Welding flux for improving obdurability and corrosion resistance of aluminum / copper welding joint
By adding Cu, Ni, La, and Ce elements to Zn-15Al brazing, the aluminum/copper welding composition is optimized, and the problem of brittle Al2Cu generation in the joint is solved, the mechanical properties and corrosion resistance of the welding structure are improved, and aluminum is realized /High strength and corrosion resistance of copper welding.
Patent Information
- Application Number
- CN202411113867.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-15
AI Technical Summary
In the existing aluminum/copper welding technology, the formation of brittle Al2Cu in the joint leads to insufficient mechanical properties and insufficient corrosion resistance, making it difficult to maintain long-term use under harsh working conditions.
Cu, Ni, La, and Ce elements are added to the Zn-15Al brazing material, and the weld structure is refined by optimizing the composition, inhibiting the generation of brittle IMCs, reducing interfacial stress and hardness, and improving corrosion resistance.
It significantly improves the mechanical properties and corrosion resistance of the aluminum/copper welded structure, reduces welding defects, extends service life, reaches 98MPa, and significantly improves corrosion resistance.
Smart Images

Figure BDA0004993079710000031 
Figure BDA0004993079710000041 
Figure HDA0004993079730000011
Abstract
Description
Technical Field
[0001] The invention relates to a solder capable of improving the toughness and corrosion resistance of an aluminum / copper welding joint, belonging to the technical field of welding of dissimilar metal materials. Technical Background
[0002] Aluminum (Al), copper (Cu) and their alloys have been widely used in the fields of electricity, refrigeration, chemical industry, automobile, aerospace, etc. due to their excellent corrosion resistance, high mechanical strength and excellent electrical and thermal transfer properties. The proven reserves of copper resources are not abundant. In the above fields, in order to control costs, reduce product weight, and use resources rationally, the welding problem of aluminum and copper dissimilar metals is often encountered. Due to the large differences in the physical properties, mechanical properties, electrical and thermal properties of these two metals, the welding of these two dissimilar metal materials is still a challenge in terms of corrosion resistance, mechanical properties, electrical and thermal conductivity, etc.
[0003] Brazing is a common method for welding aluminum / copper dissimilar materials, but when aluminum and copper are welded, the fusion interface of the joint weld can easily become the preferred location for crack initiation and expansion. At present, the brazing filler metal used in Al / Cu brazing is mainly Zn-Al brazing filler metal, whose welding temperature is lower than that of Al-Si brazing filler metal, which can reduce the overburning rate of Al base material, and has stronger corrosion resistance than Sn-Zn brazing filler metal, and has a suitable non-corrosive CsF-AlF3 flux. Among Zn-Al brazing filler metals, Zn-15Al has better fluidity than Zn-2Al and Zn-10Al, and reduces the shrinkage rate in the brazing filler metal. However, when Zn-15Al brazing filler metal is used to braze Cu / Al, a large amount of Al-Cu brittle IMCs are generated in the joint, which seriously deteriorates the mechanical properties of the Cu / Al brazed joint. In order to obtain joints with higher strength and mechanical properties, controlling the generation amount and morphology of Al-Cu brittle IMCs has become an urgent problem to be solved.
[0004] CN103317253 B discloses a Zn-Al-Cu based brazing filler metal for aluminum / copper brazing and a preparation method thereof, which comprises the following components by weight percentage: 5-16% aluminum, 3.5-12% copper, 0.5-5% germanium, 0.01-0.1% titanium, 0.01-0.2% strontium, 0.01-0.1% rare earth lanthanum and cerium, and the balance is zinc. The patent improves the shear performance and corrosion resistance of aluminum / copper brazing joints, the joint shear strength reaches up to 76.1MPa, and the tubular joint can withstand salt spray corrosion for up to 840h.
[0005] The study by Yan et al. in the literature (doi.org / 10.1016 / j.jmapro.2020.09.078) shows that adding Ni metal foil as an intermediate layer during aluminum / copper welding can inhibit the diffusion of Al elements and reduce the formation of brittle interface IMCs. At the same time, the addition of Ni elements can refine the weld structure and reduce defects such as interface holes and cracks. The tensile strength of the Al / Cu joint containing Ni foil increased by 27.1%, and the fracture surface was located in the Al2Cu+AlNi intermetallic IMC zone. The presence of hard and brittle Al2Cu intermetallic IMCs limited the further improvement of the joint strength. The addition of Ni elements alone refined the brittle IMCs in the joint to a certain extent, but failed to completely solve the problem of brittle Al2Cu formation in the joint. CN 114774843B discloses a Zn-Al-Cu-Ni-Bi multi-element powder co-infiltration agent and its application, and its application field refers to the Zn-Al-Cu-Ni-Bi multi-element powder co-infiltration agent forming a multi-element alloy infiltration layer with a thickness of 30-150 μm on a metal substrate through mechanical infiltration, and the metal mixed powder cannot be directly applied to the welding process of dissimilar metals. At present, there is no related research on Zn-Al-Cu-Ni-La-Ce solder and no precedent for Ni-containing solder used for aluminum / copper dissimilar metal welding.
