Method for preparing carbon nanotube reinforced aluminum-based composite material through heat treatment of matrix powder

By ball milling and high-temperature vacuum heat treatment on the metal matrix powder, combined with plasma sintering and hot extrusion processes, the problem of uneven dispersion of CNTs in CNTs/Al composite material powder is solved, significantly improving the strength and plasticity of the material. It is suitable for Aerospace and other fields.

CN118951015APending Publication Date: 2024-11-15NORTHWESTERN POLYTECHNICAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411179235.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

It is difficult to prepare high-content, uniformly dispersed carbon nanotubes (CNTs)/aluminum-based composite powders with high content and uniform dispersion. CNTs are mainly dispersed at grain boundaries, affecting the strong plasticity of the material.

Method used

By ball milling the metal matrix powder and high-temperature vacuum heat treatment, the growth of the matrix grains is controlled, and CNTs are added after heat treatment for secondary ball milling. Combined with plasma sintering and hot extrusion processes, the dispersion ability and mechanical properties of the CNTs are improved.

Benefits of technology

The intra-crystal dispersion of CNTs/Al composite materials is achieved, which significantly improves the strength and plastic properties of the material, simplifies the preparation process, and obtains dense and defect-free composite blocks, which are suitable for aerospace and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118951015A_ABST
    Figure CN118951015A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a carbon nano tube reinforced aluminum-based composite material through heat treatment of matrix powder, the composite material powder specifically comprises metal matrix powder and a reinforcement body, the reinforcement body is generally a one-dimensional or two-dimensional reinforcement body, and a matrix has good plastic deformation capacity and has a work hardening phenomenon in the ball milling process. Vacuum heat treatment is carried out according to the specific state of matrix powder in the high-energy ball milling process, the purposes of further improving the content of intragranular reinforcements and optimizing distribution of the reinforcements are achieved, and the intragranular reinforced metal matrix composite is obtained. Taking the carbon nanotube reinforced aluminum matrix composite (CNTs / Al) prepared by the heat treatment process as an example, the powder-state CNTs are uniformly distributed, and compared with a composite obtained in a traditional heat treatment process, the strength and plasticity of the obtained composite are improved at the same time, the strength is improved by 13.4%, and the plasticity is improved by 57.5%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of preparing intracrystalline reinforced aluminum-based composite materials by powder metallurgy, and in particular relates to a method for preparing carbon nanotube-reinforced aluminum-based composite materials by heat-treating matrix powder. Background Art

[0002] Metal-based composite materials have the properties of strong plasticity, electrical conductivity, thermal conductivity, and corrosion resistance of the matrix material. At the same time, they take advantage of the excellent properties of the reinforcement, such as low density, ultra-high room temperature and high temperature strength and modulus, and excellent electrical conductivity and thermal conductivity, and gradually play an increasingly important role in important national fields. Among them, aluminum-based composite materials are widely used in aerospace, weapons and equipment, etc. due to their light weight and high strength. However, as the service conditions become increasingly harsh, researchers hope to obtain aluminum-based composite materials with better performance. One of the main ways to achieve this goal is to select reinforcements with excellent performance. Since the discovery of carbon nanotubes (CNTs), they have become ideal reinforcements for composite materials because of their excellent mechanical properties such as extremely excellent strength (up to 100GPa) and ultra-high elastic modulus (about 1TPa). Carbon nanotube-reinforced aluminum-based composites are expected to become a new generation of lightweight and high-strength aluminum-based composites because of their excellent room temperature and high temperature mechanical properties.

[0003] At present, the preparation of CNTs / Al composite materials has certain difficulties. Due to the non-coherent interface between CNTs and Al matrix, although CNTs can be dispersed by high-energy ball milling, their distribution is mainly at the boundaries of grains. During the ball milling process, under the high-speed shear and compressive stress of the ball milling ball, the aluminum powder grains gradually become smaller, which will increase the difficulty of CNTs entering the crystal. At the same time, the longer the ball milling time, the greater the degree of damage to the CNTs structure. In addition, there are few studies on the goal of obtaining intracrystalline dispersed CNTs / Al-based composite material powders. In the prepared CNTs / Al powders, CNTs are mainly dispersed at the grain boundaries, which is not conducive to the strong plasticity of CNTs / Al-based composite materials. In order to increase the CNTs content and greatly improve the comprehensive mechanical properties of CNTs / Al, it is urgent to prepare intracrystalline dispersed CNTs / Al composite material powders with high CNTs content and uniform distribution. Summary of the invention

