Preparation method and application of oriented growth silicon dioxide nanowire

By adding triblock polyurethane surfactant to the sol-gel method, the problem of directional growth of silica nanowires was solved, and efficient and large-scale preparation of directional growth of silica nanowires was achieved, and their dispersion was improved and uniformity have expanded its application potential in multiple fields.

CN118954520APending Publication Date: 2024-11-15SOUTH CHINA UNIV OF TECH +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410876594.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the prior art, the preparation method of silica nanowires has problems such as cumbersome steps, high cost, poor uniformity and dispersion, and is especially unable to achieve directional growth, which limits its wide application in the fields of materials and electronics.

Method used

Based on the traditional sol-gel method, a small amount of triblock polyurethane surfactant is added to realize the directional growth of silica nanowires by regulating the amount added, simplifying the process and reducing costs and improving dispersion.

Benefits of technology

It has achieved efficient and large-scale preparation of directionally grown silica nanowires, significantly improving their dispersion and uniformity, and expanding their application prospects in the fields of energy storage, catalysis and aerogels.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118954520A_ABST
    Figure CN118954520A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of oriented growth silicon dioxide nanowires, and belongs to the field of nano materials and preparation methods. The invention aims to solve the problem that the direction of the nano silicon dioxide nanowire is uncertain in the growth process, and provides the preparation method of the silicon dioxide nanowire which is simple in process, uniform in finished product, easy to produce on a large scale, good in dispersity and capable of growing directionally. Specifically, according to the method, a triblock polyurethane surfactant is added into a conventional sol-gel system, so that the silicon dioxide nanowire with a regular shape is directionally generated from the silicon dioxide nanowire. The method has the advantages of simple process, mild conditions, controllable structure, easy large-scale preparation and the like, and the prepared silicon dioxide nanowire has good uniformity and dispersity, and is especially suitable for the fields of polymer fillers, energy storage, biological imaging, silicon dioxide aerogel and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of nanomaterials and preparation, and more specifically, to a preparation method of directional growth silicon dioxide nanowires and applications thereof. Background Art

[0002] One-dimensional nanomaterials (nanotubes, nanowires, nanorods, nanobelts, etc.) have broad application prospects in improving the optical properties, mechanical properties, electrical properties, etc. of materials due to their unique structural characteristics. When it comes to the rapid development of microelectronics and nanoelectronics technology, the research on one-dimensional nanomaterials related to silicon is also deepening. These one-dimensional nanomaterials include silica nanowires, carbon nanowires, silica nanotubes, carbon nanotubes, silica nanorods, and graphene nanobelts. Among them, silica nanowires stand out for their stable structure and special chemical properties, becoming the basic material in the fields of chemistry, materials, biology, and physics, with a very wide range of application space and good application potential.

[0003] At present, there are many methods for preparing silica nanowires, mainly sol-gel method, chemical vapor deposition method, thermal evaporation method, electrospinning method and laser ablation method. For example, MC Corobeaa et al. used natural soil as raw material, tetraethoxysilane as silicon source, ammonia water as main catalyst, and synthesized silica nanowires with an average diameter of 20 nm by sol-gel method, and proved that silica nanowires have mechanical properties of supporting pores; Niu et al. evaporated ZnS powder on the surface of silicon wafer, and a large number of silica nanowires were formed on the surface of silicon wafer; Li Yangyang et al. used tetraethoxysilane as silicon source, pyrrolidone as template, and used electrospinning device with a flow rate of 0.4 mL / h. The spinning was dried and sintered at 25 °C to obtain silica nanowires; D. Brodoceanu et al. used laser ablation method, metal Au nanoparticles as catalyst substrate to prepare silica nanowires on silicon source. The silicon dioxide nanowires prepared by the above method have the problems of complicated steps, high cost, poor uniformity and dispersibility, and cannot achieve directional growth of silicon dioxide nanowires.

