Production method of large steel ingot
By combining vacuum inverter and degassing and betting technology, the problem of the quality of large forging steel ingots is solved, and the production of high-quality steel ingots is achieved, reducing the risk of forging fracture and post-forging treatment time.
Patent Information
- Application Number
- CN202310540855.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-15
- Publication Date
- 2024-11-15
AI Technical Summary
The prior art cannot effectively produce steel ingots of high-quality large forgings through betting and casting, resulting in the surface and internal quality of the steel ingots not meeting the standards and cannot meet the requirements of high-quality large forgings.
The method of combining vacuum inverted and degassing and pouring is adopted to further remove harmful gases in the molten steel by vacuum inverted and degassing, control the soft blowing and pouring speed of argon gas to ensure the purity and surface quality of the molten steel.
The requirements for the quality of high-quality large forgings on steel ingots are realized, the fracture accidents of forgings are reduced during use, the post-forging treatment process is simplified, the hydrogen expansion operation is avoided, and the production efficiency is improved.
Smart Images

Figure CN118950956A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of iron-based molten steel ingot casting, and in particular to a production method of large-scale steel ingots. Background Art
[0002] Large forgings are usually made by free forging of large steel ingots due to their heavy weight, large size, complex or varied shapes. The casting methods of steel ingots include top pouring and bottom pouring:
[0003] Among them, the upper pouring method is adopted to cast large steel ingots, and the molten steel treated by vacuum refining is poured into the steel ingot mold from the upper end in the vacuum chamber to reduce the gas content in the steel ingot and cast the ingot. However, due to the large size and high height of the steel ingot mold, the molten steel drips from a high place, inevitably splashing, forming surface defects such as steel ingot scarring and subcutaneous bubbles, which have a great impact on the quality of the steel ingot.
[0004] Therefore, for high-quality large forgings (such as cross-sectional diameter of Φ1000mm or more, weight of 20 tons or more), higher requirements are placed on the surface quality of the steel ingot and the metallurgical quality of the steel ingot. For example, there should be no defects visible to the naked eye, such as dents and non-metallic inclusions on the surface of the forging, and no cracks or defects should be found in the surface ultrasonic testing to prevent microcracks from expanding and causing fracture accidents during the service of the forging. Therefore, it is impossible to produce the above-mentioned high-quality large forgings by pouring.
[0005] When pouring steel ingots, the vacuum refined molten steel is slowly poured into the ingot mold from the bottom of the ingot mold, the liquid level rises steadily, and the surface quality of the ingot is good; at the same time, the flow of molten steel is conducive to the floating and discharge of inclusions in the steel, and the metallurgical quality of the ingot is good. However, the current pouring method is limited to small and medium-sized forgings, and cannot meet the quality requirements of high-quality large forgings for steel ingots.
[0006] Therefore, it is of great significance to make product quality meet the corresponding technical requirements and realize the requirements of high-quality large forgings on ingot quality through process technology innovation without increasing traditional ingot casting equipment. Summary of the invention
[0007] In view of the above analysis, an embodiment of the present invention aims to provide a method for producing large steel ingots, so as to cast steel ingots for large forgings through the existing pouring method without adding traditional ingot casting equipment, so as to meet the quality requirements of high-quality large forgings for steel ingots.
[0008] The present invention provides a method for producing a large steel ingot, the method comprising the following steps:
[0009] S1.LF refined steel liquid is vacuum degassed in VD furnace and the chemical composition is fine-tuned according to the test results;
[0010] S2. The refined steel after vacuum degassing in the VD furnace is subjected to argon soft blowing treatment;
[0011] S3. The molten steel after argon soft blowing flows out from the LF ladle outlet, diffuses under vacuum and falls into the betting bag pre-placed in the vacuum chamber, and stirs the betting bag in the vacuum chamber with argon during the falling process;
[0012] S4. Break the air, turn off the argon gas, measure the temperature of the molten steel and cover it with an insulation cover, then lift the pouring bag out of the vacuum chamber to the pouring position;
[0013] S5. Start protective pouring and stop pouring when the under-pouring height is reached.
[0014] Preferably, in S1, the process of vacuum degassing in the VD furnace comprises: placing the LF ladle containing LF refined molten steel into the VD furnace, starting vacuum degassing, and starting timing when the vacuum degree is less than 267 Pa, and the vacuum is maintained for 15-25 minutes.
[0015] Preferably, in S2, during the argon soft blowing process, the flow rate of argon is not greater than 150NL / min, and the soft blowing time is 5-30min.
[0016] Preferably, in S3, the LF package is placed on a vacuum cover of the vacuum chamber, and evacuation is started until the vacuum degree in the vacuum chamber is no higher than 67Pa.
[0017] Preferably, in S3, before the betting bag is placed in the vacuum chamber, it is baked to a temperature not lower than 800° C., and the air-permeable bricks at the bottom of the betting bag are connected to the argon hose outside the vacuum chamber.