[0006] At present, in the field of aluminum / copper dissimilar metal welding technology, there is no solder that can completely solve the problem of brittle Al2Cu formation in joints. The solder described in the present invention, which improves the toughness and corrosion resistance of aluminum / copper welded joints, effectively reduces welding defects, improves the mechanical properties of the joints, and takes into account the improvement of the corrosion resistance of the joints, thereby effectively improving the service life of aluminum / copper welded structures under harsh working conditions. Summary of the invention
[0007] The purpose of the present invention is to provide a solder that improves the toughness and corrosion resistance of aluminum / copper welded joints, refines the weld structure, inhibits the formation of brittle IMCs, reduces defects such as interface holes and cracks, improves the mechanical properties of the aluminum / copper welded structure while taking into account the corrosion resistance of the joint. After adding the Cu element on the basis of the Zn15Al solder, the α-Al dendrites in the solder are refined into columnar crystals and equiaxed crystals; at the same time, the element diffusion of the copper side weld is inhibited, and the interface IMC layer is thinned. However, adding too much Cu to the solder will increase the hardness of the solder, and cracks are likely to initiate during the cooling process of the weld. The solder described in the present invention has determined the optimal content range of Cu through a large number of experiments based on the addition of the Cu element, which effectively refines the weld structure while reducing the interface stress and reducing defects such as interface cracks and holes.
[0008] The Ni element can reduce the hardness of Zn-Al-Cu based solder, thereby buffering the interface stress. The Ni element has a very significant effect on the refinement of the weld structure, completely inhibiting the formation of blocky brittle Al2Cu in the weld and significantly reducing the initiation of Cu side crack defects. The La and Ce elements in the solder further refine the weld structure, increase and refine the lamellar eutectic structure, and the rare earth further reduces the hardness of the solder. At the same time, the rare earth elements in the solder will generate corrosion-resistant products during corrosion, thereby improving the corrosion resistance of the joint. Based on the above purpose, we have conducted a large number of experiments, added and determined the optimal composition range of alloying elements, and obtained a solder that effectively reduces welding defects, improves the mechanical properties of the joint, and takes into account the improvement of the corrosion resistance of the joint.
[0009] The solder for improving the toughness and corrosion resistance of aluminum / copper welding joints described in the present invention is characterized in that it includes the following components by weight percentage: 13-16% aluminum, 0.1-0.9% copper, 0.1-0.5% lanthanum, 0.1-0.5% cerium, and the balance zinc.
[0010] Compared with the prior art, the present invention has the following beneficial effects.
[0011] The solder (0.1-0.9% copper, 0.1-0.5% nickel, 0.1-0.5% lanthanum, 0.1-0.5% cerium) for improving the toughness and corrosion resistance of aluminum / copper welding joints described in the present invention has significantly refined solder and weld structure compared to commercial Zn-15Al solder, and significantly improved joint strength and corrosion resistance; compared to the Zn-Al-Cu based solder (5-16% aluminum, 3.5-12% copper, 0.5-5% germanium, 0.01-0.1% titanium, 0.01-0.2% strontium, 0.01-0.1% rare earth lanthanum and cerium) disclosed in patent CN103317253 B, the types of alloy elements are relatively streamlined, the melting and casting process is simple, and the composition is stable. The Cu content in the solder is low, and no blocky brittle Al2Cu is generated during the welding process, ensuring that the solder has a low hardness, effectively refining the weld structure while reducing the interface stress. The Ni element completely inhibits the formation of massive brittle Al2Cu in the weld, significantly reducing the initiation and expansion of crack defects. The shear strength of the Cu / Al joint can reach as high as 98MPa under the conditions of traditional air furnace brazing process. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 Microstructure of Cu / Al brazed joint filled with Zn-15Al solder;
[0013] Figure 2 Example 1 Microstructure of Cu / Al brazing joint under solder filling;
[0014] Figure 3 Example 2 Microstructure of Cu / Al brazing joint under solder filling;
[0015] Figure 4 Figure 1 A magnified view of the interface microstructure on the Cu side;
[0016] Figure 5 Figure 2 A magnified view of the interface microstructure on the Cu side;
[0017] Figure 6 Figure 3 A magnified view of the interface microstructure on the Cu side; Specific implementation plan
[0018] The present invention will be described in detail below in conjunction with the accompanying drawings.
