Production process of orthotic insole

By using polyether polyol combination material and nylon composite material to prepare burr-free insole shells, combined with mold clamping foam forming technology, the problems of correcting the fracture tensile strength and environmental protection of the insole are solved, and higher tensile strength and breathability are achieved Improves the comfort and quality of the insole.

CN118952736APending Publication Date: 2024-11-15FOSHAN BAOMIN SHOES CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411065234.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The tensile strength of existing orthodontic insoles is poor in fracture and is prone to tear. The use of glue in traditional production processes leads to volatility of organic compounds and bubble problems, affecting the quality of the insole.

Method used

The burr-free insole shell is prepared by polyether polyol combination material and nylon composite material. The mold is foamed and molded, and the burrs are reserved to be closely bonded to the pads, instead of glue, and a shock absorbing block is set at the bottom to improve tensile strength and breathability. .

Benefits of technology

It improves the tensile strength and breathability of the corrected insole, reduces the use of chemical raw materials and the production of organic compound gases, and enhances environmental protection and comfort.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004979160390000091
    Figure BDA0004979160390000091
Patent Text Reader

Abstract

The invention discloses a production process of an orthotic insole, and relates to the field of insoles, and the production process comprises the following steps: S1, cutting polyurethane to obtain a shock absorption block; s2, uniformly mixing and stirring the nylon composite material, drying, twisting and weaving to obtain an insole shell with burrs; s3, mixing and stirring the polyether polyol composite material to prepare a mixed solution; s4, a release agent is sprayed to the mold; the shock absorption block is placed on the lower mold, the middle mold and the lower mold are attached and locked, the shoe pad shell with burrs is placed on the middle mold, and cloth is hung on the upper mold; and S5, injecting the mixed solution into a lower mold, attaching and locking the upper mold and the middle mold, closing the mold, foaming and forming, opening the mold to obtain a soft cushion, and trimming to obtain the orthotic insole. The orthotic insole has the effect of improving the fracture tensile strength of the orthotic insole.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of insoles, in particular to a production process of corrective insoles. Background Art

[0002] Insoles are used to be placed in shoes and can play the role of antibacterial, deodorizing, and height-increasing. Most insoles on the market are flat in shape, poorly fit the human foot, and cannot provide effective support for the arch of the foot when worn; wearing such flat insoles for a long time will make the human foot feel uncomfortable or even painful, so people usually use corrective insoles to balance the pressure on the sole of the foot to meet the needs of comfortable and healthy soles.

[0003] Existing corrective insoles are shaped and supported by insole shells, so that the outer edges of the insoles at the arch and heel are turned up and fit the sole of the foot to form an outer wall, thereby balancing the pressure on the sole of the foot; however, the existing insoles have poor breaking tensile strength, and are prone to tearing after the foot compresses the insole for a long time. Summary of the invention

[0004] In order to improve the tensile strength at break of a corrective insole, the present application provides a production process for a corrective insole.

[0005] The present application provides a production process for corrective insoles using the following technical solutions: A production process of a corrective insole comprises the following steps: S1. The polyurethane is cut to obtain a shock-absorbing block; S2. The nylon composite material is mixed and stirred evenly, and after drying, the insole shell is obtained by twisting and weaving with burrs; S3. The polyether polyol composition is mixed and stirred to obtain a mixed solution; S4. Spray the mold release agent on the mold; place the shock absorbing block on the lower mold, fit and lock the middle mold with the lower mold, place the insole shell with burrs on the middle mold, and hang the cloth on the upper mold; S5. Inject the mixed liquid into the lower mold, fit and lock the upper mold and the middle mold, close the mold for foaming, open the mold to obtain a soft cushion, and complete trimming to obtain a corrective insole.

