Hollow vacuum extrusion molding plate produced by full-industrial solid waste and production process

By preparing cementitious materials and aggregates from all industrial solid waste and combining them with vacuum extrusion molding technology to produce hollow vacuum extruded plates, the problem of low utilization rate of industrial solid waste has been solved, achieving a win-win situation of reducing production costs and environmental benefits.

CN118955075APending Publication Date: 2024-11-15CHANGZHI CARBON VALLEY TECH INCUBATOR CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411058419.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Existing technologies are insufficient for the effective utilization of industrial solid waste, resulting in high production costs and significant environmental impact.

Method used

The cementitious materials and aggregates are prepared using all industrial solid waste, and hollow vacuum extrusion molding is combined with vacuum extrusion molding process to produce hollow vacuum extrusion molded plates. Steel slag, water slag, coal gangue and other waste materials are used as the main raw materials, and carbon fiber is recovered by chemical solvent decomposition.

Benefits of technology

It has reduced production costs, solved the problem of low utilization rate of industrial solid waste, and created economic and environmental value.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955075A_ABST
    Figure CN118955075A_ABST
Patent Text Reader

Abstract

The invention relates to a hollow vacuum extrusion molding plate produced by full industrial solid waste and a production process, and belongs to the technical field of building materials, and the production process comprises the following steps: preparing a cementing material: preparing 100-300 parts of 100-800-mesh steel slag, 100-280 parts of 100-800-mesh water granulated slag, 10-30 parts of desulfurized gypsum, 10-20 parts of fly ash, 5-15 parts of slag powder and 5-15 parts of sodium silicate, and uniformly stirring in a stirrer to obtain the cementing material; and thus, the required cementing material is obtained. Aggregate: 800 to 1000 parts of coal gangue; other ingredients: preparing 30-50 parts of fly ash, 10-30 parts of slag powder and 1-15 parts of carbon fibers recovered from waste materials; the preparation method comprises the following steps: uniformly stirring the materials in a high-speed stirrer, adding 120-220 parts of water, continuously stirring to form a required blank, kneading and mixing in a mixing mill, feeding the blank into a vacuum extruder for extrusion, cutting, and feeding steam for curing at 80 DEG C to form a product. The main raw materials used by the invention are all existing industrial solid wastes, so that the production cost is greatly reduced, and the problem of consumption of industrial solid wastes left in extensive industrial production for many years in China is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of building materials, and relates to a process for producing hollow vacuum extrusion molding plates using all industrial solid waste, and also relates to a hollow vacuum extrusion molding plate produced using all industrial solid waste. The main material of the present invention adopts all industrial solid waste, which greatly reduces the production cost. Background Art

[0002] ECP board, also known as Extruded Cement Panel, is a new type of cement board made of cement, fiber and siliceous materials, manufactured by vacuum high-pressure extrusion molding equipment, and then cured by steam. ECP board has excellent properties such as high strength, light weight, fire resistance, weather resistance, earthquake resistance, and sound insulation, so it is widely used in the construction field.

[0003] Steel slag is a kind of industrial solid waste, which is the slag discharged from steelmaking. It is divided into converter slag, open-hearth slag and electric furnace slag according to the furnace type. It is mainly composed of calcium, iron, silicon, magnesium and a small amount of oxides of aluminum, manganese and phosphorus. Steel slag is formed at a temperature of 1500-1700℃. It is liquid at high temperature and becomes blocky after slow cooling. It is generally dark gray or dark brown. Sometimes the free calcium and magnesium oxides contained in it react with water or moisture to convert into hydroxides, causing the slag block to expand and break. Sometimes it breaks because a large amount of dicalcium silicate contained in it changes from β type to γ ​​type during the cooling process (about 675℃).

[0004] Water slag is formed by rapidly cooling molten blast furnace slag in water. There are two main methods: slag pool water quenching and furnace front water quenching.

