Method for preparing high-content carbon nanotube reinforced aluminum-based composite material through heat treatment circulating ball milling
By using a heat treatment cyclic ball milling method combined with vacuum heat treatment and plasma sintering, the problems of carbon nanotube dispersion and interfacial bonding in aluminum matrix composites were solved, and high-performance aluminum matrix composites were prepared to meet the application needs of aerospace and other fields.
Patent Information
- Application Number
- CN202411179740.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-15
AI Technical Summary
Existing technologies struggle to effectively disperse high-content carbon nanotubes and improve their interfacial bonding strength with the aluminum matrix, resulting in insufficient strength-plasticity matching in aluminum-based composite materials.
A high-carbon nanotube-reinforced aluminum matrix composite material was prepared by using a heat treatment cyclic ball milling method, which combines vacuum heat treatment and plasma sintering with hot extrusion. The process includes initial ball milling, vacuum heat treatment, secondary ball milling, and final sintering and extrusion, thereby improving the interfacial bonding and dispersion between the reinforcement and the matrix.
It significantly improves the strength-plasticity matching performance of carbon nanotube-reinforced aluminum matrix composites, with uniform reinforcement dispersion, tight interfacial bonding, and excellent mechanical properties, making it suitable for aerospace, weaponry, and transportation fields.
Smart Images

Figure CN118951016A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of preparing nano-reinforced aluminum-based composite materials by powder metallurgy, and in particular relates to a method for preparing high-content carbon nanotube-reinforced aluminum-based composite materials by heat treatment and cyclic ball milling. Background Art
[0002] As the most abundant metal element in the earth's crust, aluminum has been widely used in many fields. Metal materials represented by aluminum and its alloys have good strength and plasticity, heat resistance and corrosion resistance, electrical conductivity and thermal conductivity, and are widely used in important national fields such as transportation, national defense science and technology. However, as the requirements for service conditions gradually increase, people expect to obtain materials with better comprehensive performance while maintaining light weight. Aluminum-based composite materials utilize the excellent characteristics of the reinforcement while maintaining the characteristics of the matrix light weight and good plasticity, and have the potential to prepare high-performance strong plastic lightweight materials. The key to determining the performance of aluminum-based composite materials is the selection of excellent reinforcements. Since the discovery of carbon nanotubes in 1991, they have become a popular reinforcement for aluminum-based composite materials because of their extremely high strength (~100GPa), elastic modulus (~1TPa), and excellent electrical conductivity and thermal conductivity. It has received extensive attention and research at home and abroad. Carbon nanotube-reinforced aluminum-based composites have excellent comprehensive mechanical properties and are expected to become a new generation of lightweight and high-strength aluminum-based composite materials.
[0003] There are many methods for preparing carbon nanotube reinforced aluminum-based composites, such as powder metallurgy, stir friction, additive manufacturing, etc. Among them, powder metallurgy has become the main preparation method for aluminum-based composites due to its good reinforcement dispersion and the advantages of controlling interface reaction. At present, there are some difficulties in preparing carbon nanotube reinforced aluminum-based composites. On the one hand, due to its intrinsic characteristics, such as large aspect ratio and high specific surface area, carbon nanotubes are easy to agglomerate under the action of van der Waals force, and it is difficult to further disperse when the content is high. On the other hand, the improvement of the interface bonding strength between the reinforcement and the matrix is closely related to whether the load transfer mechanism of carbon nanotubes can be exerted. Therefore, how to further increase the content of dispersed carbon nanotubes and improve the interface bonding strength is of great significance for the acquisition of high-performance aluminum-based composites.
[0004] In the process of ball milling, the matrix powder of carbon nanotube reinforced aluminum matrix composite materials will inevitably undergo work hardening. These powders that are difficult to continue to plastically deform are very unfavorable for the dispersion of reinforcements. The final composite block cannot achieve a good strength-plasticity matching target due to the presence of reinforcement agglomeration. Therefore, how to further start the plastic deformation process in the powder that has already dispersed reinforcements and has undergone work hardening, so that it has the ability to further disperse reinforcements, is of great significance for obtaining high-content reinforcement composite material powders. Summary of the invention
[0005] The planetary ball milling process has a high energy input, and the reinforcements are easily dispersed evenly into the matrix under the impact and shear force of the ball milling balls. However, the work hardening of the matrix material during the ball milling deformation process is not conducive to the further dispersion of the reinforcements, resulting in the high-content reinforcements being prone to agglomeration. The present invention combines vacuum heat treatment of a specific granular powder state to improve the work hardening phenomenon while improving the interface bonding between the reinforcement and the matrix. The powder is allowed to further plastically deform and disperse the reinforcements, thereby increasing the content of the reinforcements, which has obvious advantages for preparing composite materials with high-content reinforcements. This method can lay the foundation for preparing high-energy composite materials.
