High-strength graphitized cathode carbon block and manufacturing method thereof

By using modified asphalt, calcined petroleum coke and other components and specific processes in graphitized cathode carbon blocks, the strength and electrical properties of the carbon blocks are improved, the problem of insufficient strength of the existing graphitized cathode is solved, and the electrolytic cell is extended Service life and reduce wear rate.

CN118955138APending Publication Date: 2024-11-15SHANXI LIANGYU CARBON CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411086954.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The strength of the existing graphitized cathode is low, resulting in a large mechanical wear rate in the electrolytic cell, which seriously affects the service life of the electrolytic cell and is difficult to meet the needs of high-quality graphitized cathode carbon blocks.

Method used

The overall strength of the carbon block is improved by using modified asphalt, calcined petroleum coke, silicon carbide, metal powder titanium and alumina through double-layer mixing, ball milling, CNC hydraulic molding, segmented roasting and high-pressure impregnation. Mechanical properties.

Benefits of technology

The strength and yield of the cathode carbon block are significantly improved, the wear rate is reduced, the service life of the electrolytic cell is extended, and the resistivity is reduced and electrical performance is improved by the combination of modified bitumen and metal powder titanium.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955138A_ABST
    Figure CN118955138A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of cathode carbon block manufacturing, and discloses a high-strength graphitized cathode carbon block and a manufacturing method thereof, the high-strength graphitized cathode carbon block comprises the following raw material components by weight: 23-24% of modified asphalt; 86-87% of calcined petroleum coke; 1-5% of silicon carbide; 0.5-3% of metal powder titanium; 1-5% of alumina; the modified asphalt is modified asphalt. According to the high-strength graphitized cathode carbon block and the manufacturing method thereof, the mechanical property of a finished product obtained through the two-time roasting and impregnation process step is effectively improved, the strength of the carbon block is improved, the abrasion rate of the carbon block in the using process is reduced, the service life of an electrolytic bath is prolonged, meanwhile, the carbon block is impregnated through an impregnant, pores are filled, and the service life of the electrolytic bath is prolonged. The aluminum oxide added into the raw material of the cathode carbon block can react with carbon to form an aluminum-carbon compound, so that the strength and the stability of the carbon material are enhanced, and the metal powder titanium added into the raw material of the carbon block can form a good conductive network with the carbon in the high-temperature roasting process, so that the resistivity is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of cathode carbon block manufacturing, in particular to a high-strength graphitized cathode carbon block and a manufacturing method thereof. Background Art

[0002] With the in-depth development of electrolytic aluminum towards large prebaked cells, graphitized cathodes have become a commonly used material for large prebaked cells internationally. Since graphitized cathodes have the advantages of small cathode voltage drop, excellent thermal conductivity, and superior resistance to sodium corrosion during the electrolytic production process, many old electrolytic cells in production are being replaced with graphitized cathode carbon blocks as a substitute during the overhaul process, in order to achieve the purpose of increasing current, increasing production and increasing efficiency.

[0003] However, the common graphitized cathodes currently used have a relatively low strength, which results in a high mechanical wear rate in the electrolytic cell, which is about twice that of graphite cathode carbon blocks. This seriously affects the service life of the electrolytic cell and makes it difficult to meet the current demand for high-quality graphitized cathode carbon blocks in electrolytic aluminum.

[0004] In view of the above problems, it is urgently necessary to carry out innovative design based on the original high-strength graphitized cathode carbon block. Summary of the invention

[0005] The purpose of the present invention is to provide a high-strength graphitized cathode carbon block and a method for manufacturing the same, so as to solve the problem mentioned in the above background technology that ordinary graphitized cathodes have a high mechanical wear rate in the electrolytic cell due to their low strength, which seriously affects the service life of the electrolytic cell and is difficult to meet the current demand for high-quality graphitized cathode carbon blocks in electrolytic aluminum.

