Electromagnetic shielding film and preparation method thereof
Through the design of a multi-layer structure electromagnetic shielding film, the synergy of thermoplastic resin, carbon fiber and ceramic materials is used to solve the problem of difficult regulation of thermal conductivity, insulation and electromagnetic shielding performance in the prior art, and efficient electromagnetic shielding and thermal conductivity are achieved. The preparation process is simplified and the mechanical properties and environmental protection of the material are improved.
Patent Information
- Application Number
- CN202410985207.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-22
AI Technical Summary
The prior art is difficult to achieve electronic packaging materials with high thermal conductivity, good insulation and electromagnetic shielding performance at the same time, and the preparation process is complicated, the material interface is difficult to regulate, and the electromagnetic shielding and insulation performance is difficult to regulate.
A multi-layer structure electromagnetic shielding film composed of thermoplastic resin, carbon fiber, filler A and conductive inorganic ceramic materials, including a first shielding layer, a second shielding layer, a thermally conductive layer and an insulating layer, is prepared by vacuum heat pressing composite technology, and carbon fiber is used. Synergistically with ceramic materials, it achieves improvements in electromagnetic shielding and thermal conductivity.
It realizes efficient electromagnetic shielding and thermal conductivity, simplifies the preparation process, improves the mechanical properties and environmental protection of the materials, avoids the use of solvents, and is suitable for large-scale production.
Smart Images

Figure BDA0004957550820000051 
Figure BDA0004957550820000061 
Figure BDA0004957550820000062
Abstract
Description
Technical Field
[0001] The invention belongs to the field of electromagnetic shielding film preparation, and in particular relates to an electromagnetic shielding film and a preparation method thereof. Background Art
[0002] With the rapid development of electronic devices towards miniaturization, high integration and high power density, heat dissipation seriously affects the performance, stability and service life of the equipment, restricting the further development of high power density electronic devices. In addition, the working process of highly dense electronic components will also generate a large amount of electromagnetic radiation, which will cause signal interference between adjacent devices, affect the normal operation of other precision electronic equipment, cause instrument accuracy to decrease, and may even cause the leakage of important information. At the same time, electronic packaging materials are usually required to have good electrical insulation to prevent device short circuits. Therefore, research and development of electronic packaging materials with both insulation, thermal conductivity and electromagnetic shielding functions are of great significance and great commercial prospects.
[0003] For example, Chinese patent CN114477157A provides a method for enhancing thermal conductivity, which comprehensively utilizes the large-area preparation and adjustable high thermal conductivity of raw graphene oxide (RGO) and the electrical insulation performance of boron nitride to prepare a boron nitride / RGO heterojunction, achieving the preparation of high thermal conductivity and good insulation performance fillers. However, this technology has the following disadvantages: First, the interface bonding of the two materials is difficult to control, the fixed-point transfer of boron nitride is difficult to achieve, and the process is complicated. Second, whether the material has an electromagnetic shielding function has not been verified, and it is difficult to regulate between electromagnetic shielding and insulation performance.
[0004] Chinese invention patent CN108129685A (patent name: multilayer composite thermal conductive film and preparation method thereof) constructs a composite thermal conductive film with a nanocellulose film as the middle layer, and nanocellulose / graphene film layers or (and) nanocellulose / boron nitride film layers are coated on the upper and lower surfaces in sequence, and the layers are connected by hydrogen bonds between the cellulose matrix to form a composite thermal conductive film with an ABA three-layer structure and an ACBCA five-layer structure, which has good thermal conductivity, mechanical properties and insulation properties. However, in this technology, the nanocellulose / graphene aqueous dispersion and the nanocellulose / boron nitride thin aqueous dispersion are only prepared by simple mechanical blending and ultrasonic dispersion, which is difficult to disperse evenly and cannot achieve high-content doping. The content of graphene and boron nitride is low, so the thermal conductivity of the final composite film is low (only 6.82300W / (m·K)).
[0005] Therefore, there is an urgent need for a composite film with simple structure, simple preparation process, excellent performance, and strong insulation, thermal conductivity, and electromagnetic shielding efficiency. Summary of the invention
[0006] The object of the present invention is to provide an improved electromagnetic shielding film and a preparation method thereof.
