Grouting material and preparation method thereof

By modifying the porous structure and long-chain modification of fly ash and silica fume, combined with the penetration of reinforcement agent, the problems of many gaps and poor stability of the grouting material are solved, and high-strength and high-stability grouting material are achieved .

CN118955080APending Publication Date: 2024-11-15NANJING KK CHEM ENG CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411265056.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

There are many internal gaps and poor stability in grouting materials on the market, resulting in insufficient fluidity and strength.

Method used

Modified fly ash is used to form a porous structure through alkali activation, combining the long-chain modification of silicon fume and the penetration enhancement of reinforcement agents to enhance the chemical-physical composite connection strength and stability of the grouting material.

Benefits of technology

The curing strength and connection stability of the grouting material are significantly improved, and the problems of many gaps and poor stability are solved, so that grouting material with excellent fluidity and high strength can be achieved.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the technical field of grouting, and particularly relates to a grouting material and a preparation method thereof, and the grouting material comprises the following components by mass: 40-60 parts of sand, 15-20 parts of epoxy resin, 25-30 parts of modified fly ash, 10-15 parts of silica fume, 4-8 parts of a reinforcing agent, 3-5 parts of a dispersant, 1-3 parts of a water reducer, 0.1-1 part of a retarder, and 20-30 parts of water. The invention further provides a treatment method of the modified fly ash and the silica fume and a preparation method of the grouting material. The problems of many internal gaps and poor stability of the grouting material are solved, the chemical-physical composite connection strength of the fly ash is effectively improved by utilizing a porous structure and hydration activity brought by the modified fly ash, and the curing strength of the grouting material is improved by matching with the permeation strengthening effect of the reinforcing agent; and the connection stability of the grouting material is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of grouting, and particularly relates to a grouting material and a preparation method thereof. Background Art

[0002] Grouting material is an engineering material with certain fluidity and slight expansion. It is made of high-strength materials as aggregates, cement as binder, and supplemented with construction additives. It has the advantages of good self-flowability, fast hardening speed, high early strength, high strength after hardening, no shrinkage, etc., and the grouting material does not pollute the water quality and the surrounding environment. In terms of construction, grouting materials have the advantages of reliable quality, low cost, short construction period, and easy use. However, there are many types of grouting materials on the market, and they generally have defects such as poor quality stability, poor fluidity, and many internal gaps. Therefore, the market urgently needs a grouting material with excellent fluidity, good stability, and high strength. Summary of the invention

[0003] In view of the problems in the prior art, the present invention provides a grouting material, which solves the problems of many internal gaps and poor stability of the grouting material. The porous structure and hydration activity brought by modified fly ash are utilized to effectively improve the chemical-physical composite connection strength of the fly ash. Combined with the penetration strengthening effect of the reinforcing agent, not only the curing strength of the grouting material is improved, but also the connection stability of the grouting material is improved.

[0004] In order to achieve the above technical objectives, the technical solution of the present invention is: A grouting material, the mass ratio of which is as follows: 40-60 parts of sand, 15-20 parts of epoxy resin, 25-30 parts of modified fly ash, 10-15 parts of silica fume, 4-8 parts of reinforcing agent, 3-5 parts of dispersant, 1-3 parts of water reducer, 0.1-1 parts of retarder, and 20-30 parts of water.