[0006] To achieve the above object, the present invention provides the following technical solution: a high-strength graphitized cathode carbon block, comprising the following raw material components in percentage by weight:

[0007] Among them, modified asphalt 23-24%;

[0008] Calcined petroleum coke 86-87%;

[0009] Silicon carbide 1-5%;

[0010] Metal powder titanium 0.5-3%;

[0011] Alumina 1-5%.

[0012] The above technical solution can effectively improve the overall strength of the carbon block and reduce the wear rate of the carbon block.

[0013] Preferably, the particle size composition of the calcined petroleum coke is as follows by weight percentage:

[0014] 6-3mm15-20%;

[0015] 3-1mm17-22%;

[0016] 0-1mm20-25%;

[0017] Powder coke 35-40%.

[0018] By adopting the above technical solution, the strength of the carbon block is increased, and the carbon block has better deformation ability and the fracture sensitivity is reduced.

[0019] Preferably, the calcined petroleum coke in the graphitized cathode carbon block does not include the calcined petroleum coke raw material component of the dry material in the modified asphalt.

[0020] By adopting the above technical solution, the components in the graphitized cathode carbon block can be accurately processed, so as to facilitate the maintenance of standards and efficient production during production.

[0021] A method for manufacturing a high-strength graphitized cathode carbon block, which is applied to the production of the above-mentioned graphitized cathode carbon block, comprises the following process steps:

[0022] S1. A portion of the calcined petroleum coke is sieved by a vibrating screen into 8-4 mm, 4-1 mm and 1-0 mm, wherein the purity of 8-4 mm and 4-1 mm is controlled to be above 85%, and the purity of 1-0 mm is not controlled, and the remaining portion is ground into fine powder by a ball mill to obtain powdered coke;

[0023] S2. The calcined petroleum cokes and powdered cokes obtained in S1 are preheated and dry-mixed in the upper layer of a double-layer kneading pot according to the formula, and the temperature is heated to 130-150°C to obtain dry carbon blocks. The heated dry materials and metal powders of titanium, silicon carbide and aluminum oxide are then put into the lower layer of the double-layer kneading pot, and modified asphalt is added for wet mixing. The paste temperature at the end of wet mixing is controlled at 170-180°C;

[0024] S3. The paste out of the pot in S2 is sent to the temperature-averaging pot through a belt conveyor for cooling, so that the paste temperature is reduced to 150-160 ℃, and the cooled paste is obtained;

[0025] S4. The cooled paste in S3 is placed in a mobile hopper scale for weighing. The weight control standard is the unit weight of the green block, and is sent to a high-precision mold of a CNC hydraulic molding machine, and a pressure of 250-350MPa is applied for 15-25 minutes to ensure the density uniformity and dimensional accuracy of the cathode carbon block green body;

[0026] S5. The green body obtained in S4 is sent to a cooling water pool by a catenary conveyor and cooled to room temperature, and then hoisted and sent to a green block warehouse stack for inspection;

[0027] S6. The green blocks that have passed the inspection are loaded into the roasting furnace through the overhead crane for roasting. The roasting adopts an 80-82 hour cycle curve, and the temperature is steadily increased to 900-1100°C at a heating rate of 4-8°C / h, and the temperature is kept constant for 25-35 hours. The final carbon block temperature reaches 1000-1050°C, and the insulation time is 20-40 hours;

[0028] S7. The qualified calcined blocks are loaded into the graphitization furnace through the overhead crane for graphitization, during which the temperature is raised in stages, the first stage is 1000-1800°C, the second stage is 1800-3000°C for heating, and the graphitization power supply time is 20-22 hours;

[0029] S8. The graphitized blocks that have passed the inspection are subjected to high-pressure impregnation treatment, with an impregnation pressure of 1.5-1.6Mpa and a holding time of 3-4h to ensure that the impregnation is sufficient and the pores are filled;

[0030] S9. The qualified impregnated blocks are loaded into the roasting furnace through the overhead crane for secondary roasting. The roasting cycle curve is 30-32h, and the final carbon block temperature reaches 8500-900°C, and the insulation time is 10-20 hours;

[0031] S10. Process the qualified secondary calcined blocks according to the finished cathode processing drawings to obtain high-strength graphitized cathode carbon blocks.

