Production method of titanium alloy forged part for artificial dental implant
Through the multi-stage forging and quenching treatment, the problems of long production cycle, low yield and high cost during the preparation of forged parts of titanium alloy artificial dental implants are solved, and the uniformity of metallographic structure and stability of performance are achieved. , improves efficiency and yield.
Patent Information
- Application Number
- CN202411010024.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-15
AI Technical Summary
In the preparation process of titanium alloy artificial dental implant forged parts in the prior art, the rolled sheet has a long production cycle, low yield, high cost, and the metallographic structure of the forged blank is unqualified and the performance is unstable.
By using multi-stage forging and quenching treatment, the titanium alloy ingots are prepared, and multiple forging and quenching treatments are performed, the forging temperature and deformation amount are controlled, and the annealing and mechanical finishing are finally carried out to obtain titanium alloy forging that meets medical standards. Production parts.
It achieves uniform compliance with metallographic structure, stable performance, high yield, short production cycle, high efficiency, low processing cost and stable mechanical performance.
Smart Images

Figure CN118951607A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nonferrous technology heat processing, and in particular to a production method of a titanium alloy forging for an artificial tooth implant. Background Art
[0002] Titanium and titanium alloy artificial dental implants (including crowns, bridges, inlays, posts and cores, connectors, implants, etc.) have been widely used in clinical applications to replace traditional dental restoration materials. Implants are mainly made of titanium alloy discs (eight specifications of D98×10~25mm) and blocks (eight specifications of 150×140×10~25mm; 220×150×11~25mm) through precision machining of CNC machining centers. Therefore, the key to the preparation of titanium alloy discs and blocks for implants is the production of sheet blanks (15 thickness specifications of side length or diameter 100~220mm×thickness 10~25mm). Since titanium alloy materials for dental use need to obtain Class II medical device production certification, the material properties must comply with the requirements of GB / T13810-2017 standards, and their organization must also be evaluated according to Appendix A, and the organization type should comply with A1-A9. In order to meet the organizational performance requirements, early discs and blocks were mainly loaded and unloaded from large-sized medium and thick plates produced according to GJB standards. The plates produced according to military standards are few in variety and too expensive to meet the needs of more than 15 specifications of implant discs and blocks with a thickness of 10mm to 25mm. Therefore, the key to the preparation of implant discs and blocks is to produce forged rods that meet medical standards and have a side length (or diameter) of more than 200mm.
[0003] At present, the industry attempts to use ingots with a diameter greater than 580 mm, and to prepare square billets by performing large deformation forging and high temperature multi-fire large deformation upsetting deformation at a temperature of 100-200°C above the β phase transformation point, and then multi-fire upsetting deformation production methods in the two-phase region. However, due to the large size of the finished forging billet, at least 11 fires of forging and upsetting are required to meet the organizational performance requirements of dental materials. This process has many high-temperature deformation fires, complex upsetting deformation processes, and a long process flow. The material is severely oxidized and cracked during multiple deformations in the two-phase region, the workload of billet grinding is large, the material loss exceeds 25%, and the yield rate is low. It is also not suitable for the production of dental discs and square forging billets, so new process technologies need to be developed. Summary of the invention
[0004] The present invention provides a production method of titanium alloy forgings for artificial dental implants, which is used to solve the technical problems of long production cycle of rolled plates, low yield, high cost, unqualified metallographic structure of forged blanks and unstable performance in the preparation process of forgings in the prior art, and achieves the technical effects of uniform metallographic structure, stable performance, high yield, short production cycle, high efficiency, low processing cost and stable mechanical properties.
[0005] The present invention provides a method for producing a titanium alloy forging for an artificial dental implant, the method comprising: step 1: preparing a medical titanium alloy ingot according to a preset requirement, and treating the titanium alloy ingot by a first treatment method to obtain a first qualified ingot; step 2: heating the first qualified ingot obtained in step 1 according to a first heating condition, forging it on a fast forging machine according to a first forging condition to obtain a first forging blank, and quenching the first forging blank according to a first quenching condition to obtain a first qualified forging blank; step 3: heating the first qualified ingot obtained in step 1 according to a first heating condition, and forging it on a fast forging machine according to a first forging condition to obtain a first qualified forging blank; Step 2: heating the first qualified forging blank obtained in step 3 to a temperature of Tβ+50°C above the phase transformation point, forging it according to the second forging condition to obtain a second qualified forging blank; Step 4: heating the second qualified forging blank obtained in step 3 to a temperature of Tβ-(30-60°C) below the phase transformation point, forging it according to the third forging condition to obtain a first finished blank; Step 5: heating the second qualified forging blank obtained in step 3 to a temperature of Tβ-(30-60°C) below the phase transformation point, forging it according to the fourth forging condition to obtain a third qualified forging blank; Step 6: The third qualified forging billet obtained in step 5 is heated to a temperature below the phase transformation point Tβ-(30-60°C), forged according to the fifth forging condition and a second finished billet is obtained; step 7: the third qualified forging billet obtained in step 5 is heated to a temperature below the phase transformation point Tβ-(30-60°C), forged according to the sixth forging condition and a first qualified rolled billet is obtained; step 8: the first qualified rolled billet obtained in step 7 is heated to a temperature below the phase transformation point Tβ-(40-70°C), forged according to the seventh forging condition and a first qualified rolled billet is obtained. Three finished billets; Step 9: annealing the first finished billet obtained in Step 4, the second finished billet obtained in Step 6, and the third finished billet obtained in Step 8; Step 10: reserving finishing cutting allowance for the first finished billet, the second finished billet, and the third finished billet that have been annealed in Step 9, cutting them according to the size of the titanium alloy forging for artificial dental implants, and then obtaining the titanium alloy forging for artificial dental implants through mechanical finishing.
