Artificial inorganic mosaic stone and preparation method thereof

The artificial inorganic mosaic stone is prepared through the hydration of inorganic materials assisted by vacuum compression method, which solves the problems of high production costs and unenvironmental protection of mosaic stones, realizes an environmentally friendly and energy-saving production process, and improves the stability and aesthetics of the product.

CN118955020APending Publication Date: 2024-11-15CHINA STATE CONSTR HAILONG TECH CO LTD +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411018054.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The production of existing mosaic stones has high cost and unenvironmental protection, especially natural stones are expensive, complex production processes, high energy consumption of ceramics and glass products and environmental pollution, and the bonding process requires a large amount of glue.

Method used

Artificial inorganic mosaic stone is prepared by the hydration of inorganic materials, and cement, aggregate, inorganic blends, inorganic pigments, water reducing agents and toughening agents are used to form a fixed substrate, combining acrylic plastics and polycarbonate. Mosaic materials such as plastic are made of mosaic stones through vacuum compression and maintenance.

Benefits of technology

It reduces production costs, improves product stability and environmental protection, reduces dependence on natural stone, realizes an environmentally friendly and energy-saving production process, and improves the strength and aesthetics of mosaic stone.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955020A_ABST
    Figure CN118955020A_ABST
Patent Text Reader

Abstract

The invention relates to an artificial inorganic mosaic stone and a preparation method thereof, and the artificial inorganic mosaic stone comprises a fixed base material and a mosaic material fixed in the fixed base material according to a preset pattern of the mosaic stone; the fixed base material is obtained by curing slurry comprising the following components in parts by weight: 21-23 parts of cement, 60-65 parts of aggregate, 6-10 parts of an inorganic admixture, 1-1.5 parts of inorganic pigment, 1-2 parts of a water reducing agent, 3-5 parts of a toughening agent and 1-2 parts of water. The manufacturing method has the beneficial effects that the manufacturing process is simple, and the production efficiency is high; the product quality is good, natural stone and the like are reduced, the production cost is reduced, and the environment is protected.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, and in particular to an artificial inorganic mosaic stone and a preparation method thereof. Background Art

[0002] Mosaic stone is a high-end and classic decorative material. It originated from the ancient art of mosaic, which was originally made of pebbles, tiles or glass to form patterns or designs for decorating walls and floors. In modern decoration, mosaic stone usually refers to small pieces of natural stone, glass or ceramic cut into small pieces, which are then spliced ​​into various patterns and designs.

[0003] Among them, using natural stone as the raw material for mosaics is costly and the production process is complex, resulting in high processing costs; the production of ceramic and glass products has problems such as high energy consumption and environmental pollution. At the same time, a large amount of glue is required for the bonding of mosaic stones; therefore, the current production of mosaic stones does not conform to the current development concept of green environmental protection, energy conservation and carbon reduction. Summary of the invention

[0004] 1. Technical issues to be resolved

[0005] In view of the above-mentioned shortcomings and deficiencies of the prior art, the present invention provides an artificial inorganic mosaic stone and a preparation method thereof, which solves the technical problems of high cost and environmental pollution in the production process of the existing mosaic stone.

[0006] (II) Technical solution

[0007] In order to achieve the above object, the main technical solutions adopted by the present invention include:

[0008] In the first aspect, an embodiment of the present invention provides an artificial inorganic mosaic stone, comprising a fixed substrate and a mosaic material fixed in the fixed substrate according to a preset pattern of the mosaic stone; the fixed substrate is obtained by solidifying a slurry comprising the following components in parts by weight: 21-23 parts of cement, 60-65 parts of aggregate, 6-10 parts of inorganic admixture, 1-1.5 parts of inorganic pigment, 1-2 parts of water reducer, 3-5 parts of toughening agent, and 1-2 parts of water.

[0009] As a preferred embodiment of the present invention, the artificial inorganic mosaic stone, the mosaic material is one or a combination of two or more of acrylic plastic, polycarbonate plastic, acrylonitrile butadiene styrene plastic and polyethylene board.

