Ultra-dispersed rare earth doped MoSe2 material as well as preparation method and application thereof
Synthesis of superdispersed rare earth-doped MoSe2 materials by solvent thermal method solves the problems of poor conductivity and easy aggregation of MoSe2 materials, significantly improves catalytic activity and stability, is suitable for electrocatalytic hydrogen production applications, and reduces production costs.
Patent Information
- Application Number
- CN202411067127.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-05
AI Technical Summary
The existing MoSe2 materials have problems of poor conductivity and easy aggregation in electrocatalytic hydrogen production, which limits their catalytic activity and performance.
Superdispersed rare earth doped MoSe2 material was synthesized by solvothermal method, and the MoSe2 structure was regulated by dopamine and rare earth dopants, inhibit agglomeration and introduce Se vacancy defects, and improve catalytic activity.
It significantly improves the catalytic activity and stability of MoSe2 materials, improves the electrocatalytic hydrogen production performance, reduces production costs, and is suitable for large-scale applications.
Smart Images

Figure CN118954438A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electrocatalytic hydrogen production, and in particular to an ultra-dispersed rare earth-doped MoSe2 material, a preparation method thereof and applications thereof. Background Art
[0002] Due to the increasingly serious energy issues related to energy security, environmental pollution, etc., hydrogen with high energy density and zero greenhouse gas emissions has been recognized as an ideal alternative fuel to alleviate the future global energy crisis. The electrochemical hydrogen evolution reaction (HER) is an effective method to convert intermittent electrical energy into renewable hydrogen energy. However, the high overpotential barrier and sluggish kinetics strongly limit the performance of HER. The precious metal platinum (Pt) is an efficient electrocatalyst commonly used in HER to increase the reaction rate with almost zero overpotential, but the high cost and scarcity of Pt on Earth greatly hinder its large-scale application.
[0003] In the past few decades, two-dimensional materials such as graphene, transition metal dichalcogenides (TMDs) and MXenes have attracted extensive attention due to their ultrathin layered structures, unique physicochemical properties and controllable electronic structures. Among them, transition metal dichalcogenides, especially molybdenum disulfide and diselenide (MoX2, X = S and Se), can be used to design advanced hydrogen evolution electrocatalysts to reduce overpotential and promote reaction kinetics. Moreover, transition metal dichalcogenides have become competitive candidates due to their excellent catalytic activity, excellent stability, abundant earth resources and relatively low cost. Among them, MoSe2 is a typical layered TMD composite material, similar to graphene. In many applications, MoSe2 is often regarded as an analogue of MoS2, but MoSe2 exhibits better conductivity than MoS2, which is attributed to the metallic nature of selenium atoms. Increasing Se active sites or Se vacancies in the basal plane of MoSe2 is an effective way to improve the HER performance, while integrating heterometallic content into MoSe2 can also improve the HER performance. Phase modulation of MoS2 / Diselenide drives the enhancement of electrocatalytic performance, and MoSe2-based materials have become a hot research topic in the field of energy storage and conversion due to their excellent stability, easy processing and high HER performance. However, current MoSe materials still have the constraints of poor conductivity and easy aggregation. Summary of the invention
[0004] In view of this, the technical problem to be solved by the present invention is to provide an ultra-dispersed rare earth-doped MoSe2 material, a preparation method and application thereof. The ultra-dispersed rare earth-doped MoSe2 material prepared by the present invention exhibits excellent catalytic activity in electrocatalytic hydrogen production.
[0005] The present invention provides a method for preparing an ultra-dispersed rare earth-doped MoSe2 material, comprising the following steps:
[0006] S1) mixing solution A and solution B to obtain an emulsion;
[0007] The A solution is obtained by mixing a selenium source and hydrazine hydrate; the B solution is obtained by mixing a molybdenum source and an aqueous solvent; the aqueous solvent consists of water and dopamine;
[0008] S2) mixing the rare earth dopant and the emulsion, uniformly dispersing them by ultrasonication, and then heating them for solvent thermal reaction. The obtained solid product is annealed in a mixture of hydrogen and argon to obtain an ultra-dispersed rare earth-doped MoSe2 material.
[0009] Preferably, in step S1), the selenium source is selected from at least one of selenium powder, selenomethionine and dibenzyl diselenide;
[0010] The usage ratio of the selenium source and hydrazine hydrate is 70-100 mg: 6-13 mL.