[0007] In order to achieve the above object, a technical solution adopted by the present invention is:
[0008] An electromagnetic shielding film, comprising a first shielding layer, a second shielding layer, a heat-conducting layer and an insulating layer arranged in sequence, wherein the raw materials of the first shielding layer include thermoplastic resin A, carbon fiber and filler A; the raw materials of the second shielding layer include thermoplastic resin B and filler B, and the second shielding layer is a foaming layer.
[0009] In some embodiments, the raw materials of the first shielding layer include, by weight:
[0010] Thermoplastic resin A: 100,
[0011] Carbon fiber: 100~200,
[0012] Filler A: 10-20;
[0013] The first shielding layer can absorb or attenuate electromagnetic energy propagation between the shielding area and the outside world.
[0014] In some embodiments, the thermoplastic resin A has the properties of softening by heat and hardening by cooling, and does not react chemically. No matter how many times the heating and cooling are repeated, this property can be maintained. The thermoplastic resin A can be a combination of one or more of polyethylene, polypropylene, polyvinyl chloride, polystyrene, nylon, polyoxymethylene, polycarbonate, polyphenylene ether, polysulfone, rubber, and polyester. For better mechanical properties, one or more of nylon and polypropylene are preferred. Nylon is a polymer material containing a repeating structural unit of an amide group (-CO-NH-) in the main chain of the macromolecule, and polypropylene is a polymer material containing a repeating structural unit of [CH2-CH(CH3)]n in the main chain of the macromolecule.
[0015] In some embodiments, the carbon fiber is mainly composed of carbon element, which is light in weight, has excellent conductivity, and can absorb and attenuate the electromagnetic energy propagation between the shielding area and the outside world. The carbon fiber can be carbon fiber powder, short chopped carbon fiber, long chopped carbon fiber, carbon fiber filament, carbon fiber cloth, etc. In order to achieve better electromagnetic shielding energy efficiency and thermal conductivity and heat dissipation, and for the simplicity of the preparation process, the carbon fiber is preferably one or more of carbon fiber powder or short chopped carbon fiber.
[0016] In the first shielding layer, the thermoplastic resin A contains 100 to 200 parts by weight of carbon fiber based on 100 parts by weight. If the amount of carbon fiber is small, the mechanical properties of the electromagnetic shielding film are weakened, and the small amount of carbon fiber is not conducive to the electromagnetic shielding energy efficiency of the film. If the amount of carbon fiber is large, the electromagnetic shielding energy efficiency is limited, but the preparation cost increases greatly. Therefore, the amount of carbon fiber in the first shielding layer is preferably 130 to 180 parts by weight.
[0017] In the first shielding layer, the amount of filler A is 10 to 20 parts by weight. If the amount of filler A is small, the synergistic effect between it and the carbon fiber is weakened, and the electromagnetic shielding efficiency is poor. If the amount of filler A is large, the thermoplastic resin A is easily decomposed, the film strength is reduced, and the shielding area is easily exposed to the external environment. Therefore, the amount of filler A is preferably 12 to 18 parts by weight.
[0018] In some embodiments, the filler A is a powder, which is a powder with metal or metal oxide as the main component, which can coordinate with carbon fiber to enhance electromagnetic shielding energy efficiency. The metal powder can be a combination of one or more of iron powder, cobalt powder, nickel powder, copper powder, zinc powder, aluminum powder, titanium powder, vanadium powder, chromium powder, manganese powder, silver powder, platinum powder, gold powder, iron oxide, nickel oxide, cobalt oxide, copper oxide, aluminum oxide, titanium oxide, and tungsten oxide. For better electromagnetic shielding energy efficiency, filler A is preferably one or more of copper powder and copper oxide powder.
[0019] In some embodiments, the average particle size of the filler A powder is 10 to 200 nm. If the particle size is smaller, it is easy to cause dust pollution, and if the particle size is larger, it is not conducive to uniform mixing. Therefore, the average particle size of the filler A powder is preferably 10 to 100 nm.
[0020] In some embodiments, the material of the second shielding layer includes:
[0021] Thermoplastic resin B: 100,
[0022] Filler B: 50~100.
[0023] The second shielding layer can absorb the remaining clutter after being absorbed by the first shielding layer, thereby improving the shielding energy efficiency.
[0024] In some embodiments, the thermoplastic resin B includes a combination of one or more of polystyrene, polyurethane, polyvinyl chloride, and polyethylene. Considering the synergistic effect with filler B (ease of dispersibility and processability of filler B in thermoplastic resin B) and enhancing electromagnetic shielding energy efficiency, one or more of polyethylene and polyurethane are preferred.