[0006] Preferably, in step 1, the preset requirement is to prepare an alloy ingot that meets the requirements of GB / T13810-2017 standard and has a specification of Φ620 mm; the first processing method is to cut a riser from the titanium alloy ingot, remove surface pores, and saw the material into an ingot block of Φ620×500±100 mm, and use the ingot block as the first qualified ingot.
[0007] Preferably, in step 2, the first heating condition is: heating the first qualified ingot in stages to Tβ+(160-260°C) in an electric furnace or a gas heating furnace, and the heating and holding time is 280-300 minutes; the first forging condition is: forging the first qualified ingot into the first forging blank with a side length of 490×Lmm, wherein the deformation is 20%, and the final forging temperature is greater than or equal to Tβ+50°C; the first quenching condition is: quenching the first forging blank with a side length of 490×Lmm into a water tank for rapid cooling under the condition that the final forging temperature is greater than or equal to Tβ+50°C, and the cooling water in the water tank needs to be pumped for circulation.
[0008] Preferably, in step 3, the second forging condition is: the first qualified forging blank is forged into a square billet with a side length of 270±20 mm by one fire and multiple passes, wherein the deformation of the forging pass is greater than or equal to 20%, the total deformation of the fire is 70%±10%, and the final forging temperature is greater than or equal to 750°C.
[0009] Preferably, in step 4, the third forging condition is specifically: the second qualified forging blank is forged into a finished rectangular forging blank with a side length of 225mm×155×Lmm by one fire and multiple passes, wherein the deformation amount of each pass is greater than or equal to 15%, and the total deformation amount of each fire is greater than or equal to 50%.
[0010] Preferably, in step 5, the fourth forging condition is specifically as follows: the second qualified forging blank is forged into a second forging blank with a side length of 225×Lmm through one fire and multiple forging passes, wherein the deformation amount of each pass is greater than or equal to 20%, and the deformation amount of each fire is greater than or equal to 50%.
[0011] Preferably, in step 6, the fifth forging condition is specifically: subjecting the third qualified forging blank to one fire and multiple forging passes to form a finished forging blank with a side length of 155mm×145×Lmm, wherein the deformation amount of each pass is greater than or equal to 20%, and the total deformation amount of each fire is greater than or equal to 50%.
[0012] Preferably, in step 7, the sixth forging condition is specifically: subjecting the third qualified forging blank to one fire and multiple forging passes to form a third forging blank with a side length of 155×Lmm, wherein the deformation amount of each pass is greater than or equal to 20%, and the deformation amount of each fire is greater than or equal to 50%.
[0013] Preferably, in step 8, the seventh forging condition is specifically: the first qualified billet is rolled into a finished round bar billet of Φ103×Lmm through one fire and multiple passes on a 550 type bar rolling mill, and the finished round bar billet is used as the third finished billet.
[0014] Preferably, in step 9, the annealing treatment is based on the process parameters in the GB / T13810-2017 standard.
[0015] The above one or more technical solutions in the embodiments of the present invention have at least one or more of the following technical effects:
[0016] The present invention provides a method for producing a titanium alloy forging for an artificial dental implant, the method comprising: step 1: preparing a medical titanium alloy ingot according to preset requirements, and treating the titanium alloy ingot by a first treatment method to obtain a first qualified ingot; step 2: heating the first qualified ingot obtained in step 1 according to a first heating condition, forging it on a fast forging machine according to a first forging condition to obtain a first forging blank, and quenching the first forging blank according to a first quenching condition to obtain a first qualified forging blank; step 3: heating the first qualified forging blank obtained in step 2 to a temperature above the phase transition point Tβ+50°C. temperature, forging according to the second forging condition and obtaining a second qualified forging billet; step 4: heating the second qualified forging billet obtained in step 3 to a temperature below the phase transformation point Tβ-(30-60°C), forging according to the third forging condition and obtaining a first finished billet; step 5: heating the second qualified forging billet obtained in step 3 to a temperature below the phase transformation point Tβ-(30-60°C), forging according to the fourth forging condition and obtaining a third qualified forging billet; step 6: heating the third qualified forging billet obtained in step 5 to a temperature below the phase transformation point Tβ-(30-60°C), forging according to the fifth forging condition and obtaining a first finished billet. Step 7: heating the third qualified forging billet obtained in step 5 to a temperature below the phase transformation point Tβ-(30-60°C), forging according to the sixth forging condition and obtaining a first qualified rolling billet; Step 8: heating the first qualified rolling billet obtained in step 7 to a temperature below the phase transformation point Tβ-(40-70°C), forging according to the seventh forging condition and obtaining a third finished billet; Step 9: annealing the first finished billet obtained in step 4, the second finished billet obtained in step 6, and the third finished billet obtained in step 8; Step 10: annealing the first finished billet obtained in step 9 The first finished blank, the second finished blank and the third finished blank after fire treatment are reserved with finishing cutting allowances, and are cut according to the size of the titanium alloy forging for artificial dental implants. Then, the titanium alloy forging for artificial dental implants are obtained through mechanical finishing, thereby solving the technical problems of long production cycle of rolled plates, low yield, high cost, unqualified metallographic structure of forged blanks and unstable performance in the preparation process of forgings in the prior art, and achieving the technical effects of uniform metallographic structure, stable performance, high yield, short production cycle, high efficiency, low processing cost and stable mechanical properties.
[0017] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention, it can be implemented according to the contents of the specification. In order to make the above and other purposes, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are listed below. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 The present invention is a schematic diagram of a process for producing a titanium alloy forging for an artificial dental implant according to an embodiment of the present invention.
[0019] Figure 2 The grain map of a titanium alloy forging for artificial dental implant according to an embodiment of the present invention is shown in FIG.
[0020] Figure 3 The grain map of another titanium alloy forging for artificial dental implant according to the embodiment of the present invention is shown in FIG.
[0021] Figure 4 The grain map of another titanium alloy forging for artificial dental implant according to the embodiment of the present invention is as follows: DETAILED DESCRIPTION
[0022] The embodiment of the present invention provides a method for producing titanium alloy forgings for artificial dental implants, which is used to solve the technical problems of long production cycle of rolled plates, low yield, high cost, unqualified metallographic structure of forged billets and unstable performance in the preparation process of forgings in the prior art.