[0010] As a preferred embodiment of the present invention, the artificial inorganic mosaic stone, the toughening agent is one or a combination of two of styrene-butadiene emulsion, styrene-acrylic emulsion and silicone-acrylic emulsion; the inorganic admixture is one or a combination of two or more of calcium powder, quartz powder, white silica fume, ordinary silica fume, fly ash and metakaolin with a particle size of 325-350 mesh.

[0011] As a preferred embodiment of the present invention, the artificial inorganic mosaic stone, when the inorganic admixture consists of calcium powder and white silica fume, the weight ratio of calcium powder to white silica fume is 1-6:2-4; when the inorganic admixture consists of metakaolin and quartz powder, the weight ratio of metakaolin to quartz powder is 1-3:1-3.

[0012] As a preferred embodiment of the present invention, the artificial inorganic mosaic stone, the artificial inorganic mosaic stone, the aggregate is quartz sand or calcium sand; the particle size range of the aggregate includes 16-26 mesh, 26-40 mesh, 40-70 mesh and 70-120 mesh, and they are combined in a weight ratio of 22-25:15-17:14-16:12-14.

[0013] Among them, when the endpoint values ​​of the particle size interval coincide, the upper limit values ​​are not included in this interval.

[0014] In a second aspect, an embodiment of the present invention provides a method for preparing the inorganic mosaic stone according to the first aspect, comprising the following steps:

[0015] S1. Fixing of mosaic materials: fixing the mosaic materials on the bottom of the mold according to the preset pattern of mosaic stones;

[0016] S2. Preparation of fixed substrate slurry: firstly, the aggregate and inorganic pigment are stirred and mixed, then inorganic admixture and cement are added, stirred and mixed, then a mixed solution of water reducer and water is added, stirred and mixed, and finally a toughening agent is added, stirred and mixed, and sieved to obtain a fixed substrate slurry;

[0017] S3, vacuum pressing: filling the fixed substrate slurry of step S2 into the mold of step S1, and then vacuum pressing the fixed substrate slurry and the mosaic material in the mold to prepare a rough board;

[0018] S4. Curing and polishing: After curing the rough board, polish it to obtain inorganic mosaic stone.

[0019] As a preferred embodiment of the present invention, in the preparation method, in S1, the fixing process of the mosaic material is: a base film is set at the bottom of the mold; the base film is set to a plane, and the mosaic material is pasted and fixed on the base film; or, the base film is provided with a groove according to a preset pattern of the mosaic stone, and one end of the mosaic material is inserted and fixed in the groove.

[0020] As a preferred embodiment of the present invention, in the preparation method, in S2, the sieving is performed using a sieve hole of 9-10 mm, and the sieving is performed once.

[0021] As a preferred embodiment of the present invention, in the preparation method, in S3, during the process of filling the fixed substrate slurry into the mold, when the fixed substrate slurry completely covers the mosaic material, the fixed substrate slurry that has entered the mold is first compacted, and then the remaining fixed substrate slurry is continued to be filled into the mold.

[0022] As a preferred embodiment of the present invention, in the preparation method, in S3, the vacuum pressing conditions are: holding time is 4 minutes, vacuum degree is -0.09 to -1.00 MPa, pressure is 15-17 MPa, pressing frequency is 20-80 Hz, and pressing time is 2-8 minutes.

[0023] (III) Beneficial effects

[0024] The beneficial effects of the present invention are as follows: the artificial inorganic mosaic stone and the preparation method thereof of the present invention, because the mosaic material is fixed on a surface by vacuum pressing assisted by the hydration of inorganic materials, the hydration is gradually complete with the increase of time, the strength of the inorganic artificial stone is improved, the mosaic material embedded in the inorganic artificial stone is stable, and compared with the mosaic stone formed by bonding with glue, the mosaic material in the present invention is not easy to peel off. Compared with the prior art, it can have a simple production process and high production efficiency; the product quality is good, the use of natural stone materials is reduced, the production cost is reduced, and it is environmentally friendly.