[0019] Embodiment 1, a solder for improving the toughness and corrosion resistance of aluminum / copper welding joints, characterized in that it comprises the following components by weight percentage: 13-16% aluminum, 0.1-0.9% copper, 0.1-0.5% nickel, 0.1-0.5% lanthanum, 0.1-0.5% cerium, and the balance is zinc.
[0020] Embodiment 2, a solder for improving the toughness and corrosion resistance of aluminum / copper welding joints, characterized in that it comprises the following components by weight percentage: 13-16% aluminum, 0.1-0.9% copper, 0.1-0.5% nickel, 0.1-0.5% lanthanum, and the balance is zinc.
[0021] In Example 3, the surface of 15mm*15mm*3mm thick ZL108Al aluminum alloy and 15mm*15mm*1mm thick T2Cu were mechanically broken by grinding with 400# sandpaper, and then the oil stains were broken by ultrasonic cleaning. According to the material loading method of T2 Cu / brazing agent / brazing material / brazing agent / ZL108Al, a non-corrosive commercial brazing agent cesium fluoride was used to carry out brazing experiments under fixed process parameters. During the brazing process, 15mm*15mm*0.5mm Zn-15Al solder and a solder for improving the toughness and corrosion resistance of aluminum / copper welded joints described in Example 1 and Example 2 were added respectively, and an air furnace brazing experiment was carried out to obtain 3 aluminum / copper brazing joint samples. The mechanical properties of the 3 aluminum / copper brazing joint samples obtained were tested, and the results are shown in Table 1.
[0022] Table 1 Mechanical properties of aluminum / copper brazing joint samples with different brazing fillers Table 1 Mechanical properties of aluminum / copper brazing joint samples with different solder fillings
[0023] Example 4: The aluminum / copper brazing joint samples filled with different solders prepared in Example 3 were subjected to electrochemical corrosion performance testing in 3.5% NaCl solution. The results are shown in Table 2.
[0024] Table 2 Electrochemical corrosion properties of aluminum / copper brazing joints with different brazing fillers Table 2 Electrochemical parameters of aluminum / copper brazing joint samples with different solder fillings
[0025] As shown in Table 1, the shear strength of the ZL108Al-T2 Cu brazed joint obtained by using the solders of Example 1 and Example 2 is 98 MPa and 85 MPa, respectively, which is greater than the shear strength of the brazed joint obtained by using the existing Zn-15Al, which is 59 MPa, and the mechanical properties of the joint are significantly improved.
[0026] It can be seen from Table 2 that the self-corrosion current of the ZL108Al-T2 Cu brazed joint obtained by the solder of Example 2 is significantly reduced. The lower the self-corrosion current, the slower the corrosion rate. The self-corrosion current of the joint using Example 2 is only 3.81 μA / cm2, and the corrosion resistance is significantly improved.
[0027] In order to better illustrate the innovation of the present invention, the following analysis experiments are performed:
[0028] Weld microstructure morphology Figure 1 This is the microstructure of the Cu / Al brazed joint filled with Zn-15Al solder. There are a lot of light gray long strips of Al in the brazed joint weld. 4.2 Cu 3.2 Zn 0.7 , dark gray α-Al, black Al2Cu, grayish white Zn-Al eutectic structure and bright white CuZn5. Figure 2 This is the microstructure of the Cu / Al brazing joint filled with solder in Example 1. After adding a trace amount of Cu element to the solder, the Cu element will form heterogeneous nucleation points in the weld, and α-Al will be refined into columnar crystals and equiaxed crystals. Figure 3 The microstructure of the Cu / Al brazed joint filled with solder in Example 2. The Ni-containing solder completely inhibits the formation of brittle Al2Cu in the weld. 4.2 Cu 3.2 Zn 0.7 Refined into particles.