[0032] The above technical solution is adopted to effectively improve the strength of cathode carbon block preparation and effectively improve the yield of finished products.

[0033] Preferably, the calcined petroleum coke in S1 is low-sulfur calcined petroleum coke having a sulfur content of less than 0.5%.

[0034] By adopting the above technical solution, the harm of sulfur to the environment and the risk of product cracking during the graphitization process are reduced.

[0035] Preferably, the roasting furnaces in S6 and S9 adopt segmented temperature control technology and a uniform airflow circulation system to ensure uniform temperature distribution during the roasting process and reduce internal stress.

[0036] The above technical solution is adopted to provide a stable roasting space for the internal environment of the roasting furnace and maintain uniform temperature.

[0037] Preferably, the roasting furnace in S6 and S9 is an open ring roasting furnace.

[0038] By adopting the above technical solution, the cathode carbon block can be subjected to secondary calcination to improve the strength of the carbon block.

[0039] Preferably, the graphitization furnace in S8 is an internal heat series graphitization furnace.

[0040] The above technical solution is used to achieve stable temperature control of the impregnated carbon blocks.

[0041] Compared with the prior art, the invention has the following beneficial effects: the high-strength graphitized cathode carbon block and its manufacturing method:

[0042] 1. The mechanical properties of the finished product obtained by the two roasting and impregnation process steps are effectively improved, so that the strength of the carbon block is greatly improved, and the wear rate of the carbon block during use is reduced, which is beneficial to extend the life of the electrolytic cell. At the same time, the carbon block is impregnated with an impregnating agent to fill the pores. Adding alumina to the cathode carbon block raw material can react with carbon to form aluminum-carbon compounds, thereby enhancing the strength and stability of the carbon material;

[0043] 2. The metal powder titanium added to the carbon block raw material can form a good conductive network with carbon during high-temperature roasting, reduce the resistivity, and achieve a lower resistivity in electrical performance, reduce the cathode voltage drop, and achieve better energy saving and consumption reduction. At the same time, the carbon block is bonded as a whole by internal modified asphalt, so that the carbon block has better deformation ability and reduces the fracture sensitivity of the carbon block. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1 It is a schematic diagram of the preparation process flow chart of the present invention. DETAILED DESCRIPTION

[0045] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0046] See also Figure 1 , the present invention provides a technical solution:

[0047] Example

[0048] A high-strength graphitized cathode carbon block comprises the following raw material components in percentage by weight:

[0049] Among them, modified asphalt 23-24%;

[0050] Calcined petroleum coke 86-87%;

[0051] Silicon carbide 1-5%;

[0052] Metal powder titanium 0.5-3%;

[0053] Alumina 1-5%;

[0054] The particle size composition of calcined petroleum coke is as follows by weight: 6-3mm15-20%, 3-1mm17-22%, 0-1mm20-25%, powder coke 35-40%;

[0055] The calcined petroleum coke in the graphitized cathode carbon block does not include the calcined petroleum coke raw material component of the dry material in the modified asphalt;

[0056] By clarifying the calcined petroleum coke raw materials of the calcined petroleum coke in the graphitized cathode carbon block and the calcined petroleum coke dry material in the modified asphalt, and controlling the particle size percentage of the calcined petroleum coke, it is convenient to control the overall strength and elasticity of the carbon block. By optimizing the contents to enhance the overall structural strength of the carbon block, it can effectively resist the mechanical stress in the electrolysis process and reduce the occurrence of cracks and breakage.

