Preparation method of nickel diselenide and zinc selenide / nitrogen-doped porous carbon composite material and material
By preparing nickel diselenide @ zinc selenide/nitrogen doped porous carbon composite material, the problem of performance optimization of the negative electrode material of sodium ion battery is solved, and high-efficiency sodium storage capacity and structural stability are achieved, which is suitable for the industrial production of sodium ion batteries.
Patent Information
- Application Number
- CN202411028198.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-30
AI Technical Summary
The performance optimization of existing sodium ion battery negative electrode materials is difficult, especially the problem of volume expansion of transition metal selenide during charging and discharging, resulting in capacity attenuation, poor rate performance and poor cycle stability.
Using the preparation method of nickel diselenide @ zinc selenide/nitrogen doped porous carbon composite material, nitrogen is formed by preparing alkaline nickel carbonate/zinc nanosheets, nickel/zinc metal organic frame composite material, carbonization treatment and selenization reaction. Doped with porous carbon coated structure to improve the conductivity and structural stability of the material.
It significantly improves the theoretical specific capacity, cycle stability and rate performance of the material, alleviates the volume expansion problem, extends the cycle life of the battery, and reduces production costs.
Smart Images

Figure CN118954442A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of energy storage nanomaterials, and in particular to a preparation method and material of a nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material. Background Art
[0002] With the continuous growth of global energy demand and the rapid development of renewable energy, efficient, reliable and cost-effective energy storage technology has become particularly important. Rechargeable lithium-ion batteries have made great achievements in promoting the efficient conversion and convenient utilization of clean energy. However, with the advent of a large number of lithium-ion products and the crazy expansion of market demand, the limited resources, uneven distribution and rising prices of lithium have restricted the large-scale use of lithium-ion batteries. Among them, sodium-ion batteries, as a potential alternative, have received widespread attention in recent years due to their abundant resources, low cost and environmental friendliness. However, sodium-ion batteries still face many challenges in practical applications, especially the performance optimization of negative electrode materials.
[0003] Studies have shown that transition metal sulfur compounds (TMX, X = O, S, Se) have good sodium storage properties and can react with sodium, so they have a higher theoretical specific capacity. Among them, Se has lower electronegativity and higher electronic conductivity than O and S, which is conducive to the rapid transmission of ions and electrons, and accelerates the diffusion dynamics of sodium ions. However, due to the large radius of sodium ions, the electrode material will undergo a dramatic volume expansion, which makes transition metal selenides have the disadvantages of rapid capacity decay, poor rate performance, and poor cycle stability, which seriously restricts the widespread application of transition metal selenides in sodium ion batteries.
[0004] Therefore, how to provide a simple and efficient method for preparing transition metal selenide negative electrode energy storage materials, while improving the theoretical specific capacity of the material and improving the rate performance and cycle stability, has become a technical problem that needs to be solved urgently. Summary of the invention
[0005] In view of this, in order to overcome the deficiencies of the prior art, the present invention provides a method for preparing a nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material and a material.
[0006] According to one aspect of the present invention, the present invention provides a method for preparing a nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material, the method comprising:
[0007] Step 1: Preparation of basic nickel / zinc carbonate nanosheets
[0008] A basic nickel carbonate / zinc carbonate precursor solution is prepared by using nickel nitrate hexahydrate, zinc nitrate hexahydrate, urea and deionized water according to a ratio;
[0009] placing the prepared basic nickel / zinc carbonate precursor solution in a reaction kettle for hydrothermal reaction, washing and drying the hydrothermal reaction product to obtain basic nickel / zinc carbonate nanosheets;
[0010] Step 2: Preparation of Ni / Zn metal organic framework composites
[0011] A 2-methylimidazole solution is prepared, basic nickel carbonate / zinc nanosheets are placed in the prepared 2-methylimidazole solution and stirred at room temperature, and the stirred product is washed and dried to prepare a nickel / zinc metal organic framework composite material;
[0012] Step 3: Preparation of Ni / Zn@N-doped Carbon Composite Materials
[0013] Carbonizing the nickel / zinc metal organic framework composite material in an inert gas environment to obtain a nickel / zinc@nitrogen doped carbon composite material;
[0014] Step 4: Preparation of nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material
[0015] The nickel / zinc@nitrogen doped carbon composite material and selenium powder are mixed according to a ratio and then ground, and the ground product is subjected to selenization reaction in a protective gas environment to obtain a nickel diselenide@zinc selenide / nitrogen doped porous carbon composite material.
[0016] Preferably, in the preparation method of the nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material of the present invention, in step one, nickel nitrate hexahydrate, zinc nitrate hexahydrate, urea and deionized water are used in a ratio to prepare a basic nickel carbonate / zinc precursor solution, including: when preparing the basic nickel carbonate / zinc precursor solution, 2.5 mmol of nickel nitrate hexahydrate, 2.5 mmol of zinc nitrate hexahydrate, 25 mmol of urea and 50 ml of deionized water are mixed.