[0018] Preferably, in S3, the temperature of the molten steel flowing out of the LF ladle water outlet is not less than 1580°C, and the injection flow diffuses under vacuum and falls into the injection ladle pre-placed in the vacuum chamber, and the molten steel injection flow rate is 3-15t / min.
[0019] Preferably, argon is blown into the bottom air-permeable brick of the betting bag in S3 through an argon hose outside the vacuum chamber, and the argon flow rate is 40-200NL / min.
[0020] Preferably, in S4, the argon stirring is turned off, the temperature of the molten steel is measured again, and then the ladle is covered with an insulation cover, and then the ladle is lifted out of the vacuum chamber to ensure that the temperature drop of the molten steel is no more than 1°C / min.
[0021] Preferably, in S5, the pouring ingot is protected in the atmospheric environment, and during pouring, there is argon protection between the top of the center pouring pipe and the steel outlet of the pouring ladle, as well as the upper opening of the insulation cap of the ingot mold.
[0022] Preferably, in S5, the pouring speed is not higher than 5 t / min, and the pouring speed of the riser is not higher than 2 / 3 of the pouring speed of the ingot body.
[0023] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects:
[0024] 1. The method of the present invention, without adding traditional ingot casting equipment, makes the product quality meet the corresponding technical requirements through process technology innovation, and realizes the requirements of high-quality large forgings on the quality of steel ingots. Specifically, the existing vacuum chamber, betting bag and other equipment are used without changing the existing equipment structure, which broadens the scope of application of the existing equipment and reduces the equipment research and development and transformation costs.
[0025] 2. The present invention combines vacuum degassing with pouring casting. The vacuum degassing can further remove harmful gases in the molten steel and reduce harmful gases in the steel ingot, thereby avoiding fracture accidents of forgings during use. At the same time, due to the carbon-oxygen reaction under high vacuum, the oxygen content in the molten steel is further reduced, and the purity of the molten steel is improved, thereby improving the internal metallurgical quality and surface quality of the steel ingot, thereby meeting the quality requirements of high-quality large forgings for the steel ingot.
[0026] 3. When using the existing common pouring method to produce steel ingots, the larger the steel ingot is, the longer the forging needs to undergo hydrogen expansion after forging to prevent defects such as "white spots" and hairline on the forgings. The larger the cross-section of the forging, the longer the hydrogen expansion time, which is inefficient. Compared with the existing common pouring method, the method of the present invention controls the process and specific parameters, such as argon soft blowing and vacuum ladle degassing of the molten steel before pouring, argon flow during vacuum ladle pouring, controlling the temperature drop rate of the molten steel during the transfer of the pouring ladle, and controlling the pouring speed of the pouring pouring, so that the processing time of the forging after forging is short, and the defects such as "white spots" and hairline on the forgings are effectively prevented.
[0027] 4. The steel ingot produced by the method of the present invention is forged into forgings without adding a post-forging hydrogen expansion process.
[0028] In the present invention, the above-mentioned technical solutions can also be combined with each other to achieve more preferred combination solutions. Other features and advantages of the present invention will be described in the subsequent description, and some advantages can become obvious from the description, or can be understood by practicing the present invention. The purpose and other advantages of the present invention can be realized and obtained through the contents particularly pointed out in the description and the drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] The drawings are only for the purpose of illustrating particular embodiments and are not to be considered limiting of the present invention. Like reference symbols denote like components throughout the drawings.
[0030] Figure 1 It is a process diagram of vacuum inverting degassing + pouring steel ingot in the production method of large steel ingot of the present invention;
[0031] Figure 2 Heat treatment process after forging the large steel ingot prepared in Example 1 into a forging;
[0032] Figure 3 The large steel ingot prepared in comparative example 1 is forged into a forging and then subjected to heat treatment after forging.
[0033] Reference numerals:
[0034] 1-LF bag; 2-vacuum cover; 3-betting bag; 4-vacuum chamber; 5-argon hose; 6-middle injection tube; 7-argon protection cover; 8-argon protection cover plate; 9-ingot mold; 10-betting chassis; 11-argon source. DETAILED DESCRIPTION
[0035] The preferred embodiments of the present invention are described in detail below in conjunction with the accompanying drawings, wherein the accompanying drawings constitute a part of this application and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not used to limit the scope of the present invention.
[0036] In the pouring method of the prior art, usually small steel ingots can be transferred for pouring after one vacuum treatment (such as VD). Since pouring in a vacuum chamber is limited by the size of the vacuum chamber, the larger the steel ingot, the more difficult it is to carry out smoothly. For forgings with a cross-sectional diameter of more than Φ1000mm and a weight of more than 20 tons, the pouring of large steel ingots cannot be carried out in a vacuum chamber with limited space, because the vacuum chamber is usually built for pouring. Once built, its size and capacity are determined. The pouring system cannot be placed in a vacuum chamber with limited space, or even if the pouring system is placed in a vacuum chamber, the space becomes relatively more cramped, and it will be more difficult for workers to operate, and the greater the danger for workers to work in a confined space. In the study, the inventor tried to produce the above-mentioned large steel ingots by degassing the molten steel through VD vacuum degassing and then pouring it directly under atmospheric conditions.