[0005] Gangue is a solid waste discharged during the coal mining and coal washing process. It is a black-gray rock with a low carbon content and harder than coal that accompanies the coal seam during the coal formation process. It includes excavation gangue during tunnel excavation, gangue mined from the roof, floor and interlayer during mining, and washed gangue picked out during coal washing. Its main components are Al2O3 and SiO2, and it also contains varying amounts of Fe2O3, CaO, MgO, Na2O, K2O, P2O5, SO3 and trace rare elements (gallium, vanadium, titanium, cobalt). At present, gangue is the gangue slag after pyrolysis and gasification. The original gangue is crushed by a drum-type gangue crusher, and the particles with a particle size of less than or equal to 5mm are taken and placed in a gasifier for pyrolysis and gasification. The slag obtained is gangue slag.

[0006] A large amount of industrial solid waste will be generated during the industrial production process, such as the steel slag, water slag and coal gangue mentioned above. If these industrial solid wastes are utilized, it will not only improve the utilization rate of industrial solid wastes and reduce the pressure of industrial solid wastes, but also turn waste into treasure and create economic and environmental value. Summary of the invention

[0007] The purpose of the present invention is to provide a production process for producing hollow extrusion profiles using industrial solid waste, which greatly reduces production costs and solves the problem of consuming industrial solid waste left over from my country's extensive industrial production for many years.

[0008] The technical solution adopted by the present invention to achieve its purpose is as follows:

[0009] A process for producing hollow vacuum extrusion formed plates using all industrial solid wastes comprises the following steps:

[0010] Preparation of cementitious material: prepare 100-300 parts of steel slag with a mesh size of 100-800, 100-280 parts of water slag with a mesh size of 100-800, 10-30 parts of desulfurized gypsum, 10-20 parts of fly ash and 5-15 parts of slag powder, and 5-15 parts of sodium silicate as an activator, and stir them evenly in a mixer to obtain the desired cementitious material;

[0011] Aggregate: Prepare 800-1000 parts of coal gangue with a calorific value of less than 100 kcal and a particle size of less than 5 mm; the reason for choosing coal gangue with a calorific value of less than 100 kcal is to control the carbon content and prevent it from weathering after long-term use; or use 800-1000 parts of desulfurized gypsum, or 800-1000 parts of phosphogypsum, or 800-1000 parts of iron ore to replace coal gangue.

[0012] Other ingredients: prepare 30-50 parts of fly ash, 10-30 parts of slag powder, and 1-15 parts of carbon fiber recycled from waste;

[0013] Put all the above materials into a high-speed mixer and stir them evenly, then add 120 to 220 parts of water and continue stirring to form the required blank, then put it into a mixer for kneading and mixing, and then send the blank to a vacuum extruder for extrusion (the vacuum extruder is equipped with a hollow mold to extrude a hollow vacuum extruded molded plate), cut it, and then send it to steam at 80°C for curing to form the product.

[0014] A hollow vacuum extrusion molding plate made of all industrial solid waste. The raw materials include cementitious materials, aggregates and ingredients by weight, wherein the cementitious materials include 100-300 parts of steel slag with a mesh size of 100-800, 100-280 parts of water slag with a mesh size of 100-800, 10-30 parts of desulfurized gypsum, 10-20 parts of fly ash, 5-15 parts of slag powder, and 5-15 parts of sodium silicate; the aggregate is 800-1000 parts of coal gangue with a calorific value of less than 100 kcal and a particle size of less than 5 mm, or 800-1000 parts of desulfurized gypsum, or 800-1000 parts of phosphogypsum, or 800-1000 parts of iron ore; the ingredients include 30-50 parts of fly ash, 10-30 parts of slag powder, 1-15 parts of carbon fiber recycled from waste materials, and 120-220 parts of water.

[0015] The carbon fiber recycled from waste used in the present invention is mainly obtained by chemical solvent decomposition, which generally includes the following steps:

[0016] 1. Cutting and crushing: Cut and crush the retired wind turbine blades for subsequent processing;

[0017] 2. Solvent soaking: Put the crushed blade material into a chemical solvent to separate the carbon fiber and resin. Commonly used chemical solvents include dimethyl sulfoxide (DMSO), dimethylformamide (DMF), phenol, etc.

