrogen peroxide in the piranha solution is 3:

1.

9. A calcium carbonate transparent coating, characterized in that: The calcium carbonate transparent coating is prepared by the preparation method of a calcium carbonate transparent coating according to any one of claims 1 to 8.

10. A calcium carbonate transparent coating according to claim 9, characterized in that: A calcium carbonate transparent coating is used in the technical field of oil-water separation.