[0029] Interface morphology of Cu side of weld Figure 4 This is the microstructure of the Cu side interface under Zn-15Al solder filling. There are large pieces of brittle CuAl2 near the interface on the Cu side, which induces interlayer cracking of IMCs on the Cu side interface during the cooling and shrinkage of the weld. Figure 5This is the microstructure of the Cu side interface under solder filling in Example 1. After adding Cu element to the solder, the growth of Al2Cu and will be inhibited, the interface IMCs will be thinned, and the stress concentration generated at the Cu side interface during the cooling process of the welded joint will be alleviated. Figure 6 This is the microstructure of the Cu side interface under solder filling in Example 2. The solder significantly refines the Al on the Cu side interface. 4.2 Cu 3.2 Zn 0.7 IMC, and completely inhibited the formation of brittle Al2Cu on the Cu side interface, significantly reducing the initiation of crack defects on the Cu side.
[0030] The above embodiments are only preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be regarded as equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A solder for improving the toughness and corrosion resistance of aluminum / copper welded joints, characterized in that: The invention comprises the following components by weight percentage: 13-16% aluminum, 0.1-0.9% copper, 0.1-0.5% nickel, 0.1-0.5% lanthanum, 0.1-0.5% cerium, and the balance is zinc.
2. A solder for improving the toughness and corrosion resistance of aluminum / copper welded joints, characterized in that: The composition includes the following components by weight percentage: 13-16% aluminum, 0.1-0.9% copper, 0.1-0.5% nickel, 0.1-0.5% cerium, and the balance is zinc.
3. A solder for improving the toughness and corrosion resistance of aluminum / copper welded joints according to claims 1-2, characterized in that: Compared with the commercial Zn15Al solder cast structure containing a large number of coarse α-Al dendrites, the solder cast structure contains a large number of α-Al columnar crystals and equiaxed crystals, as well as fine lamellar eutectic structure. The solder structure is significantly refined and evenly distributed.
4. A solder for improving the toughness and corrosion resistance of aluminum / copper welded joints according to claims 1-2, characterized in that: The copper content in the solder is less than 1%, and the nickel content is 0.1-0.5%. The nickel element acts as a heterogeneous nucleation point and will not generate massive brittle Al2Cu during welding, effectively inhibiting the initiation of cracks during the cooling process of the weld.
5. A solder for improving the toughness and corrosion resistance of aluminum / copper welded joints according to claims 1-2, characterized in that: The hardness of the solder is 80-90 HV, and the melting point is 400-450°C. The solder has a low hardness, which effectively refines the weld structure while reducing the interface stress, effectively inhibiting the initiation and expansion of cracks in the joint, and improving the toughness of the joint.
6. A solder for improving the toughness and corrosion resistance of aluminum / copper welded joints according to claims 1-2, characterized in that: The combined weight percentage of rare earth lanthanum and cerium does not exceed 1%, and no massive rare earth IMC will be generated in the solder, which will refine the solder structure and improve the corrosion resistance of the joint.
7. A solder for improving the toughness and corrosion resistance of aluminum / copper welded joints according to claims 1-2, characterized in that: The solder is prepared by a melting and casting method. The steps include: Step 1: preparing the materials according to the weight percentage of each component of the solder according to any one of claims 1 to 2, and placing them into the crucible in the order of pure zinc ingot, pure aluminum ingot, aluminum-copper alloy, aluminum-nickel alloy, aluminum-lanthanum alloy and aluminum-cerium alloy. The intermediate alloy ingot with high melting point is placed on the uppermost layer to reduce the burning loss of the low melting point alloy. The loaded graphite crucible is placed in a resistance melting furnace and heated to 200°C for preheating and insulation for 20 minutes. Step 2, melting and casting, heat the smelting furnace to 660℃ and keep it warm for 10 minutes; further, heat the smelting furnace to 780℃ and keep it warm for 10 minutes; further, heat the smelting furnace to 820℃ and keep it warm for 10 minutes. The temperature difference is buffered by step-by-step heating to reduce solder segregation and burning. Further, after slag removal and sufficient stirring, sprinkle a covering agent on the surface of the melt, and adjust the temperature to 660℃ and keep it warm for 30 minutes. Further, after the insulation is completed, slag removal and sufficient stirring are performed, hexachloroethane refining agent (0.1-0.2% of the weight of the solder) is added, and the refining is kept warm at 660℃ for 20 minutes. Further, after the refining and insulation time is over, the casting is cooled for 2-3 hours, and then the mold is opened to take out the solder ingot for remelting, and the melting and casting is repeated 4 times. Step three: Processing and shaping: cutting and grinding the solder ingot to the finished product size.
8. Use of the solder and element composition ratio according to any one of claims 1 to 2 in welding dissimilar metals.
Citation Information
Cited By
Toughening method of modified Zn-based intermediate layer in aluminum alloy welding
CN121156476A