Graphene stripping agent, graphene aqueous dispersion, graphene concrete and preparation method thereof
Graphene release agent prepared by phenol compounds and benzyl glycidyl ether solves the problem of poor dispersion of graphene in cement-based concrete, and a stable and regular graphene aqueous dispersion liquid is prepared, which significantly improves the mechanical properties of the concrete and durability, achieving uniform dispersion and efficient peeling of graphene in cement-based concrete.
Patent Information
- Application Number
- CN202411086083.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-15
AI Technical Summary
Graphene has poor dispersion in cement-based concrete, resulting in limited improvement in its performance. The peeling effect of existing surfactants is poor, which affects the strength and durability of concrete.
The graphene release agent prepared by epoxy ring opening and substitution reaction using phenol compounds and benzyl glycidyl ether to prepare a graphene aqueous dispersion with few defects and regular structures through mechanical peeling method to ensure that it is in cement-based concrete. Evenly dispersed.
The strength and durability of graphene concrete are improved, the mechanical properties of the concrete are enhanced, and the cost is low. The π-π interaction between graphene release agent and graphene prevents agglomeration and maintains the stability of the dispersion.
Smart Images

Figure CN118954494A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of graphene preparation, and specifically relates to a graphene exfoliator and a graphene aqueous dispersion prepared by using the graphene exfoliator, and also relates to graphene concrete containing the graphene aqueous dispersion and a preparation method thereof. Background Art
[0002] Cement concrete refers to an engineering composite material made by mixing cement as a gel material, sand and stone as aggregates, and water (which may contain admixtures and additives) in a certain proportion, through mixing, molding, curing and other processes. It has the characteristics of abundant raw materials, low price, simple production process, high compressive strength, good durability, and a wide range of strength grades. However, cement concrete has the disadvantages of being relatively brittle, low in tensile strength and easy to erode, resulting in poor durability during use and high maintenance costs.
[0003] In order to improve the performance of cement concrete materials, nanomaterials (such as nano-silicon dioxide, nano-titanium dioxide, nano-clay, graphene, carbon nanofibers or carbon nanotubes, etc.) are usually added to concrete materials to give cement concrete materials excellent mechanical properties, durability and multifunctionality. Among them, graphene, a two-dimensional carbon-based material mechanically exfoliated from graphite, has excellent tensile strength (130GPa), Young's modulus (1.1TPa), and large specific surface area (2630m 2 / g) and extremely high thermal conductivity (5000W·m -1 ·K -1 ) and electron migration properties, incorporating graphene into cement concrete materials can greatly improve the comprehensive engineering properties of cement concrete composites, thereby developing high-performance and sustainable building materials.
[0004] However, since graphene itself is neither oleophilic nor hydrophilic, and there is a large van der Waals force between graphene layers, it is prone to sedimentation, agglomeration and other problems, making its dispersibility in cement-based concrete poor, resulting in its performance improvement on concrete being very limited. At present, by preparing a stably dispersed graphene dispersion, improving its dispersibility in cement-based powder is one of the effective ways to improve concrete performance. For example, the Chinese patent application with publication number CN109467364A discloses a graphene concrete, which is prepared by a graphite flake with a surfactant through a high shear liquid phase exfoliation method to obtain a stably dispersed graphene dispersion, and the dispersion can be evenly dispersed in cement-based powder, thereby improving the strength, impermeability and durability of the concrete, and having excellent mechanical properties and thermal stability. However, the surfactant sodium cholate used therein has a general exfoliation effect on graphite, which makes the improvement effect on the performance of graphene concrete poor. Summary of the invention
[0005] In view of this, the primary purpose of the present invention is to provide a graphene exfoliator. The graphene aqueous dispersion prepared by the graphene exfoliator in the present invention has the advantages of few defects, regular structure and few layers, so that the graphene aqueous dispersion is very suitable for the preparation of graphene concrete. It can be evenly dispersed in the cement-based concrete system, supplement the strength of the concrete, reduce the pores, improve the strength and durability of the graphene concrete, and has the advantage of low cost.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] The present invention firstly provides a graphene exfoliating agent, which is prepared by epoxy ring-opening and substitution reaction of a phenolic compound and benzyl glycidyl ether.