[0005] The modified fly ash adopts alkali-activated porous fly ash; fly ash is an industrial by-product, and has a glassy layer on its surface. The glassy layer is smooth and dense, which brings chemical inertness to the surface of the fly ash. Therefore, the insufficient surface activity of the fly ash is prone to poor impermeability and poor stability. To solve this problem, the modified fly ash adopts surface silicon-aluminum-oxygen composite porous fly ash after alkali activation; a porous structure is formed on the surface of the fly ash, which not only can utilize the porous physical structure of the surface to achieve permeable connection between the fly ash and other materials such as sand, but also the alkali activation brings a stable activity to the inner and outer layers of the fly ash, thereby improving the connection stability. At the same time, the fly ash with a porous surface structure utilizes the characteristics of its own structure and the limited permeability to retain certain hydration groups while the outer layer is porous, fixed and closed, thereby improving the self-activity of the fly ash and playing a key role in the subsequent self-repair and self-sealing. The preparation method of the modified fly ash comprises the following steps: a1, putting fly ash into ethanol and stirring evenly, and wet grinding for 20-30 minutes to obtain a homogeneous slurry, then adding ethanol water solution and stirring for 2-3 hours, filtering and drying to obtain homogeneous fly ash particles, the mass ratio of the fly ash to ethanol is 3:1-2, the stirring speed is 500-800r / min, the pressure of the wet grinding is 0.3-0.5MPa, the temperature is 10-20°C, the volume ratio of the ethanol water solution to the homogeneous slurry is 3-5:1, and the drying temperature is 100-120°C. In this step, the fly ash is refined by wet grinding to form fine powder particles, and the impurities and fine particles in the fly ash are removed by the washing ability of ethanol water to obtain homogeneous fly ash particles, which effectively solves the problem of poor homogeneity of the fly ash particles; a2, adding ethyl cellulose to ether and stirring evenly, and then adding trichloromethylsilane, trichloroethylsilane and trichlorosilane in sequence. a3, placing the homogeneous fly ash particles in a mixture of ethyl cellulose and trichloromethylsilane; a4, placing the homogeneous fly ash particles in a mixture of ethyl cellulose and trichloroethylsilane; a5, placing the homogeneous fly ash particles in a mixture of ethyl cellulose and trichloroethylsilane; a6, placing the homogeneous fly ash particles in a mixture of ethyl cellulose and trichloroethylsilane; a7, placing the homogeneous fly ash particles in a mixture of ethyl cellulose and trichloroethylsilane; a8, placing the homogeneous fly ash particles in a mixture of ethyl cellulose and trichloroethylsilane; a9, placing the homogeneous fly ash particles in a mixture of ethyl cellulose and trichloroethylsilane; The mixed coating liquid is subjected to low-temperature ultrasound for 20-30 minutes, and then the hydrolyzed coated fly ash particles are blown after passing through a sieve, wherein the concentration of the homogenized fly ash particles in the mixed coating liquid is 100-200 g / L, the temperature of the low-temperature ultrasound is 5-10°C, the ultrasonic frequency is 80-100 kHz, the blowing speed is 10-20 g / min, the blowing atmosphere is a mixed atmosphere of nitrogen and water vapor, and the volume ratio of nitrogen to water vapor is 10-12:1, and the temperature is 40-50°C;In this step, the coating liquid is homogenously dispersed on the surface of the fly ash by low-temperature ultrasound, and solid-liquid separation is achieved by sieving, thereby obtaining fly ash particles with a liquid film. During the blowing process, trichloromethylsilane, trichloroethylsilane and trichlorophenylsilane are all hydrolyzed in situ, and the insolubility of ethyl cellulose itself can serve as a barrier to ensure the formation of a porous structure on the surface of the fly ash. In this temperature system, the silane product after in-situ hydrolysis forms a porous framework structure based on the condensation reaction of hydroxyl groups, and the surface of the framework structure contains methyl, ethyl and phenyl groups; a4, the hydrolyzed coated fly ash particles are placed in ether and subjected to low-temperature ultrasound for 20-40 minutes, filtered and dried, and then immersed in hydroxide The mixture is rapidly stirred in a sodium solution for 5-10 minutes, taken out and freeze-dried to obtain alkali-activated fly ash particles, wherein the concentration of the hydrolyzed coated fly ash particles in ether is 200-300 g / L, the temperature of low-temperature ultrasound is 10-20°C, the ultrasonic frequency is 80-100 kHz, and the temperature of filtration and drying is 40-50°C; the pH value of the sodium hydroxide solution is 8-9, and the temperature of freeze-drying is -20°C; in this step, the ethyl cellulose on the hydrolyzed coated fly ash particles is dissolved and removed by utilizing the solubility of ether in ethyl cellulose, and fly ash particles with a surface silicon-oxygen porous structure are obtained after filtration and drying; during the rapid stirring process, the sodium hydroxide solution enters into the fly ash particles. , not only activates the silicon-oxygen structure on the surface, but also destroys the inert glass layer on the surface of the fly ash, thereby realizing the hydration activity of the fly ash itself in the fly ash particles; freeze drying can realize in-situ water removal and retain the surface hydration activity of the fly ash itself; a5, add aluminum isopropoxide and ethyl cellulose to ethanol and stir evenly, then add alkali to activate the fly ash particles and stir for 3-5 minutes, take out and dry, let it stand for 20-40 minutes, sinter and ultraviolet light to obtain modified fly ash particles, the mass ratio of aluminum isopropoxide to ethyl cellulose is 1:1-1.5, the concentration of aluminum isopropoxide in the ethanol solution is 50-80g / L, the drying temperature is 80-90°C, and the standing atmosphere is nitrogen A mixed atmosphere with water vapor, wherein the volume ratio of nitrogen to water vapor is 7-9:1, and the temperature is 40-50°C; the sintering temperature is 200-230°C; this step utilizes the solubility of ethanol in aluminum isopropoxide and ethyl cellulose to form a coating liquid, and forms a liquid film on the porous framework of the surface of the fly ash particles by stirring for a short time. Based on the operation of low concentration and short stirring time, the liquid film slightly penetrates into the porous structure and cannot reach the fly ash body; during the standing process, aluminum isopropoxide is hydrolyzed in situ to form aluminum hydroxide, and the aluminum hydroxide is reacted to form aluminum oxide through sintering, and the ethyl cellulose is decomposed under the treatment of sintering and ultraviolet light to obtain fly ash particles with a porous surface structure;The porous fly ash particles prepared by this process have a porous structure on the surface, and the porous structure contains silicon-oxygen active and aluminum-oxygen active structures. The surface of the fly ash body inside contains hydration activity. Therefore, in the grouting material, the modified fly ash shows excellent hydration activity and physical fixation, which improves the connection strength of the fly ash and ensures the strength stability of the grouting material. The silicon-oxygen structure on the surface of the modified fly ash contains a large number of short side chains (ethyl and methyl) and benzene rings, which can form a rough silicon-oxygen framework surface, and form permeable tentacles after solidification, providing friction and improving the solidification stability. At the same time, based on the porous structure of the modified fly ash, the support structure of the silicon-oxygen system and the surface division of the aluminum-oxygen system improve the connection specific surface and physical clamping effect of the porous structure, and the hydration activity residue on the loose structure of the fly ash body surface is achieved. ;