[0025] In some embodiments, the filler B is a conductive inorganic ceramic compound, which is a functional material with ionic conductivity, electronic and hole conductivity. It has both metallic conductivity and the structural characteristics, mechanical properties and unique physical and chemical properties of ceramics, such as anti-oxidation, anti-corrosion, anti-radiation, high temperature resistance, etc. The filler B is selected from one or more of metal-based conductive ceramics, oxide-based conductive ceramics, nitride-based conductive ceramics, boride-based conductive ceramics, and carbide-based conductive ceramics, wherein metal-based conductive ceramics include metal-based ceramics such as iron, nickel powder, copper powder, and aluminum powder; oxide-based conductive ceramics include oxide-based conductive ceramics such as V2O5, TiO2, Nb2O5, CdO, CsO, MoO3, WO3, BaO, SnO2, Ta2O5, BaTiO3, PbCrO4, ZnO, Al2O3, MgFe2O4, CuFe2O4, and Fe3O4; nitride, boride, and carbide-based conductive ceramics include nitride, boride, and carbide-based conductive ceramics such as WC, TiC, NbC, Cr3C2, Mo2C, VC, ZrC, and SiC. Considering the synergistic effect with the thermoplastic resin B, the filler B is preferably one or more of SiC ceramics and Al2O3 ceramics.
[0026] In some embodiments, the second shielding layer is foamed, and foaming means that the second shielding layer material itself has countless tiny pores inside.
[0027] In some embodiments, the porosity of the second shielding layer is 20-50%, and the porosity refers to the percentage of the pore volume in the bulk material to the total volume of the material in the natural state, and the porosity is tested according to GB / T 10799-2008. If the porosity is small, the pore volume in the material is small, and the filler B cannot be coated. During the long-term use of the electronic product, the filler B is easy to fall off, reducing the thermal conductivity. If the porosity is large, it is easy to cause pore waste, preferably 25-45%.
[0028] In some embodiments, the diameter of the micropores of the second shielding layer is 0.5 to 2 μm. The large diameter micropores of the second shielding layer are conducive to better absorption of electromagnetic waves passing through the first shielding layer, and are conducive to enhancing thermal conductivity. The micropore diameter is the cross-sectional diameter of the pores in the second shielding layer, which is measured by scanning electron microscopy of the cross section. For better electromagnetic shielding energy efficiency and thermal conductivity, the diameter of the micropores of the second shielding layer is preferably 0.8 to 1.5 μm.
[0029] In some embodiments, the thermal conductive layer can dissipate heat quickly. Electronic components will generate heat energy during use. Rapid heat dissipation can extend their service life. The presence of the thermal conductive layer can enable heat to reach the surface by conduction and heat dissipation. Relying on the combined effects of thermal conductivity and radiation of the thermal conductive layer, heat can be dissipated quickly, causing the surface and internal temperatures of the object to drop, ultimately achieving the purpose of cooling and heat dissipation.
[0030] In some embodiments, the heat-conducting layer is particles attached to the second shielding layer, and the heat-conducting layer includes one or more of metal oxides and silicon nitride; the metal oxide includes a combination of one or more of iron oxide, nickel oxide, cobalt oxide, copper oxide, aluminum oxide, titanium oxide, and tungsten oxide. The silicon nitride is an inorganic substance with a chemical formula of Si3N4.
[0031] In some embodiments, the insulating layer mainly protects the thermal conductive layer, the first shielding layer, and the second shielding layer, reduces mechanical damage and chemical corrosion during use, prevents the thermal conductive layer, the first shielding layer, and the second shielding layer from contacting water vapor and getting damp, and prevents electric shock from contacting the conductor, etc., which can increase the service life of the coated electronic device. The insulating layer includes a polymer and a metal oxide, and the polymer is selected from one or more of polyimide, polytetrafluoroethylene, polyethylene, polypropylene, polyvinyl chloride, polystyrene, polyamide, polyformaldehyde, polycarbonate, polyphenylene ether, polysulfone, rubber, and polyester. In order to improve the thermal conductivity of the electromagnetic shielding film, the shielding layer is prevented from being damaged by absorbing too much heat energy from electromagnetic waves. The metal oxide is selected from a combination of one or more of iron oxide, nickel oxide, cobalt oxide, copper oxide, aluminum oxide, titanium oxide, and tungsten oxide. Considering the compatibility of the polymer and the metal oxide, it is preferably one or more of polyimide, polytetrafluoroethylene or polyethylene.