[0004] The directional growth of silica nanowires is crucial to improving their dispersibility and uniformity. At present, methods that can achieve directional growth of silica nanowires include photolithography template method and alumina template method. However, the photolithography template method has strict requirements on processing equipment, low production output and high cost; while the preparation process of the alumina template method is complicated and difficult to operate. At present, there is no simple method for large-scale preparation of directional and regulated silica nanowires. On the basis of the traditional sol-gel method, the present invention achieves the directional growth of silica nanowires by adding a small amount of triblock polyurethane surfactant, and as the amount of surfactant added changes, the morphology of silica nanowires can be regulated. Compared with the photolithography template method and the alumina template method, this process is simpler, less expensive, and can achieve large-scale preparation of directional growth of silica nanowires. Summary of the invention

[0005] The purpose of the present invention is to solve the problem of uncertain direction of silica nanowires during growth, and to provide a method for preparing silica nanowires with simple process, easy large-scale production, good dispersibility and directional growth. The present invention introduces a small amount of triblock polyurethane surfactant on the basis of the traditional sol-gel method, realizes the directional growth of silica, significantly improves the dispersibility of silica nanowires, and prepares silica nanowires with good dispersibility, which will have a broader application space in the fields of energy storage, catalysis, silica aerogel, etc.

[0006] The present invention proposes the following technical solutions to solve the above problems: The invention discloses a method for preparing directional growth silicon dioxide nanowires, which is carried out by a sol-gel method, and a tri-block polyurethane surfactant is added into the system.

[0007] Furthermore, the method comprises the following steps: A triblock polyurethane surfactant is added to a C5-C11 straight-chain alcohol solution of polyvinyl pyrrolidone, and after dispersion, C1-C4 alcohol, sodium citrate aqueous solution, water, ammonia water, and alkoxysilane are added to obtain a reaction mixture, which is allowed to stand and separated to obtain the silica nanowires.

[0008] Furthermore, the triblock polyurethane surfactant uses isocyanate, 2,2-dimethylolpropionic acid and polyethylene glycol as monomers, and the molar ratio of the isocyanate, 2,2-dimethylolpropionic acid and polyethylene glycol is 1:0.5-0.8:0.03-0.08.

[0009] Further, in the reaction mixture, the mass fraction of the polyvinyl pyrrolidone is 6%-10%; and / or, the mass fraction of the C5~C11 straight-chain alcohol is 75%-85%; and / or, the mass fraction of the triblock polyurethane surfactant is 1%-6%; and / or, the mass fraction of water is 1%-4%; and / or, the mass fraction of the C1-C4 alcohol is 6%-12%; and / or, the mass fraction of sodium citrate is 1%-3%; and / or, the mass fraction of ammonia water is 1%-3%; and / or, the mass fraction of the alkoxysilane is 1%-5%, preferably 1%-3%.

[0010] Preferably, the C5-C11 straight-chain alcohol is n-pentanol; and the C1-C4 alcohol is ethanol.

[0011] Furthermore, the preparation method of the C5-C11 straight-chain alcohol solution of polyvinyl pyrrolidone includes: adding polyvinyl pyrrolidone to the C5-C11 straight-chain alcohol and dispersing by ultrasonication.

[0012] Preferably, the ultrasonication time is 2 hours.

[0013] Furthermore, the preparation method of the triblock polyurethane surfactant comprises the following steps: heating the isocyanate to 70°C to 90°C, adding an organic tin catalyst and 2,2-dihydroxymethylpropionic acid in sequence, reacting for 1h to 3h, then adding the reaction product to polyethylene glycol at 60°C to 100°C, reacting for 1h to 3h, and vacuuming to remove the solvent to obtain the triblock polyurethane surfactant.

[0014] Preferably, the molar ratio of the isocyanate, 2,2-dimethylolpropionic acid and polyethylene glycol is 1:0.5-0.8:0.03-0.08.

[0015] Preferably, the isocyanate is selected from at least one of isophorone diisocyanate, hexamethylene diisocyanate, toluene diisocyanate, hexamethylene diisocyanate, xylylene diisocyanate, methylcyclohexyl diisocyanate or dicyclohexylmethane diisocyanate.