[0025] Mosaic materials are one or a combination of two or more of acrylic plastic, polycarbonate plastic, acrylonitrile butadiene styrene plastic or polyethylene board. Mosaic materials have a wide range of sources, various shapes and colors, low production costs, and can meet the needs of different patterns. Inorganic pigments are selected from one or a combination of two or more inorganic pigments such as titanium dioxide, iron red, iron yellow, iron black or carbon black, which enriches the color of the fixed substrate.

[0026] The inorganic admixture is one or a combination of two or more of calcium powder, quartz powder, white silica fume, ordinary silica fume, fly ash, or metakaolin with a particle size of 325-350 mesh. The components of the above inorganic admixtures have high reactivity, and the hydration products fill the pores of the material, thereby improving the density and strength of the artificial stone, and also improving its impermeability and chemical corrosion resistance, thereby extending the service life of the artificial stone. Specifically, when the inorganic admixture includes calcium powder and white silica fume, or when the inorganic admixture includes metakaolin and quartz powder, the effect is best according to a specific dosage ratio.

[0027] A base film is set at the bottom of the mold for fixing and attaching the mosaic material. The base film is provided with grooves according to the preset pattern of the mosaic stone. One end of the mosaic material is inserted and fixed in the groove, which can horizontally limit the mosaic material to avoid the movement of the mosaic material during the process of adding the fixed substrate. The prepared mosaic stone pattern has higher precision.

[0028] When pressing and fixing the base material slurry and mosaic materials, a combination of low frequency and high frequency is adopted. Low frequency is first performed evenly, and then high frequency is pressed. This is more conducive to forming a tight and delicate state between the base material slurry and the mosaic material, and is conducive to the base material slurry playing a stable fixing role on the mosaic material, ultimately ensuring the beauty and practicality of the mosaic stone. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 , Figure 2 and Figure 3 , are pictures of mosaic stones prepared in Example 3 of an artificial inorganic mosaic stone and a preparation method thereof of the present invention;

[0030] Figure 4 This is a picture of the mosaic stone prepared in Example 1 of an artificial inorganic mosaic stone and a preparation method thereof of the present invention. DETAILED DESCRIPTION

[0031] In order to better explain the present invention and facilitate understanding, the present invention is described in detail below through specific implementation modes in conjunction with the accompanying drawings.

[0032] The embodiment of the present invention proposes an artificial inorganic mosaic stone and a preparation method thereof, which aims to solve the technical problems of high cost and environmental pollution in the production process of existing mosaic stones. Since the mosaic material is fixed on a surface by vacuum pressing assisted by the hydration of inorganic materials, the hydration gradually becomes complete over time, the strength of the inorganic artificial stone is improved, and the mosaic material embedded in the inorganic artificial stone is stable. Compared with the mosaic stone formed by gluing, the mosaic material in the present invention is not easy to peel off. The production process is simple and the production efficiency is high; the product quality is good, the use of natural stone is reduced, the production cost is reduced, and it is environmentally friendly.

[0033] In order to better understand the above technical solution, exemplary embodiments of the present invention will be described in more detail below with reference to the accompanying drawings. Although exemplary embodiments of the present invention are shown in the accompanying drawings, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments described herein. On the contrary, these embodiments are provided to enable a clearer and more thorough understanding of the present invention and to fully convey the scope of the present invention to those skilled in the art.

[0034] Example 1

[0035] This embodiment provides a method for preparing an artificial inorganic mosaic stone, wherein the fixed substrate is prepared according to the following formula, and 23 parts of cement, 62 parts of quartz sand, 6 parts of inorganic admixture, 1 part of inorganic pigment, 1 part of water reducer, 5 parts of toughening agent, and 2 parts of water are added. The quartz sand particle size is in the range of 16-120 mesh, 22 parts of 16-26 mesh, 15 parts of 26-40 mesh, 14 parts of 40-70 mesh, and 12 parts of 7-120 mesh; the inorganic admixture includes 325 mesh calcium powder and white silica fume, and the mass ratio is 5:3.