[0023] The technical solution in the embodiment of the present invention has the following general idea:
[0024] The method for producing a titanium alloy forging for an artificial dental implant provided in an embodiment of the present invention comprises the following steps: 1: preparing a medical titanium alloy ingot according to preset requirements, and treating the titanium alloy ingot by a first treatment method to obtain a first qualified ingot; 2: heating the first qualified ingot obtained in step 1 according to a first heating condition, forging it on a fast forging machine according to a first forging condition to obtain a first forging blank, and quenching the first forging blank according to a first quenching condition to obtain a first qualified forging blank; 3: heating the first qualified forging blank obtained in step 2 to a temperature of Tβ+50°C above the phase transformation point, forging according to the second forging condition to obtain a second qualified forging billet; step 4: heating the second qualified forging billet obtained in step 3 to a temperature of Tβ-(30-60°C) below the phase transformation point, forging according to the third forging condition to obtain a first finished billet; step 5: heating the second qualified forging billet obtained in step 3 to a temperature of Tβ-(30-60°C) below the phase transformation point, forging according to the fourth forging condition to obtain a third qualified forging billet; step 6: heating the third qualified forging billet obtained in step 5 to a temperature of Tβ-(30-60°C) below the phase transformation point -(30~60℃), forge according to the fifth forging condition and obtain the second finished billet; Step 7: heat the third qualified forging billet obtained in step 5 to a temperature below the phase transformation point Tβ-(30~60℃), forge according to the sixth forging condition and obtain the first qualified rolled billet; Step 8: heat the first qualified rolled billet obtained in step 7 to a temperature below the phase transformation point Tβ-(40~70℃), forge according to the seventh forging condition and obtain the third finished billet; Step 9: heat the first finished billet obtained in step 4 and the first qualified rolled billet obtained in step 6 The second finished billet and the third finished billet obtained in step 8 are annealed; step 10: the first finished billet, the second finished billet and the third finished billet which have been annealed in step 9 are reserved with finishing cutting allowance, and the billets are cut according to the size of the titanium alloy forgings for artificial dental implants. After mechanical finishing, the titanium alloy forgings for artificial dental implants are obtained, achieving the technical effect of uniform metallographic structure, stable performance, high yield, short production cycle, high efficiency, low processing cost and stable mechanical properties.
[0025] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] Embodiment 1
[0027] Figure 1 FIG. 1 is a schematic diagram of a process for producing a titanium alloy forging for an artificial dental implant according to an embodiment of the present invention. Figure 1 As shown, the production method of the titanium alloy forging for artificial dental implants includes:
[0028] Step 1: According to preset requirements, a medical titanium alloy ingot is prepared, and the titanium alloy ingot is treated by a first treatment method to obtain a first qualified ingot.
[0029] Furthermore, in step 1, the preset requirement is to prepare an alloy ingot that meets the requirements of GB / T13810-2017 standard and has a specification of Φ620 mm; the first processing method is to cut a riser from the titanium alloy ingot, remove surface pores, and saw the material into an ingot block of Φ620×500±100 mm, and use the ingot block as the first qualified ingot.
[0030] Specifically, according to the requirements, it is necessary to prepare medical titanium and titanium alloy ingots first. In this embodiment, the preset requirement is to prepare alloy ingots that meet the requirements of GB / T13810-2017 standard and have a diameter of Φ620mm as a preferred method. Then the alloy ingot is treated by the first treatment method to obtain the first qualified ingot. In this embodiment, the first treatment method used is to cut the riser of the titanium alloy ingot, remove the surface pores, and saw the material into a block of Φ620×500±100mm as the first qualified ingot.
[0031] Step 2: After heating the first qualified ingot obtained in step 1 according to the first heating condition, forging it on a fast forging machine according to the first forging condition to obtain a first forging blank, and quenching the first forging blank according to the first quenching condition to obtain a first qualified forging blank.
[0032] Furthermore, in the step 2, the first heating condition is: heating the first qualified ingot in stages to Tβ+(160-260°C) in an electric furnace or a gas heating furnace, and the heating and holding time is 280-300 minutes; the first forging condition is: forging the first qualified ingot into the first forging blank with a side length of 490×Lmm, wherein the deformation is 20%, and the final forging temperature is greater than or equal to Tβ+50°C; the first quenching condition is: quenching the first forging blank with a side length of 490×Lmm into a water tank for rapid cooling under the condition that the final forging temperature is greater than or equal to Tβ+50°C, and the cooling water in the water tank needs to be pumped for circulation.
[0033] Specifically, after obtaining the first qualified ingot, the first qualified ingot needs to be heated, wherein the first heating condition is: heating the first qualified ingot in stages to Tβ+(160-260°C) in an electric furnace or a gas heating furnace, the heating and holding time is 280-300 minutes, wherein the ingot heating time is D / 2+20-40 minutes (where D is the diameter of the ingot or the side length of the billet, in mm); further forging the heated ingot on a fast forging machine according to the first forging condition, wherein the first forging condition is: heating the heated first qualified ingot Φ6 20×500 is quickly forged into a first forging blank with a side length of 490×L on a fast forging machine, the deformation is controlled to be about 20%, and the final forging temperature is controlled to be not less than Tβ+50℃; then, the first forging blank is quenched according to the first quenching condition, wherein the first quenching condition is: quickly quench the first forging blank with a side length of 490×Lmm into a water tank for rapid cooling under the condition that the final forging temperature is greater than or equal to Tβ+50℃, and the water tank is pumped to circulate to increase the cooling rate of the bar blank, therefore, the first qualified ingot is treated as the first qualified forging blank after the above forging + quenching treatment of 490×L. It is subjected to a rapid unidirectional deformation of 2500 tons in one fire and multiple passes at above the β phase transformation point Tβ+160~260℃, the deformation is controlled to be about 20%, and the final forging temperature is controlled to be not less than Tβ+50℃, and then the forging blank with a final forging temperature not less than Tβ+50℃ is quickly quenched into a water tank for rapid cooling, and the water tank is pumped to form a circulating coolant to increase the cooling rate.