[0008] In a further embodiment, the phenolic compound is one of hydroquinone, catechol, resveratrol and phloroglucinol.
[0009] In a further embodiment, the molar ratio of the hydroxyl group in the phenolic compound to the epoxy group in the benzyl glycidyl ether is 1:(1.1-1.5).
[0010] In a further embodiment, the molar ratio of the hydroxyl group in the phenolic compound to the epoxy group in the benzyl glycidyl ether is 1:1.2.
[0011] In a further embodiment, the preparation of the graphene exfoliator comprises the following steps:
[0012] adding phenolic compounds and benzyl glycidyl ether into an organic solvent to fully dissolve them to form a uniform mixed solution;
[0013] An alkaline catalyst is added to the mixed solution, reacted at a constant temperature of 60 to 90° C. for 6 to 10 hours, and then dried to obtain a graphene exfoliating agent.
[0014] In a further embodiment, the organic solvent is one or a mixture of two or more of dimethyl sulfoxide, acetone, N,N-dimethylformamide, and N-methylpyrrolidone.
[0015] In a further embodiment, the alkaline catalyst is sodium hydroxide or potassium hydroxide.
[0016] In a further embodiment, the amount of the alkaline catalyst added is 1%-2% of the total mass of the mixed solution.
[0017] The present invention further provides a method for preparing a graphene aqueous dispersion, comprising the following steps:
[0018] After the graphite powder is fully mixed with the graphene exfoliating agent and deionized water as described above, the graphene aqueous dispersion is obtained by mechanical exfoliation.
[0019] In a further embodiment, the mass ratio of the graphite powder to the graphene exfoliator is 1:(0.05-0.2).
[0020] In a further embodiment, the mechanical stripping is performed in a sand mill, the rotation speed of the sand mill is 3000-6000 rpm, and the stripping time is 2-10 hours.
[0021] In a further embodiment, the concentration of the graphene aqueous dispersion is 0.01 g / mL-0.1 g / mL.
[0022] The present invention further provides the use of a graphene aqueous dispersion in the preparation of graphene concrete, wherein the graphene aqueous dispersion is prepared by the preparation method as described above.
[0023] The present invention further provides a graphene concrete, which contains the graphene aqueous dispersion prepared by the preparation method described above.
[0024] A further solution is that, calculated by weight, it is prepared from 30-40 parts of cement, 2-5 parts of graphene aqueous dispersion, 15-20 parts of silica fume, 5-10 parts of fly ash, 6-15 parts of water reducer, 50-75 parts of natural river sand and 5-15 parts of water.
[0025] Beneficial effects of the present invention:
[0026] The graphene exfoliator in the present invention is prepared from a phenolic compound and benzyl glycidyl ether, and contains a plurality of benzene ring structures in its structure. Under the action of the graphene exfoliator, graphite powder is mechanically exfoliated to obtain a few-layer graphene with few defects and regular structure, and the yield is high. In addition, the addition amount of the graphene exfoliator is small, and the effect on the performance of the graphene is small. In addition, the graphene exfoliator in the present invention only generates a force effect on the graphene, and does not change the structure of the graphene itself.
[0027] The graphene exfoliator in the present invention has a large number of benzene ring structures, and there is a strong π-π interaction between graphene and the graphene exfoliator, thereby preventing the agglomeration of graphene sheets, so that the obtained graphene aqueous dispersion can remain stably dispersed without sedimentation after being placed for a long time, and has excellent stability and dispersibility.
[0028] Graphene has the characteristics of high mechanical strength, high specific surface area, etc., and can increase and fill cracks in the concrete microstructure, thereby improving the mechanical properties of concrete. The graphene aqueous dispersion obtained in the present invention is easy to disperse in the cement matrix, the graphene sheet is thin and the structure is regular, and the graphene plane can act as a nano nucleation point, providing a more compact and uniform microstructure. When it is added to cement-based concrete, the graphene can form a strong network structure in the cement matrix, effectively disperse external forces, reduce the formation and expansion of cracks, and improve the mechanical properties of graphene concrete, which has broad application prospects and excellent economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is a scanning electron microscope (SEM) image of graphene obtained by mechanical exfoliation in Example 1.