[0018] 3. Heating and stirring: The blade material immersed in the solvent is heated and stirred to accelerate the separation of the carbon fiber and the resin; the heating temperature and stirring time vary depending on the solvent and the blade material;

[0019] 4. Filtration and drying: Filter the separated carbon fibers from the solvent and dry them to remove residual solvent and moisture;

[0020] 5. Cleaning and purification: Clean and purify the dried carbon fiber to remove surface impurities and residual resin; the cleaning and purification methods may include water washing, acid washing, alkali washing, etc.;

[0021] 6. Stretching and curling: The purified carbon fiber is stretched and curled to improve its strength and elastic modulus.

[0022] It should be noted that in actual applications, the specific process of extracting carbon fiber by chemical solvent decomposition may vary depending on the blade material, so it needs to be optimized and improved according to actual conditions.

[0023] The beneficial effects of the present invention are:

[0024] The board produced by the present invention can achieve all the characteristics and indicators of the ECP board, and the main raw materials used are all existing industrial solid wastes, which greatly reduces the production cost and solves the problem of consuming industrial solid wastes left over from my country's extensive industrial production for many years. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a curve of sound insulation at different frequencies in 1 / 3 octave. DETAILED DESCRIPTION

[0026] The present invention is described in detail below in conjunction with specific embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work should belong to the scope of protection of the present invention. 1. Specific embodiments

[0028] Example 1

[0029] A process for producing hollow vacuum extrusion formed plates using all industrial solid wastes comprises the following steps:

[0030] S1. Prepare cementitious materials: Prepare 150 parts of 400-mesh steel slag, 130 parts of 400-mesh water slag, 25 parts of desulfurized gypsum, 13 parts of fly ash and 13 parts of slag powder, and stir 13 parts of sodium silicate as an activator in a mixer to obtain the desired cementitious material;

[0031] S2. Prepare aggregate: prepare 900 parts of coal gangue with a calorific value of less than 100 kcal and a particle size of less than 5 mm;

[0032] S3. Prepare other ingredients: prepare 40 parts of fly ash, 20 parts of slag powder, and 8 parts of recycled carbon fiber;

[0033] S4. Forming and curing: Put all the above materials into a high-speed mixer at a stirring speed of 220r / min, stir evenly, add 180 parts of water and continue stirring to form the required billet, then put it into a mixer for kneading and mixing, and then send the billet to a vacuum extruder for extrusion (the vacuum extruder is equipped with a hollow mold), cut, and then send it to steam at 80°C for curing to form a product.

[0034] Example 2

[0035] A process for producing hollow vacuum extrusion formed plates using all industrial solid wastes comprises the following steps:

[0036] S1. Prepare cementitious materials: prepare 100 parts of 300 mesh steel slag, 100 parts of 300 mesh water slag, 20 parts of desulfurized gypsum, 10 parts of fly ash and 10 parts of slag powder, and stir 10 parts of sodium silicate as an activator in a mixer to obtain the desired cementitious material;

[0037] S2. Prepare aggregate: prepare 800 parts of coal gangue with a calorific value of less than 100 kcal and a particle size of less than 5 mm;

[0038] S3. Prepare other ingredients: prepare 30 parts of fly ash, 10 parts of slag powder, and 5 parts of recycled carbon fiber;

[0039] S4. Forming and curing: Put all the above materials into a high-speed mixer at a stirring speed of 220r / min, stir them evenly, then add 150 parts of water and continue stirring to form the required billet, then put it into a mixer for kneading and mixing, and then send the billet to a vacuum extruder for extrusion (the vacuum extruder is equipped with a hollow mold), cut it, and then send it to steam at 80℃ for curing to form a product.