[0016] Preferably, the organic tin catalyst is at least one selected from dibutyltin dilaurate, stannous octoate, dibutyltin didodecylsulfide or dibutyltin diacetate.

[0017] Preferably, the number average molecular weight of the polyethylene glycol is 600 g / mol to 3500 g / mol.

[0018] Preferably, the molar ratio of the isocyanate to the organotin catalyst is 1:0.0001 to 0.001.

[0019] Further, the standing temperature is 60-85°C; and / or the standing time is 4-24 hours. Preferably, the standing time is 12-24 hours.

[0020] Furthermore, the alkoxysilane is selected from one or more of tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, tetrabutoxysilane, methyltrimethoxysilane, methyltriethoxysilane, dimethyldimethoxysilane or dimethyldiethoxysilane.

[0021] Furthermore, the dispersion is performed by ultrasound. Preferably, the duration of the ultrasound is 5-30 minutes.

[0022] Furthermore, after adding C1-C4 alcohol, sodium citrate aqueous solution and water, stir evenly. Preferably, the stirring time is 3-10 minutes.

[0023] Furthermore, after adding ammonia water and alkoxysilane, stirring is performed uniformly. Preferably, the stirring time is 3-10 minutes.

[0024] Furthermore, the separation is centrifugation.

[0025] Furthermore, after separation, the steps of washing and drying are also included. Preferably, the washing is performed by alternating ethanol and water for 5 times. Preferably, the drying is performed by oven drying; the drying temperature is 80° C.; and the drying time is 8 hours.

[0026] The present invention also protects a directed growth silicon dioxide nanowire, which is prepared according to the above method.

[0027] Preferably, the average diameter of the silicon dioxide nanowires is 80-300 nm and the length is 3-50 m.

[0028] The present invention also protects the use of the above silicon dioxide nanowires in preparing silicon dioxide aerogel or silicone rubber.

[0029] Compared with the prior art, the present invention has the following beneficial effects: The present invention provides a method for preparing directional growth of silica nanowires efficiently and on a large scale. On the basis of the traditional sol-gel method, the directional growth of silica nanowires is achieved by adding a small amount of triblock polyurethane surfactant. With the addition of the triblock polyurethane surfactant, the curvature of the silica nanowires gradually decreases. As the curvature of the silica nanowires decreases, they have better dispersibility in ethanol, and the Tyndall effect of the formed silica ethanol solution is more obvious. Compared with linear silica prepared by traditional methods, the prepared directional linear silica has better dispersion and has better application prospects in polymer fillers, energy storage, bioimaging, silica aerogels, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 Scanning electron microscope image of silicon dioxide nanowire example 1.

[0031] Figure 2 Scanning electron microscope image of silicon dioxide nanowire embodiment 2.

[0032] Figure 3 Scanning electron microscope image of silicon dioxide nanowire embodiment 3.

[0033] Figure 4 Scanning electron microscope image of silicon dioxide nanowire example 4.

[0034] Figure 5 Scanning electron microscope image of silicon dioxide nanowire comparative example 1.

[0035] Figure 6 The silica nanowire ethanol solution described in Comparative Example 1 of silica nanowires.

[0036] Figure 7 Silica nanowires The ethanol solution of silica nanowires described in Example 1. DETAILED DESCRIPTION

[0037] In order to more clearly and completely describe the technical solution of the present invention, the present invention is further described in detail through specific embodiments below. It should be understood that the specific embodiments described herein are only used to explain the present invention, and are not used to limit the present invention. Various changes can be made within the scope of the rights of the present invention.

[0038] The present invention will be further described below in conjunction with examples and drawings.

[0039] The preparation method of the triblock polyurethane surfactant comprises the following steps: heating isocyanate to 80° C., adding an organic tin catalyst and 2,2-dihydroxymethyl propionic acid in sequence, reacting for 2 hours, adding the reaction product to polyethylene glycol at 80° C., reacting for 2 hours, and vacuuming to remove the solvent to obtain the triblock polyurethane surfactant.