[0057] A method for manufacturing a high-strength graphitized cathode carbon block, which is applied to the production of the above-mentioned graphitized cathode carbon block, comprises the following process steps:

[0058] S1. A portion of the calcined petroleum coke is sieved through a vibrating screen into 8-4mm, 4-1mm and 1-0mm, wherein the purity of 8-4mm and 4-1mm is controlled to be above 85%, and the purity of 1-0mm is not controlled, and the remaining portion is ground into fine powder by a ball mill to obtain powdered coke;

[0059] The ground coke powder in S1 has a purity of 57-63%, and the calcined petroleum coke in S1 is a low-sulfur calcined petroleum coke with a sulfur content of less than 0.5%;

[0060] S2. The calcined petroleum cokes and powdered cokes obtained in S1 are preheated and dry-mixed in the upper layer of a double-layer kneading pot according to the formula, and the temperature is heated to 130-150°C to obtain dry carbon blocks. The heated dry materials and metal powders of titanium, silicon carbide and aluminum oxide are then put into the lower layer of the double-layer kneading pot, and modified asphalt is added for wet mixing. The paste temperature at the end of wet mixing is controlled at 170-180°C;

[0061] S3. The paste out of the pot in S2 is sent to the temperature-averaging pot through a belt conveyor for cooling, so that the paste temperature is reduced to 150-160 ℃, and the cooled paste is obtained;

[0062] S4. The cooled paste in S3 is placed in a mobile hopper scale for weighing. The weight control standard is the unit weight of the green block, and is sent to a high-precision mold of a CNC hydraulic molding machine, and a pressure of 250-350MPa is applied for 15-25 minutes to ensure the density uniformity and dimensional accuracy of the cathode carbon block green body;

[0063] S5. The green body obtained in S4 is sent to a cooling water pool by a catenary conveyor and cooled to room temperature, and then hoisted and sent to a green block warehouse stack for inspection;

[0064] S6. The green blocks that have passed the inspection are loaded into the roasting furnace through the overhead crane for roasting. The roasting adopts an 80-82 hour cycle curve, and the temperature is steadily increased to 900-1100°C at a heating rate of 4-8°C / h, and the temperature is kept constant for 25-35 hours. The final carbon block temperature reaches 1000-1050°C, and the insulation time is 20-40 hours;

[0065] The roasting furnaces in S6 and S9 use segmented temperature control technology and a uniform airflow circulation system to ensure uniform temperature distribution during roasting and reduce internal stress;

[0066] The roasting furnaces in S6 and S9 are open ring roasting furnaces;

[0067] S7. The qualified calcined blocks are loaded into the graphitization furnace through the overhead crane for graphitization, during which the temperature is raised in stages, the first stage is 1000-1800°C, the second stage is 1800-3000°C for heating, and the graphitization power supply time is 20-22 hours;

[0068] S8. The graphitized blocks that have passed the inspection are subjected to high-pressure impregnation treatment, with an impregnation pressure of 1.5-1.6Mpa and a holding time of 3-4h to ensure that the impregnation is sufficient and the pores are filled;

[0069] The graphitization furnace in S8 is an internal heat series graphitization furnace;

[0070] S9. The qualified impregnated blocks are loaded into the roasting furnace through the overhead crane for secondary roasting. The roasting cycle curve is 30-32h, and the final carbon block temperature reaches 8500-900°C, and the insulation time is 10-20 hours;

[0071] S10. The qualified secondary calcined block is processed according to the finished cathode processing drawing to obtain a high-strength graphitized cathode carbon block;