[0040] Example 3

[0041] A process for producing hollow vacuum extrusion formed plates using all industrial solid wastes comprises the following steps:

[0042] S1. Prepare cementitious materials: prepare 200 parts of 500-mesh steel slag, 150 parts of 500-mesh water slag, 30 parts of desulfurized gypsum, 15 parts of fly ash and 15 parts of slag powder, and stir 15 parts of sodium silicate as an activator in a mixer to obtain the desired cementitious material;

[0043] S2. Prepare aggregate: prepare 1000 parts of coal gangue with a calorific value of less than 100 kcal and a particle size of less than 5 mm;

[0044] S3. Prepare other ingredients: prepare 50 parts of fly ash, 30 parts of slag powder, and 15 parts of recycled carbon fiber;

[0045] S4. Forming and curing: put all the above materials into a high-speed mixer at a stirring speed of 220r / min, stir them evenly, add 200 parts of water and continue stirring to form the required blank, then put it into a mixer for kneading and mixing, and then send the blank to a vacuum extruder for extrusion (the vacuum extruder is equipped with a hollow mold), cut it, and then send it to steam at 80℃ for curing to form a product.

[0046] Example 4

[0047] A process for producing hollow vacuum extrusion formed plates using all industrial solid wastes comprises the following steps:

[0048] S1. Prepare cementitious materials: prepare 130 parts of 400-mesh steel slag, 120 parts of 400-mesh water slag, 26 parts of desulfurized gypsum, 11 parts of fly ash and 11 parts of slag powder, and stir 14 parts of sodium silicate as an activator in a mixer to obtain the desired cementitious material;

[0049] S2. Prepare aggregate: prepare 850 parts of coal gangue with a calorific value of less than 100 kcal and a particle size of less than 5 mm;

[0050] S3. Prepare other ingredients: prepare 38 parts of fly ash, 25 parts of slag powder, and 10 parts of recycled carbon fiber;

[0051] S4. Forming and curing: Put all the above materials into a high-speed mixer at a stirring speed of 220r / min, stir evenly, add 180 parts of water and continue stirring to form the required billet, then put it into a mixer for kneading and mixing, and then send the billet to a vacuum extruder for extrusion (the vacuum extruder is equipped with a hollow mold), cut, and then send it to steam at 80°C for curing to form a product.

[0052] Example 5

[0053] A process for producing hollow vacuum extrusion formed plates using all industrial solid wastes comprises the following steps:

[0054] S1. Prepare cementitious materials: prepare 180 parts of 400-mesh steel slag, 140 parts of 400-mesh water slag, 28 parts of desulfurized gypsum, 14 parts of fly ash and 14 parts of slag powder, and stir 12 parts of sodium silicate as an activator in a mixer to obtain the desired cementitious material;

[0055] S2. Prepare aggregate: prepare 950 parts of coal gangue with a calorific value of less than 100 kcal and a particle size of less than 5 mm;

[0056] S3. Prepare other ingredients: prepare 45 parts of fly ash, 15 parts of slag powder, and 12 parts of recycled carbon fiber;

[0057] S4. Forming and curing: Put all the above materials into a high-speed mixer at a stirring speed of 220r / min, stir evenly, add 160 parts of water and continue stirring to form the required billet, then put it into a mixer for kneading and mixing, and then send the billet to a vacuum extruder for extrusion (the vacuum extruder is equipped with a hollow mold), cut, and then send it to steam at 80°C for curing to form a product.

[0058] 2. Performance indicators

[0059] Testing basis:

[0060] 1. GB / T 14153-1993 "General rules for drop weight impact test methods for rigid plastics";

[0061] 2. GB 6566-2010 "Limits of Radioactive Nuclides in Building Materials";

[0062] 3. GB / T 19889.3-2005 "Acoustic buildings and sound insulation measurement of building elements Part 3: Laboratory measurement of airborne sound insulation of building elements";

[0063] 4. GB / T 15227-2019 "Test methods for air tightness, water tightness and wind pressure resistance of building curtain walls";

[0064] 5. JT / T 646.4-2016 "Highway sound barriers Part 4: Technical requirements and test methods for acoustic materials";

[0065] 6. GB / T 14402-2007 "Combustion performance of building materials and products - Determination of calorific value";

[0066] 7. GB / T 5464-2010 "Test method for non-combustibility of building materials";

[0067] 8. GB / T 23451-2009 "Lightweight partition boards for construction";

[0068] 9. GB / T 30100-2013 Test methods for building wall panels;

[0069] 10. GB / T 7019-2014 Test methods for fiber cement products;

[0070] 11. JGJ 144-2019 Technical Standard for External Wall Thermal Insulation Engineering;

[0071] 12.JG 149-2003 Expanded polystyrene board thin plaster exterior wall insulation system.