[0040] The molar ratio of the isocyanate, 2,2-dimethylolpropionic acid and polyethylene glycol is 1:0.7:0.05.

[0041] The isocyanate is selected from isophorone diisocyanate.

[0042] The organotin catalyst is selected from dibutyltin dilaurate.

[0043] The number average molecular weight of the polyethylene glycol is 1000 g / mol.

[0044] The molar ratio of the isocyanate to the organotin catalyst is 1:0.0005.

[0045] Example 1 A method for preparing oriented growth silicon dioxide nanowires 1. Experimental steps First, 15 g of polyvinyl pyrrolidone was weighed and dispersed in 120 g of n-pentanol. The solution was placed in a 250 mL beaker and ultrasonicated at a frequency of 60 Hz for two hours to obtain a solution A.

[0046] Then, 4.5 g of triblock polyurethane surfactant was added to Solution A, and ultrasonic treatment was continued for 10 minutes.

[0047] Then, 12 g of ethanol, 1.5 g of 0.18 M sodium citrate hydrate aqueous solution, and 4.2 g of water were added to the solution, a magnetic stirrer was added to the beaker, and the entire device was placed on a constant temperature magnetic stirrer, the heating temperature was set to 80°C, the stirring speed was 500 rpm, and stirring was carried out under this condition for 5 minutes.

[0048] Finally, add 2.5g ammonia water (mass fraction 28%) and 2.7g tetraethoxysilane to the solution, continue magnetic stirring for 5 minutes and then turn off the magnetic stirring. After standing for 24 hours, a light yellow suspension solution can be obtained. After centrifugation and alternating washing with ethanol and water, a white precipitate can be obtained. Dry it in an oven at 80°C to obtain silica nanowires.

[0049] 2. Performance Testing Scanning electron microscopy characterization of silicon dioxide nanowires Figure 1 shown.

[0050] Depend on Figure 1 It can be seen that the curvature of the silicon dioxide nanowires in this embodiment is greatly reduced compared with that in comparative example 1; the uniformity is better than that in examples 2 and 3; and the average length of the silicon dioxide nanowires is increased compared with that in example 4. The average diameter of the silicon dioxide nanowires is 300 nm and the length is 10 m.

[0051] Example 2 A method for preparing oriented growth silicon dioxide nanowires 1. Experimental steps First, 15 g of polyvinyl pyrrolidone was weighed and dispersed in 120 g of n-pentanol. The solution was placed in a 250 mL beaker and ultrasonicated at a frequency of 60 Hz for two hours to obtain a solution A.

[0052] Then, 4.5 g of triblock polyurethane surfactant was added to Solution A, and ultrasonic treatment was continued for 10 minutes.

[0053] Then, 12 g of ethanol, 1.5 g of 0.18 M sodium citrate hydrate aqueous solution, and 2.8 g of water were added to the solution, a magnetic stirrer was added to the beaker, and the entire device was placed on a constant temperature magnetic stirrer, the heating temperature was set to 80°C, the stirring speed was 500 rpm, and stirring was carried out under this condition for 5 minutes.

[0054] Finally, add 2.5g ammonia water (mass fraction 28%) and 2.7g tetraethoxysilane to the solution, continue magnetic stirring for 5 minutes and then turn off the magnetic stirring. After standing for 24 hours, a light yellow suspension solution can be obtained. After centrifugation and alternating washing with ethanol and water, a white precipitate can be obtained. Dry it in an oven at 80°C to obtain silica nanowires.

[0055] 2. Performance Testing Scanning electron microscopy characterization of silicon dioxide nanowires Figure 2 shown.

[0056] Depend on Figure 2 It can be seen that the curvature of the silica nanowires is reduced after the addition of triblock surfactants. At the same time, the reduction in the amount of water added will lead to a decrease in the uniformity of the silica nanowires. The average diameter is 300nm and the length is 10 m.