[0030] Figure 2 This is an optical photograph of the graphene aqueous dispersion obtained by mechanical exfoliation in Example 1 after being allowed to stand at 25° C. for 90 days. DETAILED DESCRIPTION
[0031] Embodiments of the present invention are described in detail below. The embodiments described below are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention.
[0032] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
[0033] A first aspect of the present invention provides a graphene exfoliator, which is prepared by epoxy ring-opening and substitution reaction of a phenolic compound and benzyl glycidyl ether.
[0034] The phenolic compounds described herein refer to organic compounds containing a benzene ring in the molecular structure and having 2 to 5 hydroxyl groups directly connected to the benzene ring. Specific examples include one of hydroquinone, catechol, resveratrol, and phloroglucinol, but are not limited thereto.
[0035] The structural formula of benzyl glycidyl ether in this article is as follows:
[0036]
[0037] Its structure contains epoxy groups, which can undergo a ring-opening reaction under alkaline conditions and then undergo a substitution reaction with phenolic compounds.
[0038] The obtained graphene exfoliator contains a large number of benzene ring structures, which can form a strong π-π conjugation with the graphene surface. With the help of mechanical exfoliation, it is gradually intercalated into the graphite, destroying the van der Waals force between the layers, thereby exfoliating the graphite to obtain graphene. The obtained graphene has the advantages of fewer defects, regular structure, fewer layers, and high yield.
[0039] In the present invention, the ratio of the phenolic compound and benzyl glycidyl ether can be determined or adjusted by methods known in the art. In some specific implementation cases of the present invention, the molar ratio of the hydroxyl group in the phenolic compound to the epoxy group in the benzyl glycidyl ether is 1:(1.1-1.5), for example, it can be 1:1.1, 1:1.2, 1:1.3, 1:1.4 or 1:1.5, preferably 1:1.2.
[0040] In the present invention, the preparation of the graphene exfoliator comprises the following steps:
[0041] adding phenolic compounds and benzyl glycidyl ether into an organic solvent to fully dissolve them to form a uniform mixed solution;
[0042] An alkaline catalyst is added to the mixed solution, reacted at a constant temperature of 60 to 90° C. for 6 to 10 hours, and then dried to obtain a graphene exfoliating agent.
[0043] The organic solvent is a good solvent for phenolic compounds and benzyl glycidyl ether, preferably an organic solvent that is easily removed by subsequent drying. Specific examples include one or a mixture of two or more of dimethyl sulfoxide, acetone, N,N-dimethylformamide, and N-methylpyrrolidone, but are not limited thereto.
[0044] The alkaline catalyst described herein is used to adjust the reaction system to be alkaline, so as to catalyze the ring-opening reaction of the epoxy group in benzyl glycidyl ether, and is preferably an alkali metal hydroxide, such as sodium hydroxide or potassium hydroxide. The specific amount thereof can be adjusted according to the materials used in the reaction, and is preferably 1%-2% of the total mass of the mixed solution.
[0045] A second aspect of the present invention provides a method for preparing a graphene aqueous dispersion, comprising the following steps:
[0046] After the graphite powder is fully and evenly mixed with the graphene exfoliating agent of the first aspect of the present invention and deionized water, it is mechanically exfoliated to obtain a graphene aqueous dispersion.
[0047] It is understood that the graphite powder used in this article is not particularly limited, and conventional or well-known graphite types in the art are suitable for the present invention. Specific examples include but are not limited to expanded graphite, expandable graphite, natural flake graphite, and artificial graphite. The specific size can be selected according to actual needs. In some typical embodiments of the present invention, the graphite powder uses 325 mesh natural flake graphite with a particle size of 45 μm.
[0048] Furthermore, during the stripping process, the specific ratio can be adjusted according to the amount of graphite powder, etc. In some specific embodiments of the present invention, the mass ratio of the graphite powder to the graphene stripping agent is 1:(0.05-0.2), for example, it can be 1:0.05, 1:0.1, 1:0.15 or 1:0.2. The amount of deionized water is mixed according to the amount of 2-10 mL of water per 1 g of graphite powder.