[0032] Another technical solution adopted by the present invention is:
[0033] A method for preparing the electromagnetic shielding film comprises:
[0034] (1) preparing a first shielding layer, a second shielding layer, a heat conducting layer and an insulating layer, wherein:
[0035] When preparing the first shielding layer, the raw material of the first shielding layer is melted to form a film, and the film is stretched to make the film twice in the transverse direction and the longitudinal direction to obtain the first shielding layer, specifically: firstly, the thermoplastic resin A is heated to 150-300°C, preferably 160-280°C (the melting point of polypropylene is 160-180°C, and the melting point of nylon PA66 is 260-280), and carbon fiber and filler A are added after melting, and then the product is extruded, and a casting process is performed on the obtained product to obtain a pre-treated sheet, and then the pre-treated sheet is stretched longitudinally and transversely to obtain the first shielding layer;
[0036] When preparing the second shielding layer, the raw material of the second shielding layer is melted and then foamed, extruded to form a foamed film, and the film is stretched so that the film is stretched twice in the transverse direction and the longitudinal direction to obtain the second shielding layer;
[0037] Prepare a heat-conducting layer, spray the heat-conducting layer material on one side of the second shielding layer to obtain the heat-conducting layer;
[0038] When preparing the insulating layer, the raw materials of the insulating layer are melted to form a film, specifically: firstly, the polymer is heated to 100-400° C., preferably 130-330° C., and the metal oxide is added after melting, and then the obtained product is extruded and subjected to a sheet casting process to obtain a pre-treated sheet, and then the pre-treated sheet is longitudinally stretched and transversely stretched to obtain the insulating layer;
[0039] (2) The first shielding layer, the second shielding layer, the heat-conducting layer, and the insulating layer are composited and hot-pressed in sequence to obtain the electromagnetic shielding film.
[0040] In some embodiments, the preparation method of the second shielding layer is as follows: the foaming is performed by supercritical fluid foaming. The advantages of supercritical foaming are: shorter time, finer pores, stronger stress structure, more uniform pore distribution and controllable particle size, thereby making the product have a lower density.
[0041] Specifically, thermoplastic resin B and filler B are placed in a reaction container, heated to 170-250°C, soaked in 10-20MPa supercritical CO2 for 1-5 hours, and then foamed under steam at 150-200°C. Subsequently, the foamed film is extruded and stretched to obtain a second shielding layer in the transverse and longitudinal directions.
[0042] Supercritical fluid refers to the state in which the density of gas and liquid phases tends to be the same and merges into a uniform phase when the temperature and pressure of the fluid reach a certain point. This specific point is called the critical point of the fluid. When the temperature and pressure of any fluid exceed the critical point and reach the supercritical state, the fluid at this time is defined as a supercritical fluid. Once a substance enters the supercritical fluid state, it presents a stable and special phase between liquid and gas. It cannot be completely classified as either liquid or gas, but it has the material properties of both. On the one hand, it has the gas state properties of low surface tension, low viscosity, and high diffusivity, and on the other hand, it also has the liquid properties of high solubility and high density.
[0043] The second shielding layer mainly shields the electromagnetic waves that pass through the first shielding layer, and because of the developed pore structure, the second shielding layer has better thermal conductivity than the first shielding layer. The electromagnetic waves that pass through the first shielding layer can be absorbed by the second shielding layer, and the heat emitted from the electronic components can be transferred to the first shielding layer by filler B, and then to the insulating layer, achieving rapid heat dissipation layer by layer.
[0044] Due to the application of the above technical solution, the present invention has the following advantages compared with the prior art:
[0045] The electromagnetic shielding film provided by the present invention is provided with a first shielding layer and a second shielding layer. The second shielding layer can absorb the clutter passing through the first shielding layer, and the electromagnetic shielding efficiency is better; the second shielding layer in the electromagnetic shielding film has large-diameter micropores, which can evenly disperse the filler B, and cooperate with the thermal conductive layer and the insulating layer, and has better thermal conductivity, and can quickly dissipate the heat energy generated by the shielding layer due to excessive absorption of electromagnetic waves, thereby avoiding overheating of electronic components; the preparation process of the electromagnetic shielding film of the present invention does not use solvents, is environmentally friendly and has a simple preparation process. DETAILED DESCRIPTION
[0046] The present invention is further described below in conjunction with the illustrated embodiments.