[0004] As a representative of high-energy ball milling, planetary ball milling is suitable for uniform dispersion of high-content reinforcements. In order to increase the content of CNTs entering the grains, the situation that the matrix grains are sharply reduced during the ball milling process, which makes it difficult for CNTs to enter the grains, occurs. The present invention controls the growth of matrix grains and eliminates the influence of powder work hardening by heat treating the ball-milled thick flaky powder. At the same time, the thick flaky powder can continue to deform plastically and has a large surface area, which is conducive to the good dispersion of CNTs. After the heat treatment, CNTs are added on this basis and ball milled to the target time. By regulating the structure of the metal matrix powder, the dispersion ability of CNTs and the possibility of dispersing CNTs into the grains are improved, laying the foundation for the preparation of high-performance CNTs / Al composite materials.

[0005] Specifically, the present invention provides a method for preparing a carbon nanotube-reinforced aluminum-based composite material by heat-treating a matrix powder, comprising: preparing a composite material powder: subjecting a certain amount of a metal matrix powder and a process control agent to a first ball milling for 4 hours, subjecting the ball-milled thick-flaked matrix powder to a high-temperature vacuum heat treatment, and subsequently adding a certain amount of a carbon nanotube reinforcement to a second ball milling for 20 hours to obtain a composite material powder; Forming of composite materials: The composite material powder is plasma sintered and then hot extruded to obtain a composite material rod with a smooth surface and no cracks.

[0006] Specifically, the content of carbon nanotubes in the composite material is 2 wt.%, and the content of the metal matrix powder is 98 wt.%.

[0007] Specifically, the metal powder is 45 μm spherical pure aluminum powder, the carbon nanotube reinforcement has a tube diameter of 20 nm and a length of 2 μm, and the process control agent is stearic acid, which accounts for 1 wt.% of the total amount of the composite material powder.

[0008] Specifically, the parameters of the first ball milling and the second ball milling are as follows: the rotation speed is 180-230 rpm / min, the ball milling mode is forward rotation for 10 min, stop for 10 min, reverse rotation for 10 min, and the cycle is performed in sequence. During the ball milling process, when the effective ball milling time reaches 2 h, stop for another 1 h, and the ambient temperature is below 20°C.

[0009] Specifically, the temperature of the high-temperature vacuum heat treatment is 550° C., and the holding time is 12 hours.

[0010] Specifically, during the plasma sintering process, a pre-pressing pressure of 0.5T is first used, the pressure is maintained for no less than 10min, and the vacuum degree is 1.5×10 -1 Pa, temperature is 590℃.

[0011] Specifically, the temperature of the hot extrusion process is 500° C., the holding time is 20 min, the extrusion ratio is 18:1, and the extrusion speed is 4 mm / s.

[0012] Compared with the prior art, the present invention has the following beneficial technical effects: (1) The preparation process of the intracrystalline reinforcement composite material powder prepared by the present invention is simple and easy to operate, the obtained reinforcement is evenly dispersed and well combined with the matrix, and the mechanical properties of the intracrystalline CNTs / Al composite block prepared by the powder metallurgy method have obvious advantages over the traditional annealing heat treatment process; (2) The present invention regulates the organization of the base metal powder during the ball milling process, effectively prevents the oxidation of the powder through vacuum heat treatment combined with sponge titanium, and effectively improves the grain size of the base structure through long-term heat treatment. On the basis of sufficient grain growth, the good dispersion ability of CNTs is maintained. At the same time, the stress of the powder after ball milling is eliminated, which is conducive to the subsequent ball milling process. CNTs can more easily enter the interior of the large grains. Subsequently, the SPS sintering process further eliminates the process control agent (stearic acid) added in the ball milling process, and the hot extrusion process is combined to further densify the organization, and finally a dense and defect-free composite material block is obtained.