[0011] Preferably, in step S1), the molybdenum source is selected from at least one of ammonium molybdate, sodium molybdate, sodium molybdate dihydrate, ammonium phosphomolybdate, molybdenum trioxide and molybdenum acetate;
[0012] The molybdenum source and the aqueous solvent are used in a ratio of 240-250 mg: 35-55 mL;
[0013] The volume ratio of water to dopamine is 30-40:5-15.
[0014] Preferably, in step S1), the mass ratio of the selenium source to the molybdenum source is 70-100:240-250.
[0015] Preferably, in step S2), the rare earth dopant is a metal salt containing rare earth ions; the rare earth ions in the rare earth dopant include Lu 3+ 、Tm 3+ 、Ru 3+ 、Sm 3+ and La 3+ At least one of .
[0016] Preferably, in step S2), the concentration of the rare earth dopant in the solution obtained by mixing the rare earth dopant with the emulsion is 0.01-0.1 mmol / L.
[0017] Preferably, in step S2), the temperature of the solvent thermal reaction is 180-220° C. and the time is 10-14 h.
[0018] Preferably, in step S2), the volume ratio of hydrogen to argon is 3-7:95-105;
[0019] The annealing temperature is 550-650° C. and the annealing time is 1-3 hours.
[0020] The present invention also provides an ultra-dispersed rare earth-doped MoSe2 material prepared by the preparation method described above.
[0021] The present invention also provides an application of the ultra-dispersed rare earth-doped MoSe2 material as described above as a hydrogen evolution electrocatalyst.
[0022] The present invention provides a method for preparing a super-dispersed rare earth doped MoSe2 material, comprising the following steps: S1) mixing solution A and solution B to obtain an emulsion; the solution A is obtained by mixing a selenium source and hydrazine hydrate; the solution B is obtained by mixing a molybdenum source and an aqueous solvent; the aqueous solvent is composed of water and dopamine; S2) mixing a rare earth dopant with the emulsion, uniformly dispersing by ultrasonication, heating for a solvothermal reaction, and annealing the obtained solid product in a mixture of hydrogen and argon to obtain a super-dispersed rare earth doped MoSe2 material. The present invention synthesizes a super-dispersed rare earth doped MoSe2 material by a solvothermal method, and in the solvothermal process, dopamine organic molecules and rare earth dopants are introduced to regulate the MoSe2 structure, and both the dopamine molecules and the rare earth dopant play multiple roles in the synthesis process. Generally, MoSe2 is prone to agglomeration during wet bottom-up synthesis due to its high surface energy; dopamine molecules carrying functional groups show strong affinity for Mo atoms and can be inserted into the Se-Mo-Se interlayer as a passivator to inhibit its overgrowth. Rare earth dopants, whose rare earth cation radius (usually 0.84-1.06pm) is much larger than the radius of Mo ions (0.68pm), easily distort the lattice of MoSe2 when they enter the Se-Mo-Se basal plane and leave Se vacancy defects in the lattice. The obtained ultra-dispersed rare earth-doped MoSe2 material exhibits excellent catalytic performance in water electrolysis. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a SEM image of the ultra-dispersed rare earth-doped MoSe2 material prepared in Example 1 of the present invention;
[0024] Figure 2 TEM image of the ultra-dispersed rare earth-doped MoSe2 material prepared in Example 1 of the present invention;
[0025] Figure 3 XRD pattern of the ultra-dispersed rare earth-doped MoSe2 material prepared in Example 1 of the present invention;
[0026] Figure 4 This is an electrochemical activity diagram of the ultra-dispersed rare earth-doped MoSe2 material of Example 1 of the present invention as a hydrogen evolution electrocatalyst. DETAILED DESCRIPTION
[0027] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] The present invention provides a method for preparing an ultra-dispersed rare earth-doped MoSe2 material, comprising the following steps:
[0029] S1) mixing solution A and solution B to obtain an emulsion;
[0030] The A solution is obtained by mixing a selenium source and hydrazine hydrate; the B solution is obtained by mixing a molybdenum source and an aqueous solvent; the aqueous solvent consists of water and dopamine;
[0031] S2) mixing the rare earth dopant and the emulsion, uniformly dispersing them by ultrasonication, and then heating them for solvent thermal reaction. The obtained solid product is annealed in a mixture of hydrogen and argon to obtain an ultra-dispersed rare earth-doped MoSe2 material.
[0032] In step S1):
[0033] Mix solution A and solution B to obtain an emulsion;
[0034] The A solution is obtained by mixing a selenium source (Se source) and hydrazine hydrate (N2H4·H2O); the B solution is obtained by mixing a molybdenum source (Mo source) and an aqueous solvent; and the aqueous solvent consists of water and dopamine.