[0017] Preferably, in the method for preparing the nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material of the present invention, in step 1, the temperature of the hydrothermal reaction is 105-135° C., and the time of the hydrothermal reaction is 10-12 h.
[0018] Preferably, in the preparation method of the nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material of the present invention, in step one, the hydrothermal reaction product is cleaned and dried to obtain basic nickel carbonate / zinc nanosheets, comprising: sequentially using deionized water and anhydrous ethanol to clean the hydrothermal reaction product cooled to room temperature, and drying the cleaned product at 80°C for 10 hours to obtain basic nickel carbonate / zinc nanosheets.
[0019] Preferably, the preparation method of the nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material of the present invention, in step 2, prepares a 2-methylimidazole solution, places the basic nickel carbonate / zinc nanosheets in the prepared 2-methylimidazole solution, and stirs at room temperature, including: preparing a 2-methylimidazole solution with a concentration of 3-7 mol / L, placing each 40 mg of the basic nickel carbonate / zinc nanosheets in 3 ml of the prepared 2-methylimidazole solution and stirring at room temperature, and the stirring time is 6-24 hours.
[0020] Preferably, in the preparation method of the nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material of the present invention, in step 2, the product after stirring is cleaned and dried to obtain a nickel / zinc metal organic framework composite material, comprising: sequentially cleaning the product after stirring with deionized water and anhydrous ethanol, and drying the cleaned product at 80°C for 10 hours to obtain a nickel / zinc metal organic framework composite material.
[0021] Preferably, in the preparation method of the nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material of the present invention, in step three, the nickel / zinc metal organic framework composite material is carbonized in an inert gas environment, including: placing the nickel / zinc metal organic framework composite material in an argon environment with an argon flow rate of 20 mL / min, heating it to 400-800°C at a heating rate of 2-5°C / min, keeping it warm for 2 hours, and then naturally cooling it to room temperature.
[0022] Preferably, in the preparation method of the nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material of the present invention, in step four, the nickel / zinc@nitrogen-doped carbon composite material and selenium powder are mixed according to a ratio and then ground, including: mixing 1 weight part of the nickel / zinc@nitrogen-doped carbon composite material with 2 weight parts of selenium powder, and grinding the mixed material for 10 minutes.
[0023] Preferably, in the preparation method of the nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material of the present invention, in step four, the ground product is subjected to a selenization reaction in a protective gas environment, including: placing the ground product in an argon environment with an argon flow rate of 20 mL / min, heating it to 400-450°C at a heating rate of 2-5°C / min, keeping it warm for 2 hours, and then naturally cooling it to room temperature.
[0024] According to another aspect of the present invention, the present invention provides a nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material, and the nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material is prepared according to the above method.
[0025] According to another aspect of the present invention, the present invention provides an application of a nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material as a negative electrode material for a sodium ion battery.
[0026] The preparation method and material of the nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material of the present invention have the following beneficial effects:
[0027] 1. By preparing basic nickel / zinc carbonate nanosheets and utilizing their large specific surface area to transform them into uniform nickel / zinc metal organic framework composite materials, the structural stability is enhanced. By introducing nitrogen elements, the conductivity and electrochemical reaction activity of the material are further improved, and more sodium ions can be adsorbed, thereby improving the sodium storage capacity of the material.
[0028] 2. The nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material prepared by the present invention is applied to the negative electrode material of sodium ion batteries, which can increase the theoretical specific capacity of the material and improve its cycle stability and rate performance through a synergistic effect. Secondly, the coating effect of the nitrogen-doped porous carbon can significantly improve the conductivity and structural stability of the material, which is beneficial to the penetration of the electrolyte and the rapid transmission of ions, and can effectively alleviate the volume expansion problem of nickel diselenide and zinc selenide during the charging and discharging process, thereby extending the cycle life of the battery and improving the performance of the battery.
[0029] 3. The preparation method of the nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material of the present invention has the characteristics of strong controllability, green environmental protection, simple process, high efficiency and low cost, and can be applied in the sodium ion battery energy storage device preparation industry, which is conducive to large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0031] Figure 1 This is a FESEM image of the nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material prepared in Example 1 of the present invention;
[0032] Figure 2 This is a FESEM image of the nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material prepared in Example 2 of the present invention;
[0033] Figure 3 This is a FESEM image of the nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material prepared in Example 3 of the present invention;
[0034] Figure 4 This is a FESEM image of the nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material prepared in Example 4 of the present invention;
[0035] Figure 5This is a FESEM image of the nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material prepared in Example 5 of the present invention;
[0036] Figure 6 This is a FESEM image of basic nickel / zinc carbonate nanosheets prepared in Example 4 of the present invention;
[0037] Figure 7 This is a FESEM image of the nickel / zinc metal organic framework composite material prepared in Example 4 of the present invention;
[0038] Figure 8 This is a FESEM image of the nickel / zinc@nitrogen-doped carbon composite material prepared in Example 4 of the present invention;
[0039] Fig. 9 XRD patterns of nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite materials prepared in Examples 1, 2, 3, 4 and 5 of the present invention;
[0040] Fig.10 Electrochemical rate performance diagram of nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite materials prepared in Examples 1, 2, 3, 4 and 5 of the present invention;
[0041] Fig.11 The nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material prepared in Example 4 of the present invention was heated to 50 mA g. -1 The charge and discharge curves of the first five cycles at a current density of . DETAILED DESCRIPTION
[0042] The embodiments of the present invention are described in detail below with reference to the accompanying drawings.