[0034] Step 3: Heat the first qualified forging blank obtained in step 2 to a temperature above the phase transformation point Tβ+50°C, forge it according to the second forging conditions and obtain a second qualified forging blank.
[0035] Furthermore, in the step 3, the second forging condition is: the first qualified forging blank is forged into a square billet with a side length of 270±20 mm by one fire and multiple passes, wherein the deformation of the forging pass is greater than or equal to 20%, the total deformation of the fire is 70%±10%, and the final forging temperature is greater than or equal to 750°C.
[0036] Specifically, after obtaining the first qualified forging blank, the first qualified forging blank needs to be heated. That is, the first qualified forging blank 490×Lmm is heated to a temperature above the phase transformation point Tβ+50℃. Then forging is performed according to the second forging condition to obtain the second qualified forging blank. Among them, the second forging condition is: the first qualified forging blank is forged into a square billet of 270±20mm by one fire and multiple passes, the deformation of the forging pass is not less than 20%, the total deformation of the fire is 70%±10%, the final forging temperature is not lower than 750℃, and the material is sawn into a rod billet with a length of 500~1200mm, and then the first qualified forging blank is transformed into a square billet with a side length of 270±20mm by 70% through the above-mentioned one fire and multiple passes as the second qualified forging blank.
[0037] Step 4: Heat the second qualified forging blank obtained in step 3 to a temperature below the phase transformation point Tβ-(30-60°C), forge it according to the third forging conditions and obtain the first finished blank.
[0038] Furthermore, in step 4, the third forging condition is specifically as follows: the second qualified forging blank is forged into a finished rectangular forging blank with a side length of 225mm×155×Lmm by one fire and multiple passes, wherein the deformation amount of each pass is greater than or equal to 15%, and the total deformation amount of each fire is greater than or equal to 50%.
[0039] Specifically, after obtaining the second qualified forging blank, it is necessary to heat the second qualified forging blank to a temperature below the phase transformation point Tβ-(30-60°C), forge it according to the third forging condition and obtain the first finished blank. Among them, the third forging condition is: adopt one fire and multiple passes to forge into a finished forging blank of 225×155×Lmm, the deformation of each pass is not less than 15%, and the total deformation of each fire is not less than 50%; and then use the second qualified forging blank after the above forging deformation process to form a finished rectangular bar forging blank with a side length of 225×155×Lmm as the first finished blank.
[0040] Step 5: Heat the second qualified forging blank obtained in step 3 to a temperature below the phase transformation point Tβ-(30-60°C), forge it according to the fourth forging condition and obtain a third qualified forging blank.
[0041] Furthermore, in step 5, the fourth forging condition is specifically as follows: the second qualified forging blank is forged into a second forging blank with a side length of 225×Lmm through one fire and multiple forging passes, wherein the deformation amount of each pass is greater than or equal to 20%, and the deformation amount of each fire is greater than or equal to 50%.
[0042] Specifically, after obtaining the second qualified forging blank, it is necessary to heat the second qualified forging blank to a temperature below the phase transformation point Tβ-(30-60°C), and then forge it according to the fourth forging condition to obtain the third qualified forging blank. Among them, the fourth forging condition is: the second qualified forging blank is forged into a second forging blank of 225×L through one fire and multiple passes, the deformation amount of each pass is not less than 20%, and the deformation amount of each fire is not less than 50%, and then the forging blank with a side length of 225×L after the above deformation is used as the third qualified forging blank.
[0043] Step 6: Heat the third qualified forging blank obtained in step 5 to a temperature below the phase transformation point Tβ-(30-60°C), forge it according to the fifth forging condition and obtain a second finished blank.
[0044] Furthermore, in step 6, the fifth forging condition is specifically as follows: subjecting the third qualified forging blank to one fire and multiple forging passes to form a finished forging blank with a side length of 155mm×145×Lmm, wherein the deformation amount of each pass is greater than or equal to 20%, and the total deformation amount of each fire is greater than or equal to 50%.
[0045] Specifically, after the third qualified forging blank obtained in step 5 is heated to a temperature below the phase transformation point Tβ-(30-60°C), it is forged according to the fifth forging condition to obtain a second finished blank. The fifth forging condition is: the third qualified forging blank is forged into a finished forging blank of 155×145×Lmm through one fire and multiple passes, the deformation of each pass is not less than 20%, and the total deformation of each fire is not less than 50%; finally, the third qualified forging blank is processed by the above forging deformation to form a finished rectangular bar forging blank with a side length of 155×145×Lmm as the second finished blank.
[0046] Step 7: Heat the third qualified forging billet obtained in step 5 to a temperature below the phase transformation point Tβ-(30-60°C), forge it according to the sixth forging condition and obtain the first qualified rolled billet.
[0047] Furthermore, in step 7, the sixth forging condition is specifically: subjecting the third qualified forging blank to one fire and multiple forging passes to form a third forging blank with a side length of 155×Lmm, wherein the deformation amount of each pass is greater than or equal to 20%, and the deformation amount of each fire is greater than or equal to 50%.
[0048] Specifically, the third qualified forging billet obtained in step 5 is heated to a temperature below the phase transformation point Tβ-(30-60°C), and then forged according to the sixth forging condition to obtain the first qualified rolling billet. The sixth forging condition is to forge the third qualified forging billet into a third forging billet of 155×Lmm through one fire and multiple passes, with the deformation amount of each pass not less than 20%, and the deformation amount of each fire not less than 50%, and then the forging billet with a side length of 155×L after the above deformation is used as the first qualified rolling billet.