[0072] In conjunction with the accompanying drawings Figure 1As shown in the figure, in the production process, the calcined petroleum coke uses low-sulfur calcined petroleum coke with a sulfur content of less than 0.5%, which reduces the harm of sulfur to the environment, reduces the risk of cracking of the product during the graphitization process, and effectively improves the yield of the finished product. As the vibrating screen grades and screens the calcined petroleum coke, the contents of 8-4mm, 4-1mm and 1-0mm inside the calcined petroleum coke are accurately controlled to provide raw materials for the output of powdered coke, which is obtained by grinding in a ball mill. As the materials of each level are batched according to the formula requirements, the prepared materials of each level are preheated and dry-mixed in the upper layer of a double-layer kneading pot, and the obtained dry materials are mixed with metal powders of titanium, silicon carbide and alumina. The lower layer of the double-layer kneading pot is wet-mixed with modified asphalt, wherein some additives that help to improve strength are added to react with carbon at high temperature to form a reinforcing phase, further improving the strength of the graphitized cathode carbon block, thereby increasing the dry material temperature, improving the kneading effect, improving the plasticity of the paste and the homogeneity of the green block, so that the material inside the produced paste is uniform. As the paste cools down, it is evenly divided by weight and then sent to the high-precision mold of the CNC hydraulic molding machine, applying a pressure of 250-350MPa and maintaining the pressure for 15-25 minutes to ensure the density uniformity and dimensional accuracy of the cathode carbon block green body and improve the quality of the finished product output;

[0073] After the first roasting of the cathode carbon block green body is completed, the silicon carbide inside the green body reduces the resistivity of the carbon block, the metal powder titanium can form a good conductive network with carbon, further reducing the resistivity, and the aluminum oxide can react with carbon to form aluminum carbon compounds, thereby enhancing the strength and stability of the carbon material. The cathode carbon block that has been roasted for the first time is put into an internal heat series graphitization furnace for graphitization, wherein the product process power consumption of the internal heat series graphitization furnace is controlled at about 2800Kwh / t, thereby reducing the production cost. After that, the graphitized cathode carbon block is put into the impregnating agent, so that the impregnating agent impregnates the carbon block and fills the pores, and then the second roasting is performed again to improve the density and strength of the carbon block so that the product compressive strength is not less than 40MPa and the flexural strength is not less than 18MPa, thereby greatly improving the mechanical strength of the product.

[0074] Comparative Example 1

[0075] A high-strength graphitized cathode carbon block comprises the following raw material components in percentage by weight:

[0076] Among them, modified asphalt 23-24%;

[0077] Calcined petroleum coke 86-87%;

[0078] The particle size composition of calcined petroleum coke is as follows by weight: 6-3mm15-20%, 3-1mm17-22%, 0-1mm20-25%, powder coke 35-40%;

[0079] A method for manufacturing a high-strength graphitized cathode carbon block, which is applied to the production of the above-mentioned graphitized cathode carbon block, comprises the following process steps:

[0080] S1. A portion of the calcined petroleum coke is sieved through a vibrating screen into 8-4mm, 4-1mm and 1-0mm, wherein the purity of 8-4mm and 4-1mm is controlled to be above 85%, and the purity of 1-0mm is not controlled, and the remaining portion is ground into fine powder by a ball mill to obtain powdered coke;

[0081] The ground coke powder in S1 has a purity of 57-63%, and the calcined petroleum coke in S1 is a low-sulfur calcined petroleum coke with a sulfur content of less than 0.5%;

[0082] S2. The calcined petroleum coke and powdered coke materials obtained in S1 are preheated and dry-mixed in the upper layer of a double-layer kneading pot according to the formula, and the temperature is heated to 130-150°C to obtain a dry carbon block, and then the heated dry material is evenly added to the lower layer of the double-layer kneading pot, and modified asphalt is added for wet mixing. The paste temperature at the end of wet mixing is controlled at 180-190°C;

[0083] S3. The paste out of the pot in S2 is sent to the temperature-averaging pot through a belt conveyor for cooling, so that the paste temperature is reduced to 140-170 ℃, and the cooled paste is obtained;

[0084] S4. The cooled paste in S3 is placed in a mobile hopper scale for weighing. The weight control standard is the single weight of the green block, and is fed into a high-precision mold of a CNC hydraulic molding machine to press the cathode carbon block green body;