[0049] Further, the mechanical exfoliation described herein can be performed using equipment or methods known in the art. In some specific implementation cases of the present invention, the mechanical exfoliation is performed in a sand mill. In the sand mill environment, a strong shearing effect is generated by the collision between the zirconium beads and the graphite powder, thereby exfoliating the graphite powder. Further, the specific sand milling parameters can be adjusted according to actual needs. In some typical embodiments of the present invention, the speed of the sand mill is 3000-6000rpm, and the exfoliation time is 2-10h. Among them, the speed of the sand mill can be, for example, 3000rpm, 3500rpm, 4000rpm, 4500rpm, 5000rpm, 5500rpm or 6000rpm, and the exfoliation time can be, for example, 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h or 10h.
[0050] In the present invention, the concentration of the graphene aqueous dispersion obtained after the final centrifugation is 0.01 g / mL to 0.1 g / mL.
[0051] In the graphene aqueous dispersion of the present invention, the strong π-π interaction between graphene and the graphene exfoliator prevents the agglomeration of graphene sheets, so that the obtained graphene aqueous dispersion can remain stably dispersed without sedimentation after being placed for a long time, and has excellent stability and dispersibility.
[0052] The third aspect of the present invention provides the use of the graphene aqueous dispersion prepared by the preparation method described in the second aspect of the present invention in the preparation of graphene concrete. Adding the graphene aqueous dispersion to cement-based concrete can significantly improve the mechanical properties of the graphene concrete.
[0053] The fourth aspect of the present invention provides a graphene concrete, which contains the graphene aqueous dispersion prepared by the preparation method of the second aspect of the present invention. It is understandable that the graphene concrete also contains other necessary components and additives in concrete, which can be selected or added as needed.
[0054] In some specific embodiments of the present invention, the graphene concrete is prepared from 30-40 parts of cement, 2-5 parts of graphene aqueous dispersion, 15-20 parts of silica fume, 5-10 parts of fly ash, 6-15 parts of water reducer, 50-75 parts of natural river sand and 5-15 parts of water, measured by mass.
[0055] Among them, cement, silica fume, fly ash, water reducing agent and natural river sand can all be of types known in the art, and specific parameters can be selected according to needs.
[0056] In some specific embodiments of the present invention, the cement used is ordinary silicate cement. The silica fume parameters used are: more than 80% of the fineness is less than 1 μm, the average particle size is 0.1-0.3 μm, and the specific surface area is 20-26 m 2 / g. The specific surface area of fly ash used is greater than 500m 2 / kg, particle size is 10-200μm, density is 2.5-2.9g / cm 3 The maximum particle size of natural river sand used is 8mm, the fineness modulus is 2.5-3.5, and the bulk density is 1600-1700kg·m -3 The water reducer used is polycarboxylic acid high-efficiency water reducer.
[0057] The preparation of graphene concrete in the present invention comprises the following steps:
[0058] After adding a water reducing agent into water and stirring evenly, adding a graphene aqueous dispersion thereto to obtain a dispersion;
[0059] Put cement, fly ash, silica fume and river sand into a blender and mix them evenly, then add the aforementioned dispersion into the blender in 2-3 portions while stirring to obtain a mixture;
[0060] The mixture is placed in a mold, lightly vibrated until dense, and graphene concrete is obtained after curing.
[0061] In the present invention, the curing conditions are specifically curing for 28 days at a temperature of 24±3°C and a relative humidity of 95±5%.
[0062] After testing, the graphene concrete in the present invention has excellent mechanical properties, with a 28d compressive strength of up to 114.7MPa, a 28d flexural strength of up to 17.4MPa, and a slump as low as 162mm.
[0063] The present invention is described below by means of specific examples. It should be noted that the following specific examples are only for illustrative purposes and do not limit the scope of the present invention in any way. In addition, unless otherwise specified, methods without specific conditions or steps are conventional methods, and the reagents and materials used can be obtained from commercial channels.
[0064] Example 1 Preparation of graphene exfoliating agent and graphene aqueous dispersion
[0065] 1. Preparation of graphene exfoliating agent
[0066] Add 5.5 g of hydroquinone and 19.7 g of benzyl glycidyl ether to 20 g of dimethyl sulfoxide, stir thoroughly to dissolve and mix evenly to form a uniform mixed solution;
[0067] Add 0.5 g of sodium hydroxide to the mixed solution, and react in an oil bath at 70° C. for 8 h to obtain a graphene pre-stripping agent;
[0068] The graphene pre-stripping agent is dried to remove the organic solvent dimethyl sulfoxide, thereby obtaining the graphene stripping agent.