[0006] Specifically, the present invention provides a method for preparing a high-content carbon nanotube-reinforced aluminum-based composite material by heat treatment and cyclic ball milling, comprising: Preparation of composite material powder: a certain amount of matrix aluminum powder and process control agent are subjected to primary ball milling, and then carbon nanotube reinforcement is added for the first time to obtain composite material powder, the composite material powder is subjected to high-energy ball milling for the first time for 24 hours, vacuum heat treatment is performed after the powder is in the form of cold-welded particles, and then carbon nanotube reinforcement is added again, and secondary high-energy ball milling is performed for 34 hours to obtain high-content carbon nanotube-reinforced aluminum-based composite material powder; Forming of the composite material: Plasma sintering of the high-content carbon nanotube-reinforced aluminum-based composite material powder is followed by hot extrusion to obtain a composite material rod with a smooth surface and no cracks.
[0007] Specifically, the carbon nanotube content in the composite material is 4 wt.%, and the aluminum powder content in the composite material is 96 wt.%.
[0008] Specifically, the content of the carbon nanotube reinforcement added for the first time in the composite material powder is 3 wt.% by mass, and the content of the carbon nanotube reinforcement added again in the high-content carbon nanotube-reinforced aluminum-based composite material powder is 1 wt.% by mass.
[0009] Specifically, the aluminum powder is 45 μm spherical pure aluminum powder, and the carbon nanotube reinforcement has a tube diameter of 20 nm and a length of 2 μm.
[0010] Specifically, the time for the initial ball milling of the matrix aluminum powder and the process control agent is 4 hours, the ball mill speed for the first high-energy ball milling and the second high-energy ball milling after adding the carbon nanotube reinforcement is 180-230 rpm / min, the ball milling method is forward rotation for 10 minutes, stop for 20 minutes, and reverse rotation for 10 minutes; the ambient temperature is below 25°C.
[0011] Specifically, the temperature of the vacuum heat treatment is 550° C., the heat preservation time is 12 hours, and the vacuum heat treatment is followed by furnace cooling, and the powder is taken out after the temperature is lower than 30° C.
[0012] Specifically, during the vacuum heat treatment, 10 to 20 g of titanium sponge is placed next to the composite material powder in advance.
[0013] Specifically, the vacuum degree of the plasma sintering is 1.5×10 -1 Pa, the sintering temperature is 590 °C, and the sintering process is kept at 450 °C to remove stearic acid.
[0014] Specifically, the temperature of the hot extrusion process is 500° C., the holding time is 20 min, the extrusion ratio is 18:1, and the extrusion speed is 4 mm / s.
[0015] Compared with the prior art, the present invention has the following beneficial technical effects: (1) The preparation process of the high-content nano-reinforced metal-based composite powder of the present invention is simple and easy to operate, the obtained nano-reinforcement content is high, the dispersion is uniform, and the combination with the matrix is good, and the ball milling time is effectively extended to achieve uniform dispersion of the reinforcement. The mechanical properties of the high-content CNTs / Al composite block prepared by the powder metallurgy method are significantly superior to those of the composite material prepared by traditional ball milling without annealing heat treatment process.
[0016] (2) The present invention regulates the organization of the composite powder during the ball milling process, effectively prevents the oxidation of the powder by vacuum heat treatment combined with titanium sponge, and effectively removes stress by long-term heat treatment, restores the ability of the powder to plastic deformation, so that the composite powder has the ability to further disperse CNTs. At the same time, after the powder is heat treated, the CNTs and the Al matrix are more tightly bonded, and then the SPS sintering process further eliminates the process control agent (stearic acid) added in the ball milling process, and the hot extrusion process is combined to further densify the organization, and finally obtain a dense and defect-free high-content CNTs / Al composite block. The coarse grains of the matrix in the organization form an effective network connection feature, which can effectively reduce the stress concentration phenomenon during the plastic deformation process.