[0036] The specific preparation steps of inorganic mosaic stone are as follows:

[0037] (1) A layer of PET base film is coated on the bottom of an 800×800 mm iron mold;

[0038] (2) Use glue to fix the front side of the patterned acrylic plate (mosaic material) on the PET base film according to the design requirements of the mosaic stone pattern; wherein the glue used for fixing can be any low-strength glue, which is only used to fix the position of the patterned acrylic plate on the PET base film.

[0039] (3) Stirring steps for fixing the substrate slurry: a. Mix quartz sand and inorganic pigment and stir evenly; b. Add inorganic admixture and cement and stir evenly; c. Add water and water reducing agent and stir evenly; d. Add toughening agent and stir evenly; e. Mechanically sieve the final mixture using a 9 mm sieve and sieve once;

[0040] (4) The partially fixed substrate slurry obtained in step (3) is evenly distributed between the acrylic plates fixed in step (1) and compacted, and then the remaining fixed substrate slurry is evenly arranged in the mold, and then vacuum vibration pressing is performed, the press holding time is 240 seconds, the vacuum degree is -0.095MPa, the press pressure is 15MPa, the press frequency is 35Hz vibration for 100s, and 50Hz vibration for 140s;

[0041] Step (5): After pressing and forming, the product is cured in a curing room and spray cured respectively. After curing, the product is polished to a certain thickness to obtain a mosaic inorganic artificial stone. The specific curing conditions refer to the prior art.

[0042] Example 2

[0043] This embodiment provides a method for preparing an artificial inorganic mosaic stone. The difference between this embodiment and embodiment 1 is that:

[0044] The inorganic admixtures are 325 mesh kaolin and quartz powder, with a mass ratio of 1:1.

[0045] Example 3

[0046] This embodiment provides a method for preparing an artificial inorganic mosaic stone. The difference between this embodiment and embodiment 1 is that:

[0047] In step (1), a layer of PET base film is coated on the bottom of the iron mold, and then a whole transparent acrylic plate is placed on the base film. The transparent acrylic plate is punched according to the design requirements of the mosaic stone pattern, and the formed holes are equivalent to the grooves formed on the base film;

[0048] In step (2), the patterned acrylic plate is inlaid in the hole of the transparent acrylic plate according to the mosaic stone pattern design, so that the patterned acrylic plate is fixed in the hole to form a mosaic stone pattern.

[0049] Compared with Example 1, this embodiment can better fix the pattern part of the mosaic stone, reduce the slight displacement of the pattern acrylic plate in the finished product, and the surface of the mosaic stone finally formed looks more coordinated as a whole.

[0050] Example 4

[0051] The difference between this embodiment and embodiment 1 is that in step (4), the pressing machine frequencies are 20 Hz and 60 Hz, respectively, and vibrate for 120 s and 120 s, respectively.

[0052] Example 5

[0053] The difference between this embodiment and embodiment 1 is that in step (4), the pressing machine frequencies are 30 Hz and 80 Hz, respectively, and vibrate for 120 s and 120 s, respectively.

[0054] Reference Figure 4 , is the inorganic mosaic stone prepared in Example 1; Figure 1 , Figure 2 , Figure 3 The inorganic mosaic stone prepared in Example 3; the inorganic mosaic stone prepared above has neat mosaic patterns, a transparent and moist surface, high aesthetics, and high overall durability.

[0055] Comparative Example 1

[0056] The difference between this comparative example and Example 1 is that in step (4), the pressing frequency is 20 Hz and the vibration is 240 s.

[0057] The Secco inorganic artificial stone prepared in this comparative example has a large number of holes inside and on the surface.

[0058] Comparative Example 2

[0059] The difference between this comparative example and Example 1 is that in step (4), the pressing frequency is 50 Hz and the vibration is 240 s.

[0060] The CYC inorganic artificial stone prepared in this comparative example was pressed using an intermediate frequency throughout the entire process, and the fixed base material slurry could not be compacted after reaching a uniform state, resulting in problems such as holes and uneven thickness in the board after final pressing.

[0061] Comparative Example 3

[0062] The difference between this comparative example and Example 1 is that in step (4), the pressing frequency is 80 Hz and the vibration is 240 s.