[0069] 2. Preparation of graphene aqueous dispersion
[0070] 10 g of natural flake graphite, 0.5 g of the graphene exfoliator in Example 1 and 89.5 g of deionized water were mixed evenly, and then homogenized and exfoliated for 10 h using a sand mill at 3000 rpm; after the exfoliation, the product was centrifuged at 3000 rpm for 30 min to obtain a graphene aqueous dispersion with a concentration of 0.03 g / mL.
[0071] in, Figure 1 This is a SEM image of the graphene aqueous dispersion obtained by mechanical exfoliation in Example 1. The existence of graphene sheets can be clearly observed, and they show obvious wrinkles; and the graphene structure is regular, with few defects and few layers.
[0072] Figure 2 This is an optical picture of the graphene aqueous dispersion in Example 1 after standing at 25° C. for 90 days. It can be seen that there is no obvious stratification phenomenon, indicating that the graphene aqueous dispersion has excellent stability and can exist stably for a long time.
[0073] Application Example 1 Preparation of Graphene Concrete
[0074] (1) According to the mass percentage, the raw material composition is: 30 parts of cement, with a specific surface area of 800m 2 / kg, 5 parts of fly ash with a particle size of 50μm and a specific surface area of 20m 2 / g silica fume 15 parts, natural river sand with a particle size of 1mm 60 parts, graphene aqueous dispersion in Example 1 3 parts, polycarboxylic acid high-efficiency water reducer 6 parts, water 10 parts;
[0075] (2) adding a polycarboxylic acid high-efficiency water reducer into water, stirring evenly, and then adding a graphene aqueous dispersion into the water and mixing evenly to obtain a dispersion;
[0076] (3) fly ash, silica fume, cement and river sand are placed in a blender and mixed evenly, and then the dispersion in step (2) is poured into the blender three times under stirring, and stirring is continued to obtain a mixture;
[0077] (4) injecting the mixture into a mold, lightly vibrating it until it is dense, and obtaining graphene concrete after curing, wherein the curing conditions are curing for 28 days at a temperature of 25° C. and a relative humidity of 95%.
[0078] Example 2 Preparation of graphene exfoliating agent and graphene aqueous dispersion
[0079] 1. Preparation of graphene exfoliating agent
[0080] Add 5.5 g of catechol and 21.35 g of benzyl glycidyl ether to 20 g of dimethyl sulfoxide, stir and dissolve them thoroughly to form a uniform mixed solution;
[0081] Add 0.5 g of sodium hydroxide to the mixed solution, and react in an oil bath at 80° C. for 8 h to obtain a graphene pre-stripping agent;
[0082] The graphene pre-stripping agent is dried to remove the organic solvent dimethyl sulfoxide, thereby obtaining the graphene stripping agent.
[0083] 2. Preparation of graphene aqueous dispersion
[0084] 10 g of natural flake graphite, 2 g of the graphene exfoliator in Example 2 and 38 g of deionized water were mixed evenly, and then homogenized and exfoliated for 8 h using a sand mill at 4000 rpm; after the exfoliation, the product was centrifuged at 3000 rpm for 30 min to obtain a graphene aqueous dispersion with a concentration of 0.06 g / mL.
[0085] Application Example 2 Preparation of Graphene Concrete
[0086] (1) According to the mass percentage, the raw material composition is: 40 parts of cement, with a specific surface area of 800m 2 / kg, 8 parts of fly ash with a particle size of 100μm and a specific surface area of 24m 2 / g silica fume 18 parts, natural river sand with a particle size of 5mm 70 parts, graphene aqueous dispersion in Example 2 5 parts, polycarboxylate high-efficiency water reducer 12 parts, water 15 parts;
[0087] (2) adding a polycarboxylic acid high-efficiency water reducer into water, stirring evenly, and then adding a graphene aqueous dispersion into the water and mixing evenly to obtain a dispersion;
[0088] (3) fly ash, silica fume, cement and river sand are placed in a blender and mixed evenly, and then the dispersion in step (2) is poured into the blender three times under stirring, and stirring is continued to obtain a mixture;
[0089] (4) injecting the mixture into a mold, lightly vibrating it until it is dense, and obtaining graphene concrete after curing, wherein the curing conditions are curing for 28 days at a temperature of 25° C. and a relative humidity of 95%.
