Preparation method of P22 stainless steel welding material

By smelting and multi-process processing in a vacuum induction furnace, the corrosion resistance of the reaction vessel in high temperature and chloride molten salt environment is solved, and the stability and strength of welding are improved.

CN118951493APending Publication Date: 2024-11-15CHINA INSTITUTE OF ATOMIC ENERGY
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411311369.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-19
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In spent fuel drying post-treatment technology, the reaction vessel needs high-temperature and corrosion-resistant materials to cope with the corrosion environment of cadmium-containing high-temperature liquid and chloride molten salt. However, the existing technology lacks suitable P22 stainless steel welding materials, resulting in poor welding. Stablize.

Method used

The steel ingot is prepared by melting the substrate in a vacuum induction furnace, and the heating, forging, hot rolling, heat treatment and cold drawing processes are carried out to regulate the chemical composition and tissue structure of the welding material, and improve its corrosion resistance to chloride salts and high-temperature liquids performance.

Benefits of technology

The prepared P22 stainless steel welding material has excellent structural strength and corrosion resistance, and can work stably under high temperature, molten chloride salt and other environments. It is suitable for welding of electrolytic refining reaction vessels.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118951493A_ABST
    Figure CN118951493A_ABST
Patent Text Reader

Abstract

The invention relates to the field of metal material welding, and provides a P22 stainless steel welding material preparation method which comprises the steps that a base material is placed in a vacuum induction furnace to be smelted to obtain a steel ingot, and chemical components of the base material comprise the carbon element, the manganese element, the silicon element, the tungsten element, the chromium element, the molybdenum element, the vanadium element, the boron element and the iron element; heating and forging the steel ingot to obtain a square rod; performing hot rolling processing on the square rod to obtain a wire rod; and after the wire rod is subjected to the heat treatment process, the wire rod is subjected to the cold drawing process to obtain the welding material. According to the preparation method of the P22 stainless steel welding material, the prepared welding material can be used for welding P22 stainless steel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of metal material welding, and in particular to a method for preparing P22 stainless steel welding material. Background Art

[0002] Spent fuel dry reprocessing technology is a key link in the integrated closed-cycle nuclear energy system. The reaction vessels used for electrolytic refining need to withstand long-term corrosion from coupled working conditions such as cadmium-containing high-temperature liquid and chloride molten salt, which brings huge challenges to the reaction vessels.

[0003] P22 stainless steel has excellent high-temperature mechanical properties and high-temperature oxidation resistance, and can be used as the main material of the reaction vessel. Therefore, in order to realize P22 stainless steel as the main material of the reaction vessel, matching welding materials are required for welding to ensure the manufacturing and forming of the reaction vessel. Summary of the invention

[0004] In view of this, the embodiments of the present application hope to provide a method for preparing a welding material capable of welding P22 stainless steel.

[0005] In order to achieve the above-mentioned purpose, the technical solution of the embodiment of the present application is implemented as follows:

[0006] The present application embodiment discloses a method for preparing a P22 stainless steel welding material, comprising:

[0007] placing a substrate in a vacuum induction furnace for smelting to obtain a steel ingot, wherein the chemical composition of the substrate includes carbon, manganese, silicon, tungsten, chromium, molybdenum, vanadium, boron and iron;

[0008] Heating and forging the steel ingot to obtain a square bar;

[0009] Hot rolling the square bar to obtain a wire rod;

[0010] After the wire rod is subjected to a heat treatment process, the wire rod is subjected to a cold drawing process to obtain a welding material.

[0011] In one embodiment, the weight percentage of the carbon element is between 0.11% and 0.13%, the weight percentage of the manganese element is not more than 0.5%, the weight percentage of the silicon element is less than 0.2%, the weight percentage of the tungsten element is not more than 0.6%, the weight percentage of the chromium element is not more than 2.4%, the weight percentage of the molybdenum element is between 0.9% and 1.1%, the weight percentage of the vanadium element is less than 0.5%, the weight percentage of the boron element is less than 0.005%, and the balance is iron element.

[0012] In one embodiment, the weight percentage of the manganese element is between 0.35% and 0.5%, the weight percentage of the tungsten element is less than 0.01%, and the weight percentage of the chromium element is between 2.1% and 2.4%.