[0047] The first shielding layer, the second shielding layer, the heat conducting layer and the insulating layer are prepared respectively, wherein the raw material formula of the first shielding layer is shown in Table 1.
[0048] Table 1 Raw materials of the first shielding layer
[0049]
[0050]
[0051] In the above table, the raw materials of the first shielding layer are as follows:
[0052] 1. Thermoplastic resin A
[0053] A1: Polypropylene, F280 polypropylene produced by Sinopec Shanghai Petrochemical Co., Ltd.
[0054] A2: Nylon, EPR27 PA66 nylon produced by Shanghai Feimai Plastic Chemical Co., Ltd.
[0055] 2. Carbon fiber
[0056] B1: Carbon fiber powder, MLD-300 carbon fiber powder produced by Toray Industries, Ltd., Japan, with a fiber length of 130 μm.
[0057] B2: Chopped carbon fiber, T700 chopped carbon fiber produced by Toray Industries, Ltd., Japan, fiber length 2mm.
[0058] 3. Filler A
[0059] C1: Copper powder, DK-Cu-001 nano copper powder produced by Beijing Dekedaojin Technology Co., Ltd., with an average particle size of 50nm.
[0060] C2: Copper oxide powder, DK-CuO nano copper oxide powder produced by Beijing Dekedaojin Technology Co., Ltd., with an average particle size of 40nm.
[0061] The preparation method of the first shielding layer is as follows:
[0062] 1. The first shielding layer (M1, M3-M9) is prepared according to the formula shown in Table 1. The thermoplastic resin A is placed in a reaction container and heated to 160°C. After melting, carbon fiber and filler A are added, followed by twin-screw extrusion at a temperature of 160°C. The obtained product is subjected to a sheet casting process to obtain a pretreated sheet, and the pretreated sheet is then longitudinally stretched and transversely stretched to obtain the first shielding layer (M1, M3-M9).
[0063] 2. The first shielding layer (M2) is prepared according to the formula shown in Table 1. Thermoplastic resin A is placed in a reaction container and heated to 260°C. Carbon fiber and filler A are added after melting. The product is then extruded through a twin-screw at a temperature of 260°C. The product is subjected to a casting process to obtain a pretreated sheet. The pretreated sheet is then longitudinally and transversely stretched to obtain the first shielding layer M2.
[0064] The raw material formula of the second shielding layer is shown in Table 2.
[0065] Table 2 Materials of the second shielding layer
[0066]
[0067]
[0068] In the above table, the materials of the second shielding layer are as follows:
[0069] 1. Thermoplastic resin B
[0070] D1: Polyethylene, LD100AC polyethylene produced by Sinopec Shanghai Petrochemical Co., Ltd.
[0071] D2: Polyurethane, FP3039D6 polyether polyurethane produced by GreenMobil.
[0072] 2. Filler B
[0073] E1: SiC ceramics, YM-SiC-50N SiC ceramics produced by Yumu (Ningbo) New Materials Co., Ltd., with an average particle size of 50nm.
[0074] E2: Al2O3 ceramics, alumina ceramics produced by Yixing Yalong Special Ceramics Co., Ltd.
[0075] The preparation method of the second shielding layer is as follows:
[0076] 1. The second shielding layer (N1, N3-N6) is prepared according to the formula shown in Table 2. The thermoplastic resin B and filler B are placed in a reaction vessel, heated to 130°C, soaked in supercritical CO2 at 130°C and 15MPa for 2 hours, and then foamed under steam at 100°C. Subsequently, the foamed film is extruded and stretched to make the film stretch twice in the transverse and longitudinal directions to obtain the second shielding layer (N1, N3-N6). The porosity of the second shielding layer (N1) is 37% and the micropore diameter is 1.2μm; the porosity of the second shielding layer (N3) is 23% and the micropore diameter is 1.5μm; the porosity of the second shielding layer (N4) is 25% and the micropore diameter is 1.3μm; the porosity of the second shielding layer (N5) is 45% and the micropore diameter is 0.8μm; the porosity of the second shielding layer (N6) is 21% and the micropore diameter is 1.8μm.