[0006] The silica fume is modified with long-chain silane before use. The silica fume is also called microsilica powder. It is collected and processed by a special capture device during the high-temperature smelting of industrial silicon and ferrosilicon in an industrial electric furnace. The smoke that escapes with the exhaust gas is collected and processed by a special capture device. However, microsilica powder itself has a certain inertia and is not easy to react with other substances. It forms particle interface gaps in the grouting material, which reduces the durability of the grouting material. The long-chain silane modification can form a stable long-chain structure on the surface of the silica fume. The long-chain structure can produce long arms with a tensile fixing effect on the surface of the microsilica powder, ensuring its connection stability in the grouting material, and the outer end of the long chain has good permeability, which can fill the gaps in the grouting material. That is, the long-chain silane-modified silica fume not only utilizes the long-chain permeability and the freeness of the outer end to form physical fixation while achieving dense gap filling, but also the silica fume itself has a very small particle size, permeability and stability, which can also improve the density of the grouting material. The preparation method of long-chain silane-modified silica ash comprises the following steps: b1, adding silica ash to ethanol for ultrasonic dispersion, then adding an acid solution and continuing ultrasonic treatment for 3-4 hours, filtering to obtain acid-modified silica ash; the mass ratio of silica ash to ethanol is 1:5-7, the ultrasonic frequency of ultrasonic dispersion is 70-90kHz, the temperature is 30-50°C, the acid solution is a sulfuric acid solution with a pH of 4-5, and the volume ratio of ethanol to the acid solution is 1:1-1.2. In this step, silica ash is dispersed in ethanol to form a suspension, and surface treatment is formed when the acid solution is added, thereby reducing the difficulty of dispersing silica ash; b2, hexadecylmethyldimethoxysilane is added to ether and stirred evenly, then the acid-modified silica ash is placed in ultrasonic treatment for 20-40 minutes, and distilled water is slowly added, filtered, and then soaked for a second time for 10-20 minutes, and long-chain silane-modified silica ash is obtained by spraying. The concentration is 5-10g / L, the stirring speed is 300-500r / min, the mass ratio of acid-modified silica fume to hexadecylmethyldimethoxysilane is 4-5:1, the temperature of the ultrasound is 5-10°C, the ultrasonic frequency is 80-100kHz, the dripping speed is 0.1-0.4mL / min, and the molar ratio of distilled water to hexadecylmethyldimethoxysilane is 2.2-2.5:1, the secondary immersion uses ether, the spraying speed is 20-30mL / min, and the temperature is 60-80°C; this step utilizes the solubility of hexadecylmethyldimethoxysilane in ether to form a dispersed solution, and after the silica fume and distilled water are added, the hexadecylmethyldimethoxysilane is hydrolyzed and reacts with the active hydroxyl groups on the silica fume, thereby fixing the hexadecylmethyldimethoxysilane on the silica fume, thereby realizing the long-chain modification of the silica fume surface.