[0043] It should be noted that the following embodiments and features in the embodiments may be combined with each other in the absence of conflict; and, based on the embodiments in the present disclosure, all other embodiments obtained by ordinary technicians in the field without making any creative work are within the scope of protection of the present disclosure.
[0044] It should be noted that various aspects of the embodiments within the scope of the appended claims are described below. It should be apparent that the aspects described herein may be embodied in a wide variety of forms, and any specific structure and / or function described herein is merely illustrative. Based on the present disclosure, it should be understood by those skilled in the art that an aspect described herein may be implemented independently of any other aspect, and two or more of these aspects may be combined in various ways. For example, any number of aspects described herein may be used to implement the device and / or practice the method. In addition, other structures and / or functionalities other than one or more of the aspects described herein may be used to implement this device and / or practice this method.
[0045] Example 1
[0046] Preparation of NiSe@ZnSe / N-doped porous carbon composites:
[0047] Step 1: Preparation of basic nickel / zinc carbonate nanosheets
[0048] A basic nickel carbonate / zinc precursor solution is prepared by using 2.5 mmol nickel nitrate hexahydrate, 2.5 mmol zinc nitrate hexahydrate, 25 mmol urea and 50 ml deionized water according to a ratio, and the prepared basic nickel carbonate / zinc precursor solution is placed in a reactor with a polytetrafluoroethylene liner for hydrothermal reaction at a temperature of 105° C. for 12 hours to obtain a hydrothermal reaction product, and the hydrothermal reaction product cooled to room temperature is washed with deionized water and anhydrous ethanol in turn, and the washed product is dried at 80° C. for 10 hours to obtain basic nickel carbonate / zinc nanosheets;
[0049] Step 2: Preparation of Ni / Zn metal organic framework composites
[0050] A 2-methylimidazole solution with a concentration of 3 mol / L was prepared, 40 mg of basic nickel carbonate / zinc nanosheets were placed in 3 ml of the prepared 2-methylimidazole solution and stirred at room temperature for 24 hours, the stirred product was washed with deionized water and anhydrous ethanol in turn, and the washed product was dried at 80° C. for 10 hours to obtain a nickel / zinc metal organic framework composite material;
[0051] Step 3: Preparation of Ni / Zn@N-doped Carbon Composite Materials
[0052] In an argon environment with an argon flow rate of 20 mL / min, the nickel / zinc metal organic framework composite material was carbonized at 800°C at a heating rate of 5°C / min, and then naturally cooled to room temperature after being kept for 2 hours to obtain a nickel / zinc@nitrogen-doped carbon composite material;
[0053] Step 4: Preparation of nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material
[0054] 1 part by weight of nickel / zinc@nitrogen-doped carbon composite material was mixed with 2 parts by weight of selenium powder, the mixed material was ground for 20 min, the ground product was placed in a porcelain boat in a tubular furnace, and the temperature was increased to 400°C at a heating rate of 5°C / min in an argon environment with an argon flow rate of 20 mL / min, and the temperature was kept at 400°C for 2 h. The product of the selenization reaction was naturally cooled to room temperature to obtain a nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material.
[0055] Example 2
[0056] Preparation of NiSe@ZnSe / N-doped porous carbon composites:
[0057] Step 1: Preparation of basic nickel / zinc carbonate nanosheets
[0058] A basic nickel carbonate / zinc precursor solution is prepared by using 2.5 mmol nickel nitrate hexahydrate, 2.5 mmol zinc nitrate hexahydrate, 25 mmol urea and 50 ml deionized water according to a ratio, and the prepared basic nickel carbonate / zinc precursor solution is placed in a reactor with a polytetrafluoroethylene liner for hydrothermal reaction at a temperature of 120° C. for 11 hours to obtain a hydrothermal reaction product, and the hydrothermal reaction product cooled to room temperature is washed with deionized water and anhydrous ethanol in turn, and the washed product is dried at 80° C. for 10 hours to obtain basic nickel carbonate / zinc nanosheets;
[0059] Step 2: Preparation of Ni / Zn metal organic framework composites
[0060] A 5 mol / L 2-methylimidazole solution was prepared, 40 mg of basic nickel / zinc carbonate nanosheets were placed in 3 ml of the prepared 2-methylimidazole solution and stirred at room temperature for 12 h, the stirred product was washed with deionized water and anhydrous ethanol in turn, and the washed product was dried at 80° C. for 10 h to obtain a nickel / zinc metal organic framework composite material;
[0061] Step 3: Preparation of Ni / Zn@N-doped Carbon Composite Materials
[0062] In an argon environment with an argon flow rate of 20 mL / min, the nickel / zinc metal organic framework composite material was carbonized at 700°C at a heating rate of 4°C / min, and then naturally cooled to room temperature after being kept at this temperature for 2 hours to obtain a nickel / zinc@nitrogen-doped carbon composite material;
[0063] Step 4: Preparation of nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material
[0064] 1 part by weight of nickel / zinc@nitrogen-doped carbon composite material was mixed with 2 parts by weight of selenium powder, the mixed material was ground for 15 min, the ground product was placed in a porcelain boat in a tubular furnace, and the temperature was increased to 430°C at a heating rate of 4°C / min in an argon environment with an argon flow rate of 20 mL / min, and the temperature was kept at 430°C for 2 h. The product of the selenization reaction was naturally cooled to room temperature to obtain a nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material.