[0037] However, vacuum degassing equipment such as VD cannot meet the quality requirements of high-quality large forgings for steel ingots because its degassing reaction is only at the interface between the two phases, which limits the improvement of molten steel purity and the removal of harmful gases in the molten steel. For example, the forging surface cannot have defects visible to the naked eye such as dents and non-metallic inclusions, and no cracks can be found in its ultrasonic detection, which prevents the microcracks from expanding during the service of the forging and causing fracture accidents.
[0038] In addition, the larger the ordinary cast steel ingot is, the longer the forging needs to undergo hydrogen expansion operation after forging to prevent defects such as "white spots" and hairline cracks in the forging. The larger the cross-section of the forging is, the longer the hydrogen expansion time is and the lower the efficiency is.
[0039] The present invention provides a method for producing a large steel ingot. Figure 1 As shown, the method comprises the following steps:
[0040] S1.LF refined steel liquid is vacuum degassed in VD furnace and the chemical composition is fine-tuned according to the test results;
[0041] S2. The refined steel after vacuum degassing in the VD furnace is subjected to argon soft blowing treatment;
[0042] S3. The molten steel after argon soft blowing flows out from the water inlet of LF bag 1, diffuses under vacuum and falls into the betting bag 3 pre-placed in the vacuum chamber 4, and the argon gas is stirred in the betting bag 3 in the vacuum chamber 4 during the falling process;
[0043] S4 break, turn off the argon stirring, measure the molten steel temperature and cover with insulation cover, then lift the betting bag 3 out of the vacuum chamber 4 transfer to the betting pouring position;
[0044] S5. Start protective pouring and stop pouring when the under-pouring height is reached.
[0045] Compared with the prior art, the present invention combines vacuum degassing with pouring. The vacuum degassing can further remove harmful gases in the molten steel, reduce harmful gases in the steel ingot, and thus avoid fracture accidents of forgings during use. At the same time, due to the carbon-oxygen reaction under high vacuum, the oxygen content in the molten steel is further reduced, the purity of the molten steel is improved, and the internal metallurgical quality of the steel ingot is further improved, meeting the quality requirements of high-quality large forgings for steel ingots. In addition, the steel ingots produced by the method of the present invention do not need to add a post-forging hydrogen expansion process when forging; the method of the present invention, on the basis of not adding traditional ingot casting equipment, through process technology innovation, makes the product quality meet the corresponding technical requirements, and achieves the quality requirements of high-quality large forgings for steel ingots.
[0046] It should be noted that the large steel ingot of the present invention refers to a steel ingot that can be forged into a large forging with a cross-sectional diameter of more than Φ1000mm and a weight of more than 20 tons, and the weight of the large steel ingot is more than 40 tons.
[0047] For example, in S1, the LF refined molten steel enters the VD furnace and starts vacuum degassing after reaching a suitable temperature (1620-1650°C) and good deoxidation ([O]≤0.0035%).
[0048] Specifically, in S1, the process of vacuum degassing in the VD furnace includes: placing the LF ladle containing LF refined molten steel into the VD furnace, starting vacuum degassing, and starting timing when the vacuum degree is less than 267 Pa, and the vacuum is maintained for 15-25 minutes.
[0049] For example, during the vacuum degassing process of the VD furnace, argon is passed into the LF bag 1, and the boiling of the molten steel in the LF bag is observed through the observation hole to adjust the argon flow rate to prevent excessive boiling of the molten steel from causing large splashing or scouring. After 15-25 minutes, the argon flow rate is reduced to no more than 150NL / min and maintained for 1-10 minutes. The total vacuum time is no more than 80 minutes. After degassing is completed, the air is broken, and the main chemical components and gas samples in the molten steel are analyzed, and the chemical composition is fine-tuned according to the test results.
[0050] Exemplarily, after the molten steel is vacuum degassed in a VD furnace, it is subjected to argon soft blowing treatment at a suitable temperature (1550-1600°C).
[0051] Specifically, in S2, in the argon soft blowing treatment, the flow rate of argon is not more than 150NL / min, such as 80NL / min, 90NL / min, 100NL / min, 110NL / min, 120NL / min, 130NL / min, 140NL / min, etc., and the soft blowing time is 5-30min, such as 10min, 15min, 20min, 25min, etc. The argon soft blowing treatment further floats and removes the inclusions in the molten steel, thereby improving the purity of the molten steel. After the soft blowing is completed, component samples and gas samples are taken to prepare for steel tapping.