[0085] S5. The green blocks that have passed the inspection are loaded into the roasting furnace through the overhead crane for roasting. The roasting adopts an 88-90 hour cycle curve, and the temperature is steadily increased to 900-1100°C at a heating rate of 4-8°C / h, and the temperature is kept constant for 25-35 hours. The final carbon block temperature reaches 1000-1500°C, and the insulation time is 20-40 hours;

[0086] S6. The qualified calcined blocks are loaded into the graphitization furnace through the overhead crane for graphitization, during which the temperature is raised in stages, the first stage is 1100-1600°C, the second stage is 1600-2500°C for heating, and the graphitization power supply time is 24-26 hours;

[0087] S7. The graphitized blocks that have passed the inspection are subjected to high-pressure impregnation treatment, with an impregnation pressure of 2-2.5Mpa and a holding time of 3-6h to ensure that the impregnation is sufficient and the pores are filled, and then loaded into the roasting furnace for secondary roasting. The roasting adopts a 30-32h cycle curve, and the final carbon block temperature reaches 8500-900°C, and the holding time is 10-20 hours;

[0088] S8. The qualified secondary calcined block is processed according to the finished cathode processing drawing to obtain a high-strength graphitized cathode carbon block;

[0089] Comparative Example 2

[0090] A high-strength graphitized cathode carbon block comprises the following raw material components in percentage by weight:

[0091] Among them, modified asphalt 23-35%;

[0092] Calcined petroleum coke 70-77%;

[0093] Silicon carbide 1-5%;

[0094] The particle size composition of calcined petroleum coke is as follows by weight: 6-3mm15-20%, 3-1mm17-22%, 0-1mm20-25%, powder coke 35-40%;

[0095] The calcined petroleum coke in the graphitized cathode carbon block does not include the calcined petroleum coke raw material component of the dry material in the modified asphalt;

[0096] The construction process steps in the preparation of the graphitized cathode carbon block are the same as the specific steps of Comparative Example 1;

[0097] Table 1: Comparison of this cathode carbon block with other similar products:

[0098] Serial number Resistivity μΩ·m Compressive strength MPa Flexural strength MPa Process power consumption Kwh / t Example 8-10 45 26 2600-2900 Comparative Example 1 16-20 38 20 3800-4500 Comparative Example 2 20-30 24 24 4200-5500

[0099] The high-strength graphitized cathode carbon block produced by the steps in the embodiment has a compressive strength of ≥40MPa, a flexural strength of ≥18MPa, and a resistivity of ≤10μΩ·m, which makes the carbon block particularly suitable for ultra-large electrolytic cells above 500KA. At the same time, the service life is effectively extended, and the generation of electrolytic cell overhaul slag is reduced. In terms of electrical properties, the cathode carbon block achieves a lower resistivity, which reduces the cathode voltage drop and achieves better energy saving and consumption reduction.

[0100] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A high-strength graphitized cathode carbon block, characterized in that: The composition includes the following raw materials by weight percentage: Among them, modified asphalt 23-24%; Calcined petroleum coke 86-87%; Silicon carbide 1-5%; Metal powder titanium 0.5-3%; Alumina 1-5%.

2. A high-strength graphitized cathode carbon block according to claim 1, characterized in that: The particle size composition of the calcined petroleum coke is as follows by weight percentage: 6-3mm15-20%; 3-1mm17-22%; 0-1mm20-25%; Powder coke 35-40%.

3. The high-strength graphitized cathode carbon block according to claim 1, characterized in that: The calcined petroleum coke in the graphitized cathode carbon block does not include the calcined petroleum coke raw material component of the dry material in the modified asphalt.