[0017] (3) The high-content CNTs / Al composite material prepared by the present invention has significantly better strength-plasticity matching than the conventional ball-milled high-content CNTs / Al composite material without heat treatment. After adding the designed heat treatment process, the plasticity of the composite material is greatly improved while maintaining the strength, and the plasticity improvement can reach 79.5% compared with the conventional powder-free heat treatment process. The present invention patent has guiding significance for further increasing the content of dispersed reinforcement in the ball milling process to prepare high-performance aluminum-based composite materials, so that aluminum-based composite materials have good application prospects in the fields of aerospace, weapons and equipment, transportation, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 This is a schematic diagram of the process for preparing the high-content CNTs / Al composite material powder designed in Example 1 of the present invention; Figure 2 Scanning photos of the powder morphology and CNTs distribution of high-content CNTs / Al composite materials prepared by the process of Example 11 of the present invention and the control group 1, wherein (a) is the powder morphology of pure aluminum ball milling for 4h + 3% CNTs@BM24h, (b) is the powder morphology of pure aluminum ball milling for 4h + 3% CNTs@BM24h + HT + 1% CNTs@BM34h, (c) is the enlarged morphology of the powder in (b), (d) is the powder morphology of pure aluminum ball milling for 4h + 1% CNTs@BM24h, (e) is the powder morphology of pure aluminum ball milling for 4h + 1% CNTs@BM24h + HT + 3% CNTs@BM34h, and (f) is the enlarged morphology of the powder in (e); Figure 3 XRD phase analysis spectra of high-content CNTs / Al composite powders prepared by the process of Example 1 and Control Group 1 of the present invention before and after ball milling and heat treatment; Figure 4 XRD phase analysis spectrum of the composite material extruded bulk prepared by the process of Example 1 and Control Group 1 of the present invention; Figure 5 EBSD band contrast images of the composite material extruded bulk prepared by the process of Example 1 and Control Group 1 of the present invention, wherein (a) is the EBSD band contrast image of the composite material extruded bulk prepared by Example 1, and (b) is the EBSD band contrast image of the composite material extruded bulk prepared by Control Group 1; Figure 6 Engineering stress-strain curves of extruded blocks of 4 wt.% CNTs / Al composite materials prepared by the processes of Example 1 and Control Groups 1 and 2 of the present invention. DETAILED DESCRIPTION
[0019] In order to make the purpose, technical solution and advantages of the embodiments of the present disclosure clearer, the technical solution of the embodiments of the present disclosure will be clearly and completely described below in conjunction with the accompanying drawings. Obviously, the described embodiments are part of the embodiments of the present disclosure, rather than all of the embodiments. Based on the described embodiments of the present disclosure, all other embodiments obtained by those skilled in the art without creative work also fall within the scope of protection of the present disclosure.
[0020] Unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as commonly understood by those skilled in the art to which the subject matter of the present disclosure belongs. It will be further understood that terms such as those defined in commonly used dictionaries should be interpreted as having a meaning consistent with their meaning in the context of the specification and the relevant art, and will not be interpreted in an idealized or overly formal form unless otherwise explicitly defined herein.
[0021] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase "embodiments" in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0022] In view of the problems that the powder in the high-energy ball milling process has work hardening that inhibits plastic deformation, the dispersion content of the reinforcement needs to be improved, and the ball milling time needs to be further extended, combined with the problems of low dispersion content of nano-level reinforcements and weak interface bonding, the present invention specifically takes nano-reinforced carbon nanotube (CNTs) reinforced aluminum-based composite material as an example through research on the ball milling, powder heat treatment, bulk organization and phase composition, tensile properties and the like of composite materials. First, the powder is ground into a flake shape, and the large surface area is used to improve the dispersion ability of the reinforcement. Then, the composite material powder is ball milled into a granular state after cold welding. At this time, the powder has obvious work hardening phenomenon and cannot be effectively plastically deformed. At this time, a vacuum heat treatment process is added to perform stress relief annealing on the powder while improving the interface bonding between the reinforcement and the matrix. Then, reinforcements are further added. Since the plastic deformation ability of the powder is restarted, the newly added reinforcements can be further effectively dispersed with the plastic deformation of the composite material powder. The prepared CNTs / Al composite material powder was sintered and extruded by a specific process, and the phase composition of the powder and block and the changes in the matrix grains were studied. Finally, the room temperature tensile properties of the high-content CNTs / Al composite material formed under powder metallurgy conditions were studied.
[0023] The present invention provides a method for preparing a high-content carbon nanotube-reinforced aluminum-based composite material by heat treatment cycle ball milling, comprising: preparing composite material powder: subjecting a certain amount of matrix aluminum powder and a process control agent to initial ball milling, and then adding a carbon nanotube reinforcement for the first time to obtain composite material powder, subjecting the composite material powder to initial high-energy ball milling for 24 hours, subjecting the powder to vacuum heat treatment after it is in a cold-welded granular state, and then adding the carbon nanotube reinforcement again, subjecting the powder to secondary high-energy ball milling for 34 hours to obtain a high-content carbon nanotube-reinforced aluminum-based composite material powder; Forming of the composite material: Plasma sintering of the high-content carbon nanotube-reinforced aluminum-based composite material powder is followed by hot extrusion to obtain a composite material rod with a smooth surface and no cracks.
[0024] In the present invention, in the process of preparing high-content reinforcement metal matrix composite material, the principle of improving the dispersion reinforcement is: the composite material powder that has been subjected to ball milling and dispersed a certain content of reinforcement has obvious work hardening phenomenon, and the composite material powder in the particle state is subjected to vacuum heat treatment to improve the interface bonding between the reinforcement and the matrix, so that the dislocation in the matrix is restored, thereby reducing the dislocation density, and reducing the internal stress of the matrix powder from a macroscopic point of view, so that it has the ability of further plastic deformation, and on this basis, a certain content of reinforcement is added again, so that the reinforcement content that can be dispersed in the composite material powder is further increased, and on the other hand, due to the further deformation of the powder, the ball milling time is extended, and the process of continuing to add reinforcement ball milling after the heat treatment is not limited to two times, and multiple heat treatment cycles can be performed. The prepared composite material powder is then subjected to plasma sintering and hot extrusion processes, and the reinforcement content in the final obtained composite material block is high and uniformly dispersed, and the combination of the reinforcement and the interface is stronger, thereby improving the mechanical properties of the composite material.