[0007] The reinforcing agent is silica sol, and the solid content of silica sol is 20-30%. Silica sol is a water sol of silicon dioxide, and the silicon dioxide particles are fine and have good permeability. They can penetrate into the grouting material through capillary action to improve the overall density, that is, the silica sol has good dispersibility; the silicon dioxide in the silica sol has high activity and is rich in silicon hydroxyl structure. After it penetrates into the grouting material, it forms an active origin and forms a stable and dense connection with materials such as fly ash, thereby achieving the effect of reinforcing the performance of concrete.

[0008] The dispersant is polyvinyl alcohol, which has good adhesion and can improve the bonding strength of the grouting material. At the same time, the material can also improve the fluidity of modified fly ash, silica fume and reinforcing agent, ensure the flow and penetration of low-size particles in the whole system, and improve the overall density.

[0009] The water reducer is a polycarboxylic acid water reducer purchased from Jiangsu Bosite Chemical Technology Co., Ltd.

[0010] The retarder is one of sodium citrate, sodium borate, sodium tartrate and sodium gluconate.

[0011] The preparation method of the grouting material comprises the following steps: Step 1, putting sand, epoxy resin, modified fly ash, silica fume and reinforcing agent into a mixer and stirring evenly for 5-10 minutes to form a mixture; Step 2, adding dispersant, water reducing agent and retarder to water and stirring evenly for 3-5 minutes to form a mixed solution; Step 3, adding the mixed solution into the mixture and stirring for 3-5 minutes to obtain grouting material.

[0012] It can be seen from the above description that the present invention has the following advantages: 1. The present invention solves the problem of many internal gaps and poor stability of the grouting material. The porous structure and hydration activity brought by the modified fly ash are utilized to effectively improve the chemical-physical composite connection strength of the fly ash. Combined with the penetration strengthening effect of the reinforcing agent, not only the curing strength of the grouting material is improved, but also the connection stability of the grouting material is improved.

[0013] 2. The present invention utilizes the surface porosification and alkali modification treatment of fly ash, which not only forms a permeable fixed connection system in the physical structure, but also the silica-alumina activity on the porous framework and the hydration activity of the internal fly ash body after alkali modification, thereby forming a stable solidification of the fly ash in the grouting material.

[0014] 3. The present invention utilizes the surface modification of silica fume to achieve the change of the surface activity of silica fume, and cooperates with the long-chain extension structure of silane to improve the surface reaction inertness of silica fume itself, thereby realizing the use of silica fume in high-strength and high-durability grouting materials. DETAILED DESCRIPTION

[0015] The present invention is described in detail with reference to the embodiments, but no limitation is imposed on the claims of the present invention. Example 1

[0016] A grouting material, the mass ratio of which is as follows: 40 parts of sand, 15 parts of epoxy resin, 25 parts of modified fly ash, 10 parts of silica fume, 4 parts of reinforcing agent, 3 parts of dispersant, 1 part of water reducer, 0.1 parts of retarder, and 20 parts of water.