[0077] 2. The second shielding layer (N2) is prepared according to the formula shown in Table 2. The thermoplastic resin B and filler B are placed in a reaction vessel, heated to 200°C, soaked in supercritical CO2 at 200°C and 15MPa for 2 hours, and then foamed under steam at 180°C. Subsequently, the foamed film is extruded and stretched to obtain a second shielding layer in the transverse and longitudinal directions. The porosity of the second shielding layer (N2) is 43%, and the micropore diameter is 0.9μm.
[0078] 3. The second shielding layer (N7) is prepared according to the formula shown in Table 2. The thermoplastic resin B and filler B are placed in a reaction container, heated to 200°C, and then extruded into a film. The film is stretched so that it is stretched twice in the transverse and longitudinal directions to obtain the second shielding layer (N7). The second shielding layer (N7) is unfoamed.
[0079] The raw materials of the thermal conductive layer are as follows:
[0080] F1: Alumina, DK410-2 nano-alumina produced by Beijing Dekedaojin Technology Co., Ltd., with an average particle size of 20nm.
[0081] F2: Silicon nitride, DK-Si3N4-01 nano silicon nitride produced by Beijing Dekedaojin Technology Co., Ltd., with an average particle size of 20nm.
[0082] Insulation material:
[0083] Polyimide: YS-20 produced by Junhua Co., Ltd.
[0084] Copper oxide: C112566 produced by Aladdin (Shanghai) Reagent Co., Ltd.;
[0085] Polytetrafluoroethylene: P434335 produced by Aladdin (Shanghai) Reagent Co., Ltd.;
[0086] Polyethylene: P434335 produced by Aladdin (Shanghai) Reagent Co., Ltd.
[0087] The preparation method of the insulating layer is as follows:
[0088] G1: Put polyimide into a reaction container, heat it to 360°C, add copper oxide powder filler after melting, then extrude it through a twin-screw extruder at a temperature of 360°C, and subject the obtained product to a sheet casting process to obtain a pretreated sheet. The pretreated sheet is then stretched longitudinally and transversely to obtain an insulating layer G1.
[0089] G2: Put polytetrafluoroethylene into a reaction container, heat it to 330°C, add copper oxide powder filler after melting, then extrude it through a twin-screw extruder at a temperature of 330°C, and subject the obtained product to a casting process to obtain a pretreated sheet. The pretreated sheet is then stretched longitudinally and transversely to obtain an insulating layer G2.
[0090] G3: Put polyethylene into a reaction container, heat it to 130°C, add copper oxide powder filler after melting, then extrude it through a twin-screw extruder at a temperature of 130°C, and subject the obtained product to a casting process to obtain a pretreated sheet. The pretreated sheet is then stretched longitudinally and transversely to obtain an insulating layer G2.
[0091] Provide examples 1-15 and comparative examples 1-7, and refer to Table 3 for the raw material formulas of examples 1-15 and comparative examples 1-7.
[0092] Table 3 Raw material formula of Examples 1-15 and Comparative Examples 1-7
[0093]
[0094]
[0095] According to the formula described in Table 3, the heat conductive layer is sprayed on one side of the second shielding layer, and then the first shielding layer, the second shielding layer, the heat conductive layer and the insulating layer are compounded to obtain an electromagnetic shielding film.
[0096] The electromagnetic shielding films of Examples 1-15 and Comparative Examples 1-7 were subjected to the following tests. Unless otherwise specified, each test was conducted at 25° C. The main indicators are as follows:
[0097] 1. Average electromagnetic shielding effectiveness: tested in accordance with GB / T30142-2013 standard;
[0098] 2. Tensile strength: tested according to GB / T 1040.1-2018;
[0099] 3. Thermal conductivity: Tested in accordance with national standard GB / T 10297-2015.
[0100] Table 4 Performance data of electromagnetic shielding films of Examples 1-15 and Comparative Examples 1-7
[0101]
[0102]
[0103] As shown in Table 4, compared with the electromagnetic shielding films of Examples 1-15 and Comparative Examples 1-7, the electromagnetic shielding films prepared in Examples 1-15 have better thermal conductivity and better electromagnetic shielding effectiveness; the electromagnetic shielding films prepared in Examples 1-15 have superior mechanical properties and a pollution-free preparation process, which is convenient for large-scale production.