4. The method for manufacturing a high-strength graphitized cathode carbon block according to claim 1 is applied to the production of the graphitized cathode carbon block according to claim 1, characterized in that: The process steps include: S1. A portion of the calcined petroleum coke is sieved by a vibrating screen into 8-4 mm, 4-1 mm and 1-0 mm, wherein the purity of 8-4 mm and 4-1 mm is controlled to be above 85%, and the purity of 1-0 mm is not controlled, and the remaining portion is ground into fine powder by a ball mill to obtain powdered coke; S2. The calcined petroleum cokes and powdered cokes obtained in S1 are preheated and dry-mixed in the upper layer of a double-layer kneading pot according to the formula, and the temperature is heated to 130-150°C to obtain dry carbon blocks. The heated dry materials and metal powders of titanium, silicon carbide and aluminum oxide are then put into the lower layer of the double-layer kneading pot, and modified asphalt is added for wet mixing. The paste temperature at the end of wet mixing is controlled at 170-180°C; S3. The paste out of the pot in S2 is sent to the temperature-averaging pot through a belt conveyor for cooling, so that the paste temperature is reduced to 150-160 ℃, and the cooled paste is obtained; S4. The cooled paste in S3 is placed in a mobile hopper scale for weighing. The weight control standard is the unit weight of the green block, and is sent to a high-precision mold of a CNC hydraulic molding machine, and a pressure of 250-350MPa is applied for 15-25 minutes to ensure the density uniformity and dimensional accuracy of the cathode carbon block green body; S5. The green body obtained in S4 is sent to a cooling water pool by a catenary conveyor and cooled to room temperature, and then hoisted and sent to a green block warehouse stack for inspection; S6. The green blocks that have passed the inspection are loaded into the roasting furnace through the overhead crane for roasting. The roasting adopts an 80-82 hour cycle curve, and the temperature is steadily increased to 900-1100°C at a heating rate of 4-8°C / h, and the temperature is kept constant for 25-35 hours. The final carbon block temperature reaches 1000-1050°C, and the insulation time is 20-40 hours; S7. The qualified calcined blocks are loaded into the graphitization furnace through the overhead crane for graphitization, during which the temperature is raised in stages, the first stage is 1000-1800°C, the second stage is 1800-3000°C for heating, and the graphitization power supply time is 20-22 hours; S8. The graphitized blocks that have passed the inspection are subjected to high-pressure impregnation treatment, with an impregnation pressure of 1.5-1.6Mpa and a holding time of 3-4h to ensure that the impregnation is sufficient and the pores are filled; S9. The qualified impregnated blocks are loaded into the roasting furnace through the overhead crane for secondary roasting. The roasting cycle curve is 30-32h, and the final carbon block temperature reaches 8500-900°C, and the insulation time is 10-20 hours; S10. Process the qualified secondary calcined blocks according to the finished cathode processing drawings to obtain high-strength graphitized cathode carbon blocks.

5. The method for manufacturing a high-strength graphitized cathode carbon block according to claim 4, characterized in that: The coke powder ground in S1 has a purity of 57-63%.

6. The method for manufacturing a high-strength graphitized cathode carbon block according to claim 4, characterized in that: The calcined petroleum coke in S1 is low-sulfur calcined petroleum coke having a sulfur content of less than 0.5%.

7. The method for manufacturing a high-strength graphitized cathode carbon block according to claim 4, characterized in that: The roasting furnaces in S6 and S9 adopt segmented temperature control technology and a uniform airflow circulation system to ensure uniform temperature distribution during the roasting process and reduce internal stress.

8. The method for manufacturing a high-strength graphitized cathode carbon block according to claim 4, characterized in that: The roasting furnaces in S6 and S9 are open ring roasting furnaces.

9. The method for manufacturing a high-strength graphitized cathode carbon block according to claim 4, characterized in that: The graphitization furnace in S8 is an internal heat series graphitization furnace.

Citation Information

Patent Citations

  • Anti-abrasion graphitization cathode carbon blocks used for aluminum electrolytic cell and manufacturing method thereof

    CN101665957A

  • Cathode graphitizing current stop block for aluminum electrolysis

    CN101949034A

  • Cathode graphite material used for electrolysis

    CN104341154A

  • Method for preparing composite graphite electrode

    CN109665845A

  • Preparation method of high-volume-density graphitized cathode carbon block for aluminum electrolysis

    CN112210791A