[0057] Example 3 A method for preparing directional growth of silicon dioxide nanowires 1. Experimental steps First, 15 g of polyvinyl pyrrolidone was weighed and dispersed in 120 g of n-pentanol. The solution was placed in a 250 mL beaker and ultrasonicated at a frequency of 60 Hz for two hours to obtain a solution A.

[0058] Then, 4.5 g of triblock polyurethane surfactant was added to Solution A, and ultrasonic treatment was continued for 10 minutes.

[0059] Then, 12 g of ethanol, 1.5 g of 0.18 M sodium citrate hydrate aqueous solution, and 4.2 g of water were added to the solution, a magnetic stirrer was added to the beaker, and the entire device was placed on a constant temperature magnetic stirrer, the heating temperature was set to 80°C, the stirring speed was 500 rpm, and stirring was carried out under this condition for 5 minutes.

[0060] Finally, add 2.5g ammonia water (mass fraction 28%) and 8.1g tetraethoxysilane to the solution, continue magnetic stirring for 5 minutes and then turn off the magnetic stirring. After standing for 24 hours, a light yellow suspension solution can be obtained. After centrifugation and alternating washing with ethanol and water, a white precipitate can be obtained. Dry it in an oven at 80°C to obtain silica nanowires.

[0061] 2. Performance Testing Scanning electron microscopy characterization of silicon dioxide nanowires Figure 3 shown.

[0062] Depend on Figure 3 It can be seen that the curvature of the silica nanowires is reduced after the addition of triblock surfactants. At the same time, the increase in the amount of TEOS added will lead to a decrease in the uniformity of the silica nanowires. The average diameter is 400nm and the length is 15 m.

[0063] Example 4 A method for preparing directional growth of silicon dioxide nanowires 1. Experimental steps First, 15 g of polyvinyl pyrrolidone was weighed and dispersed in 120 g of n-pentanol. The solution was placed in a 250 mL beaker and ultrasonicated at a frequency of 60 Hz for two hours to obtain a solution A.

[0064] Then, 4.5 g of triblock polyurethane surfactant was added to Solution A, and ultrasonic treatment was continued for 10 minutes.

[0065] Then, 12 g of ethanol, 1.5 g of 0.18 M sodium citrate hydrate aqueous solution, and 4.2 g of water were added to the solution, a magnetic stirrer was added to the beaker, and the entire device was placed on a constant temperature magnetic stirrer, the heating temperature was set to 80°C, the stirring speed was 500 rpm, and stirring was carried out under this condition for 5 minutes.

[0066] Finally, add 2.5g ammonia water (mass fraction 28%) and 2.7g tetraethoxysilane to the solution, continue magnetic stirring for 5 minutes and then turn off the magnetic stirring. After standing for 4 hours, a light yellow suspension solution can be obtained. After centrifugation and alternating washing with ethanol and water, a white precipitate can be obtained. Dry it in an oven at 80°C to obtain silica nanowires.

[0067] 2. Performance Testing Scanning electron microscopy characterization of silicon dioxide nanowires Figure 4 shown.

[0068] Depend on Figure 4 It can be seen that the curvature of the silica nanowires is reduced after the addition of the triblock surfactant. At the same time, when the reaction time is short, the length of the silica nanowires is shorter. The average diameter is 300nm and the length is 5 m.

[0069] Comparative Example 1 A method for preparing silicon dioxide nanowires 1. Experimental steps First, 15 g of polyvinyl pyrrolidone was weighed and dispersed in 120 g of n-pentanol. The solution was placed in a 250 mL beaker and ultrasonicated at a frequency of 60 Hz for two hours to obtain a solution A.

[0070] Then, 12 g of ethanol, 1.5 g of 0.18 M sodium citrate hydrate aqueous solution, and 4.2 g of water were added to the solution, a magnetic stirrer was added to the beaker, and the entire device was placed on a constant temperature magnetic stirrer, the heating temperature was set to 80°C, the stirring speed was 500 rpm, and stirring was carried out under this condition for 5 minutes.