[0013] In one embodiment, the weight percentage of the manganese element is less than 0.1%, the weight percentage of the tungsten element is between 0.2% and 0.6%, the weight percentage of the chromium element is between 1.1% and 1.4%, the weight percentage of the vanadium element is between 0.15% and 0.35%, and the weight percentage of the boron element is between 0.001% and 0.003%.

[0014] In one embodiment, the step of heating and forging the steel ingot to obtain a square bar comprises:

[0015] The steel ingot is placed in a heating furnace for heating, wherein the heating temperature is between 1100° C. and 1150° C., and the holding time is 3 hours;

[0016] After being evenly heat-insulated, the steel ingot is forged, and then forged into the square rod by two-fire forging through drawing and roughening.

[0017] In one embodiment, the holding temperature of the hot rolling process is between 1100° C. and 1150° C., the holding time of the hot rolling process is between 1 h and 1.5 h, and the wire rod is formed by hot continuous rolling.

[0018] In one embodiment, the temperature of the heat treatment process is between 640° C. and 760° C., and the insulation time of the heat treatment process is between 1 hour and 1.5 hours.

[0019] In one embodiment, the cold drawing process includes:

[0020] Firstly, the wire rod is surface-grinded and coated with a coating agent, then single-pass cold drawing, vacuum annealing and continuous cold drawing are performed, and finally the wire is wound around a coil to obtain the welding material.

[0021] In one embodiment, the impurities in the welding material include sulfur and phosphorus, the weight percentage of the sulfur element is less than 0.003%, and the weight percentage of the phosphorus element is not more than 0.007%.

[0022] In one embodiment, the tensile yield strength of the welding material is between 360 MPa and 530 MPa, the tensile strength of the welding material is between 510 MPa and 690 MPa, and the elongation of the welding material is between 25% and 40%.

[0023] The embodiment of the present application discloses a method for preparing a P22 stainless steel welding material. By placing a substrate in a vacuum induction furnace for smelting to obtain a steel ingot, the precipitate of carbide can be melted back into the substrate to improve the homogenization of the subsequent welding material, wherein the carbon element in the substrate can be strengthened by solid solution to increase the structural strength of the welding material; the manganese element can improve the corrosion resistance of the welding material to chloride salts; silicon is a deoxidizer in the steelmaking process, and its content is inevitable; the tungsten element can further improve the corrosion resistance of the welding material to chloride salts and cadmium-containing high-temperature liquids; the chromium element is a ferrite-forming element, which can improve the corrosion resistance and structural strength of the welding material; the molybdenum element can further improve the corrosion resistance of the welding material to chloride salts to adapt to the corrosive environment of chloride molten salts; the vanadium element can improve the structural strength of the welding material and improve the corrosion resistance of the welding material to cadmium-containing high-temperature liquids; the boron element can improve the grain boundary strength of the welding material, reduce the occurrence of failure of the welding material's radiation resistance, and improve the corrosion resistance of the welding material to cadmium-containing high-temperature liquids; the iron element can also improve the corrosion resistance of the welding material to cadmium-containing high-temperature liquids to a certain extent. After smelting to obtain the steel ingot, the steel ingot can be heated and forged to obtain a square bar, and then the square bar can be hot-rolled to obtain a wire rod, and then the wire rod is subjected to a heat treatment process, and finally the heat-treated wire rod is subjected to a cold drawing process to obtain the welding material. In this way, the organizational structure and grain size of the subsequently formed welding material can be regulated, and the impurities in the welding material can be reduced to improve the cleanliness of the welding material. In this way, after welding the reaction vessel of the electrolytic refining, the welding point of the reaction vessel can adapt to the corrosion of coupled working conditions such as high temperature and chloride molten salt, and has good working stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 A schematic flow chart of a method for preparing a P22 stainless steel welding material provided in an embodiment of the present application. DETAILED DESCRIPTION

[0025] It should be noted that, in the absence of conflict, the embodiments and technical features in the embodiments of the present application can be combined with each other, and the detailed description in the specific implementation method should be understood as an explanation of the purpose of the present application and should not be regarded as an improper limitation on the present application.

[0026] The present application will be further described in detail below with reference to the accompanying drawings and specific embodiments.

[0027] This application embodiment provides a method for preparing P22 stainless steel welding material, please refer to Figure 1 , the preparation method comprises:

[0028] S1. placing a substrate in a vacuum induction furnace for smelting to obtain a steel ingot, wherein the chemical composition of the substrate includes carbon, manganese, silicon, tungsten, chromium, molybdenum, vanadium, boron and iron;

[0029] S2, heating and forging the steel ingot to obtain a square bar;

[0030] S3, hot rolling the square bar to obtain a wire rod;

[0031] S4. After the wire rod is subjected to a heat treatment process, the wire rod is subjected to a cold drawing process to obtain welding material.