[0035] In certain embodiments of the present invention, the selenium source is selected from at least one of selenium powder, selenomethionine and dibenzyl diselenide, preferably selenium powder. The usage ratio of the selenium source to hydrazine hydrate is 70-100 mg: 6-13 mL, such as 79 mg: 10 mL.
[0036] In certain embodiments of the present invention, the molybdenum source is selected from at least one of ammonium molybdate, sodium molybdate, sodium molybdate dihydrate (Na2MoO4·2H2O), ammonium phosphomolybdate, molybdenum trioxide and molybdenum acetate; preferably sodium molybdate. The volume ratio of water to dopamine is 30-40:5-15, such as 35:10. The amount ratio of the molybdenum source to the aqueous solvent is 240-250 mg:35-55 mL, such as 242 mg:45 mL.
[0037] In certain embodiments of the present invention, the mass ratio of the selenium source to the molybdenum source is 70-100:240-250, such as 79:242.
[0038] In step S2):
[0039] The rare earth dopant and the emulsion are mixed, ultrasonically dispersed evenly, and then heated for solvent thermal reaction. The obtained solid product is annealed in a mixture of hydrogen and argon to obtain an ultra-dispersed rare earth-doped MoSe2 material.
[0040] In some embodiments of the present invention, the rare earth dopant is a metal salt containing rare earth ions; preferably, the rare earth ions in the rare earth dopant include Lu 3+ 、Tm 3+ 、Ru 3+ 、Sm 3+ and La 3+ Specifically, the rare earth dopant is a ruthenium salt, such as Ru(NO3)3·2H2O, La(NO3)3·2H2O, Sm(NO3)3·2H2O, Lu(NO3)3·2H2O or Tm(NO3)3·2H2O.
[0041] In certain embodiments of the present invention, in the solution obtained by mixing the rare earth dopant with the emulsion, the concentration of the rare earth dopant is 0.01-0.1 mmol / L, such as 0.05 mmol / L.
[0042] In certain embodiments of the present invention, the temperature of the solvent thermal reaction is 180-220°C, such as 200°C, and the time is 10-14h, such as 12h. The solvent thermal reaction is carried out in an autoclave. After the solvent thermal reaction, the steps include cooling, filtering, washing and drying. The cooling is natural cooling to room temperature. The solid product obtained by filtration is washed. The washing agent used for the washing is deionized water and ethanol. The drying is vacuum drying, and the vacuum drying temperature is 100-140°C, such as 120°C.
[0043] In some embodiments of the present invention, the volume ratio of hydrogen to argon is 3-7:95-105, for example, 5:100.
[0044] In some embodiments of the present invention, the annealing temperature is 550-650° C., such as 600° C., and the annealing time is 1-3 hours, such as 2 hours.
[0045] The present invention also provides an ultra-dispersed rare earth-doped MoSe2 material prepared by the preparation method described above.
[0046] The present invention also provides an application of the ultra-dispersed rare earth-doped MoSe2 material described above as a hydrogen evolution electrocatalyst (catalyst for electrochemical hydrogen evolution reaction (HER)).
[0047] The present invention controls the synthesis of precursors and dopes the MoSe2 material with various rare earth elements, thereby significantly improving the HER activity of the material.
[0048] The preparation process provided by the invention is simple, green and environmentally friendly, cheap, and has low production cost, which is conducive to large-scale market promotion.
[0049] The present invention uses a series of rare earth elements for doping to form a comparison, trying to find the best electrocatalytic activity. It can be seen that the corresponding electrocatalytic activities are significantly improved, proving that our doping is very effective.
[0050] In the present invention, dopamine molecules carrying functional groups show a strong affinity for Mo atoms and can be inserted into the Se-Mo-Se interlayer as a passivator to inhibit its overgrowth. The rare earth cation radius of the rare earth dopant (usually 0.84-1.06 pm) is much larger than the radius of the Mo ion (0.68 pm). When it enters the Se-Mo-Se basal plane, it is easy to distort the lattice of MoSe2 and leave Se vacancy defects in the lattice.
[0051] The ultra-dispersed rare earth-doped MoSe2 material obtained by the present invention has a large specific surface area, which can be 180 to 190 m 2 g -1 , with many active sites, containing 14% to 15% Se vacancy defects, good cycle stability, simple process, low production cost, low environmental pollution, and the activity is greatly improved after doping with a series of rare earth metals.
[0052] The present invention has no particular limitation on the sources of the raw materials used above, and they can be generally commercially available.
[0053] In order to further illustrate the present invention, an ultra-dispersed rare earth-doped MoSe2 material, a preparation method and an application thereof provided by the present invention are described in detail below in combination with embodiments, but it should not be understood as limiting the scope of protection of the present invention.
