Modified cement-based micro-expansive mortar for vertical joints and preparation method of modified cement-based micro-expansive mortar
By adding specific components such as grouting materials, water reducing agents and polymer emulsions to the mortar, the problems of poor fluidity and large shrinkage in the prefabricated concrete wall panel structure are solved, and high fluidity, crack resistance and stickiness are achieved The improvement of junction performance meets the joint performance requirements and optimizes the construction process.
Patent Information
- Application Number
- CN202411208864.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-15
AI Technical Summary
The existing mortar materials have problems such as poor fluidity, large shrinkage, brittle damage, and poor bonding performance in the prefabricated concrete wall panel structure, which cannot meet the joint performance requirements, and the existing construction technology has the inability to completely fill the joints and The problem of easy water leakage affects the overall performance of the structure.
Develop a modified cement-based micro-expanded mortar for vertical joints, which improves the use of components such as grouting materials, high-efficiency water reducers, defoamers, foaming agents, polymer emulsions, rubber particles and emulsified asphalt. Flowability, adhesion and crack resistance ensure that the hardening process does not shrink or slightly expand, and optimize the process to suit industrial production.
It has achieved high flowability, early high strength, micro-expansion, crack resistance and bonding performance of the mortar during hardening, meet the joint performance requirements of prefabricated concrete wall panel structures, improve construction quality and overall stress performance. Shorten the construction cycle.
Smart Images

Figure BDA0005019799540000071 
Figure BDA0005019799540000072 
Figure BDA0005019799540000081
Abstract
Description
Technical Field
[0001] The invention relates to a mortar material, in particular to a modified cement-based micro-expansion mortar for vertical joints and a preparation method thereof, belonging to the field of cement-based material preparation. Background Art
[0002] As a representative of new building industrialization, prefabricated buildings have broad development prospects. Among them, prefabricated concrete wall panel structural system has obvious advantages in low-rise and multi-story prefabricated buildings. Compared with traditional cast-in-place concrete structures, prefabricated concrete wall panel structural system has a series of advantages, such as short construction period, controllable construction quality, good seismic performance, etc. Since prefabricated concrete structures mainly realize overall force through the connection of prefabricated components, the joint performance is particularly important to the overall performance of prefabricated concrete wall panels.
[0003] There are two main factors that affect the performance of joints: the first is the structural design and connection method of the joints; the second is the type and performance of the joint connection materials, including the strength and volume stability of the joint materials. The quality of the material performance will also have a significant impact on the overall performance of the entire structure. Therefore, it is necessary to pay attention to both the structural optimization design of the joints and the selection and performance control of the connection materials.
[0004] Ordinary mortar has problems such as poor fluidity, large shrinkage, easy brittle failure, and poor bonding performance, which cannot meet the requirements of joint performance of prefabricated concrete wall panels. In addition, the existing wall panel horizontal joint construction process "sitting mortar method" also has some defects, such as the mortar cannot completely fill the joint and is easy to seep water, which leads to quality problems at the joint and seriously affects the overall performance of the structure.
[0005] Domestic and foreign scholars have conducted extensive research on the seismic performance and joint connection forms of prefabricated concrete wall panels, and have achieved some important results. However, there are relatively few in-depth studies on cement-based materials for structural joints. Most of the existing research focuses on concrete road and bridge deck caulking materials, channel anti-seepage materials and crack repair materials, but no special new material development has been carried out to meet the performance requirements of PC wall panel structure joints.
[0006] Therefore, it is of great significance to develop a new type of connection material that can meet the performance requirements and construction quality requirements of PC wall panel structures. This can not only solve the various problems existing in ordinary mortars and improve the performance of joints, but also optimize the overall stress performance of prefabricated concrete wall panel structures and enhance their bearing capacity and seismic performance. At the same time, improving the joint construction process can also improve the construction quality and shorten the construction period, thereby promoting the widespread application of prefabricated construction technology in actual projects. Summary of the invention
[0007] In view of the shortcomings of the prior art, the first object of the present invention is to provide a modified cement-based micro-expansion mortar for vertical joints. The material has the advantages of high fluidity, high early strength, no shrinkage or micro-expansion during hardening, high toughness, crack resistance, etc.