[0052] In the present invention, S3 is a vacuum inverted steel flow degassing process. In this process, after the steel flow enters the vacuum chamber, gases [H] and the like escape rapidly, and carbon-oxygen reaction occurs in the molten steel, resulting in carbon monoxide bubbles escaping, so that the steel flow is sprayed with droplets at a certain diffusion angle, which greatly increases the surface area of the molten steel, achieves the purpose of degassing, and reduces the occurrence of defects such as bubbles and white spots in forgings.
[0053] Specifically, in S3, the LF bag 1 is placed on the vacuum cover 2 of the vacuum chamber 4, and vacuuming is started until the vacuum degree in the vacuum chamber 4 is not higher than 67Pa.
[0054] Exemplarily, before placing the LF bag 1 on the vacuum cover 2 of the vacuum chamber 4, the qualified molten steel after argon soft blowing treatment is first transferred to the vicinity of the vacuum chamber 4, and the slide plate is opened for drainage. The drainage time is greater than 10s, so that the water inlet of the LF bag 1 is fully preheated. After preheating, the slide plate is closed, and then the LF bag 1 is placed on the vacuum cover 2 of the vacuum chamber 4. After sealing, vacuuming is started. When the vacuum degree of the vacuum chamber 4 is not higher than 67Pa, for example, 20Pa, 30Pa, 40Pa, 50Pa, 60Pa, etc., the slide plate is opened again, and the steel flow is ejected from the water inlet of the LF bag 1 and diffuses in the vacuum chamber 4, and falls into the betting bag 3 placed in the vacuum chamber 4 in advance, thereby completing the degassing operation.
[0055] For example, in S3, before the betting ladle 3 is placed in the vacuum chamber 4, it is baked to a temperature not lower than 800°C, such as 850°C, 900°C, 950°C, 1000°C, 1100°C, 1200°C, etc., and the air-permeable bricks at the bottom of the betting ladle 3 are connected to the argon hose 5 outside the vacuum chamber 4. Baking the betting ladle 3 to a temperature not lower than 800°C can prevent the subsequent pouring temperature from being unable to be controlled due to excessive temperature drop of the molten steel.
[0056] Specifically, in S3, argon is blown into the bottom air bricks of the betting ladle 3 through the argon hose 5 outside the vacuum chamber 4, and the argon flow rate is 40-200NL / min, such as 50NL / min, 60NL / min, 80NL / min, 100NL / min, 120NL / min, 140NL / min, 160NL / min, 180NL / min, 190NL / min, etc. The purpose of blowing argon is to make the temperature of the molten steel uniform and avoid accidents such as pouring failure. The size of the flow rate is suitable for uniform stirring intensity. Too large a flow rate will seriously scour the ladle and the air bricks and reduce the purity of the molten steel. Too small a flow rate cannot achieve the purpose of uniform temperature.
[0057] For example, in S3, the temperature of the molten steel flowing out of the nozzle of the LF ladle 1 is not less than 1580°C, which is to ensure the subsequent pouring temperature. The pouring temperature will affect the solidification process of the steel ingot and the final quality of the steel ingot, and too low a temperature will cause the "cold steel" to condense and the pouring will fail; the injection flow diffuses under vacuum and falls into the injection ladle 3 pre-placed in the vacuum chamber 4, and the injection speed of the molten steel is 3-15t / min, such as 4t / min, 5t / min, 6t / min, 7t / min, 8t / min, 9t / min, 10t / min, 11t / min, 12t / min, 13t / min, 14t / min. If the speed is too slow, the temperature drop will be large, and the subsequent pouring temperature cannot be guaranteed. If the speed is too fast, the degassing time will be too short, and the degassing effect will not reach the expected goal.
[0058] In the present invention, after the vacuum ladle steel flow is degassed, the water inlet of the LF ladle 1 is closed, the air is broken, the vacuum cover 2 is removed, the lower ladle 3 is lifted, and after the temperature measurement and sampling work is completed, the lower ladle 3 is transferred to the lower pouring position for pouring.
[0059] Specifically, in S4, during the process of lifting the pouring ladle 3 out of the vacuum chamber 4 to the pouring position, the cooling rate of the molten steel in the pouring ladle 3 is not greater than 1°C / min to prevent excessive temperature drop from failing to meet the final pouring speed.
[0060] Exemplarily, the pouring package 3 is lifted out of the vacuum chamber 4 to the pouring position within 10 minutes.
[0061] Specifically, in S4, the heat-insulating cover may be a cover made of refractory material to prevent heat radiation and convection heat dissipation.
[0062] In the present invention, the pouring process in S5 includes: the molten steel in the pouring ladle 3 flows from the top of the middle pouring pipe 6 into the steel flow channel in the pouring bottom plate 10, and then enters the ingot mold 9 from the bottom of the ingot mold 9.
[0063] For example, in S5, the pouring ingot is protected in the atmospheric environment, and during pouring, there is argon protection between the top of the middle pouring pipe 6 and the steel outlet of the pouring ladle 3 and the upper opening of the insulation cap of the ingot mold 9. Argon protection can prevent the purity of the molten steel from being reduced due to secondary oxidation of the refined molten steel.