[0049] Step 8: heating the first qualified rolled billet obtained in step 7 to a temperature below the phase transformation point Tβ-(40-70° C.), forging according to the seventh forging condition to obtain a third finished billet;
[0050] Furthermore, in the step 8, the seventh forging condition is specifically: the first qualified billet is subjected to one fire and multiple passes on a 550 type bar rolling mill to be rolled into a finished round bar billet of Φ103×Lmm, and the finished round bar billet is used as the third finished billet.
[0051] Specifically, the first qualified billet obtained in step 7 is heated to a temperature below the phase transformation point Tβ-(40~70℃), and then forged according to the seventh forging condition to obtain the third finished billet; wherein the seventh forging condition is: the first qualified billet is subjected to one fire and multiple passes on a 550 type bar mill to be rolled into a Φ103×L finished round bar billet, and then the finished round bar billet is used as the third finished billet.
[0052] Step 9: annealing the first finished blank obtained in step 4, the second finished blank obtained in step 6, and the third finished blank obtained in step 8;
[0053] Furthermore, in step 9, the annealing treatment is based on the process parameters in the GB / T13810-2017 standard.
[0054] Specifically, when heat treating the material, the following is done: the first finished rectangular bar blank, the second finished rectangular bar blank and the third finished round bar blank obtained in step 4, step 6 and step 8 are annealed, and in this embodiment, the annealing process is preferably based on the process parameters recommended in the GB / T13810-2017 standard. For example, pure titanium is: 600-700℃ / 1-2hrAC, and titanium alloy is: 700-850℃ / 1-2hrAC.
[0055] Step 10: reserve finishing cutting allowance for the first finished blank, the second finished blank, and the third finished blank that have undergone the annealing treatment in step 9, cut them according to the size of the titanium alloy forging for artificial dental implants, and then obtain the titanium alloy forging for artificial dental implants through mechanical finishing.
[0056] Specifically, after the heat treatment process is completed, mechanical processing is required. Specifically: reserve finishing cutting allowance for the three sizes of finished rod blanks after annealing in step 9, and use sawing or electric spark cutting method to cut the first and second finished rectangular rod blanks and the third finished round rod blank obtained in steps 4, 6, and 8 into disc and square blank sizes. The cut disc and square blanks are mechanically finished on a CNC machining center into titanium alloy discs (eight thickness specifications of D98×10-25mm) and blocks (150×140×10~25mm; 220×150×11~25mm, eight thickness specifications each) for artificial dental implants.
[0057] Therefore, the present invention can be used to produce titanium alloy discs (eight thickness specifications of D98×10~25mm) and blocks (eight thickness specifications of 150×140×10~25mm; 220×150×11~25mm) for artificial dental implants, without the need for a plate process method with complex process, long production cycle and high cost, so that the microstructure of large-sized rectangular block forging billets (150×140×L; 220×150×Lmm) and large-sized round disc rolling billets (Φ98×Lmm) for dental implants can meet the rating requirements. The invention discloses a method for forging a square billet of 490×L mm by heating a Φ620 mm diameter ingot to 160-260°C above the phase transformation point, controlling the total deformation to be about 20%, controlling the final forging temperature to be not less than Tβ+50°C, and then rapidly quenching the billet; forging the quenched 490×L billet into a 270×L mm forging billet with a total deformation of 70% or more in a β phase region 50°C above the phase transformation point; and forging the 270×L mm forging billet with a deformation of 70% and a total deformation of 50% or more in a single fire into a rectangular 225×155×L mm square finished forging billet and a 225×L mm forging billet; and then heating forging and rolling the billet at 40-70°C below the phase transformation point to forge a rectangular 155×145×L mm square finished forging billet and roll a disc finished rolling billet with a diameter of Φ105×L mm. The titanium alloy discs and blocks for artificial dental implants produced by the present invention achieve the technical and economic effects of eliminating the traditional large-size bar and thick plate production forging blanks with multiple firings, large deformation, three piers and three draws, and the use of large-scale plate rolling mill equipment with high processing costs. The intermediate process grinding loss is small, the yield is high, the processing cost is low, the product metallographic structure meets the rating requirements, and the mechanical properties are stable.
[0058] Furthermore, the production method of the present invention is easy to implement in industrial standardized production, and the production equipment used is the most commonly used equipment in the current processing plant. The production and preparation process has few fires, very little grinding, and a high yield rate. Only the forging process is used, and at most one rolling process is added to produce all three models of 24 specifications and sizes of discs and blocks forging blanks. The processing cost is low, and it is most suitable for the production and processing of titanium and titanium alloy forging bar blanks for dentistry. In addition, the titanium alloy discs and blocks for artificial dental implants produced by the method of the present invention have microstructures that meet the rating requirements, stable mechanical properties, and good end face consistency. Furthermore, the production process of the present invention is not limited by the alloy type. The technical effect of the present invention can be achieved by adjusting the common parameters according to the corresponding alloy type. At the same time, the Ti6Al4V, Ti6Al4VELI, Ti6Al7Nb dental discs and block forging bar blanks and rolling blanks produced by the present invention have a bar microstructure rating of: 3 to 9 levels.
[0059] Embodiment 2
[0060] The embodiment of the present invention also provides a method for producing a titanium alloy forging for an artificial dental implant, which specifically comprises the following steps:
[0061] Step 21: Prepare a Ti6Al4V alloy ingot with a specification of Φ620mm. Cut the riser from the ingot, remove the surface pores, and saw it into sections with a length of Φ620×500mm;
[0062] Step 22: The ingot cut in step 21 is heated to 1200° C. in an electric furnace for 280 minutes of heating and heat preservation time. The heated Φ620×500 ingot is quickly forged into a square billet with a side length of 490×L on a 2500T fast forging machine (with a deformation amount of about 20%). When the final forging temperature is 1050° C., the square billet with a side length of 490×L is quickly quenched into a water tank for rapid cooling. The water tank is pumped with circulating water. The billet is cooled for 30 minutes and then discharged from the water. The water is then air-cooled to room temperature to repair surface defects.