[0008] The second object of the present invention is to provide a method for preparing a modified cement-based micro-expansion mortar for vertical joints. The method is simple, low-cost and suitable for industrial production.
[0009] In order to achieve the above technical objectives, the present invention provides a modified cement-based slightly expansive mortar for vertical joints, which comprises the following components by weight:
[0010] 650-670 parts of cement;
[0011] 355-365 parts of limestone powder;
[0012] 277-285 parts of water;
[0013] Sand 859-877 parts;
[0014] 53 to 53.8 parts of expansion agent;
[0015] Water reducing agent 3.56-3.64 parts;
[0016] 0.29-0.31 parts of foaming agent;
[0017] 1.78-1.82 parts of defoaming agent;
[0018] 39-40 parts of polymer emulsion;
[0019] 9.43-9.63 parts of rubber particles;
[0020] 1.42 to 1.46 parts of emulsified asphalt.
[0021] The present invention selects grouting material as the modification object and utilizes its advantages of no vibration, high fluidity and low price to achieve the purpose of improving fluidity and reducing costs; utilizes the functions of high-efficiency water reducing agent in dispersing, reducing surface tension, retaining water and regulating hydration, and utilizes the function of defoaming agent in eliminating bubbles that are unfavorable to mortar, thereby achieving the purpose of improving mortar fluidity; utilizes the function of foaming agent in generating micro bubbles, utilizes the function of micro-expansion agent in shrinking mortar volume, and maintains micro-expansion of slurry by adding foaming agent in the plastic stage of mortar, and utilizes expansion agent in the hardening stage to compensate for mortar volume shrinkage, thereby achieving the purpose of making mortar non-shrinking or micro-expansion; utilizes the function of polymer emulsion in cement to form a dense spatial network structure, thereby achieving the purpose of improving the fluidity, adhesion and other properties of mortar; utilizes the filling and dispersion effect of rubber particles in cement-based materials, utilizes the function of emulsified asphalt in film formation to cover the surface of rubber particles, and improves the bonding force of the interface between rubber particles and cement matrix, thereby improving the tensile strength, toughness and crack resistance of cement-based.
[0022] As a preferred solution, the cement is silicate cement.
[0023] As a preferred solution, the silicate cement is P·II52.5 silicate cement.
[0024] As a preferred solution, the particle size of the limestone powder is -300 mesh.
[0025] As a preferred solution, the sand is quartz sand or machine-made sand.
[0026] As a preferred solution, the sand includes coarse sand with a particle size of -16 mesh to +30 mesh and fine sand with a particle size of -30 mesh to +50 mesh.
[0027] As a preferred solution, the mass amount of the coarse sand is 364 to 372 parts; the mass amount of the fine sand is 495 to 505 parts.
[0028] As a preferred solution, the expansion agent is a calcium oxide expansion agent.
[0029] As a preferred solution, the water reducer is a polycarboxylate water reducer.
[0030] As a preferred solution, the foaming agent is a rubber foaming agent.
[0031] As a preferred solution, the defoaming agent is tributyl phosphate defoaming agent.
[0032] As a preferred solution, the polymer emulsion is anionic chloroprene rubber latex.
[0033] As a preferred solution, the rubber particles are waste tire rubber particles.
[0034] As a preferred solution, the emulsified asphalt is anionic emulsified asphalt.
[0035] As a preferred solution, the rubber particles have a particle size of -20 mesh.
[0036] The present invention also provides a method for preparing a modified cement-based micro-expansive mortar for vertical joints, which comprises mixing cement, limestone powder, sand, an expansion agent, a water reducer, a foaming agent, a defoaming agent and rubber particles, and then adding materials containing water, a polymer emulsion and emulsified asphalt to mix the mortar.
[0037] Compared with the prior art, the present invention has the following beneficial effects:
[0038] 1) The modified cement-based micro-expansive mortar of the present invention achieves the purpose of improving fluidity and reducing costs by selecting grouting material as the modification object and utilizing its advantages of no vibration, high fluidity and low price.