[0006] By adopting the above technical scheme, in the traditional process of producing corrective insoles, the burrs at the edge of the insole shell after molding are removed, and the process of cleaning the burrs increases the difficulty and cost of producing corrective insoles. After the burrs and burrs are cleaned, the insole shell needs to be bonded with the foamed soft pad by glue. During the foaming process, the glue will produce volatile organic compounds and other substances due to the high temperature, which are harmful to human health. At the same time, it is easy to cause bubbles at the connection position between the insole shell and the soft pad, making the edge of the corrective insole uneven, affecting the quality of the corrective insole. However, in the process of preparing the insole shell, the burrs are reserved in advance in the present application. When the corrective insole is molded, the reserved burrs are tightly bonded to the soft pad, instead of using glue to bond the soft pad and the insole shell. The burrs remaining when producing the insole shell are reasonably used, reducing the use of chemical raw materials and the generation of organic compound gases, which has an environmental protection effect. At the same time, the edge position of the corrective insole is made flat, and the appearance quality of the insole is improved. A shock-absorbing block is set at the bottom of the corrective insole of the present application, so that the insole has good air permeability, elasticity and shock absorption. The polyether polyol combination material is used as the raw material in the soft pad, which can effectively improve the tensile strength of the corrective insole and improve the tensile strength at break of the corrective insole.

[0007] Preferably, in step S2, the burr has a width of 2-4 mm and a thickness of 0.1-0.5 mm.

[0008] By adopting the above technical solution, the width and thickness of the burr are controlled, so that the burr can be more tightly bonded to the corrective insole during molding, and is not likely to affect the normal molding of the corrective insole.

[0009] Preferably, the preparation method of the polyether polyol combination is: adding the second component to the first component while stirring, and stirring evenly after adding to obtain the polyether polyol combination; the preparation method of the first component is: mixing and heating 400-600 parts by weight of polyether polyol A and 600-800 parts by weight of polyether polyol B, adding 80-120 parts by weight of nano zinc oxide and dispersing evenly, then heating 40-60 parts by weight of 2,4-diphenylmethane diisocyanate for heating reaction, adding 10-20 parts by weight of defoamer, 80-100 parts by weight of butyl acetate and 40-100 parts by weight of ethylene glycol ethyl ether acetate after cooling, and stirring evenly to obtain the first component; the preparation method of the second component is: mixing 20-60 parts by weight of dibutyltin dilaurate, 100-200 parts by weight of water and 500-900 parts by weight of isocyanate to obtain the second component.

[0010] By adopting the above technical scheme, polyether polyol A and polyether polyol B are first fully mixed, and then nano zinc oxide and 2,4-diphenylmethane diisocyanate are added to obtain a first component, and then the first component is evenly mixed with the isocyanate in the second component, so as to give full play to the synergistic effect between polyether polyol A and polyether polyol B, and obtain a corrective insole with excellent tensile strength and mildew and antibacterial strength; polyether polyol A and polyether polyol B react with 2,4-diphenylmethane diisocyanate, and at the same time, during the foaming molding process, nano zinc oxide will be evenly dispersed in the pores of the material, so that the voids inside the material become smaller, and the strength limit of the pores is increased, thereby improving the tensile strength at break of the corrective insole.

[0011] Preferably, the hydroxyl value of the polyether polyol A is 400-500 mg / g; the hydroxyl value of the polyether polyol B is 100-120 mgKOH / g, and the functionality is 2.

[0012] By adopting the above technical solution, the combination of polyether polyol A and polyether polyol B effectively overcomes the problem of poor material dimensional stability when using water as a foaming agent, so that the soft pad can still maintain good elasticity and strength, thereby improving the wearing comfort of the insole.

[0013] Preferably, in step S2, the preparation method of the nylon composite material is: 100-150 parts by weight of nylon, 80-100 parts by weight of flax fiber and 50-70 parts by weight of tea polyphenols are uniformly stirred to obtain the nylon composite material.

[0014] By adopting the above technical scheme, nylon, flax fiber and tea polyphenols are used as raw materials to prepare a nylon composite material, which is used as an insole shell, the hardness and air permeability of the insole shell can be improved, thereby further improving the air permeability of the corrective insole.

[0015] Preferably, the nano zinc oxide is modified nano zinc oxide; the preparation method of the modified nano zinc oxide is: 100-150 parts by weight of nano zinc oxide is mixed with 200-240 parts by weight of propylene glycol, 10-20 parts by weight of concentrated sulfuric acid, 50-100 parts by weight of triclosan and 50-80 parts by weight of polyethylene glycol, then 50-60 parts by weight of ammonium polyphosphate is added and continued to be stirred, and the modified zinc oxide is obtained after filtering and drying.