[0065] Example 3
[0066] Preparation of NiSe@ZnSe / N-doped porous carbon composites:
[0067] Step 1: Preparation of basic nickel / zinc carbonate nanosheets
[0068] A basic nickel carbonate / zinc precursor solution is prepared by using 2.5 mmol nickel nitrate hexahydrate, 2.5 mmol zinc nitrate hexahydrate, 25 mmol urea and 50 ml deionized water according to a ratio, and the prepared basic nickel carbonate / zinc precursor solution is placed in a reactor with a polytetrafluoroethylene liner for hydrothermal reaction at a temperature of 135° C. for 10 hours to obtain a hydrothermal reaction product, and the hydrothermal reaction product cooled to room temperature is washed with deionized water and anhydrous ethanol in turn, and the washed product is dried at 80° C. for 10 hours to obtain basic nickel carbonate / zinc nanosheets;
[0069] Step 2: Preparation of Ni / Zn metal organic framework composites
[0070] A 7 mol / L 2-methylimidazole solution was prepared, 40 mg of basic nickel carbonate / zinc nanosheets were placed in 3 ml of the prepared 2-methylimidazole solution and stirred at room temperature for 6 h, the stirred product was washed with deionized water and anhydrous ethanol in turn, and the washed product was dried at 80° C. for 10 h to obtain a nickel / zinc metal organic framework composite material;
[0071] Step 3: Preparation of Ni / Zn@N-doped Carbon Composite Materials
[0072] In an argon environment with an argon flow rate of 20 mL / min, the nickel / zinc metal organic framework composite material was carbonized at 600°C at a heating rate of 2°C / min, and then naturally cooled to room temperature after being kept for 2 hours to obtain a nickel / zinc@nitrogen-doped carbon composite material;
[0073] Step 4: Preparation of nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material
[0074] Every 1 weight part of nickel / zinc@nitrogen-doped carbon composite material was mixed with 2 weight parts of selenium powder, the mixed material was ground for 10 min, the ground product was placed in a porcelain boat and set in a tubular furnace, and the temperature was increased to 400°C at a heating rate of 2°C / min in an argon environment with an argon flow rate of 20 mL / min, and the temperature was kept for 2 h. The product of the selenization reaction was naturally cooled to room temperature to obtain a nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material.
[0075] Example 4
[0076] Preparation of NiSe@ZnSe / N-doped porous carbon composites:
[0077] Step 1: Preparation of basic nickel / zinc carbonate nanosheets
[0078] A basic nickel / zinc carbonate precursor solution is prepared by using 2.5 mmol nickel nitrate hexahydrate, 2.5 mmol zinc nitrate hexahydrate, 25 mmol urea and 50 ml deionized water according to a ratio, and the prepared basic nickel / zinc carbonate precursor solution is placed in a reactor with a polytetrafluoroethylene liner for hydrothermal reaction at a temperature of 120° C. for 10 h to obtain a hydrothermal reaction product, and the hydrothermal reaction product cooled to room temperature is washed with deionized water and anhydrous ethanol in turn, and the washed product is dried at 80° C. for 10 h to obtain basic nickel / zinc carbonate nanosheets;
[0079] Step 2: Preparation of Ni / Zn metal organic framework composites
[0080] A 5 mol / L 2-methylimidazole solution was prepared, 40 mg of basic nickel / zinc carbonate nanosheets were placed in 3 ml of the prepared 2-methylimidazole solution and stirred at room temperature for 12 h, the stirred product was washed with deionized water and anhydrous ethanol in turn, and the washed product was dried at 80° C. for 10 h to obtain a nickel / zinc metal organic framework composite material;
[0081] Step 3: Preparation of Ni / Zn@N-doped Carbon Composite Materials
[0082] In an argon environment with an argon flow rate of 20 mL / min, the nickel / zinc metal organic framework composite material was carbonized at 500°C at a heating rate of 2°C / min, and then naturally cooled to room temperature after being kept at this temperature for 2 hours to obtain a nickel / zinc@nitrogen-doped carbon composite material;
[0083] Step 4: Preparation of nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material
[0084] 1 part by weight of nickel / zinc@nitrogen-doped carbon composite material was mixed with 2 parts by weight of selenium powder, and the mixed material was ground for 10 minutes. The ground product was placed in a porcelain boat and set in a tubular furnace. In an argon environment with an argon flow rate of 20 mL / min, the temperature was increased to 450°C at a heating rate of 2°C / min and kept for 2 hours. The product of the selenization reaction was naturally cooled to room temperature to obtain a nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material.