[0064] Specifically, an argon protective cover 7 is arranged between the top end of the middle pouring pipe 6 and the molten steel outlet of the lower pouring bag 3, and an argon protective cover plate 8 is arranged on the upper opening of the insulation cap of the ingot mold 9.
[0065] In the present invention, the bottom air-permeable bricks, argon protective cover 7 and argon protective cover plate 8 of the betting bag 3 are respectively connected to the argon source 11 through the argon hose 5, and the argon source 11 provides argon therefor.
[0066] For example, in S5, the pouring speed is not higher than 5t / min, such as 1t / min, 2t / min, 3t / min, 4t / min, etc., and the pouring speed of the riser is not higher than 2 / 3 of the pouring speed of the ingot body. The pouring speed can be controlled by controlling the opening size of the steel tapping nozzle of the pouring ladle 3. The pouring speed can improve the final surface quality and core metallurgical quality of the steel ingot.
[0067] Example 1
[0068] This embodiment provides a method for producing a large-scale support roller steel ingot, wherein the corresponding forging cross-section diameter of the support roller steel ingot is Φ1120 mm, the length is 4795 mm, and the weight is 25 tons. The production method includes:
[0069] VD furnace vacuum degassing: LF refined molten steel enters the VD furnace for vacuum degassing when the temperature is appropriate and the deoxidation is good. When the vacuum degree reaches 250Pa, the timing starts, and the vacuum is maintained for 20 minutes. The boiling of the molten steel in the LF ladle is observed through the observation hole to adjust the argon flow rate to prevent excessive boiling of the molten steel from causing large splashing or scouring. After 20 minutes, the argon flow rate is reduced to 140NL / min and maintained for a certain period of time. The total vacuum time is 50 minutes. After degassing is completed, the main chemical components and gas samples of the molten steel are analyzed after breaking the air, and the chemical composition is fine-tuned according to the test results.
[0070] Argon soft blowing treatment: After the molten steel is vacuum degassed in the VD furnace, the temperature is suitable for argon soft blowing treatment, the flow rate is 140NL / min, and the soft blowing time is 20min, so that the inclusions in the molten steel can be further floated and removed, and the purity of the molten steel can be improved. After the soft blowing is completed, the component samples and gas samples are taken to prepare for steelmaking.
[0071] Degassing of the steel flow in the vacuum ladle: After the qualified molten steel is soft-blown with argon, it is transferred to the vicinity of the vacuum chamber 4, and the slide plate is opened for drainage. The drainage time is 15s to fully preheat the water inlet of the LF ladle 1. Then close the slide plate, place the LF ladle 1 directly on the vacuum cover 2, and start vacuuming after sealing. When the vacuum degree of the vacuum chamber 4 is 65Pa, open the slide plate again, the steel flow sprays out from the ladle water inlet and diffuses in the vacuum chamber, and falls into the betting ladle 3 pre-placed in the vacuum chamber 4, thereby completing the degassing operation. Before the steel flow is degassed, the betting ladle 3 is well baked before entering the vacuum chamber 4, the temperature is 900℃, and the argon hose 5 outside the vacuum chamber 4 is connected. The degassing pouring temperature is 1600℃, and the degassing pouring speed is controlled to be 7t / min. From the start of steel flow degassing to the pouring of the steel ingot, argon is blown into the bottom air brick of the betting ladle 3 through the argon hose 5 outside the vacuum chamber, and the flow rate is 80NL / min. After the degassing pouring is completed, the water inlet is closed, the air is broken, the vacuum cover 2 is removed and the pouring bag 3 is lifted, the temperature measurement and sampling work is completed, and it is transferred to the pouring position to prepare for pouring.
[0072] Protect the pouring ingot in the atmospheric environment: after breaking through the air, lift out the pouring bag 3, measure the temperature, take samples, and transfer to the pouring position within 10 minutes. During the transfer process, cover the pouring bag 3 with an insulation cover to prevent excessive temperature drop. The temperature drop rate of the molten steel is 0.6℃ / min. After the transfer is completed, start the protective pouring, and stop pouring when the under-pouring height is reached. Before pouring, the ingot system is baked with hot air; during pouring, there is an argon protective cover 7 between the top of the middle pouring pipe 6 and the molten steel outlet of the pouring bag 3, and there is an argon protective cover plate 8 on the upper mouth of the insulation cap of the ingot mold 9; the molten steel rises steadily in the mold, and the pouring speed is controlled by the size of the water inlet opening. The pouring speed is 4t / min, and the pouring speed of the riser is 1 / 3 of the pouring speed of the ingot body.