[0016] By adopting the above technical scheme, the present application modifies nano zinc oxide, and both triclosan and nano zinc oxide have good bactericidal effects. The modified nano zinc oxide is added to the soft pad and dispersed evenly in the micropores of the insole, thereby improving the air permeability of the corrective insole and improving the wearing comfort of the corrective insole; the modified zinc oxide has a microporous structure and can absorb the odor generated inside the shoe, thereby improving the anti-mildew and antibacterial effect of the corrective insole.

[0017] Preferably, the weight ratio of the nano zinc oxide, ammonium polyphosphate and polyethylene glycol is (2.4-2.72):1:(1.28-1.44).

[0018] By adopting the above technical scheme, when nano zinc oxide, ammonium polyphosphate and polyethylene glycol are in a specific weight ratio, the tensile strength performance of the corrective insole can be further improved. Polyethylene glycol makes the ammonium polyphosphate evenly dispersed in the nano zinc oxide, making the gaps between the nano zinc oxide smaller, thereby improving the compressive strength of the polyether polyol combination supporting the insole, and further improving the air permeability of the corrective insole.

[0019] Preferably, the isocyanate is a modified isocyanate, and the preparation method of the modified isocyanate is as follows: dissolve 15-25 parts by weight of sodium alginate in water, add 30-50 parts by weight of sodium periodate and stir evenly, add 5-15 parts by weight of ethylene glycol and 8-16 parts by weight of cinnamamide ethanol solution and continue stirring; then add 24-48 parts by weight of isocyanate and 0.2-0.6 parts by weight of sodium dodecyl sulfate and stir evenly to obtain the modified isocyanate.

[0020] Preferably, the isocyanate is isophorone diisocyanate.

[0021] By adopting the above technical solution, sodium alginate has a certain surface activity. After sodium alginate is mixed and modified with isocyanate, the hydrophilicity of the isocyanate surface can be adjusted, so that the second component of the isocyanate can be better combined with the first component, thereby further improving the breathability and antibacterial effect of the corrective insole.

[0022] Preferably, the weight ratio of the sodium alginate, isocyanate and cinnamamide ethanol is 1:(1.4-1.6):(0.6-0.75).

[0023] By adopting the above technical scheme, when sodium alginate, isocyanate and cinnamamide ethanol are in a specific weight ratio, cinnamamide is grafted into ammonium alginate, and ammonium alginate is filled into isocyanate, so that the modified isocyanate is combined with the first component, the emulsification effect of isocyanate is improved, and a corrective insole with good elasticity and strength is obtained.

[0024] In summary, this application has the following beneficial technical effects: 1. In the process of preparing the insole shell, the present application reserves burrs. When the corrective insole is molded, the reserved burrs are tightly bonded to the soft pad, instead of using glue to bond the soft pad and the insole shell. The burrs and burrs remaining in the production of the insole shell are reasonably used, which reduces the use of chemical raw materials and the generation of organic compound gases, has an environmental protection effect, and at the same time makes the edge position of the corrective insole flat, thereby improving the appearance quality of the insole. A shock-absorbing block is arranged at the bottom of the corrective insole of the present application, so that the insole has good air permeability, elasticity and shock absorption. The polyether polyol combination material is used as the raw material in the soft pad, which can effectively improve the tensile strength of the corrective insole and improve the tensile strength at break of the corrective insole.