[0032] The preparation method of P22 stainless steel welding material provided in the embodiment of the present application is to place the substrate in a vacuum induction furnace for smelting to obtain a steel ingot, and the precipitate of carbide can be melted back into the substrate to improve the homogenization of the subsequent welding material, wherein the carbon element in the substrate can be strengthened by solid solution to increase the structural strength of the welding material; the manganese element can improve the corrosion resistance of the welding material to chloride salts; silicon is a deoxidizer in the steelmaking process, and its content is inevitable; the tungsten element can further improve the corrosion resistance of the welding material to chloride salts and cadmium-containing high-temperature liquids; the chromium element is a ferrite-forming element, which can improve the corrosion resistance and structural strength of the welding material; the molybdenum element can further improve the corrosion resistance of the welding material to chloride salts to adapt to the corrosive environment of chloride molten salts; the vanadium element can improve the structural strength of the welding material and improve the corrosion resistance of the welding material to cadmium-containing high-temperature liquids; the boron element can improve the grain boundary strength of the welding material, reduce the occurrence of failure of the welding material's radiation resistance, and improve the corrosion resistance of the welding material to cadmium-containing high-temperature liquids; the iron element can also improve the corrosion resistance of the welding material to cadmium-containing high-temperature liquids to a certain extent. After smelting to obtain the steel ingot, the steel ingot can be heated and forged to obtain a square bar, and then the square bar can be hot-rolled to obtain a wire rod, and then the wire rod is subjected to a heat treatment process, and finally the heat-treated wire rod is subjected to a cold drawing process to obtain the welding material. In this way, the organizational structure and grain size of the subsequently formed welding material can be regulated, and the impurities in the welding material can be reduced to improve the cleanliness of the welding material. In this way, after welding the reaction vessel of the electrolytic refining, the welding point of the reaction vessel can adapt to the corrosion of coupled working conditions such as high temperature and chloride molten salt, and has good working stability.

[0033] Exemplarily, in one embodiment, the size of the square rod may be 45 mm×45 mm.

[0034] In one embodiment, the weight percentage of carbon element is between 0.11% and 0.13%, the weight percentage of manganese element is not more than 0.5%, the weight percentage of silicon element is less than 0.2%, the weight percentage of tungsten element is not more than 0.6%, the weight percentage of chromium element is not more than 2.4%, the weight percentage of molybdenum element is between 0.9% and 1.1%, the weight percentage of vanadium element is less than 0.5%, the weight percentage of boron element is less than 0.005%, and the balance is iron element.

[0035] For example, the weight percentage of carbon element can be 0.11%, 0.12% or 0.13%, etc. In this way, by setting the appropriate weight percentage, not only can the situation that carbides precipitate from austenite grain boundaries due to excessive carbon content, resulting in intergranular corrosion and reduced mechanical properties, be reduced, but also better welding with 430SS stainless steel can be performed.

[0036] The weight percentage of manganese is not more than 0.5%. It should be noted that if the proportion of manganese is too large, the corrosion resistance of the welding material to chloride salts will decrease. Therefore, by setting a suitable weight percentage of manganese, the corrosion resistance of the welding material to chloride salts can be improved.

[0037] The weight percentage of silicon element may be 0.05%, 0.1%, 0.15% or 0.18%, etc.

[0038] The weight percentage of tungsten element is not more than 0.6%, thus, the corrosion resistance of the welding material to chloride salts and high-temperature liquid containing cadmium can be improved.

[0039] The weight percentage of chromium is not more than 2.4%. It should be noted that too high a chromium content will lead to an increase in the ferrite content, which will reduce the structural strength and mechanical properties of the material. In this way, by setting an appropriate weight percentage of chromium, the solubility of nitrogen in the welding material can be increased to improve the structural strength and mechanical properties of the welding material.

[0040] The weight percentage of the molybdenum element can be 0.9%, 0.95%, 1%, 1.05% or 1.1%, etc. Here, since the molybdenum element is a ferrite-forming element, by setting the appropriate weight percentage of the molybdenum element, not only the pitting corrosion resistance of the welding material can be improved, but also the increase of ferrite can be reduced, thereby reducing the precipitation of harmful phases and improving the homogeneity of the welding material.