[0073] Example 2
[0074] This embodiment provides a method for producing a large steel ingot, comprising:
[0075] VD furnace vacuum degassing: LF refined molten steel enters the VD furnace for vacuum degassing when the temperature is appropriate and the deoxidation is good. When the vacuum degree reaches 260Pa, the timing starts, and the vacuum is maintained for 15 minutes. The boiling of the molten steel in the LF ladle is observed through the observation hole to adjust the argon flow rate to prevent excessive boiling of the molten steel from causing large splashing or scouring. After 15 minutes, the argon flow rate is reduced to 130NL / min and maintained for a certain period of time. The total vacuum time is 40 minutes. After degassing is completed, the main chemical components and gas samples of the molten steel are analyzed after breaking the air, and the chemical composition is fine-tuned according to the test results.
[0076] Argon soft blowing treatment: After the molten steel is vacuum degassed in the VD furnace, the temperature is suitable for argon soft blowing treatment, the flow rate is 130NL / min, and the soft blowing time is 5min, so that the inclusions in the molten steel can be further floated and removed, and the purity of the molten steel can be improved. After the soft blowing is completed, the component samples and gas samples are taken to prepare for steelmaking.
[0077] Degassing of the steel flow in the vacuum ladle: After the qualified molten steel is soft-blown with argon, it is transferred to the vicinity of the vacuum chamber 4, and the slide plate is opened for drainage. The drainage time is 12s to fully preheat the water inlet of the LF ladle 1. Then close the slide plate, place the LF ladle 1 directly on the vacuum cover 2, and start vacuuming after sealing. When the vacuum degree of the vacuum chamber 4 is 60Pa, open the slide plate again, the steel flow sprays out from the ladle water inlet and diffuses in the vacuum chamber, and falls into the betting ladle 3 pre-placed in the vacuum chamber 4, thereby completing the degassing operation. Before the steel flow is degassed, the betting ladle 3 is well baked before entering the vacuum chamber 4, the temperature is 800℃, and the argon hose 5 outside the vacuum chamber 4 is connected. The degassing pouring temperature is 1580℃, and the degassing pouring speed is controlled to be 3t / min. From the start of steel flow degassing to the pouring of the steel ingot, argon is blown into the bottom air brick of the betting ladle 3 through the argon hose 5 outside the vacuum chamber, and the flow rate is 40NL / min. After the degassing pouring is completed, the water inlet is closed, the air is broken, the vacuum cover 2 is removed and the pouring bag 3 is lifted, the temperature measurement and sampling work is completed, and it is transferred to the pouring position to prepare for pouring.
[0078] Protect the pouring ingot in the atmospheric environment: after breaking through the air, lift out the pouring bag 3, measure the temperature, take samples, and transfer it to the pouring position within 10 minutes. During the transfer process, cover the pouring bag 3 with an insulation cover to prevent excessive temperature drop. The temperature drop rate of the molten steel is 0.8℃ / min. After the transfer is completed, start the protective pouring, and stop pouring when the under-pouring height is reached. Before pouring, the ingot system is baked with hot air; during pouring, there is an argon protective cover 7 between the top of the middle pouring pipe 6 and the molten steel outlet of the pouring bag 3, and there is an argon protective cover plate 8 on the upper mouth of the insulation cap of the ingot mold 9; the molten steel rises steadily in the mold, and the pouring speed is controlled by the size of the water inlet opening. The pouring speed is 3t / min, and the pouring speed of the riser is 1 / 3 of the pouring speed of the ingot body.
[0079] Example 3
[0080] This embodiment provides a method for producing a large steel ingot, comprising:
[0081] VD furnace vacuum degassing: LF refined molten steel enters the VD furnace for vacuum degassing when the temperature is appropriate and the deoxidation is good. When the vacuum degree reaches 265Pa, the timing starts, and the vacuum is maintained for 25 minutes. The boiling of the molten steel in the LF ladle is observed through the observation hole to adjust the argon flow rate to prevent excessive boiling of the molten steel from causing large splashing or scouring. After 25 minutes, the argon flow rate is reduced to 150NL / min and maintained for a certain period of time. The total vacuum time is 60 minutes. After degassing is completed, the main chemical components and gas samples of the molten steel are analyzed after breaking the air, and the chemical composition is fine-tuned according to the test results.
[0082] Argon soft blowing treatment: After the molten steel is vacuum degassed in the VD furnace, the temperature is suitable for argon soft blowing treatment, the flow rate is 150NL / min, and the soft blowing time is 30min, so that the inclusions in the molten steel can be further floated and removed, and the purity of the molten steel can be improved. After the soft blowing is completed, the component samples and gas samples are taken to prepare for tapping.