[0085] Example 5
[0086] Preparation of NiSe@ZnSe / N-doped porous carbon composites:
[0087] Step 1: Preparation of basic nickel / zinc carbonate nanosheets
[0088] A basic nickel / zinc carbonate precursor solution is prepared by using 2.5 mmol nickel nitrate hexahydrate, 2.5 mmol zinc nitrate hexahydrate, 25 mmol urea and 50 ml deionized water according to a ratio, and the prepared basic nickel / zinc carbonate precursor solution is placed in a reactor with a polytetrafluoroethylene liner for hydrothermal reaction at a temperature of 120° C. for 10 h to obtain a hydrothermal reaction product, and the hydrothermal reaction product cooled to room temperature is washed with deionized water and anhydrous ethanol in turn, and the washed product is dried at 80° C. for 10 h to obtain basic nickel / zinc carbonate nanosheets;
[0089] Step 2: Preparation of Ni / Zn metal organic framework composites
[0090] A 5 mol / L 2-methylimidazole solution was prepared, 40 mg of basic nickel / zinc carbonate nanosheets were placed in 3 ml of the prepared 2-methylimidazole solution and stirred at room temperature for 12 h, the stirred product was washed with deionized water and anhydrous ethanol in turn, and the washed product was dried at 80° C. for 10 h to obtain a nickel / zinc metal organic framework composite material;
[0091] Step 3: Preparation of Ni / Zn@N-doped Carbon Composite Materials
[0092] In an argon environment with an argon flow rate of 20 mL / min, the nickel / zinc metal organic framework composite material was carbonized at 400°C at a heating rate of 2°C / min, and then naturally cooled to room temperature after being kept warm for 2 hours to obtain a nickel / zinc@nitrogen-doped carbon composite material;
[0093] Step 4: Preparation of nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material
[0094] 1 part by weight of nickel / zinc@nitrogen-doped carbon composite material was mixed with 2 parts by weight of selenium powder, and the mixed material was ground for 10 minutes. The ground product was placed in a porcelain boat and set in a tubular furnace. In an argon environment with an argon flow rate of 20 mL / min, the temperature was increased to 450°C at a heating rate of 2°C / min and kept for 2 hours. The product of the selenization reaction was naturally cooled to room temperature to obtain a nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material.
[0095] Example 6
[0096] A thermal field emission scanning electron microscope (FESEM) of model SIGMA 500 produced by Zeiss of Germany was used to observe the microscopic morphology of the nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite materials prepared in Examples 1, 2, 3, 4 and 5 and the basic nickel carbonate / zinc nanosheets, nickel / zinc metal organic framework composite materials and nickel / zinc@nitrogen-doped carbon composite materials prepared in Example 4; the test process and test parameters include: the materials prepared in each example were made into powder material samples, the samples were pasted on the sample table with conductive glue and observed by the instrument, and the acceleration voltage was 5 kV.
[0097] The microstructure of the nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material prepared in Example 1 is shown in Figure 1 , the magnification is 100,000 times; the microscopic morphology of the nickel diselenide @ zinc selenide / nitrogen-doped porous carbon composite material prepared in Example 2 is shown in Figure 2 , the magnification is 100,000 times; the microscopic morphology of the nickel diselenide @ zinc selenide / nitrogen-doped porous carbon composite material prepared in Example 3 is shown in Figure 3 , the magnification is 100,000 times; the microscopic morphology of the nickel diselenide @ zinc selenide / nitrogen-doped porous carbon composite material prepared in Example 4 is shown in Figure 4 , the magnification is 100,000 times; the microscopic morphology of the nickel diselenide @ zinc selenide / nitrogen-doped porous carbon composite material prepared in Example 5 is shown in Figure 5 , the magnification is 100,000 times; the microscopic morphology of the basic nickel carbonate / zinc nanosheet prepared in Example 4 is shown in Figure 6 , the magnification is 100,000 times; the microscopic morphology of the nickel / zinc metal organic framework composite material prepared in Example 4 is shown in Figure 7 , the magnification is 100,000 times; the microscopic morphology of the nickel / zinc@nitrogen-doped carbon composite material prepared in Example 4 is shown in Figure 8 , the magnification is 100,000 times.
[0098] Figure 1 This is a FESEM image of the nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material prepared in Example 1 of the present invention. Figure 1 As shown, the nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material is composed of nickel diselenide and zinc selenide nanoparticles and nitrogen-doped porous carbon. After carbonization treatment and selenization reaction, the surface is relatively rough and has a larger specific surface area, which increases the active sites, is beneficial to the adsorption of sodium ions, and helps to improve the capacity of sodium ion batteries.