[0041] The weight percentage of vanadium is less than 0.5%. It should be noted that when the content of vanadium is excessive, the toughness and ductility of the welding material may be reduced. In this way, by setting an appropriate weight percentage of vanadium, the structural strength of the welding material can be improved.

[0042] The weight percentage of boron is less than 0.005%. It should be noted that boron is an element with a large neutron absorption cross section, and excessive addition will cause the welding material to fail under neutron irradiation conditions. In this way, by setting an appropriate weight percentage of boron, not only can the grain boundary strength of the welding material be improved, but also the failure of the welding material's radiation resistance can be reduced.

[0043] In one embodiment, the weight percentage of manganese element is between 0.35% and 0.5%, the weight percentage of tungsten element is less than 0.01%, and the weight percentage of chromium element is between 2.1% and 2.4%.

[0044] For example, the weight percentage of manganese element may be 0.35%, 0.4%, 0.45% or 0.5%, etc. Thus, by setting a suitable weight percentage of manganese element, the corrosion resistance of the welding material to chloride salts may be improved to a certain extent.

[0045] The weight percentage of the tungsten element can be 0.02%, 0.04%, 0.06% or 0.08%. In this way, by setting the tungsten element, the corrosion resistance of the welding material to chloride salts and cadmium-containing high-temperature liquids can be improved to a certain extent.

[0046] The weight percentage of chromium element can be 2.1%, 2.15%, 2.2%, 2.25%, 2.3%, 2.35% or 2.4%, etc., which can significantly improve the corrosion resistance of the welding material to cadmium-containing high-temperature liquid and the structural strength of the welding material.

[0047] In one embodiment, the weight percentage of carbon is between 0.11% and 0.13%, the weight percentage of manganese is between 0.35% and 0.5%, the weight percentage of silicon is less than 0.2%, the weight percentage of tungsten is less than 0.01%, the weight percentage of chromium is between 2.1% and 2.4%, the weight percentage of molybdenum is between 0.9% and 1.1%, the weight percentage of vanadium is less than 0.5%, the weight percentage of boron is less than 0.005%, and the balance is iron. In this way, on the one hand, it can not only improve the corrosion resistance of the welding material to chloride salts and cadmium-containing high-temperature liquids to a certain extent, but also significantly improve the structural strength and mechanical properties of the welding material; on the other hand, it can also improve the compatibility with P22 stainless steel materials and achieve welding of the same material.

[0048] In one embodiment, the weight percentage of manganese element is less than 0.1%, the weight percentage of tungsten element is between 0.2% and 0.6%, the weight percentage of chromium element is between 1.1% and 1.4%, the weight percentage of vanadium element is between 0.15% and 0.35%, and the weight percentage of boron element is between 0.001% and 0.003%.

[0049] Exemplarily, the weight percentage of manganese element can be 0.02%, 0.04%, 0.06% or 0.08%. Thus, by setting a suitable manganese element, the corrosion resistance of the welding material to chloride salts can be significantly improved.

[0050] The weight percentage of the tungsten element can be 0.2%, 0.3%, 0.4%, 0.5% or 0.6%, etc. Here, by setting a suitable tungsten element, the corrosion resistance of the welding material to chloride salts and cadmium-containing high-temperature liquids can be significantly improved.

[0051] The weight percentage of chromium element can be 1.1%, 1.2%, 1.3% or 1.4%, etc. In this way, by setting the appropriate weight percentage of chromium element, the structural strength of the welding material can be improved to a certain extent.

[0052] The weight percentage of the vanadium element may be 0.15%, 0.2%, 0.25%, 0.3% or 0.35%, etc. Here, by setting a suitable weight percentage of the vanadium element, the structural strength of the welding material may be improved to a certain extent.

[0053] The weight percentage of boron can be 0.001%, 0.002% or 0.003%, etc. Here, by setting a suitable weight percentage of boron, not only the grain boundary strength of the welding material can be improved to a certain extent, but also the failure of the welding material's radiation resistance can be reduced.