[0025] In the following embodiments, high-content carbon nanotube-reinforced aluminum-based composite material (CNTs / Al) powder is used as an example for description.
[0026] Raw materials, planetary ball milling, plasma sintering, hot extrusion and performance testing equipment used in the following examples: The high-content composite material powder was prepared using a German Pulverisette 5 planetary ball mill; The composite material powder after ball milling was subjected to vacuum heat treatment process using Henan Chengyi 1200℃ vacuum heat treatment tube furnace equipment; The composite material blocks in SPS state were prepared using Shanghai Chenhua SPS-20T-10-ⅠⅠⅠⅠ plasma sintering equipment; Ningbo Pavol vertical hot extrusion equipment YP61-315 is used for the hot extrusion process of sintered samples; The German ZEISS Gemini 500 was used to characterize the powder morphology and its CNTs distribution state; The powder was subjected to XRD characterization analysis using a D8 Discover X-ray diffractometer; The British Oxford c nano probe was used to perform EBSD characterization analysis on the extruded high-content CNTs / Al composite bulk; The tensile properties of high-content CNTs / Al composites were tested using an American INSTRON 3382 electronic universal testing machine; The powder used was 45 micron spherical pure Al powder prepared by Shanghai Buwei Company, the CNTs powder used multi-walled carbon nanotubes (Baytubes C150P), and the stearic acid was produced by Macklin Company with the chemical formula of C 18 H 36 O2.
[0027] The following embodiments all utilize high-energy ball milling. The ball milling process first changes the morphology of the matrix powder so that it obtains a larger surface area, which can more efficiently disperse CNTs. At the same time, when the composite material powder is cold-welded into particles, a vacuum heat treatment process is combined to remove the ball milling stress and improve the interface bonding between the reinforcement and the matrix, so that the composite material powder can further plastically deform, further extending the ball milling time. Subsequently, the ball milling is performed to the target time to obtain CNTs / Al powder with a good CNTs dispersion state, and the powder is sintered. Finally, the block is further densified by hot extrusion, and finally a dense composite material rod without obvious defects is obtained. Example 1
[0028] The preparation method of the high-content CNTs / Al composite material in this embodiment includes high-energy ball milling combined with vacuum heat treatment to improve the ability of the composite material powder to further disperse the reinforcement, and then add CNTs to continue ball milling, while further increasing the CNTs content, improving the interface bonding between CNTs and the matrix, extending the ball milling time, and then sintering and extruding the prepared CNTs / Al composite powder to finally obtain a composite material block. On the other hand, by adjusting the content of the reinforcement added before and after the heat treatment, the improvement effect of the heat treatment on the interface bonding is compared. In addition, the traditional ball milling method without the heat treatment process is also compared, and the composite material powder prepared by ball milling is also sintered and hot extruded, and finally the mechanical properties are compared and analyzed.
[0029] The specific method for preparing high-content CNTs / Al composite material powder comprises the following steps: Step 101, powder proportioning and ball milling: A total of 115.2 g of 45 μm spherical pure aluminum powder was loaded into the ball mill.
[0030] Powder ratio: the content of spherical pure Al powder with a particle size of 45 μm is 96 wt.%, the amount of stearic acid added is 1 wt.%, and the ball milling ball is a zirconia ball with a diameter of 10 mm, and the ball-to-material ratio is 5:1.
[0031] In the above preparation process, in step 1, the order of loading the materials into the tank is to add the ball milling balls first, then add the pure aluminum powder and stearic acid particles evenly at the same time, and stir evenly with a spoon to make the initial CNTs and Al powder and stearic acid particles pre-mixed evenly.
[0032] Step 102, ball milling process and parameter design: First, open the outlet valve to ensure that the gas path is normal, adjust the gas flow rate to 0.5 L / min, and introduce argon gas into the air inlet to ensure that the ventilation time is not less than 8 minutes; when stopping the air intake, first close the air inlet valve, and then close the outlet valve. The relatively low gas flow rate in the above operation is conducive to the slow exhaust of air by the argon protective gas, and will not cause a decrease in the quality of the powder.
[0033] The ball milling parameters are set to a speed of 200 rpm / min, and the ball milling method is forward rotation for 10 min, stop for 20 min, reverse rotation for 10 min, and then cycle in sequence. This process can effectively avoid the chemical reaction caused by excessive temperature in the ball milling tank. On the other hand, the ambient temperature is controlled below 25°C to ensure the consistency of temperature each time the ball milling is started. For the added pure aluminum powder, the effective ball milling time is set to 4 h. When the base powder is ball milled into a thick flake, the tank is opened in the glove box and the reinforcement is added.