[0063] Step 23: The square billet with a side length of 490×L prepared in step 22 is heated to 1050°C and kept warm for 260 minutes. The square billet with a side length of 490×L is forged into a square billet with a side length of 270×Lmm by a single-fire multi-pass drawing forging on a 2500T fast forging machine. The final forging temperature is about 750°C. After air cooling, the surface defects are ground and the billet is cut into 270×1000mm on a sawing machine.
[0064] Step 24: The square billet with a side length of 270×1000mm prepared in step 23 is added to 950°C and heated for 160 minutes. The heated square billet with a side length of 270×1000mm is forged into a finished rectangular bar billet with a side length of 225×155×Lmm by multi-pass drawing and forging on a 1600T fast forging machine, and then air-cooled.
[0065] Step 25: The finished rectangular bar blank with a side length of 225×155×L mm prepared in step 24 is subjected to AC heat treatment at 750°C / 2.0 hr.
[0066] Step 26: Cut the blank with a side length of 225×155×Lmm heat-treated in step 25 into 225×155×12-26mm (eight thickness specifications) artificial dental implant blanks by wire cutting, and take samples from the blank with a side length of □225×155×Lmm, 750℃ / 2.0hr, AC annealing heat treatment, and the transverse metallographic structure is shown in FIG. Figure 2 As shown, according to Appendix A of GB / T13810-2017, its organizational type meets the A8 rating standard.
[0067] Step 27: Cut the artificial dental implant blanks prepared in step 26 into 225×155×12~26mm (eight thickness specifications), and make them into grade / annealed (TC4G / M) titanium blocks on a CNC machining center. The specifications are 220×150×(11, 13, 15, 17, 19, 21, 23, 25)mm.
[0068] Embodiment 3
[0069] The embodiment of the present invention also provides a method for producing a titanium alloy forging for an artificial dental implant, which specifically comprises the following steps:
[0070] Step 31: Prepare an alloy ingot of Φ620 mm Ti6Al4V. Cut the riser from the ingot, remove the surface pores, and saw it into sections of Φ620 × 500 mm in length.
[0071] Step 32: Heat the ingot cut in step 31 to 1200°C in an electric furnace, and heat and hold for 280 minutes. Rapidly forge the heated Φ620×500 ingot on a 2500T fast forging machine into a square billet with a side length of 490×L (deformation of about 20%). When the final forging temperature is 1050°C, quickly quench the square billet with a side length of 490×L into a water tank for rapid cooling. Add a pump to circulate water in the water tank. The billet is cooled for 30 minutes and then air-cooled to room temperature to repair surface defects.
[0072] Step 33: Heat the 490×L square billet prepared in step 32 to 1050°C and keep it warm for 260 minutes. Forge the heated 490×L square billet on a 2500T fast forging machine through multiple passes of drawing and forging into a square billet with a side length of 270×Lmm. The final forging temperature is about 750°C. After air cooling, the surface defects are ground and the material is cut into 270×1000mm on a sawing machine.
[0073] Step 34: Heat the square billet with a side length of 270×1000mm prepared in step 33 to 950°C and keep it warm for 160 minutes. Forge the heated square billet with a side length of 270×1000mm on a 1600T fast forging machine through multiple passes of drawing and forging to form a square bar billet with a side length of 225×2000mm. After air cooling, grind away surface defects and saw the material to 225×1000mm.
[0074] Step 35: Heat the square billet with a side length of 225×1000mm prepared in step 34 to 950°C and heat and keep warm for 140 minutes. Forge the heated square billet with a side length of 225×1000mm on a 1600T fast forging machine through multiple passes of drawing and forging to form a finished square bar billet with a side length of 155×145×Lmm.
[0075] Step 36: Heat treat the finished rectangular bar blank with a side length of 155×145×Lmm prepared in step 35 at 700℃ / 2.0hr, AC
[0076] Step 37: The blank with a side length of 155×145×Lmmmm heat-treated in step 36 is cut into 155×145×11-26mm (eight thickness specifications) artificial dental implant blanks by wire cutting, and samples are taken from the blanks subjected to AC annealing heat treatment at 750℃ / 2.0hr. The transverse metallographic structure is shown in FIG. Figure 3 As shown, according to Appendix A of GB / T13810-2017, its organizational type meets the A7 rating standard.
[0077] Step 38: Cut the artificial dental implant blanks prepared in step 37 into 1555×145×12~26mm (eight thickness specifications), and make them into grade / annealed (TC4G / M) titanium blocks on a CNC machining center. The specifications are 1500×140×(10, 12, 14, 16, 18, 20, 22, 25)mm.
[0078] Embodiment 4
[0079] The embodiment of the present invention also provides a method for producing a titanium alloy forging for an artificial dental implant, which specifically comprises the following steps:
[0080] Step 41: Prepare an alloy ingot of Φ620 mm Ti6Al4V. Cut the riser from the ingot, remove the surface pores, and saw it into sections of Φ620 × 500 mm in length.
[0081] Step 42: Heat the ingot cut in step 41 to 1200°C in an electric furnace for 280 minutes of heating and heat preservation time. Rapidly forge the heated Φ620×500 ingot on a 2500T fast forging machine into a square billet with a side length of 490×L (deformation of about 20%). When the final forging temperature is 1050°C, quickly quench the square billet with a side length of 490×L into a water tank for rapid cooling. Add a pump to circulate water in the water tank. The billet is cooled for 30 minutes and then discharged from the water. Then, it is air-cooled to room temperature to repair surface defects.
[0082] Step 43: Heat the 490×L square billet prepared in step 42 to 1050°C and keep it warm for 260 minutes. Forge the heated 490×L square billet on a 2500T fast forging machine through multiple passes of drawing and forging into a square billet with a side length of 270×Lmm. The final forging temperature is about 750°C. After air cooling, the surface defects are ground and the billet is cut into 270×1000mm on a sawing machine.