[0039] 2) The modified cement-based micro-expansive mortar of the present invention achieves the purpose of improving the fluidity of the mortar by adding a high-efficiency water reducing agent and a defoaming agent, utilizing the dispersion, surface tension reduction, water retention and hydration regulation effects of the high-efficiency water reducing agent, and utilizing the effect of the defoaming agent to eliminate bubbles that are detrimental to the mortar.
[0040] 3) The modified cement-based micro-expansive mortar of the present invention adds a foaming agent and an expansive agent, utilizes the effect of the foaming agent to generate tiny bubbles, utilizes the effect of the micro-expansive agent to shrink the volume of the mortar, maintains the micro-expansion of the mortar by adding a foaming agent in the plastic stage of the mortar, and uses an expansive agent to compensate for the volume shrinkage of the mortar in the hardening stage, thereby achieving the purpose of making the mortar shrink-free or micro-expanding.
[0041] 4) The modified cement-based micro-expansive mortar of the present invention achieves the purpose of improving the fluidity, adhesion and other properties of the mortar by adding polymer emulsion and utilizing the function of the polymer emulsion to form a dense spatial network structure in cement.
[0042] 5) The modified cement-based micro-expansive mortar of the present invention uses the filling and dispersion effects of rubber particles in cement-based materials by adding rubber particles and emulsified asphalt, and uses the emulsified asphalt to cover the surface of rubber particles after film formation, thereby improving the bonding force at the interface between rubber particles and cement matrix, thereby improving the tensile strength, toughness and crack resistance of the cement matrix. DETAILED DESCRIPTION
[0043] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0044] Example 1
[0045] Prepare the raw materials according to the following mass components:
[0046] 660 parts of P·Ⅱ52.5 silicate cement, 360 parts of limestone powder passing through a 300-mesh sieve, 53.4 parts of calcium oxide expansion agent, 281.2 parts of water, 368 parts of quartz sand passing through a 16-mesh sieve but not passing through a 30-mesh sieve, 500 parts of quartz sand passing through a 30-mesh sieve but not passing through a 50-mesh sieve, 3.6 parts of high-performance polycarboxylic acid water-reducing agent, 0.30 parts of rubber foaming agent, 1.8 parts of tributyl phosphate defoaming agent, 39.6 parts of anionic chloroprene rubber latex, 9.53 parts of waste tire rubber particles passing through a 20-mesh sieve, and 1.44 parts of anionic emulsified asphalt.
[0047] The preparation process is as follows:
[0048] 1) P·Ⅱ52.5 silicate cement, limestone powder through 300 mesh sieve, calcium oxide expansion agent, quartz sand with a particle size of -16 mesh to +30 mesh, quartz sand with a particle size of -30 mesh to +50 mesh, high-performance polycarboxylic acid water reducer, rubber foaming agent, tributyl phosphate defoamer and waste tire rubber particles through 20 mesh sieve are first put into a mixer and dry mixed for 30 seconds to ensure that all materials are mixed evenly.
[0049] 2) After the dry mixing is completed, add the pre-mixed water-anionic chloroprene latex-anionic emulsified asphalt mixture, stir at 140 r / min for 90 s, stop for 30 s, and then continue stirring at 285 r / min for 120 s, so as to obtain a modified cement-based micro-expansive mortar with uniform dispersion of each component.
[0050] Comparative Example 1
[0051] 660 parts of P·Ⅱ52.5 silicate cement, 360 parts of limestone powder passing through a 300-mesh sieve, 53.4 parts of calcium oxide expansion agent, 253.4 parts of water, 368 parts of quartz sand with a particle size of -16 mesh to +30 mesh, 500 parts of quartz sand with a particle size of -30 mesh to +50 mesh, 3.5 parts of high-performance polycarboxylic acid water-reducing agent, 0.26 parts of rubber foaming agent, 1.4 parts of tributyl phosphate defoaming agent, 26.4 parts of anionic chloroprene rubber latex, 9.53 parts of waste tire rubber particles passing through a 20-mesh sieve, and 1.44 parts of anionic emulsified asphalt.
[0052] The preparation method is the same as Example 1.