[0017] The modified fly ash adopts alkali-activated porous fly ash; and the modified fly ash adopts surface silica-alumina composite porous fly ash after alkali activation; the preparation method of the modified fly ash comprises the following steps: a1, putting fly ash into ethanol and stirring evenly, and wet grinding for 20 minutes to obtain a homogeneous slurry, and then adding ethanol aqueous solution and stirring for 2 hours, filtering and drying to obtain homogeneous fly ash particles, the mass ratio of the fly ash to ethanol is 3:1, the stirring speed is 500r / min, the pressure of the wet grinding is 0.3MPa, the temperature is 10°C, the volume ratio of the ethanol aqueous solution to the homogeneous slurry is 3:1, and the drying is carried out. The drying temperature is 100°C; a2, ethyl cellulose is added to ether and stirred evenly, and then trichloromethylsilane, trichloroethylsilane and trichlorophenylsilane are added in sequence to obtain a mixed coating solution, wherein the concentration of ethyl cellulose in ether is 200g / L, the molar ratio of trichloromethylsilane, trichloroethylsilane and trichlorophenylsilane is 3:1:1, and the mass ratio of trichloromethylsilane to ethyl cellulose is 1:3; a3, homogeneous fly ash particles are placed in the mixed coating solution and ultrasonicated at low temperature for 20 minutes, and then blown through a sieve to obtain hydrolyzed coated fly ash particles, and the concentration of the homogeneous fly ash particles in the mixed coating solution is 100 g / L, the temperature of low-temperature ultrasound is 5°C, the ultrasonic frequency is 80kHz, the blowing speed is 10g / min, the blowing atmosphere is a mixed atmosphere of nitrogen and water vapor, and the volume ratio of nitrogen to water vapor is 10:1, and the temperature is 40°C; a4, the hydrolyzed coated fly ash particles are placed in ether and subjected to low-temperature ultrasound for 20 minutes, filtered and dried, and then immersed in a sodium hydroxide solution and rapidly stirred for 5 minutes, taken out and freeze-dried to obtain alkali-activated fly ash particles, wherein the concentration of the hydrolyzed coated fly ash particles in ether is 200g / L, the temperature of low-temperature ultrasound is 10°C, the ultrasonic frequency is 80kHz, the temperature of filtration and drying is 4 0℃; the pH value of the sodium hydroxide solution is 8, and the freeze-drying temperature is -20℃; a5, adding aluminum isopropoxide and ethyl cellulose to ethanol and stirring evenly, then adding alkali-activated fly ash particles and stirring for 3 minutes, taking out and drying and standing for 20 minutes, sintering and ultraviolet light to obtain modified fly ash particles, the mass ratio of aluminum isopropoxide to ethyl cellulose is 1:1, the concentration of aluminum isopropoxide in the ethanol solution is 50g / L, the drying temperature is 80℃, the standing atmosphere is a mixed atmosphere of nitrogen and water vapor, and the volume ratio of nitrogen to water vapor is 7:1, and the temperature is 40℃; the sintering temperature is 200℃.

[0018] The silica ash is modified with long-chain silane before use. The preparation method of the long-chain silane-modified silica ash comprises the following steps: b1, adding silica ash to ethanol for ultrasonic dispersion, then adding acid solution and continuing ultrasonic treatment for 3 hours, filtering to obtain acid-modified silica ash; the mass ratio of silica ash to ethanol is 1:5, the ultrasonic frequency of ultrasonic dispersion is 70kHz, the temperature is 30°C, the acid solution is a sulfuric acid solution with a pH of 4, and the volume ratio of ethanol to the acid solution is 1:1; b2, adding hexadecylmethyldimethoxysilane to ether and stirring evenly, then putting in acid-modified silica ash for ultrasonic treatment for 20 minutes, and slowly adding distilled water, filtering and then distilling for 2 hours. The mixture was immersed for 10 minutes, and long-chain silane-modified silica ash was obtained by spraying. The concentration of hexadecylmethyldimethoxysilane in ether was 5g / L, the stirring speed was 300r / min, the mass ratio of acid-modified silica ash to hexadecylmethyldimethoxysilane was 4:1, the temperature of the ultrasound was 5°C, the frequency of the ultrasound was 80kHz, the speed of the dripping was 0.1mL / min, and the molar ratio of distilled water to hexadecylmethyldimethoxysilane was 2.2:1. Ether was used for the second immersion, the spraying speed was 20mL / min, and the temperature was 60°C.

[0019] The reinforcing agent is silica sol, and the solid content of the silica sol is 20%.

[0020] The dispersant is polyvinyl alcohol.

[0021] The water reducer is a polycarboxylic acid water reducer purchased from Jiangsu Bosite Chemical Technology Co., Ltd.

[0022] The retarder is sodium citrate.

[0023] The preparation method of the grouting material comprises the following steps: Step 1, putting sand, epoxy resin, modified fly ash, silica fume and reinforcing agent into a mixer and stirring evenly for 5 minutes to form a mixture; Step 2, adding the dispersant, water reducing agent and retarder into water and stirring evenly for 3 minutes to form a mixed solution; Step 3, adding the mixed solution into the mixture and stirring for 3 minutes to obtain the grouting material. Example 2

[0024] A grouting material, the mass ratio of which is as follows: 60 parts of sand, 20 parts of epoxy resin, 30 parts of modified fly ash, 15 parts of silica fume, 8 parts of reinforcing agent, 5 parts of dispersant, 3 parts of water reducer, 1 part of retarder, and 30 parts of water.