[0083] Degassing of the steel flow in the vacuum ladle: After the qualified molten steel is soft-blown with argon, it is transferred to the vicinity of the vacuum chamber 4, and the slide plate is opened for drainage. The drainage time is 20s to fully preheat the water inlet of the LF ladle 1. Then close the slide plate, place the LF ladle 1 directly on the vacuum cover 2, and start vacuuming after sealing. When the vacuum degree of the vacuum chamber 4 is 67Pa, open the slide plate again, the steel flow sprays out from the ladle water inlet and diffuses in the vacuum chamber, and falls into the betting ladle 3 pre-placed in the vacuum chamber 4, thereby completing the degassing operation. Before the steel flow is degassed, the betting ladle 3 is well baked before entering the vacuum chamber 4, the temperature is 1000℃, and the argon hose 5 outside the vacuum chamber 4 is connected. The degassing pouring temperature is 1630℃, and the degassing pouring speed is controlled to be 12t / min. From the start of steel flow degassing to the pouring of the steel ingot, argon is blown into the bottom air brick of the betting ladle 3 through the argon hose 5 outside the vacuum chamber, and the flow rate is 200NL / min. After the degassing pouring is completed, the water inlet is closed, the air is broken, the vacuum cover 2 is removed and the pouring bag 3 is lifted, the temperature measurement and sampling work is completed, and it is transferred to the pouring position to prepare for pouring.
[0084] Protect the pouring ingot in the atmospheric environment: after breaking through the air, lift out the pouring bag 3, measure the temperature, take samples, and transfer it to the pouring position within 10 minutes. During the transfer process, cover the pouring bag 3 with an insulation cover to prevent excessive temperature drop. The temperature drop rate of the molten steel is 0.9℃ / min. After the transfer is completed, start the protective pouring, and stop pouring when the under-pouring height is reached. Before pouring, the ingot system is baked with hot air; during pouring, there is an argon protective cover 7 between the top of the middle pouring pipe 6 and the molten steel outlet of the pouring bag 3, and there is an argon protective cover plate 8 on the upper mouth of the insulation cap of the ingot mold 9; the molten steel rises steadily in the mold, and the pouring speed is controlled by the size of the water inlet opening. The pouring speed is 5t / min, and the pouring speed of the riser is 2 / 3 of the pouring speed of the ingot body.
[0085] Example 4
[0086] This embodiment provides a method for producing large steel ingots similar to that of Embodiment 1, except that the temperature drop rate of the molten steel during the transfer of the pouring ladle 3 is 1.5°C / min.
[0087] The forgings forged from the steel ingot prepared in this embodiment have defects visible to the naked eye, such as non-metallic inclusions, on the surface, and a small amount of inclusions are found in the ultrasonic test. This is because the temperature drop of the molten steel is too large, part of the molten steel condenses or has difficulty in flowing, resulting in unsmooth pouring. At the same time, the temperature of the molten steel is too low, and the inclusions in the steel are quickly captured, resulting in poor metallurgical quality of the steel ingot.
[0088] Example 5
[0089] This embodiment provides a method for producing large steel ingots similar to that of Embodiment 1, except that the pouring speed of the bottom pouring is 6 t / min.
[0090] Ultrasonic testing of the forged steel ingots prepared in this embodiment revealed multiple 2-3 mm defects on the surface. This is because the pouring speed is too fast, which easily produces internal defects such as bubbles and inclusions, uneven thermal stress inside the steel ingot, which easily produces cracks, and scarring and heavy skin on the surface of the steel ingot.
[0091] Example 6
[0092] This embodiment provides a method for producing large steel ingots similar to that of Embodiment 1, except that argon is blown into the bottom air-permeable bricks of the betting bag 3 through the argon hose 5 outside the vacuum chamber 4, and the argon flow rate is 20NL / min.
[0093] In this embodiment, because the argon gas flow rate is too small, the temperature of the molten steel in the pouring ladle is uneven, resulting in defects inside and on the surface of the final steel ingot, casting failure, and no steel ingot can be produced.
[0094] Comparative Example 1
[0095] This embodiment provides a method for producing large steel ingots similar to that of Embodiment 1, except that there is no step of vacuum pouring steel flow degassing, and the molten steel after argon soft blowing is directly poured and cast ingots under atmospheric protection.
[0096] The forgings forged from the steel ingot prepared in this embodiment have a large number of defects visible to the naked eye, such as dents and non-metallic inclusions on their surfaces. A large number of cracks and defects are found in ultrasonic testing, and fracture accidents have occurred in the forgings during service.
[0097] The surface quality, internal quality and service fracture conditions of the forgings forged from the steel ingots produced in Examples 1-6 and Comparative Example 1 are listed in Table 1.
[0098] Table 1
[0099]
[0100] EN10228 has 4 quality levels, with level 1 being the worst and level 4 being the best.
[0101] Test example:
[0102] The large steel ingots prepared in Example 1 and Comparative Example 1 were forged into forgings, and then subjected to post-forging heat treatment. When the hydrogen content in the steel is 4ppm, the pressure of more than 1000 atmospheres can be caused in the steel below 200 degrees Celsius due to the accumulation of hydrogen and the contraction of the steel. When the stress caused by this exceeds the tensile strength of the steel, the steel will be cracked. Therefore, one of the main purposes of post-forging heat treatment is to expand hydrogen and reduce the hydrogen content of the forging. Taking the forging with the largest cross-section of Φ1230 as an example, the post-forging heat treatment process of normalizing + tempering is performed.