[0025] 2. First, polyether polyol A and polyether polyol B are fully mixed, and then nano zinc oxide and 2,4-diphenylmethane diisocyanate are added to obtain a first component, and then the first component is evenly mixed with the isocyanate in the second component to give full play to the synergistic effect between polyether polyol A and polyether polyol B to obtain a corrective insole with excellent tensile strength and mildew and antibacterial strength; polyether polyol A and polyether polyol B react with 2,4-diphenylmethane diisocyanate, and during the foaming process, nano zinc oxide will be evenly dispersed in the pores of the material, so that the voids inside the material become smaller and the strength limit of the pores is increased, thereby improving the tensile strength at break of the corrective insole. DETAILED DESCRIPTION

[0026] The present application is further described in detail below in conjunction with embodiments and comparative examples. Example

[0027] Example 1 A production process of a corrective insole comprises the following steps: S1. The polyurethane is cut into round blocks to obtain shock-absorbing blocks; wherein the polyurethane is selected from PORON polyurethane foam, model 41-30031; S2. The nylon composite material was mixed and stirred evenly, and then dried and twisted to obtain an insole shell; wherein the edge of the insole shell retained burrs, the width of the burrs was 2 mm; the thickness was 0.1 mm; the preparation method of the nylon composite material was: 100 g of nylon 66, 80 g of flax fiber and 50 g of tea polyphenols were put into an electric stirrer, stirred at a temperature of 75 ° C and a speed of 200 r / min for 15 minutes to obtain a nylon composite material; wherein the nylon 66 selected from the US DuPont model is 70G30HSLR; S3. The polyether polyol composition is mixed and stirred to obtain a mixed solution; wherein the preparation method of the polyether polyol is: 400g of polyether polyol A and 600g of polyether polyol B were mixed and heated, and then 80g of nano zinc oxide was added and dispersed evenly. Then 40g of 2,4-diphenylmethane diisocyanate was heated to 75°C and reacted for 1.5h. After cooling to 45°C, 10g of defoamer, 80g of butyl acetate and 40g of ethylene glycol ethyl ether acetate were added and stirred evenly for 30s at a speed of 150r / s to obtain a first component. 20 g of dibutyltin dilaurate, 100 g of water and 500 g of isophorone diisocyanate were uniformly mixed to obtain the second component; The first component and the second component are placed in a stirring kettle and stirred for 30 seconds at a temperature of 40° C. and a rotation speed of 400 r / s to obtain a polyether polyol composite material; The hydroxyl value of polyether polyol A is 400 mg / g, the hydroxyl value of polyether polyol B is 100 mgKOH / g, and the functionality is 2; the defoamer is specifically Jusheng Chemical WDXP; S4. Spray a release agent on the middle mold and the lower mold of the mold, wherein the release agent is specifically stearic acid; place the shock absorbing block in the lower mold, fit the middle mold with the lower mold, and lock the middle mold and the lower mold, and place the insole shell with burrs on the middle mold; hang a cloth on the side of the upper mold close to the middle mold; S5. Inject the polyether polyol combination material into the lower mold with an injection gun, fit and lock the upper mold and the middle mold, and foam and mold at a temperature of 60°C for 10 seconds after the mold is closed. Open the upper mold and the middle mold in turn, take out the soft cushion and trim it to obtain a corrective insole.

[0028] Example 2 A production process of a corrective insole comprises the following steps: S1. The polyurethane is cut into round blocks to obtain shock-absorbing blocks; wherein the polyurethane is selected from PORON polyurethane foam, model 41-30031; S2. The nylon composite was mixed and stirred evenly, and then dried and twisted to obtain an insole shell; wherein the edge of the insole shell retained burrs, the width of the burrs was 4 mm; the thickness was 0.5 mm; the preparation method of the nylon composite was: 100 g of nylon 66, 80 g of flax fiber and 50 g of tea polyphenols were put into an electric stirrer, stirred at a temperature of 75 ° C and a speed of 200 r / min for 15 min to obtain a nylon composite; wherein the nylon 66 selected from the US DuPont model is 70G30HSLR; S3. The polyether polyol composition is mixed and stirred to obtain a mixed solution; wherein the preparation method of the polyether polyol is: 600g of polyether polyol A and 800g of polyether polyol B were mixed and heated, and then 120g of nano zinc oxide was added and dispersed evenly. Then 60g of 2,4-diphenylmethane diisocyanate was heated to 75°C and reacted for 1.5h. After cooling to 45°C, 20g of defoamer, 100g of butyl acetate and 100g of ethylene glycol ethyl ether acetate were added and stirred evenly for 30s at a speed of 150r / s to obtain a first component. 60 g of dibutyltin dilaurate, 200 g of water and 900 g of isophorone diisocyanate were uniformly mixed to obtain the second component; The first component and the second component are placed in a stirring kettle and stirred for 30 seconds at a temperature of 40° C. and a rotation speed of 400 r / s to obtain a polyether polyol composite material; The hydroxyl value of polyether polyol A is 500 mg / g, the hydroxyl value of polyether polyol B is 120 mgKOH / g, and the functionality is 2; the defoamer is specifically Jusheng Chemical WDXP; S4. Spray a release agent on the middle mold and the lower mold of the mold, wherein the release agent is specifically stearic acid; place the shock absorbing block in the lower mold, fit the middle mold with the lower mold, and lock the middle mold and the lower mold, and place the insole shell with burrs on the middle mold; hang a cloth on the side of the upper mold close to the middle mold; S5. Inject the polyether polyol combination material into the lower mold with an injection gun, fit and lock the upper mold and the middle mold, and foam and mold at a temperature of 60°C for 10 seconds after the mold is closed. Open the upper mold and the middle mold in turn, take out the soft cushion and trim it to obtain a corrective insole.