[0083] Step 44: Heat the square billet with a side length of 270×1000mm prepared in step 43 to 950°C and keep it warm for 160 minutes. Forge the heated square billet with a side length of 270×1000mm on a 1600T fast forging machine through multiple passes of drawing and forging to form a square forging billet with a side length of 225×2000mm. After air cooling, grind away surface defects and saw the billet to 225×1000mm.
[0084] Step 45: Heat the square billet with a side length of 225×1000mm prepared in step 44 to 920°C and keep it warm for 140 minutes. Forge the heated square billet with a side length of 225×1000mm through multiple passes on a 1600T fast forging machine to form a rolled billet with a side length of 155×2000mm. After air cooling, grind away surface defects and saw the billet to 155×1000mm.
[0085] Step 46: Heat the square billet with a side length of 155×1000 mm prepared in step 45 to 930° C. and keep it warm for 120 minutes. Roll the heated square billet with a side length of 155×1000 mm on a 550 type bar rolling mill into a Φ105×L finished round bar billet.
[0086] Step 47: Heat treatment of the Φ105×L finished round bar blank prepared in step 46 at 700°C / 1.5hr, AC
[0087] Step 48: Cut the finished round bar blank with a diameter of Φ105×L prepared in step 47 into artificial dental implant blanks with a diameter of Φ105×11-26mm (eight thickness specifications) by wire cutting. Samples are taken from the blanks after AC annealing at 750℃ / 2.0hr, and the transverse metallographic structure is shown in FIG. Figure 4 As shown, according to Appendix A of GB / T13810-2017 standard, its organizational type meets the A4 rating standard.
[0088] Step 49: Cut the artificial dental implant blanks prepared in step 48 into Φ105×11~26mm (eight thickness specifications) by wire cutting, and make them into grade / annealed (TC4G / M) titanium blocks on a CNC machining center, with eight specifications of Φ98×(10, 12, 14, 16, 18, 20, 22, 25)mm.
[0089] It can be seen that the present invention includes the production of Φ105×Lmm diameter disc billets and rectangular 155×145×Lmm, 225×155×Lmm square forging billets, and the microstructure of the prepared medical two-phase titanium alloy billets meets the assessment requirements of Appendix A of GB / T13810-2017 standard, and its organizational type meets the A1-A9 rating standard. The Φ105×Lmm disc billets and rectangular 155×145×Lmm, 225×155×Lmm square forging billets only need to be annealed in an electric furnace, and then cut by band saw or wire cutting, and machined to prepare titanium alloy discs (eight thickness specifications of D98×10-25mm) and blocks (eight thickness specifications of 150×140×10-25mm; 220×150×11-25mm) for implants. A method for producing large-size medical forged rods with a simple production method and low cost is proposed. The method adopts an ingot with a specific diameter of 620 mm. According to the process scheme, process parameters and process flow proposed in the present invention, the original grains can be crushed through two firings, the high-temperature β phase structure can be refined, and the structure is prepared for two-phase processing, so that the minimum forging process of producing finished forged rods with four forging firings is achieved. Taking TC4 alloy as an example, a sample is taken from a rod with a maximum side length of 220×150×L mm, and its metallographic structure is rated as level 7. The method of the present invention is used to prepare titanium alloy discs and blocks for dentistry, and the metallographic structure is uniform and meets the standards, the performance is stable, the yield is high, the production cycle is short, the efficiency is high, the cost is low, and the production is flexible, which completely solves the technical problems of long production cycle, low yield, high cost, and inconsistent metallographic structure and unstable performance of forged billets in the traditional preparation process.
[0090] The above one or more technical solutions in the embodiments of the present invention have at least one or more of the following technical effects:
[0091] The present invention provides a method for producing a titanium alloy forging for an artificial dental implant, the method comprising: step 1: preparing a medical titanium alloy ingot according to preset requirements, and treating the titanium alloy ingot by a first treatment method to obtain a first qualified ingot; step 2: heating the first qualified ingot obtained in step 1 according to a first heating condition, forging it on a fast forging machine according to a first forging condition to obtain a first forging blank, and quenching the first forging blank according to a first quenching condition to obtain a first qualified forging blank; step 3: heating the first qualified forging blank obtained in step 2 to a temperature above the phase transition point Tβ+50°C. temperature, forging according to the second forging condition and obtaining a second qualified forging billet; step 4: heating the second qualified forging billet obtained in step 3 to a temperature below the phase transformation point Tβ-(30-60°C), forging according to the third forging condition and obtaining a first finished billet; step 5: heating the second qualified forging billet obtained in step 3 to a temperature below the phase transformation point Tβ-(30-60°C), forging according to the fourth forging condition and obtaining a third qualified forging billet; step 6: heating the third qualified forging billet obtained in step 5 to a temperature below the phase transformation point Tβ-(30-60°C), forging according to the fifth forging condition and obtaining a first finished billet. Step 7: heating the third qualified forging billet obtained in step 5 to a temperature below the phase transformation point Tβ-(30-60°C), forging according to the sixth forging condition and obtaining a first qualified rolling billet; Step 8: heating the first qualified rolling billet obtained in step 7 to a temperature below the phase transformation point Tβ-(40-70°C), forging according to the seventh forging condition and obtaining a third finished billet; Step 9: annealing the first finished billet obtained in step 4, the second finished billet obtained in step 6, and the third finished billet obtained in step 8; Step 10: annealing the first finished billet obtained in step 9 The first finished blank, the second finished blank and the third finished blank after fire treatment are reserved with finishing cutting allowances, and are cut according to the size of the titanium alloy forging for artificial dental implants. Then, the titanium alloy forging for artificial dental implants are obtained through mechanical finishing, thereby solving the technical problems of long production cycle of rolled plates, low yield, high cost, unqualified metallographic structure of forged blanks and unstable performance in the preparation process of forgings in the prior art, and achieving the technical effects of uniform metallographic structure, stable performance, high yield, short production cycle, high efficiency, low processing cost and stable mechanical properties.