[0072] Judgment basis:

[0073] 1. JT / T 646.4-2016 "Highway sound barriers Part 4: Technical requirements and test methods for acoustic materials";

[0074] 2. GB / T23451-2009 "Lightweight partition boards for construction".

[0075] Table 1 80mm thick plate properties

[0076]

[0077]

[0078] Note: The fire performance test project was completed at the Jiaozuo branch site; 3. Weighted sound insulation test piece area: 7.5m 2 .

[0079] Table 2 Sound insulation at different frequencies in 1 / 3 octave band

[0080] Frequency f / Hz 100 125 160 200 250 315 400 500 630 Sound insulation R / dB 32.7 37.9 35.4 33.6 35.5 35.8 36.3 36.9 36.9 Frequency f / Hz 800 1000 1250 1600 2000 2500 3150 4000 5000 Sound insulation R / dB 37.4 39.3 40.0 41.5 42.9 45.1 45.1 44.3 45.7

Claims

1. A process for producing hollow vacuum extrusion molded boards using all industrial solid waste, characterized in that: The following steps are involved: S1. Prepare cementitious materials: Prepare 100 to 300 parts of steel slag of 100 to 800 mesh, 100 to 280 parts of water slag of 100 to 800 mesh, 10 to 30 parts of desulfurized gypsum, 10 to 20 parts of fly ash and 5 to 15 parts of slag powder, and 5 to 15 parts of sodium silicate in a mixer to obtain a cementitious material; S2. Prepare aggregates: Prepare 800-1000 parts by mass of coal gangue with a calorific value of less than 100 kcal and a particle size of less than 5 mm; or 800-1000 parts of desulfurized gypsum, or 800-1000 parts of phosphogypsum, or 800-1000 parts of iron ore; S3. Prepare ingredients: Prepare 30 to 50 parts of fly ash, 10 to 30 parts of slag powder, and 1 to 15 parts of recycled carbon fiber by mass; S4. Molding and curing: The cementitious material prepared in step S1, the aggregate prepared in step S2, and the ingredients prepared in step S3 are all placed in a high-speed mixer, stirred, 120 to 220 parts by weight of water are added and continued to be stirred to form a blank, which is then placed in a mixer for kneading and mixing, and then the blank is sent to a vacuum extruder for extrusion, cut, and steam cured to form a product.

2. A process for producing hollow vacuum extrusion molded boards using all industrial solid waste according to claim 1, characterized in that: In step S1, the steel slag is selected to be 100-800 mesh steel slag, and the water slag is selected to be 100-800 mesh water slag.

3. The process for producing hollow vacuum extrusion molded boards using all industrial solid waste according to claim 1, characterized in that: The stirring speed of the high-speed stirrer in step S4 is 220 r / min.

4. The process for producing hollow vacuum extrusion formed boards using all industrial solid waste according to claim 1, characterized in that: After cutting in step S4, the product is cured by steam at 80°C.

5. A hollow vacuum extrusion molded board produced using all industrial solid waste, characterized in that: Calculated by mass, the raw materials include cementitious materials, aggregates and ingredients, among which the cementitious materials include 100-300 parts of steel slag with a mesh size of 100-800, 100-280 parts of water slag with a mesh size of 100-800, 10-30 parts of desulfurized gypsum, 10-20 parts of fly ash and 5-15 parts of slag powder, and 5-15 parts of sodium silicate; the aggregate is 800-1000 parts of coal gangue with a calorific value below 100 kcal and a particle size of less than 5 mm, or 800-1000 parts of desulfurized gypsum, or 800-1000 parts of phosphogypsum, or 800-1000 parts of iron ore; the ingredients include 30-50 parts of fly ash, 10-30 parts of slag powder, 1-15 parts of carbon fiber recycled from waste, and 120-220 parts of water.