[0099] Figure 2 This is a FESEM image of the nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material prepared in Example 2 of the present invention. Figure 2As shown, by adjusting the concentration of 2-methylimidazole solution, the surface of the nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material after carbonization and selenization is made rougher and has a larger specific surface area. When the material is used as the negative electrode material of sodium ion battery, it is beneficial to embed more sodium ions and improve the capacity of the sodium ion battery.
[0100] Figure 3 This is a FESEM image of the nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material prepared in Example 3 of the present invention. Figure 3 As shown, by regulating the hydrothermal temperature and time, the distribution of the nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material after carbonization and selenization is made more uniform, and the number of nickel diselenide and zinc selenide nanoparticles increases. When the material is used as the negative electrode material of a sodium ion battery, it is beneficial to the rapid embedding and extraction of sodium ions, which is beneficial to improving the first coulombic efficiency of the sodium ion battery.
[0101] Figure 4 This is a FESEM image of the nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material prepared in Example 4 of the present invention. Figure 4 As shown, a large number of nickel diselenide and zinc selenide nanoparticles are attached to the carbon skeleton. When the material is used in the negative electrode material of sodium ion battery, the presence of the carbon skeleton is beneficial to alleviate the volume expansion caused by the electrochemical charge and discharge process. The heterogeneous structure formed by nickel diselenide and zinc selenide helps to improve the specific capacity of the electrode material.
[0102] Figure 5 This is a FESEM image of the nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material prepared in Example 5 of the present invention. Figure 5 As shown, by regulating the temperature of the carbonization treatment, the original dodecahedral structure is made more obvious, so that the nickel diselenide and zinc selenide nanoparticles formed by the subsequent selenization reaction are more evenly distributed. When the material is applied to the negative electrode material of the sodium ion battery, it is beneficial to the embedding and extraction of sodium ions, which is beneficial to improving the structural stability of the sodium ion battery during the electrochemical reaction process.
[0103] Figure 6 This is a FESEM image of the basic nickel carbonate / zinc nanosheet prepared in Example 4 of the present invention, as shown Figure 6 As shown, the basic nickel / zinc carbonate nanosheets are uniform in size and have no agglomeration phenomenon, which is conducive to the subsequent process of preparing nickel / zinc metal organic framework composite materials with uniform size.
[0104] Figure 7 This is a FESEM image of the nickel / zinc metal organic framework composite material prepared in Example 4 of the present invention, as shown in Figure 7As shown, the nickel / zinc metal organic framework composite material presents a regular dodecahedral structure, and clustered nanoparticles are attached to the surface. The particle size distribution is relatively uniform, which provides a stable structure for subsequent processes. When the material is used in the negative electrode material of sodium ion batteries, it is beneficial to enhance the structural stability during the electrochemical reaction process.
[0105] Figure 8 This is a FESEM image of the nickel / zinc@nitrogen-doped carbon composite material prepared in Example 4 of the present invention, as shown in Figure 8 As shown, after high-temperature carbonization, the original dodecahedral structure shrinks to form a stable carbon skeleton, which enhances the structural stability of the material, and nickel / zinc nanoparticles are attached to the surface, further enhancing the conductivity of the material.
[0106] Example 7
[0107] The phase composition of the nickel diselenide @ zinc selenide / nitrogen-doped porous carbon composite materials prepared in Example 1, Example 2, Example 3, Example 4 and Example 5 was analyzed by an X-ray diffractometer (XRD) of model XRD-6000 (3KW) produced by Shimadzu Corporation of Japan; the test process and test parameter settings include: placing the nickel diselenide @ zinc selenide / nitrogen-doped porous carbon composite materials prepared in each embodiment into a groove (2.0 * 2.0 cm) of a glass slide, preferably to fill the groove, and then placing it in an X-ray diffractometer, the ray source is a Cu target Kα ray (λ = 0.15418 nm), the scanning range is 10-80°, the scanning rate is 4° / min, the tube voltage is 40 kV, the tube current is 30 mA, and the test results are shown in Fig. 9 .
[0108] Fig. 9 The XRD patterns of the nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite materials prepared in Examples 1, 2, 3, 4 and 5 of the present invention are as follows: Fig. 9 As shown, the XRD patterns of the nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite materials prepared in Example 1, Example 2, Example 3, Example 4 and Example 5 correspond to the standard PDF cards NiSe2-JCPDS#88-1711 and ZnSe-JCPDS#88-2345, indicating that the materials prepared in Example 1, Example 2, Example 3, Example 4 and Example 5 contain nickel diselenide and zinc selenide.
[0109] Example 8
[0110] The nickel diselenide @ zinc selenide / nitrogen-doped porous carbon composite materials prepared in Example 1, Example 2, Example 3, Example 4 and Example 5 were mixed with a conductive agent Super P and polyvinylidene fluoride in a mass ratio of 8:1:1, respectively, and stirred evenly to obtain a mixed product; then N-methylpyrrolidone was added to the mixed product as a solvent, stirred evenly, and a viscous and suitable slurry was obtained; finally, the slurry was coated on a copper foil with a thickness of 9 μm using a SZQ four-sided preparation device (thickness of 150 μm) produced by Kexin Testing Machine Factory, Jinghai District, Tianjin, and the coated copper foil was vacuum dried at 80°C for 12 hours to obtain an electrode sheet made of the nickel diselenide @ zinc selenide / nitrogen-doped porous carbon composite materials prepared in Example 1, Example 2, Example 3, Example 4 and Example 5.