[0090] Example 3 Preparation of graphene exfoliating agent and graphene aqueous dispersion
[0091] 1. Preparation of graphene exfoliating agent
[0092] Add 11 g of resveratrol and 29.7 g of benzyl glycidyl ether to 20 g of N,N-dimethylformamide, stir thoroughly to dissolve and mix evenly to form a uniform mixed solution;
[0093] Add 0.6 g of sodium hydroxide to the mixed solution, and react in an oil bath at 70° C. for 10 h to obtain a graphene pre-stripping agent;
[0094] The graphene pre-stripping agent is dried to remove the organic solvent N,N-dimethylformamide, thereby obtaining the graphene stripping agent.
[0095] 2. Preparation of graphene aqueous dispersion
[0096] 10 g of natural flake graphite, 1.5 g of the graphene exfoliator in Example 3 and 23.5 g of deionized water were mixed evenly, and then homogenized and exfoliated using a sand mill at 6000 rpm for 9 h. After the exfoliation was completed, the product was centrifuged at 3000 rpm for 30 min to obtain a graphene aqueous dispersion with a concentration of 0.08 g / mL.
[0097] Application Example 3 Preparation of Graphene Concrete
[0098] (1) According to the mass percentage, the raw material composition is: 50 parts of cement, with a specific surface area of 800m 2 / kg, 10 parts of fly ash with a particle size of 150μm, and a specific surface area of 26m 2 / g silica fume 20 parts, natural river sand with a particle size of 5mm 70 parts, graphene aqueous dispersion in Example 3 5 parts, polycarboxylate high-efficiency water reducer 15 parts, water 15 parts;
[0099] (2) adding a polycarboxylic acid high-efficiency water reducer into water, stirring evenly, and then adding a graphene aqueous dispersion into the water and mixing evenly to obtain a dispersion;
[0100] (3) fly ash, silica fume, cement and river sand are placed in a blender and mixed evenly, and then the dispersion in step (2) is poured into the blender three times under stirring, and stirring is continued to obtain a mixture;
[0101] (4) injecting the mixture into a mold, lightly vibrating it until it is dense, and obtaining graphene concrete after curing, wherein the curing conditions are curing for 28 days at a temperature of 25° C. and a relative humidity of 95%.
[0102] Example 4 Preparation of graphene exfoliating agent and graphene aqueous dispersion
[0103] 1. Preparation of graphene exfoliating agent
[0104] Add 5.5 g of phloroglucinol and 25.8 g of benzyl glycidyl ether to 20 g of N,N-dimethylformamide, stir thoroughly to dissolve and mix evenly to form a uniform mixed solution;
[0105] Add 0.25 g of potassium hydroxide to the mixed solution, and react in an oil bath at 60° C. for 8 h to obtain a graphene pre-stripping agent;
[0106] The graphene pre-stripping agent is dried to remove the organic solvent N,N-dimethylformamide, thereby obtaining the graphene stripping agent.
[0107] 2. Preparation of graphene aqueous dispersion
[0108] 10 g of expanded graphite, 2 g of the graphene exfoliator in Example 4 and 55 g of deionized water were mixed evenly, and then homogenized and exfoliated for 9 h using a sand mill at 5000 rpm; after the exfoliation, the product was centrifuged at 3000 rpm for 30 min to obtain a graphene aqueous dispersion with a concentration of 0.07 g / mL.
[0109] Application Example 4 Preparation of Graphene Concrete
[0110] (1) According to the mass percentage, the raw material composition is: 40 parts of cement, with a specific surface area of 800m 2 / kg, 5 parts of fly ash with a particle size of 150μm and a specific surface area of 22m 2 / g silica fume 16 parts, natural river sand with a particle size of 5mm 50 parts, graphene aqueous dispersion in Example 4 2 parts, polycarboxylic acid high-efficiency water reducer 10 parts, water 12 parts;
[0111] (2) adding a polycarboxylic acid high-efficiency water reducer into water, stirring evenly, and then adding a graphene aqueous dispersion into the water and mixing evenly to obtain a dispersion;
[0112] (3) fly ash, silica fume, cement and river sand are placed in a blender and mixed evenly, and then the dispersion in step (2) is poured into the blender three times under stirring, and stirring is continued to obtain a mixture;
[0113] (4) injecting the mixture into a mold, lightly vibrating it until it is dense, and obtaining graphene concrete after curing, wherein the curing conditions are curing for 28 days at a temperature of 25° C. and a relative humidity of 95%.