[0013] (3) The intracrystalline CNTs / Al composite material prepared by the present invention has significantly better strength-plasticity matching than the traditional stress relief annealing. After adding the designed heat treatment process, compared with the traditional powder heat treatment stress relief process, the designed process has significantly improved the strength and plasticity of the composite block prepared by the traditional method when the effective ball milling time of the CNTs / Al composite powder is 4 hours less. The strength is increased by 13.4% and the plasticity is increased by 57.5%. The patent of the present invention has guiding significance for the stress relief annealing process of the ball milling process and the preparation of high-performance aluminum-based composite materials, so that aluminum-based composite materials have good application prospects in the fields of aerospace, weapons and equipment, transportation, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 This is a schematic diagram of the process of preparing CNTs / Al composite material powder in Example 1 of the present invention; Figure 2 The following are scanning photos of the powder morphology and CNTs distribution of the intracrystalline CNTs / Al composite material prepared in Example 1 of the present invention, wherein (a) is the powder morphology of pure aluminum after ball milling for 4 hours, heat treatment and ball milling again for 20 hours, (b) is the dispersion state of CNTs after pure aluminum is ball milled for 4 hours, heat treatment and ball milling again for 20 hours, (c) is the powder morphology of the CNTs / Al composite material after ball milling for 4 hours, heat treatment and ball milling again for 20 hours, and (d) is the dispersion state of CNTs after the CNTs / Al composite material is ball milled for 4 hours, heat treatment and ball milling again for 20 hours; Figure 3 XRD phase analysis spectrum of the intracrystalline CNTs / Al composite material powder prepared in Example 1 of the present invention before and after heat treatment; Figure 4 TEM data of the change in the grain structure of the matrix powder before and after heat treatment in Example 1 of the present invention, wherein (a) is the TEM bright field phase of the thick flaky pure aluminum powder ball-milled for 4 hours before heat treatment, (b) is the corresponding diffraction pattern of the thick flaky pure aluminum powder ball-milled for 4 hours before heat treatment, (c) is the dark field pattern of the thick flaky pure aluminum powder ball-milled for 4 hours before heat treatment, (d) is the TEM bright field phase of the thick flaky pure aluminum powder ball-milled for 4 hours after heat treatment, (e) is the corresponding diffraction pattern of the thick flaky pure aluminum powder ball-milled for 4 hours after heat treatment, and (f) is the dark field pattern of the thick flaky pure aluminum powder ball-milled for 4 hours after heat treatment; Figure 5 Mechanical property data of 2 wt.% CNTs / Al composite block prepared in Example 1 of the present invention and the control group. DETAILED DESCRIPTION

[0015] In order to make the purpose, technical solution and advantages of the embodiments of the present disclosure clearer, the technical solution of the embodiments of the present disclosure will be clearly and completely described below in conjunction with the accompanying drawings. Obviously, the described embodiments are part of the embodiments of the present disclosure, rather than all of the embodiments. Based on the described embodiments of the present disclosure, all other embodiments obtained by those skilled in the art without creative work also fall within the scope of protection of the present disclosure.

[0016] Unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as commonly understood by those skilled in the art to which the subject matter of the present disclosure belongs. It will be further understood that terms such as those defined in commonly used dictionaries should be interpreted as having a meaning consistent with their meaning in the context of the specification and the relevant art, and will not be interpreted in an idealized or overly formal form unless otherwise explicitly defined herein.

[0017] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase "embodiments" in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0018] In view of the problems that the reinforcements in the current powder metallurgy preparation of nano-reinforced metal-based composite materials are easily distributed at the grain boundaries and the performance improvement is limited, combined with the demand for increasing the content of reinforcements in the crystal to further improve the performance of the composite material, combined with the research on ball milling, powder heat treatment, bulk organization and phase composition, tensile properties, etc. of the composite material. The present invention specifically takes the nano-reinforced carbon nanotube (CNTs) reinforced aluminum-based composite material as an example. First, starting from the matrix pure aluminum powder organization, vacuum heat treatment is performed after ball milling to the powder into thick flakes to control the grain size, and then CNTs are added for a long time of ball milling to achieve the uniform dispersion of CNTs and the process of entering the crystal. The prepared CNTs / Al composite powder is sintered and extruded, and the phase composition of the powder and the block and the change of the matrix grains are studied. Finally, the room temperature tensile properties of the CNTs / Al composite material formed under powder metallurgy conditions are studied.

[0019] The present invention provides a method for preparing a carbon nanotube reinforced aluminum-based composite material by heat-treating a matrix powder, comprising: Preparation of composite material powder: a certain amount of metal matrix powder and process control agent are first ball-milled for 4 hours, the thick flake matrix powder after ball milling is subjected to high-temperature vacuum heat treatment, and then a certain amount of carbon nanotube reinforcement is added for secondary ball milling for 20 hours to obtain composite material powder; Forming of composite materials: The composite material powder is plasma sintered and then hot extruded to obtain a composite material rod with a smooth surface and no cracks.