[0029] Example 3 A production process of a corrective insole comprises the following steps: S1. The polyurethane is cut into round blocks to obtain shock-absorbing blocks; wherein the polyurethane is selected from PORON polyurethane foam, model 41-30031; S2. The nylon composite was mixed and stirred evenly, and then dried and twisted to obtain an insole shell; wherein the edge of the insole shell retains burrs, the width of the burrs is 3mm; the thickness is 0.3mm; the preparation method of the nylon composite is: 100g nylon 66, 80g flax fiber and 50g tea polyphenols are put into an electric stirrer, stirred at a temperature of 75°C and a speed of 200r / min for 15min to obtain a nylon composite; wherein the nylon 66 is selected from the American DuPont model 70G30HSLR; S3. The polyether polyol composition is mixed and stirred to obtain a mixed solution; wherein the preparation method of the polyether polyol is: 500g of polyether polyol A and 700g of polyether polyol B were mixed and heated, and then 100g of nano zinc oxide was added to disperse evenly, and then 50g of 2,4-diphenylmethane diisocyanate was heated to 75°C for reaction for 1.5h, and then 15g of defoamer, 90g of butyl acetate and 70g of ethylene glycol ethyl ether acetate were added after cooling to 45°C, and stirred evenly for 30s at a speed of 150r / s to obtain a first component; 40 g of dibutyltin dilaurate, 150 g of water and 700 g of isophorone diisocyanate were mixed to obtain the second component; The first component and the second component are placed in a stirring kettle and stirred for 30 seconds at a temperature of 40° C. and a rotation speed of 400 r / s to obtain a polyether polyol composite material; The hydroxyl value of polyether polyol A is 400 mg / g, the hydroxyl value of polyether polyol B is 100 mgKOH / g, and the functionality is 2; the defoamer is specifically Jusheng Chemical WDXP; S4. Spray a release agent on the middle mold and the lower mold of the mold, wherein the release agent is specifically stearic acid; place the shock absorbing block in the lower mold, fit the middle mold with the lower mold, and lock the middle mold and the lower mold, and place the insole shell with burrs on the middle mold; hang a cloth on the side of the upper mold close to the middle mold; S5. Inject the polyether polyol combination material into the lower mold with an injection gun, fit and lock the upper mold and the middle mold, and foam and mold at a temperature of 60°C for 10 seconds after the mold is closed. Open the upper mold and the middle mold in turn, take out the soft cushion and trim it to obtain a corrective insole.

[0030] Example 4 A production process for corrective insoles, which is different from Example 3 in that, in step S3, an equal amount of nano zinc oxide is replaced by modified zinc oxide, and the preparation method of the modified zinc oxide is as follows: 100g of nano zinc oxide, 200g of propylene glycol, 10g of concentrated sulfuric acid, 50g of triclosan and 60g of polyethylene glycol are put into a water bath, mixed and stirred for 120min at a temperature of 70°C, 50g of ammonium polyphosphate is added and continued to be stirred for 15min, and after filtering, the modified zinc oxide is obtained after drying in an oven at a temperature of 80°C for 4h; wherein the ammonium polyphosphate is specifically Xinxindi model 25799; and the polyethylene glycol is specifically Shanghai Ximeng PEG4000.