[0114] Comparative Example 1
[0115] This comparative example provides a concrete and a preparation method thereof, which adopts the same implementation as in Application Example 1, except that no graphene aqueous dispersion is added. Other process conditions and steps are the same as in Application Example 1, and the specific steps are as follows:
[0116] (1) According to the mass percentage, the raw material composition is: 30 parts of cement, with a specific surface area of 800m 2 / kg, 5 parts of fly ash with a particle size of 50μm and a specific surface area of 20m 2 / g silica fume 15 parts, river sand with a particle size of 1mm 60 parts, polycarboxylic acid high-efficiency water reducing agent 6 parts, water 10 parts;
[0117] (2) adding the polycarboxylate high-efficiency water reducer into water and stirring evenly to obtain a dispersion;
[0118] (3) fly ash, silica fume, cement and river sand are placed in a blender and mixed evenly, and then the dispersion in step (2) is poured into the blender three times under stirring, and stirring is continued to obtain a mixture;
[0119] (4) injecting the mixture into a mold, lightly vibrating it until it is dense, and obtaining graphene concrete after curing, wherein the curing conditions are curing for 28 days at a temperature of 25° C. and a relative humidity of 95%.
[0120] Comparative Example 2
[0121] This comparative example provides a method for preparing a graphene aqueous dispersion, which adopts the same implementation as in Example 1, except that no graphene exfoliating agent is added. Other process conditions and steps are the same as in Example 1, and the specific steps are as follows:
[0122] 10 g of natural flake graphite and 90 g of deionized water were mixed evenly, and then homogenized and peeled using a sand mill at 3000 rpm for 10 h. After the peeling was completed, the product was centrifuged at 3000 rpm for 30 min to obtain a graphene aqueous dispersion.
[0123] This comparative example also provides the preparation of graphene concrete, and its process conditions and steps are the same as those of Application Example 1, with the only difference being that the graphene aqueous dispersion is prepared in Comparative Example 2.
[0124] Comparative Example 3
[0125] This comparative example provides a method for preparing a graphene aqueous dispersion, which adopts the same implementation as Example 1, except that the graphene exfoliator is replaced with an equal mass of sodium dodecylbenzene sulfonate. Other process conditions and steps are the same as those in Example 1, and the specific steps are as follows:
[0126] 10 g of natural flake graphite, 0.5 g of sodium dodecylbenzene sulfonate and 89.5 g of deionized water were mixed evenly, and then homogenized and peeled off using a sand mill at 3000 rpm for 10 h. After the peeling was completed, the product was centrifuged at 3000 rpm for 30 min to obtain a graphene aqueous dispersion.
[0127] This comparative example also provides the preparation of graphene concrete, and its process conditions and steps are the same as those of Application Example 1, with the only difference being that the graphene aqueous dispersion is prepared in Comparative Example 3.
[0128] Comparative Example 4
[0129] This comparative example provides a method for preparing a graphene aqueous dispersion, which adopts the same implementation as Example 1, except that the graphene exfoliator is replaced with an equal mass of sodium cholate. The other process conditions and steps are the same as those in Example 1, and the specific steps are as follows:
[0130] 10 g of natural flake graphite, 0.5 g of sodium cholate and 89.5 g of deionized water were mixed evenly, and then homogenized and peeled off using a sand mill at 3000 rpm for 10 h. After the peeling was completed, the product was centrifuged at 3000 rpm for 30 min to obtain a graphene aqueous dispersion.
[0131] This comparative example also provides the preparation of graphene concrete, and its process conditions and steps are the same as those of Application Example 1, with the only difference being that the graphene aqueous dispersion is prepared in Comparative Example 4.