[0054] Example 1
[0055] The preparation of the chemical formula Ru-MoSe2 includes the following steps:
[0056] (1) Dissolve 79 mg of Se source (selenium powder) in 10 mL of hydrazine hydrate to obtain solution A;
[0057] 242 mg of Mo source (Na2MoO4·2H2O) was dissolved in 45 mL of aqueous solvent (water and dopamine, volume ratio of 35:10) to obtain solution B;
[0058] Mix solution A and solution B to obtain an emulsion;
[0059] (2) Rare earth dopant (Ru(NO3)3·2H2O) was added to the emulsion, and after being uniformly dispersed by ultrasonication, the emulsion was transferred to an autoclave and heated to 200°C for a solvothermal reaction for 12 hours. After the autoclave was naturally cooled to room temperature, the solid product obtained by filtration was washed with deionized water and ethanol, and dried in a vacuum drying furnace at 120°C. The dried material was annealed at 600°C for 2 hours in a mixture of hydrogen and argon (the volume ratio of hydrogen to argon was 5:100) to obtain an ultra-dispersed rare earth doped MoSe2 material (Ru-MoSe2).
[0060] Figure 1 This is a SEM image of the ultra-dispersed rare earth-doped MoSe2 material prepared in Example 1 of the present invention. Figure 1 It can be seen that the ultra-dispersed rare earth-doped MoSe2 material is a 3D nanolayered structure, and the doped rare earth elements are evenly dispersed on the surface of the material.
[0061] Figure 2 TEM image of the ultra-dispersed rare earth-doped MoSe2 material prepared in Example 1 of the present invention. Figure 2 It can be seen that the ultra-dispersed rare earth-doped MoSe2 material has good dispersion.
[0062] Figure 3 This is the XRD pattern of the ultra-dispersed rare earth-doped MoSe2 material prepared in Example 1 of the present invention. Figure 3 It can be seen that doping does not change the corresponding peaks of the raw materials.
[0063] The specific method of electrochemical performance test is: using Chenhua 660e electrochemical workstation, adopting a three-electrode system, the counter electrode is a graphite rod, the reference electrode is a Hg / HgO reference electrode; the electrolyte is a 1 mol / L KOH aqueous solution.
[0064] 5 mg of sample (ultra-dispersed rare earth-doped MoSe2 material) was dissolved in 375 mL of water and 120 μL of ethanol, and then 5 μL of nafion solution was added. After ultrasonication for 1 h, 25 μL was dropped on a 0.025 cm 2 The samples were placed on hydrophilic carbon paper and air-dried. Cyclic voltammetry (scanning potential from -0.8 V to -1.8 V, scan rate 0.2 Vs -1 ) to activate the material, and then perform linear voltammetry (LSV) performance test (scanning potential from -0.8 V to -1.8 V, scan rate of 0.005 Vs -1 ) to obtain the overpotential value and the polarization curve of the catalyst in the electrolyte (KOH aqueous solution). Figure 4 This is an electrochemical activity diagram of the ultra-dispersed rare earth-doped MoSe2 material of Example 1 of the present invention as a hydrogen evolution electrocatalyst.
[0065] from Figure 4 It can be seen that the application of the ultra-dispersed rare earth-doped MoSe2 material of Example 1 in the electrocatalytic HER hydrogen production can significantly improve its overpotential, which is -10A / cm under alkaline conditions. 2 It reaches 214mV, which is significantly improved compared with pure MoSe2 material (397mV).
[0066] Example 2
[0067] The difference from Example 1 is:
[0068] In step (2), the rare earth dopant is replaced by La(NO3)3·2H2O, and the remaining steps are the same as those in Example 1 to obtain an ultra-dispersed rare earth-doped MoSe2 material (La-MoSe2).
[0069] The electrochemical activity of the ultra-dispersed rare earth-doped MoSe2 material as a hydrogen evolution electrocatalyst was studied according to the method of Example 1. The results are as follows: Figure 4 As shown. Figure 4 It can be seen that the overpotential of La-MoSe2 material is -10A / cm under alkaline conditions. 2 It reaches 338mv.
[0070] Example 3
[0071] The difference from Example 1 is:
[0072] In step (2), the rare earth dopant is replaced by Sm(NO3)3·2H2O, and the remaining steps are the same as those in Example 1 to obtain an ultra-dispersed rare earth-doped MoSe2 material (Sm-MoSe2).