[0025] The modified fly ash adopts alkali-activated porous fly ash; and the modified fly ash adopts surface silica-alumina composite porous fly ash after alkali activation; the preparation method of the modified fly ash comprises the following steps: a1, putting the fly ash into ethanol and stirring evenly, and wet grinding for 30 minutes to obtain a homogeneous slurry, and then adding ethanol aqueous solution and stirring for 3 hours, filtering and drying to obtain homogeneous fly ash particles, the mass ratio of the fly ash to ethanol is 3:2, the stirring speed is 800r / min, the pressure of the wet grinding is 0.5MPa, the temperature is 20°C, the volume ratio of the ethanol aqueous solution to the homogeneous slurry is 5:1, and the drying is carried out. The temperature is 120°C; a2, ethyl cellulose is added to ether and stirred evenly, and then trichloromethylsilane, trichloroethylsilane and trichlorophenylsilane are added in sequence to obtain a mixed plating solution, wherein the concentration of the ethyl cellulose in the ether is 300 g / L, the molar ratio of the trichloromethylsilane, trichloroethylsilane and trichlorophenylsilane is 3:1:2, and the mass ratio of the trichloromethylsilane to the ethyl cellulose is 1:4; a3, homogeneous fly ash particles are placed in the mixed plating solution and subjected to low-temperature ultrasound for 30 minutes, and then blown through a sieve to obtain hydrolyzed coated fly ash particles, and the concentration of the homogeneous fly ash particles in the mixed plating solution is 200 g / L , the temperature of low-temperature ultrasound is 10°C, the ultrasonic frequency is 100kHz, the blowing speed is 20g / min, the blowing atmosphere is a mixed atmosphere of nitrogen and water vapor, and the volume ratio of nitrogen to water vapor is 12:1, and the temperature is 50°C; a4, the hydrolyzed coated fly ash particles are placed in ether and low-temperature ultrasound is performed for 40 minutes, filtered and dried, and then immersed in a sodium hydroxide solution and rapidly stirred for 10 minutes, taken out and freeze-dried to obtain alkali-activated fly ash particles, the concentration of the hydrolyzed coated fly ash particles in ether is 300g / L, the temperature of low-temperature ultrasound is 20°C, the ultrasonic frequency is 100kHz, the temperature of filtration and drying is 50 ℃; the pH value of the sodium hydroxide solution is 9, and the freeze-drying temperature is -20℃; a5, adding aluminum isopropoxide and ethyl cellulose to ethanol and stirring evenly, then adding alkali-activated fly ash particles and stirring for 5 minutes, taking out and drying and standing for 40 minutes, sintering and ultraviolet light to obtain modified fly ash particles, the mass ratio of aluminum isopropoxide to ethyl cellulose is 1:1.5, the concentration of aluminum isopropoxide in the ethanol solution is 80g / L, the drying temperature is 90℃, the standing atmosphere is a mixed atmosphere of nitrogen and water vapor, and the volume ratio of nitrogen to water vapor is 9:1, and the temperature is 50℃; the sintering temperature is 230℃.

[0026] The silica ash is modified with long-chain silane before use. The preparation method of the long-chain silane-modified silica ash comprises the following steps: b1, adding silica ash to ethanol for ultrasonic dispersion, then adding acid solution and continuing ultrasonic treatment for 4 hours, filtering to obtain acid-modified silica ash; the mass ratio of silica ash to ethanol is 1:7, the ultrasonic frequency of ultrasonic dispersion is 90kHz, the temperature is 50°C, the acid solution is a sulfuric acid solution with a pH of 5, and the volume ratio of ethanol to acid solution is 1:1.2; b2, adding hexadecylmethyldimethoxysilane to ether and stirring evenly, then putting in acid-modified silica ash for ultrasonic treatment for 40 minutes, and slowly adding distilled water, filtering and then re-cleaning. Soak for 20 minutes and obtain long-chain silane-modified silica ash by spraying. The concentration of hexadecylmethyldimethoxysilane in ether is 10 g / L, the stirring speed is 500 r / min, the mass ratio of acid-modified silica ash to hexadecylmethyldimethoxysilane is 5:1, the temperature of the ultrasound is 10°C, the ultrasonic frequency is 100 kHz, the dropping speed is 0.4 mL / min, and the molar ratio of distilled water to hexadecylmethyldimethoxysilane is 2.5:1. Ether is used for the secondary soaking, the spraying speed is 30 mL / min, and the temperature is 80°C.

[0027] The reinforcing agent is silica sol, and the solid content of the silica sol is 30%.

[0028] The dispersant is polyvinyl alcohol.

[0029] The water reducer is a polycarboxylic acid water reducer purchased from Jiangsu Bosite Chemical Technology Co., Ltd.

[0030] The retarder is sodium borate.