[0104] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. An electromagnetic shielding film, characterized in that: The electromagnetic shielding film includes a first shielding layer, a second shielding layer, a heat-conducting layer and an insulating layer arranged in sequence. The raw materials of the first shielding layer include thermoplastic resin A, carbon fiber and filler A; the raw materials of the second shielding layer include thermoplastic resin B and filler B, and the second shielding layer is a foaming layer.
2. The electromagnetic shielding film according to claim 1, characterized in that In parts by weight, the raw materials of the first shielding layer include: thermoplastic resin A: 100, carbon fiber: 100-200, filler A: 10-20; The raw materials of the second shielding layer include: thermoplastic resin B: 100, filler B: 50-100.
3. The electromagnetic shielding film according to claim 1, characterized in that The thermoplastic resin A includes one or more of polyethylene, polypropylene, polyvinyl chloride, polystyrene, nylon, polyoxymethylene, polycarbonate, polyphenylene ether, polysulfone, rubber, and polyester.
4. The electromagnetic shielding film according to claim 1, characterized in that The filler A contains metal elements, and the filler A includes one or more combinations of iron, cobalt, nickel, copper, zinc, aluminum, titanium, vanadium, chromium, manganese, silver, platinum, gold, iron oxide, nickel oxide, cobalt oxide, copper oxide, aluminum oxide, titanium oxide, and tungsten oxide.
5. The electromagnetic shielding film according to claim 1, characterized in that The thermoplastic resin B includes one or more combinations of polystyrene, polyurethane, polyvinyl chloride, and polyethylene; and\or, the filler B is a conductive ceramic, and the filler B includes one or more combinations of metal-based conductive ceramics, oxide-based conductive ceramics, nitride-based conductive ceramics, boride-based conductive ceramics, and carbide-based conductive ceramics.
6. The electromagnetic shielding film according to claim 1, characterized in that The porosity of the second shielding layer is 20-50%, and the diameter of the micropores of the second shielding layer is 0.5-2 μm.
7. The electromagnetic shielding film according to claim 1, characterized in that The thermal conductive layer is particles attached to the second shielding layer, and the thermal conductive layer includes one or more of metal oxides and silicon nitride; the metal oxide includes a combination of one or more of iron oxide, nickel oxide, cobalt oxide, copper oxide, aluminum oxide, titanium oxide, and tungsten oxide.
8. The electromagnetic shielding film according to claim 1, characterized in that The insulating layer includes a polymer and a metal oxide, the polymer is selected from a combination of one or more of polyimide, polytetrafluoroethylene, polyethylene, polypropylene, polyvinyl chloride, polystyrene, polyamide, polyformaldehyde, polycarbonate, polyphenylene ether, polysulfone, rubber, and polyester, and the metal oxide is selected from a combination of one or more of iron oxide, nickel oxide, cobalt oxide, copper oxide, aluminum oxide, titanium oxide, and tungsten oxide.
9. A method for preparing an electromagnetic shielding film according to any one of claims 1 to 8, characterized in that: include: (1) preparing a first shielding layer, a second shielding layer, a heat-conducting layer and an insulating layer, wherein when preparing the second shielding layer, the raw material of the second shielding layer is melted and then foamed to form a foamed film; (2) The first shielding layer, the second shielding layer, the heat conducting layer and the insulating layer are compounded in sequence to obtain the electromagnetic shielding film.
10. The method for preparing an electromagnetic shielding film according to claim 9, characterized in that: In step (1), when preparing the second shielding layer, the raw material of the second shielding layer is melted and then mixed with a supercritical fluid, and foamed under steam to form a foamed film.
Citation Information
Patent Citations
Multilayer composite thermal conductive film and preparation method thereof
CN108129685A
Method for enhancing thermal conductivity of reduced graphene oxide
CN114477157A
Wide band electromagnetic wave-shielded polyethylene compound film containing carbonyl iron powder and preparation method thereof
CN101362390A
Insulating heat-conducting polymer composite material with frequency selective electromagnetic shielding and preparation method thereof
CN111391440A
Epoxy resin-based high-thermal-conductivity insulating material and preparation method thereof
CN112961469A
Cited By
Foaming type metal-based wave-absorbing shielding sheet and preparation method thereof
CN120697345A
A foamed metal-based wave-absorbing and shielding sheet and a method for preparing the same
CN120697345B