[0111] The nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite electrode sheets prepared in Example 1, Example 2, Example 3, Example 4 and Example 5 were cut using a tablet press model SZ-50-14 produced by Shenzhen Kejing Material Technology Co., Ltd. The test process and test parameters include: the materials prepared in each example were cut into round sheets with a diameter of 12 mm as electrode materials for standby use, and CR2025 battery shells, 1M NaCF3SO3 in DIGLYME (100%) electrolyte, glass fiber diaphragm and metal sodium sheet are put into a glove box with a water and oxygen content of less than 0.1ppm, the electrode material is placed in the center of the positive electrode shell, two drops of electrolyte are added to fully infiltrate the electrode material, and then the glass fiber diaphragm is covered on the electrode plate with tweezers, and then the metal sodium sheet, gasket, shrapnel and negative electrode shell are placed in sequence, and finally the battery is sealed with a battery sealing machine model PX-HS-20 produced by Shenzhen Kejing Material Technology Co., Ltd. to obtain a sodium ion battery composed of nickel diselenide @ zinc selenide / nitrogen-doped porous carbon composite materials prepared in Example 1, Example 2, Example 3, Example 4 and Example 5 as the negative electrode material.
[0112] The sodium ion battery assembled from the nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite materials prepared in Examples 1, 2, 3, 4 and 5 was electrochemically tested using a Blue Electric battery test system model CT3002A produced by Wuhan Blue Electric Electronics Co., Ltd. The test process and test parameters include: taking the current density as 0.05Ag, -1 , 0.1Ag -1 , 0.2A g -1 , 0.5Ag -1 , 1.0Ag -1 , 2.0Ag -1 , 5.0Ag -1 and 10.0Ag -1The electrochemical performance of each embodiment is reflected by constant current charge and discharge test.
[0113] Fig.10 The electrochemical rate performance diagram of the nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material prepared in Example 1, Example 2, Example 3, Example 4 and Example 5 of the present invention is as follows: Fig.10 As shown, the nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite materials prepared in Example 1, Example 2, Example 3, Example 4 and Example 5 have good sodium storage performance, and the charge and discharge capacity overlap is high under different current densities, and its efficiency is maintained at about 100%.
[0114] Fig.11 The sodium ion battery assembled with the nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material prepared in Example 4 of the present invention is 50 mAg -1 The first five cycles of charge and discharge curves under current density, of which the first cycle charge capacity is 576.80mAh g -1 , the discharge capacity is 588.43 mAh g -1 , the first-round efficiency is as high as 98.02%.
[0115] The sodium ion battery assembled with the nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material prepared in Examples 1 to 5 was -1 The first cycle charge and discharge capacity and first coulombic efficiency of the charge and discharge test under the current density are shown in Table 1.
[0116] Table 1
[0117]
[0118] It can be seen from Table 1 that the nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite materials prepared in Examples 1-5 of the present invention have excellent electrochemical properties when used as negative electrode materials for sodium ion batteries. Among them, the negative electrode material prepared in Example 4 has excellent electrochemical performance at 50 mAg -1 The first charge and discharge specific capacity of the charge and discharge test under the current density is 576.80 / 588.43mAh g -1 The first coulombic efficiency is as high as 98.02%. The other embodiments have higher charge and discharge specific capacities, and the first coulombic efficiency is above 95%.
[0119] The preparation method and material of the nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material of the present invention have the following beneficial effects:
[0120] 1. By preparing basic nickel / zinc carbonate nanosheets and utilizing their large specific surface area to transform them into uniform nickel / zinc metal organic framework composite materials, the structural stability is enhanced. By introducing nitrogen elements, the conductivity and electrochemical reaction activity of the material are further improved, and more sodium ions can be adsorbed, thereby improving the sodium storage capacity of the material.
[0121] 2. The nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material prepared by the present invention is applied to the negative electrode material of sodium ion batteries, which can increase the theoretical specific capacity of the material and improve its cycle stability and rate performance through a synergistic effect. Secondly, the coating effect of the nitrogen-doped porous carbon can significantly improve the conductivity and structural stability of the material, which is beneficial to the penetration of the electrolyte and the rapid transmission of ions, and can effectively alleviate the volume expansion problem of nickel diselenide and zinc selenide during the charging and discharging process, thereby extending the cycle life of the battery and improving the performance of the battery.
[0122] 3. The preparation method of the nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material of the present invention has the characteristics of strong controllability, green environmental protection, simple process, high efficiency and low cost, and can be applied in the sodium ion battery energy storage device preparation industry, which is conducive to large-scale industrial production.