[0073] The electrochemical activity of the ultra-dispersed rare earth-doped MoSe2 material as a hydrogen evolution electrocatalyst was studied according to the method of Example 1. The results are as follows: Figure 4 As shown. Figure 4 It can be seen that the overpotential of Sm-MoSe2 material is -10A / cm under alkaline conditions. 2 It reaches 273mv.
[0074] Example 4
[0075] The difference from Example 1 is:
[0076] In step (2), the rare earth dopant is replaced by Lu(NO3)3·2H2O, and the remaining steps are the same as those in Example 1 to obtain an ultra-dispersed rare earth-doped MoSe2 material (Lu-MoSe2).
[0077] The electrochemical activity of the ultra-dispersed rare earth-doped MoSe2 material as a hydrogen evolution electrocatalyst was studied according to the method of Example 1. The results are as follows: Figure 4 As shown. Figure 4 It can be seen that the overpotential of Lu-MoSe2 material is -10A / cm under alkaline conditions. 2 It reaches 233mv.
[0078] Example 5
[0079] The difference from Example 1 is:
[0080] In step (2), the rare earth dopant is replaced by Tm(NO3)3·2H2O, and the remaining steps are the same as those in Example 1 to obtain an ultra-dispersed rare earth-doped MoSe2 material (Tm-MoSe2).
[0081] The electrochemical activity of the ultra-dispersed rare earth-doped MoSe2 material as a hydrogen evolution electrocatalyst was studied according to the method of Example 1. The results are as follows: Figure 4 As shown. Figure 4 It can be seen that the overpotential of Tm-MoSe2 material is -10A / cm under alkaline conditions. 2 For pure MoSe2, after doping with different rare earth elements, its electrocatalytic HER activity has been improved accordingly, among which the effect of ruthenium doping is the best and its stability is also very good.
[0082] The description of the above embodiments is only used to help understand the method of the present invention and its core idea. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing ultra-dispersed rare earth-doped MoSe2 material, comprising the following steps: S1) mixing solution A and solution B to obtain an emulsion; The A solution is obtained by mixing a selenium source and hydrazine hydrate; the B solution is obtained by mixing a molybdenum source and an aqueous solvent; the aqueous solvent consists of water and dopamine; S2) mixing the rare earth dopant and the emulsion, uniformly dispersing them by ultrasonication, and then heating them for solvent thermal reaction. The obtained solid product is annealed in a mixture of hydrogen and argon to obtain an ultra-dispersed rare earth-doped MoSe2 material.
2. The preparation method according to claim 1, characterized in that: In step S1), the selenium source is selected from at least one of selenium powder, selenomethionine and dibenzyl diselenide; The usage ratio of the selenium source and hydrazine hydrate is 70-100 mg: 6-13 mL.
3. The preparation method according to claim 1, characterized in that: In step S1), the molybdenum source is selected from at least one of ammonium molybdate, sodium molybdate, sodium molybdate dihydrate, ammonium phosphomolybdate, molybdenum trioxide and molybdenum acetate; The molybdenum source and the aqueous solvent are used in a ratio of 240-250 mg: 35-55 mL; The volume ratio of water to dopamine is 30-40:5-15.
4. The preparation method according to claim 1, characterized in that: In step S1), the mass ratio of the selenium source to the molybdenum source is 70-100:240-250.
5. The preparation method according to claim 1, characterized in that: In step S2), the rare earth dopant is a metal salt containing rare earth ions; the rare earth ions in the rare earth dopant include Lu 3+ 、Tm 3+ 、Ru 3+ 、Sm 3+ and La 3+ At least one of .
6. The preparation method according to claim 1, characterized in that: In step S2), the rare earth dopant and the emulsion are mixed to obtain a solution in which the concentration of the rare earth dopant is 0.01 to 0.1 mmol / L.
7. The preparation method according to claim 1, characterized in that: In step S2), the temperature of the solvent thermal reaction is 180-220° C. and the time is 10-14 hours.
8. The preparation method according to claim 1, characterized in that: In step S2), the volume ratio of hydrogen to argon is 3-7:95-105; The annealing temperature is 550-650° C. and the annealing time is 1-3 hours.
9. The ultra-dispersed rare earth-doped MoSe2 material obtained by the preparation method according to any one of claims 1 to 8.
10. Use of the ultra-dispersed rare earth-doped MoSe2 material according to claim 9 as a hydrogen evolution electrocatalyst.
Citation Information
Patent Citations
Catalyst as well as preparation method and application thereof
CN117626344A
Monatomic metal-doped few-layer molybdenum disulfide electrocatalytic material, preparing method thereof, and method for electrocatalytic nitrogen fixation