[0053] Comparative Example 2
[0054] 660 parts of P·Ⅱ52.5 silicate cement, 360 parts of limestone powder passing through a 300-mesh sieve, 53.4 parts of calcium oxide expansion agent, 250.8 parts of water, 360 parts of quartz sand with a particle size of -16 mesh to +30 mesh, 500 parts of quartz sand with a particle size of -30 mesh to +50 mesh, 4.0 parts of high-performance polycarboxylic acid water-reducing agent, 0.28 parts of rubber foaming agent, 1.6 parts of tributyl phosphate defoaming agent, 33.0 parts of anionic chloroprene rubber latex, 11.91 parts of waste tire rubber particles passing through a 20-mesh sieve, and 1.80 parts of anionic emulsified asphalt.
[0055] The preparation method is the same as Example 1.
[0056] Comparative Example 3
[0057] 660 parts of P·Ⅱ52.5 silicate cement, 360 parts of limestone powder passing through a 300-mesh sieve, 53.4 parts of calcium oxide expansion agent, 248.2 parts of water, 352 parts of quartz sand with a particle size of -16 mesh to +30 mesh, 500 parts of quartz sand with a particle size of -30 mesh to +50 mesh, 4.4 parts of high-performance polycarboxylic acid water-reducing agent, 0.30 parts of rubber foaming agent, 1.8 parts of tributyl phosphate defoaming agent, 39.6 parts of anionic chloroprene rubber latex, 14.29 parts of waste tire rubber particles passing through a 20-mesh sieve, and 2.16 parts of anionic emulsified asphalt.
[0058] The preparation method is the same as Example 1.
[0059] Comparative Example 4
[0060] 660 parts of P·Ⅱ52.5 silicate cement, 360 parts of limestone powder passing through a 300-mesh sieve, 53.4 parts of calcium oxide expansion agent, 286.4 parts of water, 360 parts of quartz sand with a particle size of -16 mesh to +30 mesh, 500 parts of quartz sand with a particle size of -30 mesh to +50 mesh, 2.5 parts of high-performance polycarboxylic acid water-reducing agent, 0.26 parts of rubber foaming agent, 1.4 parts of tributyl phosphate defoaming agent, 26.4 parts of anionic chloroprene rubber latex, 11.91 parts of waste tire rubber particles passing through a 20-mesh sieve, and 1.80 parts of anionic emulsified asphalt.
[0061] The preparation method is the same as Example 1.
[0062] Comparative Example 5
[0063] 660 parts of P·Ⅱ52.5 silicate cement, 360 parts of limestone powder passing through a 300-mesh sieve, 53.4 parts of calcium oxide expansion agent, 283.8 parts of water, 352 parts of quartz sand with a particle size of -16 mesh to +30 mesh, 500 parts of quartz sand with a particle size of -30 mesh to +50 mesh, 3.0 parts of high-performance polycarboxylic acid water-reducing agent, 0.28 parts of rubber foaming agent, 1.6 parts of tributyl phosphate defoaming agent, 33.0 parts of anionic chloroprene rubber latex, 14.29 parts of waste tire rubber particles passing through a 20-mesh sieve, and 2.16 parts of anionic emulsified asphalt.
[0064] The preparation method is the same as Example 1.
[0065] Comparative Example 6
[0066] 660 parts of P·Ⅱ52.5 silicate cement, 360 parts of limestone powder passing through a 300-mesh sieve, 53.4 parts of calcium oxide expansion agent, 319.4 parts of water, 352 parts of quartz sand with a particle size of -16 mesh to +30 mesh, 500 parts of quartz sand with a particle size of -30 mesh to +50 mesh, 2.3 parts of high-performance polycarboxylic acid water-reducing agent, 0.26 parts of rubber foaming agent, 1.4 parts of tributyl phosphate defoaming agent, 26.4 parts of anionic chloroprene rubber latex, 14.29 parts of waste tire rubber particles passing through a 20-mesh sieve, and 2.16 parts of anionic emulsified asphalt.
[0067] The preparation method is the same as Example 1.