[0034] Step 103, adding the reinforcement for the first time and high energy ball milling: The matrix powder with an effective ball milling time of 4 h was operated and mixed with 3 wt.% of reinforcement powder. The ball mill was opened in the glove box, and the reinforcement weighed in advance was added and stirred evenly with a spoon. Then the ball mill lid was closed and the ball mill was reloaded into the planetary ball mill for ball milling.
[0035] The ball mill speed was set at 180-230 rpm / min, and the ball milling method was forward rotation for 10 min, stop for 20 min, reverse rotation for 10 min, and the cycle was repeated in sequence. At this time, the composite material powder was ball milled to a granular powder state after cold welding. Taking the carbon nanotube reinforced aluminum-based composite material as an example, the ball milling was continued for 24 h, and the ambient temperature was controlled below 25 °C.
[0036] In order to compare and illustrate the superiority of this patent, two control groups were set up under the premise of controlling the total added CNTs content to 4 wt.%, wherein control group 1 was to add 1 wt.% CNTs and then ball-milled to a granular composite material powder for 24 hours, followed by heat treatment, and 3 wt.% CNTs were added again after the heat treatment; control group 2 was to add 2 wt.% CNTs and then ball-milled to a granular composite material powder for 24 hours, without heat treatment, and then 2 wt.% CNTs were added again and ball-milled for the same time, and the operation method was consistent with the designed process.
[0037] Step 104, powder vacuum heat treatment process: The composite material powder after ball milling for 24 h is granular. At this stage, 1 g of the powder before and after heat treatment is selected for morphology and phase characterization. It should be noted that the powder should be prevented from direct contact with the air during the powder collection process, and the operation needs to be carried out in a glove box. The vacuum heat treatment temperature is 550 ° C, the holding time is 12 h, and then the furnace is cooled. At the same time, 10-20 g of sponge titanium is placed next to the heat-treated powder in advance to further prevent the powder from being oxidized.
[0038] As a further explanation of the present invention, in order to highlight the material performance advantages of this design scheme, a control group is used for illustration. The design process of control group 1 in this step is as follows: ball milling for 24 hours, and the granular CNTs / Al composite material powder containing 1 wt.% of reinforcement is also vacuum heat treated, and the parameter selection and steps are consistent with the above-mentioned design process. The process of control group 2 adopts a heat-free treatment method, that is, no heat treatment is performed after ball milling for 24 hours, and then CNTs are added again to continue ball milling.
[0039] Step 105, after heat treatment, the powder is again added with reinforcement and ball milled: After heat treatment of the granular composite powder after ball milling for 24 hours, the stress of the matrix powder has been removed, and it is added to the ball mill again, and 1 wt.% of CNTs reinforcement is added, and 1 wt% of the process control agent (stearic acid) is added, followed by ball milling. The ball milling speed is 200 rpm / min, and the ball milling time is 34 hours. Together with the initial 4 hours of pure aluminum and the 24 hours of ball milling to granular powder, the total effective ball milling time is 62 hours.
[0040] In order to illustrate the material performance advantages of the present invention, the control group 1 is used for illustration. The design process of the control group 1 in this step is as follows: after the CNTs / Al composite material powder is ball-milled for 24 hours, it is heat-treated and then added to the ball mill again, and 3 wt.% of CNTs reinforcement is added, and 1 wt.% of the process control agent (stearic acid) is added, followed by ball milling. The ball milling speed is 200 rpm / min, and the ball milling time is 34 hours. In addition to the initial 4 hours of pure aluminum and the 24 hours of ball milling to granular powder, the total effective ball milling time is 62 hours.
[0041] The ball milling process without heat treatment was used as the control group 2. The specific steps were as follows: the CNTs / Al composite material powder with a content of 2 wt.% was ball-milled to granular form for 24 h, and then 1 wt.% stearic acid and 2 wt.% CNTs were added again without heat treatment, and ball-milled for 34 h. Finally, the ball-milled composite material was powdered in a glove box.
[0042] Step 106, high content CNTs / Al composite material powder spark plasma sintering process: The CNTs / Al composite powder obtained after ball milling is loaded into a graphite mold with a diameter of 29.8 mm, and pre-pressed with a pressure of 0.5T, and the pressure holding time is not less than 5 minutes. Then, the outside of the graphite mold is wrapped with high-temperature resistant fiber felt, which plays a role in heat preservation of the mold during the sintering process. The graphite mold is loaded into the plasma sintering equipment furnace for sintering, and the sintering procedure is as follows: a. Temperature rises to 450℃ in 5 min, and pressure rises to 1 T; b. Maintain temperature and pressure at 450℃ (1 T) for 10 min; c. Heat to 590°C for 4 min, pressure remains at 1 T; d. Increase the pressure to 2.2 T (30 MPa) in 1 min; e. Keep at 590℃ and 2.2T pressure for 30 min; f. Cooling; The vacuum degree during sintering is 1.5×10 -1 Pa. Finally, a sintered composite material block with a diameter of 29.8 mm was obtained. The temperature measurement during the sintering process was measured by K-type thermocouple contact temperature measurement to ensure the sensitivity and accuracy of the temperature test. The insulation under the conditions of 450°C and 1T is to allow the stearic acid to fully volatilize, thereby ensuring a lower oxygen content in the composite material. The sintering process of the designed control group samples was the same, and finally a sintered composite block sample was obtained.