[0063] The CYC inorganic artificial stone prepared in this comparative example was directly subjected to high frequency at the beginning, which resulted in most of the fixed substrate slurry being compacted, and a small part being unable to be compacted. The surface of the prepared CYC inorganic artificial stone was partially smooth and partially had a large number of holes.

[0064] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. An artificial inorganic mosaic stone, characterized in that: It includes a fixed substrate and a mosaic material fixed in the fixed substrate according to a preset pattern of mosaic stone; The fixed substrate is obtained by solidifying a slurry comprising the following components in parts by weight: 21-23 parts of cement, 60-65 parts of aggregate, 6-10 parts of inorganic admixture, 1-1.5 parts of inorganic pigment, 1-2 parts of water reducer, 3-5 parts of toughening agent, and 1-2 parts of water.

2. The artificial inorganic mosaic stone according to claim 1, characterized in that: The mosaic material is one or a combination of two or more of acrylic plastic, polycarbonate plastic, acrylonitrile butadiene styrene plastic and polyethylene board.

3. The artificial inorganic mosaic stone according to claim 1, characterized in that: The toughening agent is one or a combination of two of styrene-butadiene emulsion, styrene-acrylic emulsion and silicone-acrylic emulsion; The inorganic admixture is one or a combination of two or more of calcium powder, quartz powder, white silica fume, ordinary silica fume, fly ash and metakaolin with a particle size of 325-350 meshes.

4. The artificial inorganic mosaic stone according to claim 3, characterized in that: When the inorganic admixture consists of calcium powder and white silica fume, the weight ratio of calcium powder to white silica fume is 1-6:2-4; When the inorganic admixture consists of metakaolin and quartz powder, the weight ratio of the metakaolin to the quartz powder is 1-3:1-3.

5. The artificial inorganic mosaic stone according to claim 1 or 2, characterized in that: The aggregate is quartz sand or calcium sand; The particle size ranges of the aggregates include 16-26 mesh, 26-40 mesh, 40-70 mesh and 70-120 mesh, and they are combined in a weight ratio of 22-25:15-17:14-16:12-14.

6. A method for preparing the inorganic mosaic stone according to any one of claims 1 to 5, characterized in that: The following steps are involved: S1. Fixing of mosaic materials: fixing the mosaic materials on the bottom of the mold according to the preset pattern of mosaic stones; S2. Preparation of fixed substrate slurry: firstly, the aggregate and inorganic pigment are stirred and mixed, then inorganic admixture and cement are added, stirred and mixed, then a mixed solution of water reducer and water is added, stirred and mixed, and finally a toughening agent is added, stirred and mixed, and sieved to obtain a fixed substrate slurry; S3, vacuum pressing: filling the fixed substrate slurry of step S2 into the mold of step S1, and then vacuum pressing the fixed substrate slurry and the mosaic material in the mold to prepare a rough board; S4. Curing and polishing: After curing the rough board, polish it to obtain inorganic mosaic stone.

7. The preparation method according to claim 6, characterized in that: In S1, the fixing process of the mosaic material is as follows: a base film is arranged at the bottom of the mold; The base film is set to be a flat surface, and the mosaic material is adhered and fixed on the base film; Alternatively, the base film is provided with a groove according to a preset pattern of the mosaic stone, and one end of the mosaic material is inserted and fixed in the groove.

8. The preparation method according to claim 6, characterized in that: In S2, the sieve is sieved once using a sieve with a mesh size of 9-10 mm.

9. The preparation method according to claim 6, characterized in that: In S3, during the process of filling the fixed substrate slurry into the mold, when the fixed substrate slurry completely covers the mosaic material, the fixed substrate slurry that has entered the mold is compacted first, and then the remaining fixed substrate slurry is continued to be filled into the mold.

10. The preparation method according to claim 6, characterized in that: In S3, the vacuum pressing conditions are: holding time is 4 min, vacuum degree is -0.09 to -1.00 MPa, and pressure is 15-17 MPa; The pressing frequency is 20-80Hz, and the pressing time is 2-8min.

Citation Information

Cited By

  • Method for preparing mosaic inorganic artificial stone by utilizing leftover materials left after stone cutting

    CN120155991A