[0020] In the present invention, for the metal matrix powder with a certain plastic deformation ability during the high-energy ball milling process, it is ensured that the metal matrix powder can be deformed into an ellipsoidal or flaky powder through the ball milling process, and the content of the intracrystalline reinforcement is increased by the powder metallurgy method. The principle of improving the comprehensive mechanical properties of the composite material is: by heat treating the matrix metal powder in a specific state (thick flakes in this patent), the grains are significantly grown, which reduces the powder work hardening caused by ball milling on the one hand, so that the ability of the powder to continue to deform is significantly improved. On the other hand, the thick flake powder with a large grain structure has two advantages. One is that the large surface area of ​​the flake powder can improve the dispersion ability of the nano reinforcement, and the other is that the large grains are easier to make the nano reinforcement enter the grain than the small grains during the ball milling process. On this basis, ball milling is carried out, followed by powder metallurgy sintering and hot extrusion processes. The reinforcement is evenly dispersed in the composite material finally obtained, and the possibility of the reinforcement being distributed in the grain is greatly improved, thereby improving the mechanical properties of the composite material.

[0021] The content of carbon nanotubes in the composite material is 2 wt.% by mass, and the content of the metal matrix powder is 98 wt.% by mass.

[0022] In the present invention, the composite material powder is specifically a uniformly dispersed intracrystalline carbon nanotube reinforced aluminum-based composite material powder, the CNTs are uniformly dispersed and well combined with the matrix, the powder is vacuum heat treated and the SPS sintering process controls the sintering temperature, and the reaction amount in the obtained material is low.

[0023] The metal powder is 45 μm spherical pure aluminum powder, the carbon nanotube reinforcement has a tube diameter of 20 nm and a length of 2 μm, and the process control agent is stearic acid, which accounts for 1 wt.% of the total amount of the composite material powder.

[0024] In the present invention, a 500 ml zirconia ball mill is used in the powder processing process. To ensure the ball milling efficiency, the volume of the powder and ball milling balls finally added to the jar does not exceed 50% of the volume of the ball mill. The ball milling balls are added first, followed by the base metal powder and the process control agent. The ball milling balls are made of zirconia, with a size of 10 mm, and the ball-to-material ratio is 5:1.

[0025] The parameters of the first ball milling and the second ball milling are as follows: the rotation speed is 180-230 rpm / min, the ball milling mode is forward rotation for 10 minutes, stop for 10 minutes, reverse rotation for 10 minutes, and the cycle is performed in sequence. During the ball milling process, when the effective ball milling time reaches 2 hours, stop for another hour, and the ambient temperature is below 20°C.

[0026] In the present invention, during the ball milling process, the zirconia ball milling jar that has been loaded with base metal powder, process control agent and ball milling balls is sealed, and the air is discharged by filling high-purity argon gas into the ball milling jar using the characteristic that the density of argon gas is greater than that of air. The specific process is to first open the outlet valve to ensure that the gas path is normal, adjust the gas flow rate to 1.0 L / min, and introduce argon gas into the air inlet to ensure that the ventilation time is not less than 8 minutes; when stopping the air intake, first close the air inlet valve and then close the air outlet valve. The relatively low gas flow rate in the above operation is conducive to the slow discharge of air by the argon protective gas, and will not cause a reduction in the quality of the powder.

[0027] The goal of the heat treatment is to grow the metal matrix grains and to allow the carbon nanotube reinforcement to enter the interior of the grains during the secondary ball milling process.

[0028] In the present invention, vacuum heat treatment is performed on the matrix powder ball-milled to a thick sheet shape. The setting principle of the heat treatment temperature is: to remove the ball milling stress, the temperature shall not be lower than the annealing temperature of the material. If the material contains a reinforcement, the temperature shall not be higher than the reaction temperature of the matrix material and the reinforcement, and shall not be lower than the volatilization temperature of the process control agent. In the subsequent continuous ball milling, a quantitative process control agent needs to be added again to keep the amount added each time the same and to facilitate the realization of repeated experiments. At the same time, sponge titanium is placed around the powder during the heat treatment process to prevent the powder from being oxidized. The target state after heat treatment is that the matrix grains grow up, which is conducive to the reinforcement entering the interior of the grains during the subsequent ball milling process.

[0029] The temperature of high temperature vacuum heat treatment is 550℃, and the holding time is 12h.

[0030] During plasma sintering, a pre-pressing pressure of 0.5T is used, the pressure is maintained for no less than 10min, and the vacuum degree is 1.5×10 -1 Pa, temperature is 590℃.