[0054] In one embodiment, the weight percentage of carbon is between 0.11% and 0.13%, the weight percentage of manganese is less than 0.1%, the weight percentage of silicon is less than 0.2%, the weight percentage of tungsten is between 0.2% and 0.6%, the weight percentage of chromium is between 1.1% and 1.4%, the weight percentage of molybdenum is between 0.9% and 1.1%, the weight percentage of vanadium is between 0.15% and 0.35%, the weight percentage of boron is between 0.001% and 0.003%, and the balance is iron. In this way, on the one hand, not only can the corrosion resistance of the welding material to chloride salts and cadmium-containing high-temperature liquids be significantly improved, but also the structural strength and mechanical properties of the welding material can be improved to a certain extent; on the other hand, the compatibility with P22 stainless steel material can be improved to achieve welding of the same material.

[0055] In one embodiment, S2, the step of heating and forging the steel ingot to obtain a square bar, comprises:

[0056] S21, placing the steel ingot in a heating furnace for heating, wherein the heating temperature is between 1100° C. and 1150° C., and the holding time is 3 hours;

[0057] S22. After uniform heat preservation, the steel ingot is forged, and then forged into the square rod by two-fire forging through drawing and roughening.

[0058] Exemplarily, the steel ingot is placed in a heating furnace for heating, and the heating temperature can be 1100°C, 1110°C, 1120°C, 1130°C, 1140°C or 1150°C, etc., and the insulation time can be 3 hours. In this way, after uniform insulation, that is, after the temperature of various parts on the steel ingot is roughly the same, it can be forged. Through multiple lengthening and roughening, as well as quenching and tempering, it can be forged into a square rod. In this way, the mechanical properties of subsequent welding materials can be improved.

[0059] In one embodiment, the holding temperature of the hot rolling process is between 1100° C. and 1150° C., the holding time of the hot rolling process is between 1 h and 1.5 h, and the wire rod is formed by hot continuous rolling.

[0060] Exemplarily, the holding temperature of hot rolling can be 1100°C, 1110°C, 1120°C, 1130°C, 1140°C or 1150°C, etc. The holding time of hot rolling can be 1h, 1.1h, 1.2h, 1.3h, 1.4h or 1.5h, etc., and finally the square bar can be rolled into a wire rod by a hot rolling mill. In this way, on the one hand, the square bar can be easily rolled into a required shape and size after hot rolling, with strong processing flexibility and high production efficiency; on the other hand, the hot rolling process can refine the grains inside the metal, make the surface oxidation of the wire rod obvious, the oxide scale becomes loose, and there are no defects such as cracks, folds and scars, so that the strength, toughness and ductility of subsequent welding materials can be improved.

[0061] In one embodiment, the diameter of the wire rod can be 8.5 mm, so that it is convenient to draw it into welding wire.

[0062] In one embodiment, the temperature of the heat treatment process is between 640° C. and 760° C., and the holding time of the heat treatment process is between 1 hour and 1.5 hours.

[0063] For example, the temperature of the heat treatment process may be 640°C, 650°C, 660°C, 670°C, 680°C, 690°C, 700°C, 710°C, 720°C, 730°C, 740°C, 750°C or 760°C, etc. The holding time of the heat treatment process may be 1h, 1.1h, 1.2h, 1.3h, 1.4h or 1.5h, etc. In this way, by setting the appropriate temperature and holding time of the heat treatment process, not only the microstructure and grain size of the metal can be regulated, but also the precipitates of carbides can be melted back into the matrix to improve the homogenization of the welding material.

[0064] In one embodiment, the cold drawing process includes: firstly grinding the surface of the wire rod and applying a coating agent on the surface, then performing single-pass cold drawing, vacuum annealing and continuous cold drawing, and finally winding the wire into a coil to obtain the welding material.

[0065] For example, the surface of the wire rod can be polished first, so that not only can the surface attachments such as oxide scale be removed, but also the surface roughness can be improved, which is convenient for subsequent processing. By applying a film agent on the surface, on the one hand, a protective film can be formed on the surface of the wire rod to prevent moisture, oxygen and other corrosive media from contacting the matrix of the wire rod, thereby slowing down or preventing the occurrence of corrosion reactions; on the other hand, it can be used for subsequent cold drawing to reduce wear. Then a single-pass cold drawing can be used to draw the wire rod for the first time, so that the wire rod is roughly drawn into the required size and shape, and then it is vacuum annealed to improve the microstructure in the metal material, improve the ductility and toughness, and also discharge the impurities inside the metal to improve the cleanliness of the subsequent welding material. Finally, it can be drawn into the welding material of the required size by continuous cold drawing, and then collected around the disk, which can protect the welding material.