[0123] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the protection scope of the claims.
Claims
1. A method for preparing a nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material, characterized in that: The method comprises: Step 1: Preparation of basic nickel / zinc carbonate nanosheets A basic nickel carbonate / zinc carbonate precursor solution is prepared by using nickel nitrate hexahydrate, zinc nitrate hexahydrate, urea and deionized water according to a ratio; placing the prepared basic nickel / zinc carbonate precursor solution in a reaction kettle for hydrothermal reaction, washing and drying the hydrothermal reaction product to obtain basic nickel / zinc carbonate nanosheets; Step 2: Preparation of Ni / Zn metal organic framework composites A 2-methylimidazole solution is prepared, basic nickel carbonate / zinc nanosheets are placed in the prepared 2-methylimidazole solution, stirred at room temperature, and the stirred product is washed and dried to prepare a nickel / zinc metal organic framework composite material; Step 3: Preparation of Ni / Zn@N-doped Carbon Composite Materials The nickel / zinc metal organic framework composite material is carbonized in an inert gas environment to obtain a nickel / zinc@nitrogen doped carbon composite material; Step 4: Preparation of nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material The nickel / zinc@nitrogen doped carbon composite material and selenium powder are mixed according to a ratio and then ground, and the ground product is subjected to selenization reaction in a protective gas environment to obtain a nickel diselenide@zinc selenide / nitrogen doped porous carbon composite material.
2. The method for preparing the nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material according to claim 1, characterized in that: In step 1, nickel nitrate hexahydrate, zinc nitrate hexahydrate, urea and deionized water are used to prepare a basic nickel carbonate / zinc precursor solution according to a ratio, including: when preparing the basic nickel carbonate / zinc precursor solution, 2.5mmol nickel nitrate hexahydrate, 2.5mmol zinc nitrate hexahydrate, 25mmol urea and 50ml deionized water are mixed.
3. The method for preparing the nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material according to claim 1, characterized in that: In step 1, the temperature of the hydrothermal reaction is 105-135° C., and the time of the hydrothermal reaction is 10-12 h.
4. The method for preparing the nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material according to claim 1, characterized in that: In step one, the hydrothermal reaction product is cleaned and dried to obtain basic nickel carbonate / zinc nanosheets, including: using deionized water and anhydrous ethanol to clean the hydrothermal reaction product cooled to room temperature in sequence, and drying the cleaned product at 80° C. for 10 hours to obtain basic nickel carbonate / zinc nanosheets.
5. The method for preparing the nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material according to claim 1, characterized in that: In step 2, a 2-methylimidazole solution is prepared, and the basic nickel carbonate / zinc nanosheets are placed in the prepared 2-methylimidazole solution and stirred at room temperature, including: preparing a 2-methylimidazole solution with a concentration of 3-7 mol / L, placing 40 mg of the basic nickel carbonate / zinc nanosheets in 3 ml of the prepared 2-methylimidazole solution and stirring at room temperature, and the stirring time at room temperature is 6-24 hours.
6. The method for preparing the nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material according to claim 1, characterized in that: In step 2, the stirred product is washed and dried to obtain a nickel / zinc metal organic framework composite material, including: washing the stirred product with deionized water and anhydrous ethanol in sequence, and drying the washed product at 80° C. for 10 hours to obtain a nickel / zinc metal organic framework composite material.
7. The method for preparing the nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material according to claim 1, characterized in that: In step three, the nickel / zinc metal organic framework composite material is carbonized in an inert gas environment, including: placing the nickel / zinc metal organic framework composite material in an argon environment with an argon flow rate of 20 mL / min, heating it to 400-800°C at a heating rate of 2-5°C / min, keeping it warm for 2 hours, and then naturally cooling it to room temperature.
8. The method for preparing the nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material according to claim 1, characterized in that: In step 4, the nickel / zinc@nitrogen-doped carbon composite material and selenium powder are mixed according to a ratio and then ground, including: mixing 1 weight part of the nickel / zinc@nitrogen-doped carbon composite material with 2 weight parts of selenium powder, and grinding the mixed material for 10 minutes.
9. The method for preparing the nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material according to claim 1, characterized in that: In step 4, the ground product is subjected to selenization reaction in a protective gas environment, including: placing the ground product in an argon environment with an argon flow rate of 20 mL / min, heating to 400-450°C at a heating rate of 2-5°C / min, keeping warm for 2 hours, and then naturally cooling to room temperature.
10. A nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material, characterized in that: The nickel diselenide@zinc selenide / nitrogen-doped porous carbon composite material is prepared according to any one of claims 1 to 9.
Citation Information
Patent Citations
Cobalt diselenide@porous nitrogen-doped carbon nano composite material, potassium ion battery and preparation method thereof
CN113410440A
Azole metal organic framework material as well as preparation method and application thereof
CN118165280A
Preparation method for metal organic framework material
WO2023236139A1
Cited By
Nitrogen-doped carbon composite cobalt-nickel diselenide nanocube material and preparation method and application thereof in battery
CN120097318A