[0031] In the present invention, during the sintering process, the composite material powder obtained after ball milling is loaded into a graphite mold with a diameter of 29.5 mm, and pre-pressed with a pressure of 0.5 T, and the pressure holding time is not less than 10 minutes, and then the outside of the graphite mold is wrapped with high-temperature resistant fiber felt to play a role in heat preservation of the mold during the sintering process. The graphite mold is loaded into a plasma sintering equipment furnace for sintering; the temperature is quickly raised to the target sintering temperature of 590 ° C, the pressure is increased to 2.2 T (30 MPa), and the vacuum degree is 1.5×10 -1 Pa, holding time 30min, a dense cylindrical block was obtained. The temperature during the sintering process was measured using a K-type thermocouple contact temperature measurement to ensure the sensitivity and accuracy of the temperature test.

[0032] The temperature of the hot extrusion process was 500 °C, the holding time was 20 min, the extrusion ratio was 18:1, and the extrusion speed was 4 mm / s.

[0033] In the present invention, during the hot extrusion process, the surface of the sample is first polished with sandpaper to remove the oxide scale, high-temperature grease is applied to the inner wall of the extrusion die and the sleeve, the sample is kept warm at 500°C for 20 minutes in a box furnace, and then immediately placed in an extrusion device preheated at 370°C, with an extrusion ratio of 18:1 and an extrusion speed of 4 mm / s, and finally a composite material extruded rod with a diameter of 7 mm and a smooth surface without cracks is obtained.

[0034] In the following embodiments, the powder of carbon nanotubes reinforced aluminum-based composite material (CNTs / Al) distributed in the crystal is used as an example for explanation.

[0035] Raw materials, planetary ball milling, plasma sintering, hot extrusion and performance testing equipment used in the following examples: The intra-crystalline and grain boundary composite material powders were prepared using a German Pulverisette 5 planetary ball mill. The composite material blocks in SPS state were prepared using Shanghai Chenhua SPS-20T-10-ⅠⅠⅠⅠ plasma sintering equipment; The sintered block samples were subjected to vacuum heat treatment using Henan Chengyi's 1200℃ vacuum heat treatment tube furnace. Ningbo Pavol vertical hot extrusion equipment YP61-315 is used for the hot extrusion process of sintered samples; The powder morphology and internal morphology were characterized using the German ZEISS Sigma 300; The powder and bulk TEM analysis and characterization were performed using the American FEI Talos F200X high-resolution transmission equipment; The powder was subjected to XRD characterization analysis using a D8 Discover X-ray diffractometer; The tensile properties of the extruded intracrystalline and grain boundary distributed CNTs / Al composites were tested using an American INSTRON 3382 electronic universal testing machine. The powder used was 45 micron spherical pure Al powder prepared by Shanghai Buwei Company, the CNTs powder used multi-walled carbon nanotubes (Baytubes C150P), and the stearic acid was produced by Macklin Company with the chemical formula of C 18 H 36 O2.

[0036] In the following examples, high-energy ball milling is used. The ball milling process first changes the morphology of the matrix powder to obtain a larger surface area, which can disperse CNTs more efficiently. At the same time, a vacuum heat treatment process is combined to remove the ball milling stress and make the matrix grains grow, thereby improving the ability of CNTs to enter the grains. The ball milling is repeated to the target time to obtain CNTs / Al powder with good CNT dispersion. The powder is then sintered, and finally the block is further densified by hot extrusion, and finally a composite material rod without obvious defects and dense is obtained. Example 1

[0037] In this embodiment, the preparation method of the intracrystalline CNTs / Al composite material includes high-energy ball milling combined with vacuum heat treatment to improve the metal matrix structure, and then adding CNTs to further improve the dispersion ability of CNTs while increasing the possibility of CNTs entering the crystal, and then sintering and extruding the prepared CNTs / Al composite powder to finally obtain a composite material block. On the other hand, the composite material powder is directly heat treated, the powder is annealed, and then ball milled again as a control group of the present invention, and the composite material powder prepared by ball milling is also sintered and hot extruded.

[0038] The specific method for preparing high-content CNTs / Al composite material powder comprises the following steps: Step 101, powder proportioning and ball milling: A total of 117.6 grams of 45 micron spherical pure aluminum powder was loaded into the ball mill.

[0039] Powder ratio: the content of spherical pure Al powder with a particle size of 45 μm is 98 wt.%, the amount of stearic acid added is 1 wt.%, and the ball milling ball is a zirconia ball with a diameter of 10 mm, and the ball-to-material ratio is 5:1.

[0040] In the above preparation process, in step 1, the order of loading the materials into the tank is to add the ball milling balls first, then add the pure aluminum powder and stearic acid particles evenly at the same time, and stir evenly with a spoon to make the initial CNTs and Al powder and stearic acid particles pre-mixed evenly.