[0132] Performance Testing
[0133] The compressive strength, flexural strength and slump of the graphene concrete in the application examples and comparative examples in this article were tested, wherein the compressive strength and flexural strength were tested according to the methods in the Standard for Test Methods for Physical and Mechanical Properties of Concrete (GB / T50081-2019). The slump was tested according to the method in the Standard for Test Methods for Performance of Ordinary Concrete Mixtures (GB / T50080-2016). The test results are shown in Table 1.
[0134] Table 1 Graphene concrete performance test results
[0135]
[0136] It can be seen from the test results in Table 1 that after adding the graphene aqueous dispersion prepared by the graphene stripping agent in the present invention, the mechanical properties of the graphene concrete are significantly improved. This is mainly due to the fact that the graphene stripping agent can well strip graphite and obtain a regular graphene structure with few defects and few layers, which can be stably and evenly dispersed in cement-based concrete, thereby significantly improving the mechanical properties of the graphene concrete.
[0137] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0138] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A graphene exfoliating agent, characterized in that: It is prepared by epoxy ring-opening and substitution reaction of phenolic compounds and benzyl glycidyl ether; Preferably, the phenolic compound is one of hydroquinone, catechol, resveratrol and phloroglucinol; Preferably, the molar ratio of the hydroxyl group in the phenolic compound to the epoxy group in the benzyl glycidyl ether is 1:(1.1-1.5).
2. The graphene exfoliating agent according to claim 1, characterized in that The molar ratio of the hydroxyl group in the phenolic compound to the epoxy group in the benzyl glycidyl ether is 1:1.
2.
3. The graphene exfoliating agent according to claim 1, characterized in that Its preparation comprises the following steps: Adding phenolic compounds and benzyl glycidyl ether into an organic solvent to fully dissolve them to form a uniform mixed solution; Adding an alkaline catalyst to the mixed solution, reacting at a constant temperature of 60 to 90° C. for 6 to 10 hours, and drying to obtain a graphene exfoliating agent; Preferably, the organic solvent is one or a mixture of two or more of dimethyl sulfoxide, acetone, N,N-dimethylformamide, and N-methylpyrrolidone; Preferably, the alkaline catalyst is sodium hydroxide or potassium hydroxide; Preferably, the amount of the alkaline catalyst added is 1%-2% of the total mass of the mixed solution.
4. A method for preparing a graphene aqueous dispersion, characterized in that: The following steps are involved: After the graphite powder is fully mixed with the graphene exfoliating agent according to any one of claims 1 to 3 and deionized water, the graphene aqueous dispersion is obtained by mechanical exfoliation.
5. The method for preparing a graphene aqueous dispersion according to claim 4, wherein: The mass ratio of the graphite powder to the graphene exfoliating agent is 1:(0.05-0.2).
6. The method for preparing a graphene aqueous dispersion according to claim 4, wherein: The mechanical stripping is carried out in a sand mill, the rotation speed of the sand mill is 3000-6000 rpm, and the stripping time is 2-10 hours.
7. The method for preparing a graphene aqueous dispersion according to claim 4, wherein: The concentration of the graphene aqueous dispersion is 0.01 g / mL-0.1 g / mL.
8. Application of graphene aqueous dispersion in the preparation of graphene concrete, characterized in that: The graphene aqueous dispersion is prepared by the preparation method according to any one of claims 4 to 7.
9. A graphene concrete, characterized in that: Contains a graphene aqueous dispersion prepared by the preparation method according to any one of claims 4 to 7.
10. The graphene concrete according to claim 9, characterized in that: Calculated by weight, it is prepared from 30-40 parts of cement, 2-5 parts of graphene aqueous dispersion, 15-20 parts of silica fume, 5-10 parts of fly ash, 6-15 parts of water reducer, 50-75 parts of natural river sand and 5-15 parts of water.
Citation Information
Patent Citations
Preparation method of functionalized graphene and application thereof
CN104403130A
Graphene aqueous dispersion liquid, graphene concrete and preparation methods of graphene aqueous dispersion liquid and graphene concrete
CN110498634A
Modified graphene cement-based material and preparation method thereof
CN115231860A
Aqueous dispersions for antioxidants
CN1643099A
Photocurable resin composition containing modified graphene
KR1020170042051A