[0043] Step 106, hot extrusion process of high-content CNTs / Al sintered block: The designed sample and the samples of control group 1 and control group 2 after sintering in step 105 are hot extruded. The samples are first heated and kept warm, and then placed in a preheated extrusion device for hot extrusion operation, and finally an extruded composite material rod with a smooth surface and no cracks is obtained. The hot extrusion process specifically includes the following steps: Firstly, the surface of the sample was polished with sandpaper to remove the oxide scale, high-temperature grease was applied to the extrusion die and the inner wall of the sleeve, and the sample was heated and insulated with an insulation sleeve. The insulation temperature was not less than 350°C. The sample was kept at 500°C for 20 min in a box furnace and then immediately placed in the preheated extrusion sleeve. The extrusion ratio was 18:1 and the extrusion speed was 4 mm / s. Finally, a composite extruded rod with a diameter of 7 mm and a smooth surface without cracks was obtained.
[0044] In the above-mentioned forming process, in step 106, in the sample, the process of control group 1 is to add 1% CNTs after ball milling pure aluminum for 4 h, and vacuum heat treat the composite powder after ball milling for 24 h, then add 3% CNTs again, and ball mill again for 34 h. The ball milling process of control group 2 is to initially add 2% CNTs and ball mill for 24 h, and then add 2% CNTs again and ball mill for 24 h. Note that vacuum heat treatment of powder is not performed in control group 2. Finally, the two control groups are subjected to the same sintering and extrusion process as the composite powder designed by the present invention. The room temperature tensile properties of the three composite materials are shown in Table 1. In the control groups 1 and 2 of this patent and design, the CNTs reinforcement content is 4 wt%. The yield strength of the sample designed and prepared by the present invention reaches 458.6±17.3 MPa, the tensile strength is 500.0±2.6 MPa, and the elongation at break reaches 7.0±0.3%. Compared with control group 1, the yield strength is increased by 10%, the tensile strength is increased by 11.4%, and the elongation at break is increased by 32.1%. Compared with control group 2, the yield strength increased by 5.1%, the tensile strength remained almost unchanged, and the elongation at break increased by 79.5%. The preparation process of the high-content CNTs / Al composite material designed in this patent has obvious performance advantages. Table 1 Mechanical properties of high-content CNTs / Al composites and control group
[0045] Material Name Yield strength (MPa) Tensile strength (MPa) Elongation at break (%) 3%HT1% (this patent) 458.6±17.3 500.0±2.6 7.0±0.3 1%HT3% (control group 1) 416.9±13.9 451.3±1.5 5.3±1.0 2%+2% (control group 2) 436.3±19.5 505.6±1.0 3.9±1.6 The following tests and analyses were performed on the high-content CNTs / Al composite powder prepared by vacuum heat treatment, plasma sintering, and hot extrusion in this embodiment: (1) Morphology analysis of the high-content CNTs / Al composite powder prepared by ball milling in this example: The morphology of the composite powders obtained at different ball milling times was characterized by SEM scanning. Figure 2 The morphology of the CNTs / Al composite powder obtained at different stages of ball milling in the process designed for Example 1 and Control Group 1, where Figure 2 (a) and (d) respectively represent the morphology of the ball milling process designed by the present invention (pure aluminum ball milling for 4h + 3% CNTs@BM24h) and the control group 1 (pure aluminum ball milling for 4h + 1% CNTs@BM24h). It can be seen that after 24h of ball milling, the powder designed by the present invention has become more regular particles, while the powder of the control group is larger particles. Figure 2(b) and (e) show the powder morphology of the process designed by the present invention (pure aluminum ball milling 4h + 3% CNTs@BM24h + HT + 1% CNTs@BM34h) and the control group 1 (pure aluminum ball milling 4h + 1% CNTs@BM24h + HT + 3% CNTs@BM34h). It can be seen that the powder size obtained by the process designed by the present invention is still granular and has a uniform size distribution, while the composite powder obtained by the control group 1 is larger in size and unevenly distributed, with fine powder. Further zooming in on the powder, such as Figure 2 As shown in (c) and (f), it can be seen that the powder surfaces are significantly different. The composite powder surface obtained by the process flow designed by the present invention is smooth and has no obvious pores, while the powder surface prepared by the control group 1 has a lot of debris. These debris are broken composite powders. Due to the naturally formed aluminum oxide layer on the powder surface, the bonding between these debris powders and large particle powders is significantly reduced. On the other hand, the dispersion of CNTs is characterized by Figure 2 (a) and (d) show that before heat treatment, the surface of the composite powder that was ball-milled for 24 hours showed that the CNTs were basically in a single state, and a large number of CNTs were buried in the matrix, indicating that the first step had a good dispersion state for the CNTs. This is because the good plastic deformation ability of the initial Al matrix allowed the CNTs to be well dispersed as the Al powder deformed. After the powder was vacuum heat treated, it was ball-milled for 34 hours. In the composite powder finally obtained, the composite powder prepared by the present invention showed good sphericity, indicating that the powder properties after heat treatment were similar to those of the initial Al powder and could be fully plastically deformed. At the same time, no obvious CNTs were found under high-magnification observation of the powder surface, further verifying that the CNTs had been fully buried in the matrix and were well dispersed under a strong bond with the matrix. In contrast, high-magnification observation of the surface of the composite powder prepared in control group 1 showed obvious CNTs, even including small-scale CNT agglomerations, indicating that the dispersion state of the CNTs was not ideal ( Figure 2 (High magnification image in (f)).