[0041] In order to compare and illustrate the superiority of this patent, traditional stress relief annealing was used for preparation and comparison. Pure aluminum, 2wt.% CNTs and 1wt.% stearic acid were added during the initial ball milling process, and the operation method was consistent with the designed process.

[0042] Step 102, ball milling process and parameter design: First, open the outlet valve to ensure that the gas path is normal, adjust the gas flow rate to 1.0 L / min, and introduce argon gas into the air inlet to ensure that the ventilation time is not less than 8 minutes; when stopping the air intake, first close the air inlet valve, and then close the outlet valve. The relatively low gas flow rate in the above operation is conducive to the slow exhaust of air by the argon protective gas, and will not cause a decrease in the quality of the powder.

[0043] The ball milling parameters are set to a speed of 200 rpm / min, and the ball milling method is forward rotation for 10 min, stop for 10 min, reverse rotation for 10 min, and then cycle in sequence. In order to avoid chemical reactions caused by excessive temperature in the ball mill, on the one hand, when the effective ball milling time reaches 2 h, a stop time of 1 h is added to allow the ball mill to cool fully, and on the other hand, the ambient temperature is controlled below 20°C to ensure that the temperature is consistent each time the ball mill is started. When the base powder is ball milled to a thick flake (4h in this patent), the base powder is taken out for vacuum heat treatment.

[0044] In addition, the control group is CNTs / Al composite material powder, and the argon filling and ball milling parameters are consistent with the design patent. After ball milling for 4 hours, the composite material is also powdered and prepared for vacuum heat treatment operation.

[0045] Step 103, powder vacuum heat treatment process: Pure aluminum was ball-milled for 4 hours to form thick slices. 1 g of powder was taken out at this stage and after heat treatment for morphological characterization analysis. Note that the powder should be prevented from direct contact with air during the powder collection process, and the operation should be completed in a glove box. The vacuum heat treatment temperature was 550°C, the holding time was 12 hours, and then the furnace was cooled. At the same time, 20 g of sponge titanium was placed in advance next to the heat-treated powder to further prevent the powder from being oxidized.

[0046] As a further explanation of the present invention, in order to highlight the material performance advantages of this design scheme, a control group is used for illustration. The design process of the control group in this step is as follows: the thick sheet CNTs / Al composite material powder that has been ball-milled for 4 hours is also heat-treated, and the parameter selection and steps are consistent with the above-mentioned design process.

[0047] Step 104, continue high-energy ball milling on the heat-treated powder: After heat treatment of the pure aluminum powder after ball milling for 4 hours, the Al grains have grown and are added to the ball mill again. A process control agent (stearic acid) at a content of 1wt% is added, followed by ball milling at a speed of 200rpm / min and a ball milling time of 20h. Together with the initial 4h ball milling time for pure aluminum, the total effective ball milling time is 24h.

[0048] As a further explanation of the present invention, in order to highlight the material performance advantages of the present design, a control group is used for illustration. The design process of the control group in this step is as follows: after the CNTs / Al composite material powder is ball-milled for 4 hours, it is heat-treated and then added to the ball mill again, and a process control agent (stearic acid) with a content of 1wt% is added, followed by ball milling. The ball milling speed is 200rpm / min and the ball milling time is 20 hours. Together with the initial 4 hours of ball milling of the CNTs / Al composite material powder, the total effective ball milling time is 28 hours.

[0049] The whole ball milling process flow chart is as follows: Figure 1 As shown, it can be seen that the process designed in this patent is for the matrix powder, and CNTs are added after its structure is optimized and adjusted. Specifically, the powder is ball-milled to a certain thickness and then vacuum heat treated. This process can make the grains grow and eliminate the ball-milling stress, which helps the CNTs to further disperse and enter the crystal.

[0050] The morphology analysis of the intracrystalline CNTs / Al composite material powder prepared by ball milling in this example is as follows: The morphology of the composite powders obtained at different ball milling times was characterized by SEM scanning. Figure 2 The powder morphology of CNTs / Al composite material obtained by the process designed in Example 1 and the final ball milling state of the control group, wherein Figure 2(a) and (b) respectively represent the powder morphology of the designed pure aluminum after ball milling for 4 hours, heat treatment and ball milling again for 20 hours and the dispersion state of CNTs. Figure 2 (c) and (d) show the morphology and CNTs dispersion state of the control group CNTs / Al composite material after ball milling for 4 hours, heat treatment and ball milling for another 20 hours. It can be seen that the morphology of both powders is flaky powder. After magnifying the local surface, a small amount of dispersed CNTs can be found on the surface of the powder, and the remaining CNTs have been buried in the matrix powder during the ball milling process.