[0092] Although the preferred embodiments of the present invention have been described, those skilled in the art may make additional changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.
[0093] Obviously, those skilled in the art can make various changes and modifications to the embodiments of the present invention without departing from the spirit and scope of the embodiments of the present invention. Thus, if these modifications and variations of the embodiments of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.
Claims
1. A method for producing a titanium alloy forging for artificial dental implants, characterized in that: The method comprises: Step 1: preparing a medical titanium alloy ingot according to preset requirements, and treating the titanium alloy ingot by a first treatment method to obtain a first qualified ingot; Step 2: After heating the first qualified ingot obtained in step 1 according to the first heating condition, forging it on a fast forging machine according to the first forging condition to obtain a first forging blank, and quenching the first forging blank according to the first quenching condition to obtain a first qualified forging blank; Step 3: heating the first qualified forging blank obtained in step 2 to a temperature above the phase transformation point Tβ+50° C., forging according to the second forging conditions to obtain a second qualified forging blank; Step 4: heating the second qualified forging blank obtained in step 3 to a temperature below the phase transformation point Tβ-(30-60° C.), forging it according to the third forging condition and obtaining a first finished blank; Step 5: heating the second qualified forging blank obtained in step 3 to a temperature below the phase transformation point Tβ-(30-60° C.), forging according to the fourth forging condition to obtain a third qualified forging blank; Step 6: heating the third qualified forging blank obtained in step 5 to a temperature below the phase transformation point Tβ-(30-60° C.), forging according to the fifth forging condition and obtaining a second finished blank; Step 7: heating the third qualified forging billet obtained in step 5 to a temperature below the phase transformation point Tβ-(30-60° C.), forging according to the sixth forging condition and obtaining a first qualified rolling billet; Step 8: heating the first qualified rolled billet obtained in step 7 to a temperature below the phase transformation point Tβ-(40-70° C.), forging according to the seventh forging condition to obtain a third finished billet; Step 9: annealing the first finished blank obtained in step 4, the second finished blank obtained in step 6, and the third finished blank obtained in step 8; Step 10: reserve finishing cutting allowance for the first finished blank, the second finished blank, and the third finished blank that have undergone the annealing treatment in step 9, cut them according to the size of the titanium alloy forging for artificial dental implants, and then obtain the titanium alloy forging for artificial dental implants through mechanical finishing.
2. The method for producing a titanium alloy forging for artificial dental implant according to claim 1, characterized in that: In the step 1, the preset requirement is to prepare an alloy ingot that meets the requirements of GB / T13810-2017 and has a specification of Φ620 mm; The first processing method is to cut a riser from the titanium alloy ingot, remove surface pores, and saw the material into an ingot block of Φ620×500±100mm, and use the ingot block as the first qualified ingot.
3. The method for producing a titanium alloy forging for artificial dental implant according to claim 1, characterized in that: In the step 2, the first heating condition is: heating the first qualified ingot in an electric furnace or a gas heating furnace to Tβ+ (160-260° C.) in stages, and the heating and holding time is 280-300 minutes; The first forging condition is: forging the first qualified ingot into the first forging blank with a side length of 490×Lmm, wherein the deformation amount is 20% and the final forging temperature is greater than or equal to Tβ+50°C; The first quenching condition is: quenching the first forging blank with a side length of 490×Lmm into a water tank for rapid cooling under the condition that the final forging temperature is greater than or equal to Tβ+50°C, and the cooling water in the water tank needs to be circulated by a pump.
4. The method for producing a titanium alloy forging for artificial dental implant according to claim 1, characterized in that: In step 3, the second forging condition is: the first qualified forging blank is forged into a square billet with a side length of 270±20 mm by one fire and multiple passes, wherein the deformation of the forging pass is greater than or equal to 20%, the total deformation of the fire is 70%±10%, and the final forging temperature is greater than or equal to 750°C.
5. The method for producing a titanium alloy forging for artificial dental implant according to claim 1, characterized in that: In step 4, the third forging condition is specifically: the second qualified forging blank is forged into a finished rectangular forging blank with a side length of 225mm×155×Lmm by one fire and multiple passes, wherein the deformation amount of each pass is greater than or equal to 15%, and the total deformation amount of each fire is greater than or equal to 50%.
6. The method for producing a titanium alloy forging for artificial dental implant according to claim 1, characterized in that: In step 5, the fourth forging condition is specifically as follows: the second qualified forging blank is forged into a second forging blank with a side length of 225×Lmm through one fire and multiple passes, wherein the deformation amount of each pass is greater than or equal to 20%, and the deformation amount of each fire is greater than or equal to 50%.
7. The method for producing a titanium alloy forging for artificial dental implant according to claim 1, characterized in that: In step 6, the fifth forging condition is specifically: subjecting the third qualified forging blank to one fire and multiple forging passes to form a finished forging blank with a side length of 155mm×145×Lmm, wherein the deformation amount of each pass is greater than or equal to 20%, and the total deformation amount of each fire is greater than or equal to 50%.
8. The method for producing a titanium alloy forging for artificial dental implant according to claim 1, characterized in that: In step 7, the sixth forging condition is specifically: subjecting the third qualified forging blank to one fire and multiple forging passes to form a third forging blank with a side length of 155×Lmm, wherein the deformation amount of each pass is greater than or equal to 20%, and the deformation amount of each fire is greater than or equal to 50%.
9. The method for producing a titanium alloy forging for artificial dental implant according to claim 1, characterized in that: In step 8, the seventh forging condition is specifically: the first qualified billet is rolled into a finished round bar billet of Φ103×Lmm through one fire and multiple passes on a 550 type bar rolling mill, and the finished round bar billet is used as the third finished billet.
10. The method for producing a titanium alloy forging for artificial dental implant according to claim 1, characterized in that: In step 9, the annealing treatment is based on the process parameters in the GB / T13810-2017 standard.