[0071] Finally, add 2.5g ammonia water (mass fraction 28%) and 2.7g tetraethoxysilane to the solution, continue magnetic stirring for 5 minutes and then turn off the magnetic stirring. After standing for 24 hours, a light yellow suspension solution can be obtained. After centrifugation and alternating washing with ethanol and water, a white precipitate can be obtained. Dry it in an oven at 80°C to obtain silica nanowires.

[0072] 2. Performance Testing Scanning electron microscopy characterization of silicon dioxide nanowires Figure 5 shown.

[0073] Depend on Figure 1 It can be seen that the silicon dioxide in this comparative example is linear, has a high degree of curvature, an average diameter of 300nm, and a length of 10 m.

[0074] Test Example 1: Dispersibility Test The silicon dioxide nanowires prepared in Comparative Example 1 and Example 1 were added to the ethanol solution respectively, and ultrasonicated for 30 minutes to form a silicon dioxide ethanol solution, wherein the addition amount of the silicon dioxide nanowires was 0.2 wt %.

[0075] Test results such as Figure 6 and Figure 7 shown.

[0076] exist Figure 6 As shown in the figure, in ethanol, the silica nanowires synthesized without adding triblock surfactant have poor dispersibility and are easy to form agglomerates; Figure 7 As shown, the silica nanowires synthesized by adding triblock surfactants have better dispersibility in ethanol and more obvious Tyndall effect.

[0077] The dispersibility of the silicon dioxide nanowires prepared in Examples 2-4 is also better than that in Comparative Example 1.

[0078] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.

Claims

1. A method for preparing directional growth of silica nanowires, using a sol-gel method, characterized in that: A triblock polyurethane surfactant is added into the system.

2. The method according to claim 1, characterized in that The steps include: A triblock polyurethane surfactant is added to a C5-C11 straight-chain alcohol solution of polyvinyl pyrrolidone, and after dispersion, C1-C4 alcohol, sodium citrate aqueous solution, water, ammonia water, and alkoxysilane are added to obtain a reaction mixture, which is allowed to stand and separated to obtain the silica nanowires.

3. The method according to claim 1 or 2, characterized in that: The triblock polyurethane surfactant uses isocyanate, 2,2-dimethylol propionic acid and polyethylene glycol as monomers, and the molar ratio of the isocyanate, 2,2-dimethylol propionic acid and polyethylene glycol is 1:0.5-0.8:0.03-0.

08.

4. The method according to claim 3, characterized in that The preparation method of the triblock polyurethane surfactant comprises the following steps: heating isocyanate to 70°C to 90°C, adding an organic tin catalyst and 2,2-dihydroxymethyl propionic acid in sequence, reacting for 1h to 3h, adding the reaction product to polyethylene glycol at 60°C to 100°C, reacting for 1h to 3h, and removing the solvent by vacuum to obtain the triblock polyurethane surfactant.

5. The method according to claim 3 or 4, characterized in that: The isocyanate is selected from at least one of isophorone diisocyanate, hexamethylene diisocyanate, toluene diisocyanate, hexamethylene diisocyanate, xylylene diisocyanate, methylcyclohexyl diisocyanate or dicyclohexylmethane diisocyanate.

6. The method according to claim 3 or 4, characterized in that: The organic tin catalyst is at least one of dibutyltin dilaurate, stannous octoate, dibutyltin didodecylsulfide or dibutyltin diacetate.

7. The method according to claim 2, characterized in that: The standing temperature is 60-85°C.

8. The method according to claim 2, characterized in that: The standing time is 4-24 hours.

9. A directed growth of silicon dioxide nanowires, characterized in that: Prepared according to any one of claims 1 to 8.

10. Use of the directional growth silica nanowires according to claim 9 in the preparation of silica aerogel or silicone rubber.

Citation Information

Patent Citations

  • Preparation method of silicon dioxide nanorod array

    CN111137897A

  • Silicon dioxide microsphere as well as preparation method and application thereof

    CN114917847A

  • Method to product silica powder having huge particle,high purity and globular shape