[0051] Step 105, high content CNTs / Al composite material powder spark plasma sintering process: The composite material powder obtained after ball milling was loaded into a graphite mold with a diameter of 30, and pre-pressed with a pressure of 0.5T, and the pressure was maintained for no less than 10min. Then the mold was loaded into the plasma sintering equipment furnace for sintering. The sintering temperature was 590℃, the pressure was 30MPa, and the vacuum degree was 1.5×10 -1 Pa, and the holding time is 30min, so that the sample can be densified. The temperature is measured by contact temperature measurement using a K-type thermocouple to ensure the accuracy of the temperature.

[0052] Step 106, hot extrusion process: The powder obtained by ball-milling the pure aluminum for 4 hours, vacuum heat treatment, and then ball-milling for 20 hours in step 105 is sintered, and the obtained block composite material sample and the control group (the composite material is ball-milled for 4 hours, heat-treated, and then ball-milled for 20 hours and sintered) are hot extruded. The surface of the extruded sample is first polished with a sanding machine to remove the outer oxide scale. The sample is then kept at 500°C in a box furnace for 20 minutes, and then placed in an extrusion equipment preheated at 370°C. The extrusion ratio is 18:1 and the extrusion speed is 4 mm / s. Finally, a composite material extruded rod with a diameter of 7 mm and a smooth surface without cracks is obtained.

[0053] In the above-mentioned forming process, in step 106, in the sample, the control group, i.e., the initial state, is the composite material powder, and the sheet of ball milling for 4 hours is heat treated and ball milled again to prepare the powder, and the composite material block is obtained through the sintering and extrusion process, and the yield strength average value is 133.7MPa, the tensile strength average value is 168.2MPa, and the elongation at break average value is 10.0%. The performance of the intracrystalline CNTs / Al composite material designed in this patent is that the yield strength averages 142.9MPa, the tensile strength average value is 183.7MPa, and the elongation at break average value is 15.3%. The specific data are shown in Table 1. It can be seen that although the ball milling time experienced by the composite material powder after adding CNTs in the designed ball milling process is only 20h, its strength and plasticity are significantly higher than the performance of the composite material powder after heat treatment annealing, and the preparation process of the intracrystalline CNTs / Al composite material designed in this patent has obvious advantages.

[0054] Table 1 Mechanical properties of intracrystalline CNTs / Al composites and control group Material Name Yield strength (MPa) Tensile strength (MPa) Elongation at break (%) Control group 133.7±5.7 168.2±2.1 10.0±0.6 Intracrystalline CNTs / Al 142.9±7.5 183.7±9.5 15.3±1.4 The following tests and analyses were performed on the intracrystalline CNTs / Al composite material powder prepared by vacuum heat treatment, plasma sintering, and hot extrusion in this embodiment: (1) Characterization of phase change of pure aluminum before and after heat treatment Figure 3 This is the XRD characterization spectrum of pure aluminum powder before and after vacuum heat treatment after ball milling for 4 hours. No obvious alumina peak was found through calibration, indicating that the powder did not undergo obvious oxidation, verifying the stability of the vacuum heat treatment process. At the same time, the peak position after heat treatment shifted slightly to the left compared with before heat treatment. The decrease in the θ angle indicates an increase in the interplanar spacing d, which may be due to the presence of large compressive stress in the powder after ball milling, resulting in a decrease in the lattice spacing. After heat treatment, the internal stress of the powder is removed, and the interplanar spacing d increases, which leads to a decrease in the θ angle, verifying that the internal stress of the powder is fully removed.

[0055] (2) Characterization of grain changes before and after heat treatment of pure aluminum Combining the XRD results and TEM analysis of the powder, the changes in the matrix powder grains were characterized. First, the grain size was statistically analyzed using the Scherrer formula through the XRD spectrum, and the results are shown in Table 2. It can be seen that the grain sizes of the powder grains obtained from different crystal planes after heat treatment are significantly improved, indicating that the matrix grains have grown significantly.