[0066] Exemplarily, in one embodiment, the shape of the welding material can be strip or wire.

[0067] In one embodiment, the temperature of vacuum annealing is between 640° C. and 760° C., and the time of vacuum annealing is between 1 hour and 1.5 hours.

[0068] Exemplarily, the temperature of vacuum annealing can be 640°C, 650°C, 660°C, 670°C, 680°C, 690°C, 700°C, 710°C, 720°C, 730°C, 740°C, 750°C or 760°C, etc. The holding time of vacuum annealing can be 1h, 1.1h, 1.2h, 1.3h, 1.4h or 1.5h, etc. In this way, by setting the appropriate temperature and time of vacuum annealing, the tensile properties of the metal can be effectively improved, and the impurities in the metal can be significantly reduced, and the cleanliness is high.

[0069] In one embodiment, the impurities in the welding material include sulfur and phosphorus, the weight percentage of sulfur is less than 0.003%, and the weight percentage of phosphorus is not more than 0.007%.

[0070] In this way, the toughness of the welding material can be improved and the thermal cracking of the welding material can be reduced, so that the welding material can adapt to the high-temperature electrolytic refining environment.

[0071] In one embodiment, the tensile yield strength of the welding material is between 360 MPa and 530 MPa, the tensile strength of the welding material is between 510 MPa and 690 MPa, and the elongation of the welding material is between 25% and 40%.

[0072] In this way, the tensile properties of the weld can be improved to meet subsequent welding requirements.

[0073] It should be noted that the chemical composition and corresponding weight percentage of the substrate are substantially the same as the chemical composition and corresponding weight percentage of the prepared welding material.

[0074] Exemplarily, in one embodiment, the chemical components of the substrate and the corresponding weight percentages are: carbon: 0.11%; manganese: less than 0.03%; silicon: less than 0.1%; tungsten: 0.4%; chromium: 1.23%; molybdenum: between 1.0% and 1.1%; vanadium: 0.26%; boron: 0.0026%; nitrogen: 0.0012%; the balance is iron. The substrate is first placed in a vacuum induction furnace for smelting to prepare a steel ingot. The steel ingot can be forged after a holding time of 3 hours at any temperature between 1100°C and 1150°C in a heating furnace, and after being stretched and roughened, it is forged into a square bar with a size of 45mm×45mm. The square rod is hot-rolled, and the holding temperature of the hot rolling process is kept at any temperature between 1100℃ and 1150℃ for 1h to 1.5h, and hot-rolled to a wire rod with a final diameter of 8.5mm; the surface oxidation of the wire rod is obvious, the oxide scale is relatively loose, and there are no defects such as cracks, folds and scars. Then the heat treatment process of the wire rod is carried out, and the heat treatment process is: keep warm at a temperature of 760℃ for 1.5h. Then the wire rod is further processed by the cold drawing process, and the process includes: surface grinding, surface coating agent, single-pass cold drawing, vacuum annealing (temperature is 760℃, holding time is 1.5h), continuous cold drawing, winding and coiling, and finally the finished welding wire is obtained. The impurity content of the welding wire is: sulfur element is less than 0.0025%, and phosphorus element is less than 0.006%. Then, the prepared welding wire was subjected to a room temperature tensile performance test according to GB / T 228.8-2021 "Tensile Test of Metallic Materials Part 1: Room Temperature Test Method", and the results showed that its tensile yield strength was 401 MPa, the tensile strength was 555 MPa, and the elongation was 34%.