[0031] Example 5 A production process for corrective insoles, which is different from that of Example 3 in that, in step S3, an equal amount of nano zinc oxide is replaced by modified zinc oxide, and the preparation method of the modified zinc oxide is as follows: 150g of nano zinc oxide, 240g of propylene glycol, 20g of concentrated sulfuric acid, 100g of triclosan and 80g of polyethylene glycol are put into a water bath, mixed and stirred for 120min at a temperature of 70°C, and then 60g of ammonium polyphosphate is added and continued to be stirred for 15min. After filtering, the modified zinc oxide is obtained after drying in an oven at a temperature of 80°C for 4h; wherein the ammonium polyphosphate is specifically Xinxindi model 25799; and the polyethylene glycol is specifically Shanghai Ximeng PEG4000.

[0032] Example 6 A production process for a corrective insole, which is different from Example 5 in that the input amount of nano zinc oxide is 120g, the input amount of ammonium polyphosphate is 50g, and the input amount of polyethylene glycol is 64g.

[0033] Example 7 A production process for a corrective insole, which is different from Example 5 in that the input amount of nano zinc oxide is 136 g, the input amount of ammonium polyphosphate is 50 g, and the input amount of polyethylene glycol is 72 g.

[0034] Example 8 A production process for corrective insoles, which is different from that of Example 7 in that, in step S3, the isocyanate of the second component is a modified isocyanate, and the preparation method of the modified isocyanate is as follows: 15g of sodium alginate is dissolved in 500g of water and put into a stirrer, 30g of sodium periodate is added and stirred evenly for 4h, 5g of ethylene glycol and 8g of cinnamamide ethanol solution are added and heated to 50°C and stirred for 4h; then 24g of isocyanate and 0.2g of sodium dodecyl sulfate are added and stirred evenly for 30min under the condition of heating in a water bath to obtain the modified isocyanate.

[0035] Example 9 A production process for corrective insoles, which is different from that of Example 7 in that, in step S3, the isocyanate of the second component is a modified isocyanate, and the preparation method of the modified isocyanate is as follows: 15g of sodium alginate is dissolved in 500g of water and put into a stirrer, 30g of sodium periodate is added and stirred evenly for 4h, 5g of ethylene glycol and 8g of cinnamamide ethanol solution are added and heated to 50°C and stirred for 4h; then 24g of isocyanate and 0.2g of sodium dodecyl sulfate are added and stirred evenly for 30min under the condition of heating in a water bath to obtain the modified isocyanate.

[0036] Example 10 A production process for corrective insoles, which is different from Example 9 in that, in the preparation method of modified isocyanate, the input amount of sodium alginate is 20g, the input amount of isocyanate is 28g, and the input amount of cinnamamide ethanol is 12g.

[0037] Embodiment 11 A production process for corrective insoles, which is different from Example 9 in that, in the preparation method of modified isocyanate, the input amount of sodium alginate is 20g, the input amount of isocyanate is 32g, and the input amount of cinnamamide ethanol is 15g.

[0038] Example 12 A production process for corrective insoles, which is different from Example 11 in that, in step S2, the preparation method of the nylon composite is: 150g of nylon 66, 100g of flax fiber and 70g of tea polyphenols are put into an electric stirrer, and stirred for 15min at a temperature of 75°C and a rotation speed of 200r / min to obtain the nylon composite; wherein the nylon 66 selected is the American DuPont model 70G30HSLR.

[0039] Comparative Example Comparative Example 1 A production process for a corrective insole, which is different from that of Example 3 in that, in step S2, the insole shell with burrs is trimmed to remove the burrs.

[0040] Comparative Example 2 A production process for a corrective insole, which is different from that of Example 3 in that an equal amount of polyether polyol A is used instead of polyether polyol B.

[0041] Comparative Example 3 A production process for a corrective insole, which is different from that of Example 3 in that an equal amount of polyether polyol B is used instead of polyether polyol A.