[0046] (2) Phase composition of composite powder before and after heat treatment Figure 3The XRD characterization analysis of the composite material powder prepared by the present invention and the powder of the control group 1 at different ball milling stages and before and after heat treatment. For the process designed by the present patent, the first ball milling powder is 3%@BM24h, and the control group 1 (1%@BM24h) is a composite material powder after ball milling for 24 hours. From the XRD results, it can be seen that there is no obvious other phase except the peak of the Al matrix, indicating that the temperature and parameters of the ball milling process are reasonably set, and no obvious oxidation and interface reaction will occur. With the addition of the heat treatment process, in addition to the Al peak, a weaker Al4C3 peak is produced in the XRD spectrum of the present invention (3%@BM24h-HT) and the control group 1 (1%@BM24h-HT), indicating that the heat treatment process causes a partial reaction between CNTs and the matrix, but because the peak intensity is very low, it can be considered that the degree of interface reaction is not high. After CNTs were added to the heat-treated powder again and ball milled, the Al4C3 content in the composite powder of the present invention and the control group 1 decreased to a certain extent compared with the powder after heat treatment. This is because there is no obvious interface reaction between the carbon tubes added after heat treatment and the matrix, thereby reducing the total aluminum carbide content of the system.
[0047] (3) Phase composition of extruded bulk Combined with the XRD results and EBSD analysis of the powder, the changes in the matrix powder grains are characterized. First, the XRD spectrum is used. The results are as follows Figure 4 As shown, both the present invention (3%-HT-1%) and the control group 1 (1%-HT-3%) have Al4C3 peaks, proving that the finally obtained CNTs / Al composite materials have a certain degree of interfacial reaction. However, since the Al4C3 peak intensity is not high, it means that the CNTs in the block are not completely converted into Al4C3, and only a certain degree of interfacial reaction exists.
[0048] In addition, EBSD was used to analyze the specific phase content, grain size, grain structure and dislocation density of the extruded microstructure. Figure 5 The EBSD contrast image shows that the bulk structure of the composite material prepared by the process of the present invention is significantly different from that of the control group 1. Although both organizations have a heterogeneous structure with large grains and small grains coexisting, the organization of the present invention has two characteristics in comparison. First, the large grains (white grains in the figure) are relatively more regularly distributed and present a continuous network structure. At the same time, the size of the large grains is larger than that of the large grains in the control group 1, which also leads to the final grain size of 1.84 μm prepared by the present invention. 2 , while the control group 1 was only 0.88 μm 2, the continuous network coarse grain structure is more conducive to the uniform transmission of stress and strain during the force process, and more effectively avoids adverse phenomena such as stress concentration, so it has better mechanical properties than the control group 1. Through the analysis of other data, it can be seen from Table 2 that the content of Al2O3 in the block prepared by the present invention is 0.5%, which is lower than 0.8% of the control group 1. Considering that the sintering and extrusion process parameters and conditions are the same, it shows that the process of the present invention can more effectively avoid the oxygen absorption of the powder during the ball milling process. On the other hand, the content of Al4C3 is the same in the two materials, indicating that the degree of reaction is similar. In addition, the dislocation density was statistically analyzed, and it was found that the dislocation density in the extruded composite block prepared by the process of the present invention is 56.28×10 14 , while that of control group 1 was 55.85×10 14 The composite material prepared by the present invention has a higher dislocation density, indicating that it has a higher strength. Table 2 EBSD results of high-content CNTs / Al composites and control group 1
[0049] Material Name <![CDATA[Al2O3 phase content (%)]]> <![CDATA[Al4C3 phase content (%)]]> <![CDATA[Grain size (μm 2 )]]> Dislocation density (Al, 1 / 2 <110> ) 3%HT1% (this patent) 0.5 0.1 1.84 <![CDATA[56.28×10 14 ]]> 1%HT3% (control group 1) 0.8 0.1 0.88 <![CDATA[55.85×10 14 ]]> (4) Mechanical and room temperature properties test of high content CNTs / Al composites The composite material block prepared by the present invention and control group 1 and control group 2 were subjected to room temperature tensile performance test. The engineering stress-strain results are as follows: Figure 6 As shown, by comparison with the control group, the composite material block prepared by the present invention has obvious advantages in strength and elongation at break. The composite material prepared by the present invention has obvious organizational advantages. First, there are continuous mesh matrix grains in the organization to avoid stress concentration during plastic deformation. On the other hand, after the composite material powder is heat treated, some CNTs in the organization react with the matrix to a certain extent, thereby improving the interface bonding between the CNTs and the matrix, which is conducive to the load transfer strengthening mechanism in the plastic deformation process to be better exerted. If the content of CNTs in the composite material powder is relatively small during heat treatment (i.e., control group 1), the content of CNTs with obvious interface enhancement in the composite material finally obtained will be reduced, resulting in a decrease in the strength of the final composite material. If the composite material powder is not heat treated, the composite material powder after ball milling for a certain period of time cannot be effectively further plastically deformed due to obvious work hardening, so that the CNTs cannot be effectively dispersed again, resulting in the agglomeration of CNTs in the final matrix, and the plasticity is poor in the final mechanical properties test. The heat treatment ball milling method of the present invention provides a method for obtaining metal-based composite materials with high content and strong interface bonding, and is expected to obtain nano-reinforced metal-based composite materials with excellent comprehensive mechanical properties to meet the application of composite materials in important national fields such as aerospace, weapons and armaments.