[0075] Exemplarily, in one embodiment, the chemical components of the substrate and the corresponding weight percentages are: carbon: 0.091%; manganese: 0.39%; silicon: less than 0.1%; tungsten: 0.005%; chromium: 2.22%; molybdenum: 1.02%; vanadium: less than 0.03%; boron: less than 0.0005%; nitrogen: 0.0008%; the balance is iron. The substrate is first placed in a vacuum induction furnace for smelting to prepare a steel ingot. The steel ingot can be forged after being held in a heating furnace at any temperature between 1100°C and 1150°C for 3 hours, and then forged, stretched and roughened, and forged into a square bar with a size of 45mm×45mm. The square bars are hot rolled, and the holding temperature of the hot rolling process is kept at any temperature between 1100℃ and 1150℃ for 1h to 1.5h, and hot rolled to a wire rod with a final diameter of 8.5mm; the surface oxidation of the wire rod is obvious, the oxide scale is relatively loose, and there are no defects such as cracks, folds and scars. Then the heat treatment process of the wire rod is carried out, and the heat treatment process is: keep warm at a temperature of 760℃ for 1.5h. Then the wire rod is further processed by the cold drawing process, and the process includes: surface grinding, surface coating agent, single-pass cold drawing, vacuum annealing (temperature is 760℃, holding time is 1.5h), continuous cold drawing, winding and coiling, and finally the finished welding wire is obtained. The impurity content of the welding wire is: sulfur element is less than 0.0025%, and phosphorus element is less than 0.005%. Then, the prepared welding wire was subjected to a room temperature tensile performance test according to GB / T 228.8-2021 "Tensile Test of Metallic Materials Part 1: Room Temperature Test Method", and the results showed that its tensile yield strength was 529 MPa, the tensile strength was 680 MPa, and the elongation was 27%.

[0076] The above is only a preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. All modifications, equivalent substitutions, improvements, etc. within the spirit and principles of the present application are included in the protection scope of the present application.

Claims

1. A method for preparing P22 stainless steel welding material, characterized in that: include: placing a substrate in a vacuum induction furnace for smelting to obtain a steel ingot, wherein the chemical composition of the substrate includes carbon, manganese, silicon, tungsten, chromium, molybdenum, vanadium, boron and iron; Heating and forging the steel ingot to obtain a square bar; Hot rolling the square bar to obtain a wire rod; After the wire rod is subjected to a heat treatment process, the wire rod is subjected to a cold drawing process to obtain a welding material.

2. The preparation method according to claim 1, characterized in that: The weight percentage of the carbon element is between 0.11% and 0.13%, the weight percentage of the manganese element is not more than 0.5%, the weight percentage of the silicon element is less than 0.2%, the weight percentage of the tungsten element is not more than 0.6%, the weight percentage of the chromium element is not more than 2.4%, the weight percentage of the molybdenum element is between 0.9% and 1.1%, the weight percentage of the vanadium element is less than 0.5%, the weight percentage of the boron element is less than 0.005%, and the balance is iron element.

3. The preparation method according to claim 2, characterized in that: The weight percentage of the manganese element is between 0.35% and 0.5%, the weight percentage of the tungsten element is less than 0.01%, and the weight percentage of the chromium element is between 2.1% and 2.4%.

4. The preparation method according to claim 2, characterized in that: The weight percentage of the manganese element is less than 0.1%, the weight percentage of the tungsten element is between 0.2% and 0.6%, the weight percentage of the chromium element is between 1.1% and 1.4%, the weight percentage of the vanadium element is between 0.15% and 0.35%, and the weight percentage of the boron element is between 0.001% and 0.003%.

5. The preparation method according to claim 1, characterized in that: The step of heating and forging the steel ingot to obtain a square bar comprises: The steel ingot is placed in a heating furnace for heating, wherein the heating temperature is between 1100° C. and 1150° C., and the holding time is 3 hours; After being evenly heat-insulated, the steel ingot is forged, and then forged into the square rod by two-fire forging through drawing and roughening.

6. The preparation method according to claim 1, characterized in that: The holding temperature of the hot rolling process is between 1100° C. and 1150° C., the holding time of the hot rolling process is between 1 h and 1.5 h, and the wire rod is formed by hot continuous rolling.

7. The preparation method according to claim 1, characterized in that: The temperature of the heat treatment process is between 640° C. and 760° C., and the insulation time of the heat treatment process is between 1 hour and 1.5 hours.

8. The preparation method according to claim 1, characterized in that: The cold drawing process comprises: Firstly, the wire rod is surface-grinded and coated with a coating agent, then single-pass cold drawing, vacuum annealing and continuous cold drawing are performed, and finally the wire is wound around a coil to obtain the welding material.

9. The preparation method according to claim 1, characterized in that: The impurities in the welding material include sulfur and phosphorus, the weight percentage of the sulfur is less than 0.003%, and the weight percentage of the phosphorus is not more than 0.007%.

10. The preparation method according to claim 1, characterized in that: The tensile yield strength of the welding material is between 360MPa and 530MPa, the tensile strength of the welding material is between 510MPa and 690MPa, and the elongation of the welding material is between 25% and 40%.

Citation Information

Cited By

  • Welding material for stainless steel hot roll and surfacing process thereof

    CN120587753A