[0042] Comparative Example 4 A production process for a corrective insole, which is different from that of Example 3 in that an equal amount of nano zinc oxide is replaced by nano silicon dioxide.

[0043] Comparative Example 5 A production process for a corrective insole, which is different from Example 3 in that polyether polyol C is used instead of polyether polyol A, wherein the polyether polyol C has a hydroxyl value of 28 mgKOH / g, a molecular weight of 5000, and a functionality of 3.

[0044] Comparative Example 6 A production process for a corrective insole, which is different from Example 3 in that polyether polyol C is used instead of polyether polyol A and polyether polyol B, wherein the polyether polyol C has a hydroxyl value of 28 mgKOH / g, a molecular weight of 5000, and a functionality of 3.

[0045] Comparative Example 7 A production process for a corrective insole, which is different from Example 3 in that polyether polyol C is used instead of polyether polyol B, wherein the polyether polyol C has a hydroxyl value of 28 mgKOH / g, a molecular weight of 5000, and a functionality of 3.

[0046] Performance testing Tensile strength performance: The tensile strength at break of the corrective insoles of Examples 1-12 and Comparative Examples 1-7 was tested according to GB / T 528-2009 “Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber”.

[0047] Antibacterial performance: Taking Staphylococcus aureus ATCC6538 as an example, at a temperature of 25°C, the corrective insole samples of Examples 1-12 and Comparative Examples 1-7 were placed in special plastic bags, each 10 cm 2 Add 2 mL of inoculum solution to the sample, introduce air into the plastic bag, irradiate under sunlight for 30 minutes, then oscillate at 37℃±1° for 24 hours, determine the number of surviving bacteria by dilution plate culture method, and calculate the antibacterial rate.

[0048] Air permeability: The air permeability (ml / m 2 ), the test gas is nitrogen, the test time is 24 hours, and the test pressure is 0.2MPa.

[0049] According to the data comparison of Examples 1-3 and Comparative Examples 1-7, the present application reserves burrs in the process of preparing the insole shell. When the corrective insole is molded, the reserved burrs are tightly bonded to the soft pad, instead of using glue to bond the soft pad and the insole shell. The burrs and burrs remaining in the production of the insole shell are reasonably used, the use of chemical raw materials and the generation of organic compound gases are reduced, which has an environmental protection effect. At the same time, the edge position of the corrective insole is made flat, and the appearance quality of the insole is improved. A shock-absorbing block is set at the bottom of the corrective insole of the present application, so that the insole has good air permeability, elasticity and shock absorption. The polyether polyol combination material is used as a raw material in the soft pad, which can effectively improve the tensile strength of the corrective insole and improve the tensile strength at break of the corrective insole.

[0050] According to the data comparison of Examples 3-7, the present application modifies nano zinc oxide, and both triclosan and nano zinc oxide have good bactericidal effects. The modified nano zinc oxide is added to the soft pad and dispersed evenly in the micropores of the insole, thereby improving the air permeability of the corrective insole and improving the wearing comfort of the corrective insole; the modified zinc oxide has a microporous structure and can absorb the odor generated inside the shoe, thereby improving the mildew and antibacterial effect of the corrective insole; polyethylene glycol makes ammonium polyphosphate evenly dispersed in the nano zinc oxide, making the gaps between the nano zinc oxide smaller, thereby increasing the compressive strength of the polyether polyol combination supporting the insole, and further improving the air permeability of the corrective insole.

[0051] According to the data comparison of Examples 7-11, the present application modifies isocyanate, and the hydrophilicity of the isocyanate surface can be adjusted after the sodium alginate and isocyanate are mixed and modified, so that the second component of the isocyanate can be better combined with the first component, thereby further improving the air permeability and antibacterial effect of the corrective insole; when the sodium alginate, isocyanate and cinnamamide ethanol are in a specific weight ratio, cinnamamide is grafted into ammonium alginate, and ammonium alginate is filled in isocyanate, so that the modified isocyanate is combined with the first component, the emulsification effect of the isocyanate is improved, and a corrective insole with good elasticity and strength is obtained.