[0050] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention.
Claims
1. A method for preparing a high-content carbon nanotube-reinforced aluminum-based composite material by heat treatment and cyclic ball milling, characterized in that: The method comprises: Preparation of composite material powder: a certain amount of matrix aluminum powder and process control agent are subjected to primary ball milling, and then carbon nanotube reinforcement is added for the first time to obtain composite material powder, the composite material powder is subjected to high-energy ball milling for the first time for 24 hours, vacuum heat treatment is performed after the powder is in the form of cold-welded particles, and then carbon nanotube reinforcement is added again, and secondary high-energy ball milling is performed for 34 hours to obtain high-content carbon nanotube-reinforced aluminum-based composite material powder; Forming of the composite material: Plasma sintering of the high-content carbon nanotube-reinforced aluminum-based composite material powder is followed by hot extrusion to obtain a composite material rod with a smooth surface and no cracks.
2. The method for preparing a high-content carbon nanotube-reinforced aluminum-based composite material by heat treatment and cyclic ball milling according to claim 1, characterized in that: The content of carbon nanotubes in the high-content carbon nanotube-reinforced aluminum-based composite material powder is 4 wt.% by mass, and the content of aluminum powder in the high-content carbon nanotube-reinforced aluminum-based composite material powder is 96 wt.% by mass.
3. The method for preparing a high-content carbon nanotube-reinforced aluminum-based composite material by heat treatment and cyclic ball milling according to claim 1, characterized in that: The content of the carbon nanotube reinforcement added for the first time in the composite material powder is 3 wt.% by mass, and the content of the carbon nanotube reinforcement added again in the high-content carbon nanotube-reinforced aluminum-based composite material powder is 1 wt.% by mass.
4. The method for preparing a high-content carbon nanotube-reinforced aluminum-based composite material by heat treatment and cyclic ball milling according to claim 1, characterized in that: The aluminum powder is 45 μm spherical pure aluminum powder, and the carbon nanotube reinforcement has a tube diameter of 20 nm and a length of 2 μm.
5. The method for preparing a high-content carbon nanotube-reinforced aluminum-based composite material by heat treatment and cyclic ball milling according to claim 1, characterized in that: The time for the initial ball milling of the matrix aluminum powder and the process control agent is 4 hours, the ball mill speed for the first high-energy ball milling and the second high-energy ball milling after adding the carbon nanotube reinforcement is 180-230 rpm / min, the ball milling method is forward rotation for 10 minutes, stop for 20 minutes, and reverse rotation for 10 minutes; the ambient temperature is below 25°C.
6. The method for preparing a high-content carbon nanotube-reinforced aluminum-based composite material by heat treatment and cyclic ball milling according to claim 1, characterized in that: The temperature of the vacuum heat treatment is 550° C., the heat preservation time is 12 hours, and the furnace is cooled after the vacuum heat treatment, and the powder is taken out after the temperature is lower than 30° C.
7. The method for preparing a high-content carbon nanotube-reinforced aluminum-based composite material by heat treatment and cyclic ball milling according to claim 1, characterized in that: During the vacuum heat treatment, 10-20 g of titanium sponge is placed next to the composite material powder in advance.
8. The method for preparing a high-content carbon nanotube-reinforced aluminum-based composite material by heat treatment and cyclic ball milling according to claim 1, characterized in that: The vacuum degree of the plasma sintering is 1.5×10 -1 Pa, the sintering temperature is 590 °C, and the sintering process is kept at 450 °C to remove stearic acid.
9. The method for preparing a high-content carbon nanotube-reinforced aluminum-based composite material by heat treatment and cyclic ball milling according to claim 1, characterized in that: The temperature of the hot extrusion process is 500° C., the holding time is 20 min, the extrusion ratio is 18:1, and the extrusion speed is 4 mm / s.