[0031] The preparation method of the grouting material comprises the following steps: Step 1, putting sand, epoxy resin, modified fly ash, silica fume and reinforcing agent into a mixer and stirring evenly for 10 minutes to form a mixture; Step 2, adding the dispersant, water reducing agent and retarder to water and stirring evenly for 5 minutes to form a mixed solution; Step 3, adding the mixed solution into the mixture and stirring for 5 minutes to obtain a grouting material. Example 3

[0032] A grouting material, the mass ratio of which is as follows: 50 parts of sand, 18 parts of epoxy resin, 28 parts of modified fly ash, 13 parts of silica fume, 6 parts of reinforcing agent, 4 parts of dispersant, 2 parts of water reducer, 0.6 parts of retarder, and 25 parts of water.

[0033] The modified fly ash adopts alkali-activated porous fly ash; and the modified fly ash adopts surface silica-alumina composite porous fly ash after alkali activation; the preparation method of the modified fly ash comprises the following steps: a1, putting fly ash into ethanol and stirring evenly, and wet grinding for 25 minutes to obtain a homogeneous slurry, and then adding ethanol aqueous solution and stirring for 3 hours, filtering and drying to obtain homogeneous fly ash particles, the mass ratio of the fly ash to ethanol is 3:2, the stirring speed is 700r / min, the pressure of the wet grinding is 0.4MPa, the temperature is 15°C, the volume ratio of the ethanol aqueous solution to the homogeneous slurry is 4:1, and the drying is carried out. The temperature is 110°C; a2, ethyl cellulose is added to ether and stirred evenly, and then trichloromethylsilane, trichloroethylsilane and trichlorophenylsilane are added in sequence to obtain a mixed coating solution, wherein the concentration of the ethyl cellulose in the ether is 200-300 g / L, the molar ratio of the trichloromethylsilane, trichloroethylsilane and trichlorophenylsilane is 3:1:1, and the mass ratio of the trichloromethylsilane to the ethyl cellulose is 1:4; a3, homogeneous fly ash particles are placed in the mixed coating solution and subjected to low-temperature ultrasound for 25 minutes, and then blown through a sieve to obtain hydrolyzed coated fly ash particles, wherein the concentration of the homogeneous fly ash particles in the mixed coating solution is 15 0g / L, the temperature of low-temperature ultrasound is 8°C, the ultrasonic frequency is 90kHz, the blowing speed is 15g / min, the blowing atmosphere is a mixed atmosphere of nitrogen and water vapor, and the volume ratio of nitrogen to water vapor is 11:1, and the temperature is 45°C; a4, the hydrolyzed coated fly ash particles are placed in ether and subjected to low-temperature ultrasound for 30min, filtered and dried, and then immersed in a sodium hydroxide solution and rapidly stirred for 8min, taken out and freeze-dried to obtain alkali-activated fly ash particles, wherein the concentration of the hydrolyzed coated fly ash particles in ether is 250g / L, the temperature of low-temperature ultrasound is 15°C, the ultrasonic frequency is 90kHz, the temperature of filtration and drying is 45 ℃; the pH value of the sodium hydroxide solution is 9, and the freeze-drying temperature is -20℃; a5, adding aluminum isopropoxide and ethyl cellulose to ethanol and stirring evenly, then adding alkali-activated fly ash particles and stirring for 4 minutes, taking out and drying and standing for 30 minutes, sintering and ultraviolet light to obtain modified fly ash particles, the mass ratio of aluminum isopropoxide to ethyl cellulose is 1:1.3, the concentration of aluminum isopropoxide in the ethanol solution is 70g / L, the drying temperature is 85℃, the standing atmosphere is a mixed atmosphere of nitrogen and water vapor, and the volume ratio of nitrogen to water vapor is 8:1, and the temperature is 45℃; the sintering temperature is 220℃.

[0034] The silica ash is modified with long-chain silane before use. The preparation method of the long-chain silane-modified silica ash includes the following steps: b1, adding silica ash to ethanol for ultrasonic dispersion, then adding acid solution and continuing ultrasonic treatment for 4 hours, filtering to obtain acid-modified silica ash; the mass ratio of silica ash to ethanol is 1:6, the ultrasonic frequency of ultrasonic dispersion is 80kHz, the temperature is 40°C, the acid solution is a sulfuric acid solution with a pH of 5, and the volume ratio of ethanol to acid solution is 1:1.1; b2, adding hexadecylmethyldimethoxysilane to ether and stirring evenly, then putting in acid-modified silica ash for ultrasonic treatment for 30 minutes, and slowly adding distilled water, filtering and then The secondary immersion was carried out for 15 minutes, and long-chain silane-modified silica ash was obtained by spraying. The concentration of hexadecylmethyldimethoxysilane in ether was 8 g / L, the stirring speed was 400 r / min, the mass ratio of acid-modified silica ash to hexadecylmethyldimethoxysilane was 5:1, the temperature of the ultrasound was 8°C, the ultrasonic frequency was 90 kHz, the dropping speed was 0.3 mL / min, and the molar ratio of distilled water to hexadecylmethyldimethoxysilane was 2.4:1. Ether was used for the secondary immersion, the spraying speed was 25 mL / min, and the temperature was 70°C.