[0052] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.

Claims

1. A production process for corrective insoles, characterized in that: The following steps are involved: S1. The polyurethane is cut to obtain a shock-absorbing block; S2. The nylon composite material is mixed and stirred evenly, and after drying, the insole shell is obtained by twisting and weaving with burrs; S3. The polyether polyol composition is mixed and stirred to obtain a mixed solution; S4. Spray the mold release agent on the mold; place the shock absorbing block on the lower mold, fit and lock the middle mold with the lower mold, place the insole shell with burrs on the middle mold, and hang the cloth on the upper mold; S5. Inject the mixed liquid into the lower mold, fit and lock the upper mold and the middle mold, close the mold for foaming, open the mold to obtain a soft cushion, and complete trimming to obtain a corrective insole.

2. The production process of a corrective insole according to claim 1, characterized in that: In the step S2, the burr has a width of 2-4 mm and a thickness of 0.1-0.5 mm.

3. The production process of a corrective insole according to claim 1, characterized in that: The preparation method of the polyether polyol combination material is as follows: adding the second component to the first component while stirring, and stirring evenly after adding, so as to obtain the polyether polyol combination material; the preparation method of the first component is as follows: mixing and heating 400-600 parts by weight of polyether polyol A and 600-800 parts by weight of polyether polyol B, adding 80-120 parts by weight of nano zinc oxide and dispersing evenly, then heating 40-60 parts by weight of 2,4-diphenylmethane diisocyanate for heating reaction, and adding 10-20 parts by weight of defoamer, 80-100 parts by weight of butyl acetate and 40-100 parts by weight of ethylene glycol ethyl ether acetate after cooling, and stirring evenly, so as to obtain the first component; the preparation method of the second component is as follows: mixing 20-60 parts by weight of dibutyltin dilaurate, 100-200 parts by weight of water and 500-900 parts by weight of isocyanate evenly, so as to obtain the second component.

4. The production process of a corrective insole according to claim 3, characterized in that: The hydroxyl value of the polyether polyol A is 400-500 mg / g; the hydroxyl value of the polyether polyol B is 100-120 mgKOH / g, and the functionality is 2.

5. The production process of a corrective insole according to claim 1, characterized in that: In step S2, the preparation method of the nylon composite material is: 100-150 parts by weight of nylon, 80-100 parts by weight of flax fiber and 50-70 parts by weight of tea polyphenols are uniformly stirred to obtain the nylon composite material.

6. The production process of a corrective insole according to claim 3, characterized in that: The nano zinc oxide is modified nano zinc oxide; the preparation method of the modified nano zinc oxide is: 100-150 parts by weight of nano zinc oxide is mixed with 200-240 parts by weight of propylene glycol, 10-20 parts by weight of concentrated sulfuric acid, 50-100 parts by weight of triclosan and 50-80 parts by weight of polyethylene glycol, then 50-60 parts by weight of ammonium polyphosphate is added and stirred continuously, and the modified zinc oxide is obtained after filtering and drying.

7. The production process of a corrective insole according to claim 6, characterized in that: The weight ratio of the nano zinc oxide, ammonium polyphosphate and polyethylene glycol is (2.4-2.72):1:(1.28-1.44).

8. The production process of a corrective insole according to claim 3, characterized in that: The isocyanate is a modified isocyanate, and the preparation method of the modified isocyanate is as follows: dissolving 15-25 parts by weight of sodium alginate in water, adding 30-50 parts by weight of sodium periodate and stirring evenly, adding 5-15 parts by weight of ethylene glycol and 8-16 parts by weight of cinnamamide ethanol solution and continuing to stir; then adding 24-48 parts by weight of isocyanate and 0.2-0.6 parts by weight of sodium dodecyl sulfate and stirring evenly to obtain the modified isocyanate.

9. The production process of a corrective insole according to claim 8, characterized in that: The isocyanate is isophorone diisocyanate.

10. The production process of a corrective insole according to claim 8, characterized in that: The weight ratio of the sodium alginate, isocyanate and cinnamamide ethanol is 1: (1.4-1.6): (0.6-0.75).