[0056] Table 2 Statistics of grain size of pure aluminum powder before and after heat treatment Statistical crystal plane Before heat treatment After heat treatment (111) 585 988 (200) 533 997 (220) 455 947 (311) 417 973 average 497.5±74.7 976.3±21.9 On the other hand, the changes in grain size can be directly observed through TEM data, e.g. Figure 4The TEM bright field phase and corresponding diffraction and dark field images of thick flake pure aluminum powder ball-milled for 4 hours before and after heat treatment are shown, where (ac) is before heat treatment and (df) is after heat treatment. By performing selected area electron diffraction on the circled areas in (a) and (b), it is found that the diffraction spots of the powder before heat treatment are polycrystalline rings, indicating that the area is mainly polycrystalline and the grains are small, as can be seen in Figure (c). And from Figure (e), it can be seen that the diffraction of the same size area after heat treatment is a set of diffraction spots, indicating that there is basically only one grain in this area, proving the obvious growth of the grains. At the same time, the dark field operation of the diffraction spots in the set shows that the grain size that lights up is very large, which further verifies the realization of the heat treatment plan goal.

[0057] (3) Mechanical and room temperature properties test of intracrystalline CNTs / Al composites The room temperature tensile properties of the designed and prepared intracrystalline CNTs / Al composite materials and the control group were tested. The engineering stress-strain results are shown in Figure 5 As shown, it can be seen that after the process designed by this patent, the strength and plasticity of the material are significantly improved compared with the composite material obtained by traditional stress relief annealing, proving that the invention has a good effect on the improvement of the initial metal matrix grains, the method of selecting a thick sheet state for heat treatment and then adding CNTs for ball milling to prepare composite material powder. On the other hand, the total ball milling time for the CNTs / Al composite material powder in the control group is 24h, while the ball milling time for the CNTs / Al composite material powder designed by this patent is 20h, and the strength and plasticity are further improved in a shorter time, which not only saves time cost, but also increases the possibility of CNTs entering the crystal. This method provides ideas for obtaining metal-based composite materials with intracrystalline reinforcements, and is expected to obtain nano-reinforced metal-based composite materials with excellent comprehensive mechanical properties, which can meet the application of composite materials in important national fields such as aerospace, weapons and armaments.

[0058] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention.

Claims

1. A method for preparing a carbon nanotube-reinforced aluminum-based composite material by heat treating a matrix powder, characterized in that: include: Preparation of composite material powder: a certain amount of metal matrix powder and process control agent are first ball-milled for 4 h, the thick flake matrix powder after ball milling is subjected to high temperature vacuum heat treatment, and then a certain amount of carbon nanotube reinforcement is added for secondary ball milling for 20 h to obtain composite material powder; Forming of the composite material: The composite material powder is subjected to plasma sintering and then hot extrusion to obtain a composite material rod with a smooth surface and no cracks.

2. The method for preparing carbon nanotube reinforced aluminum-based composite materials by heat treatment ball milling according to claim 1, characterized in that: The content of carbon nanotubes in the composite material is 2 wt.%, and the content of the metal matrix powder is 98 wt.%.

3. The method for preparing carbon nanotube reinforced aluminum-based composite materials by heat treatment ball milling according to claim 1, characterized in that: The metal powder is 45 μm spherical pure aluminum powder, the carbon nanotube reinforcement is a tube with a diameter of 20 nm and a length of 2 μm, and the process control agent is stearic acid, which accounts for 1 wt.% of the total amount of the composite material powder.

4. The method for preparing carbon nanotube reinforced aluminum-based composite materials by heat treatment ball milling according to claim 1, characterized in that: The parameters of the first ball milling and the second ball milling are as follows: the rotation speed is 180-230 rpm / min, the ball milling mode is forward rotation for 10 minutes, stop for 10 minutes, reverse rotation for 10 minutes, and the cycle is performed in sequence. During the ball milling process, when the effective ball milling time reaches 2 hours, stop for another hour, and the ambient temperature is below 20°C.

5. The method for preparing carbon nanotube reinforced aluminum-based composite materials by heat treatment ball milling according to claim 1, characterized in that: The temperature of the high temperature vacuum heat treatment is 550° C., and the holding time is 12 h.

6. The method for preparing carbon nanotube reinforced aluminum-based composite materials by heat treatment and ball milling according to claim 1, characterized in that: During the plasma sintering process, a pre-pressing pressure of 0.5 T is first used, and the pressure is maintained for no less than 10 min. The vacuum degree is 1.5×10 -1 Pa, the temperature is 590℃.

7. The method for preparing carbon nanotube reinforced aluminum-based composite materials by heat treatment and ball milling according to claim 1, characterized in that: The temperature of the hot extrusion process is 500° C., the holding time is 20 min, the extrusion ratio is 18:1, and the extrusion speed is 4 mm / s.