[0103] The heat treatment process after forging of the large steel ingot prepared in Example 1 is as follows: Figure 2 As shown in the figure, the specific process is as follows: the forging blank is heated in a 600-650℃ soaking furnace for 15h, then heated to the normalizing temperature (950±10℃) at a rate of no more than 80℃ / h, kept warm for 15h and then taken out of the furnace for air cooling. When the surface temperature of the forging blank drops to 350-400℃, it is heated to the tempering temperature (600±10℃) at a rate of no more than 60℃ / h, then kept warm for 60h and then taken out of the furnace to complete the post-forging heat treatment process; the post-forging heat treatment process of the large steel ingot prepared in comparative example 1 is as follows Figure 3 As shown in the figure, the specific process is basically the same as above, except that the tempering and heat preservation stage needs to be extended for 100 hours before it can be taken out of the furnace. This is because the larger the cross-section, the slower the diffusion of harmful gases such as hydrogen, the longer the diffusion time required, the more energy consumption, and the greater the heating loss of the forging. Figure 2 and Figure 3 From the process comparison, it can be seen that the scheme of the present invention does not need to add a post-forging hydrogen expansion process. This is because the present invention combines vacuum inverting degassing with the down-pouring pouring method. The vacuum inverting degassing can further remove harmful gas hydrogen in the molten steel, thereby reducing the hydrogen content in the steel ingot. There is no need for a post-forging hydrogen expansion process, thereby shortening the post-forging heat treatment time, simplifying the post-forging heat treatment process, and also making the energy consumption of the post-forging heat treatment small and the cost low.
[0104] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.
Claims
1. A method for producing a large steel ingot, characterized in that: The method comprises the following steps: S1.LF refined steel liquid is vacuum degassed in VD furnace and the chemical composition is fine-tuned according to the test results; S2. The refined steel after vacuum degassing in the VD furnace is subjected to argon soft blowing treatment; S3. The molten steel after argon soft blowing flows out from the LF ladle outlet, diffuses under vacuum and falls into the betting bag pre-placed in the vacuum chamber, and stirs the betting bag in the vacuum chamber with argon during the falling process; S4. Break the air, turn off the argon gas, measure the temperature of the molten steel and cover it with an insulation cover, then lift the pouring bag out of the vacuum chamber to the pouring position; S5. Start protective pouring and stop pouring when the under-pouring height is reached.
2. The method for producing a large steel ingot according to claim 1, characterized in that: In S1, the process of vacuum degassing in the VD furnace includes: placing the LF bag containing LF refined molten steel into the VD furnace, starting vacuum degassing, and starting timing when the vacuum degree is less than 267 Pa, and the vacuum is maintained for 15-25 minutes.
3. The method for producing a large steel ingot according to claim 1, characterized in that: In S2, during the argon soft blowing process, the flow rate of argon is not greater than 150NL / min, and the soft blowing time is 5-30min.
4. The method for producing a large steel ingot according to claim 1, characterized in that: In S3, the LF package is placed on the vacuum cover of the vacuum chamber, and vacuuming is started until the vacuum degree in the vacuum chamber is no higher than 67Pa.
5. The method for producing a large steel ingot according to claim 1, characterized in that: In S3, before the betting bag is placed in the vacuum chamber, it is baked to a temperature not less than 800° C., and the air-permeable bricks at the bottom of the betting bag are connected to the argon hose outside the vacuum chamber.
6. The method for producing a large steel ingot according to claim 1, characterized in that: In S3, the temperature of the molten steel flowing out of the LF ladle water outlet is not less than 1580°C, and the injection flow diffuses under vacuum and falls into the injection ladle pre-placed in the vacuum chamber, and the injection flow rate of the molten steel is 3-15t / min.
7. The method for producing a large steel ingot according to claim 5, characterized in that: Argon gas is blown into the bottom air-permeable brick of the S3 middle betting bag through the argon hose outside the vacuum chamber, and the argon gas flow rate is 40-200NL / min.
8. The method for producing a large steel ingot according to claim 1, characterized in that: In S4, during the process of lifting the pouring ladle out of the vacuum chamber to the pouring position, the temperature drop rate of the molten steel in the pouring ladle is not greater than 1°C / min.
9. The method for producing a large steel ingot according to claim 1, characterized in that: In the above S5, the pouring ingot is protected in the atmospheric environment. During pouring, the space between the top of the center pouring pipe and the outlet of the pouring ladle and the upper opening of the insulation cap of the ingot mold are all protected by argon gas.
10. The method for producing a large steel ingot according to claims 1-5, characterized in that: In S5, the pouring speed is not higher than 5 t / min, and the pouring speed of the riser is not higher than 2 / 3 of the pouring speed of the ingot body.