[0035] The reinforcing agent is silica sol, and the solid content of the silica sol is 25%.

[0036] The dispersant is polyvinyl alcohol.

[0037] The water reducer is a polycarboxylic acid water reducer purchased from Jiangsu Bosite Chemical Technology Co., Ltd.

[0038] The retarder is sodium gluconate.

[0039] The preparation method of the grouting material comprises the following steps: Step 1, putting sand, epoxy resin, modified fly ash, silica fume and reinforcing agent into a mixer and stirring evenly for 8 minutes to form a mixture; Step 2, adding the dispersant, water reducing agent and retarder to water and stirring evenly for 4 minutes to form a mixed solution; Step 3, adding the mixed solution into the mixture and stirring for 4 minutes to obtain a grouting material.

[0040] Comparative Example 1 The formula and preparation method of Comparative Example 1 are the same as those of Example 3, except that the silica fume used in Comparative Example 1 is not modified with long-chain silane.

[0041] Comparative Example 2 The formula and preparation method of Comparative Example 2 are the same as those of Example 3, except that the fly ash used in Comparative Example 2 is not modified.

[0042] Comparative Example 3 The formula and preparation method of Comparative Example 3 are the same as those of Comparative Example 1, except that the fly ash in Comparative Example 2 is not modified, but only wet ground and cleaned to obtain homogeneous fly ash particles.

[0043] Comparative Example 4 Comparative Example 4 uses commercially available grouting materials purchased from: a certain material company in Nanjing.

[0044] Performance Testing The grouting materials of Examples 1-3 and Comparative Examples 1-4 were used as test samples to carry out the following tests: Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Layering none none none none none none none Compressive strength MPa (7d) 104 106 104 101 100 87 80 Flexural strength MPa (7d) 30 31 30 28 26 24 21 Compression elastic modulus GPa 16 17 17 16 16 16 16 Linear shrinkage% 0.003 0.002 0.003 0.005 0.005 0.006 0.007 Exothermic temperature peak ℃ 33 31 33 35 36 39 41 It is understood that the above specific description of the present invention is only used to illustrate the present invention and is not limited to the technical solutions described in the embodiments of the present invention. Those skilled in the art should understand that the present invention can still be modified or replaced by equivalents to achieve the same technical effects; as long as the use requirements are met, they are within the protection scope of the present invention.

Claims

1. A grouting material, Features: The quality ratio is as follows: 40-60 parts of sand, 15-20 parts of epoxy resin, 25-30 parts of modified fly ash, 10-15 parts of silica fume, 4-8 parts of reinforcing agent, 3-5 parts of dispersant, 1-3 parts of water reducer, 0.1-1 parts of retarder, and 20-30 parts of water.

2. The grouting material according to claim 1, Features: The modified fly ash adopts alkali-activated porous fly ash.

3. The grouting material according to claim 2, Features: The modified fly ash adopts surface silica-alumina composite porous fly ash activated by alkali.

4. The grouting material according to claim 1, Features: The silica fume is modified with long-chain silane before use.

5. The grouting material according to claim 1, Features: The reinforcing agent is silica sol, and the solid content of the silica sol is 20-30%.

6. The grouting material according to claim 1, Features: The dispersant is polyvinyl alcohol.

7. The grouting material according to claim 1, Features: The water reducer is a polycarboxylic acid water reducer purchased from Jiangsu Bost Chemical Technology Co., Ltd.

8. The grouting material according to claim 1, Features: The retarder is one of sodium citrate, sodium borate, sodium tartrate and sodium gluconate.

9. The grouting material according to claim 1, Features: The preparation method of the grouting material comprises the following steps: Step 1, putting sand, epoxy resin, modified fly ash, silica fume and reinforcing agent into a mixer and stirring evenly for 5-10 minutes to form a mixture; Step 2, adding dispersant, water reducing agent and retarder to water and stirring evenly for 3-5 minutes to form a mixed solution; Step 3, adding the mixed solution into the mixture and stirring for 3-5 minutes to obtain grouting material.