[0068] Comparative Example 7
[0069] 660 parts of P·Ⅱ52.5 silicate cement, 360 parts of limestone powder passing through a 300-mesh sieve, 53.4 parts of calcium oxide expansion agent, 316.8 parts of water, 368 parts of quartz sand with a particle size of -16 mesh to +30 mesh, 500 parts of quartz sand with a particle size of -30 mesh to +50 mesh, 2.7 parts of high-performance polycarboxylic acid water-reducing agent, 0.28 parts of rubber foaming agent, 1.6 parts of tributyl phosphate defoaming agent, 33.0 parts of anionic chloroprene rubber latex, 9.53 parts of waste tire rubber particles passing through a 20-mesh sieve, and 1.44 parts of anionic emulsified asphalt.
[0070] The preparation method is the same as Example 1.
[0071] Comparative Example 8
[0072] 660 parts of P·Ⅱ52.5 silicate cement, 360 parts of limestone powder passing through a 300-mesh sieve, 53.4 parts of calcium oxide expansion agent, 314.2 parts of water, 360 parts of quartz sand with a particle size of -16 mesh to +30 mesh, 500 parts of quartz sand with a particle size of -30 mesh to +50 mesh, 3.2 parts of high-performance polycarboxylic acid water-reducing agent, 0.30 parts of rubber foaming agent, 1.8 parts of tributyl phosphate defoaming agent, 39.6 parts of anionic chloroprene rubber latex, 11.91 parts of waste tire rubber particles passing through a 20-mesh sieve, and 1.80 parts of anionic emulsified asphalt.
[0073] The preparation method is the same as Example 1.
[0074] Table 1 is the orthogonal factor level table, and Table 2 is the material mix ratio of each group in the orthogonal experiment.
[0075] Tables 3 to 5 show the performance test results of various embodiments and comparative examples.
[0076] Table 1 Orthogonal factor level table In Table 1, the basis for the polymer emulsion dosage is the sum of the masses of cement, limestone powder and expansion agent; the basis for the rubber particle dosage is the volume of coarse sand.
[0077] Table 2 Material proportions of each group in orthogonal experiment / unit: g·L -1
[0078]
[0079]
[0080] Table 3 Analysis of test results of fluidity and vertical expansion rate
[0081]
[0082] Table 4 Mechanical properties test results
[0083]
[0084]
[0085] Table 5 Expansion rate and bonding performance test results
[0086]
[0087] According to the experimental research results, the following optimal combination can be obtained for the mix ratio design of the joint materials of the prefabricated concrete wall panel structure:
[0088] When the 28-day flexural strength and compressive strength are used as control indicators, the best ratio is A1B3C1 or A1B1C1. This is because the mortar strength decreases significantly with the increase of water-cement ratio, and decreases with the increase of rubber particle content. The CR emulsion content is not the main factor affecting this indicator. Therefore, a lower water-cement ratio (A1), a suitable CR emulsion content (B1 or B3), and a lower rubber particle content (C1) can improve the strength performance of the mortar.
[0089] When the 28-day compression ratio is used as the control index, the best ratio is A3B3C1 or A3B3C3. This is because the compression ratio increases with the increase of water-cement ratio, decreases first and then increases with the increase of CR emulsion content, and the compression ratio is higher when the rubber particle content is C1 or C3. Therefore, a higher water-cement ratio (A3), a higher CR emulsion content (B3) and a suitable rubber particle content (C1 or C3) help improve the toughness performance of the mortar.
[0090] Taking the 21-day limited expansion rate in air as an indicator, the best ratio is A3B1C3. This is because when the water-cement ratio is A3, the mortar expansion performance is optimal, and when the rubber particle content is C1 or C3, the mortar expansion performance is relatively high, and the CR emulsion content is not the main factor affecting the mortar expansion performance. Therefore, a higher water-cement ratio (A3), a suitable CR emulsion content (B1), and a suitable rubber particle content (C1 or C3) can improve the expansion performance of the mortar.
[0091] Taking the 7-day bond strength as an indicator, the best ratio is A1B2C1. This is because the 7-day bond strength decreases significantly with the increase of water-cement ratio, decreases with the increase of rubber particle content, and the CR emulsion content is not the main factor affecting the 7-day bond strength. Therefore, a lower water-cement ratio (A1), a moderate CR emulsion content (B2) and a lower rubber particle content (C1) are conducive to improving the bond strength between the mortar and the substrate.
[0092] After comprehensively balancing various performance indicators, the optimal mix ratio was finally determined to be A2B3C1, that is, the water-cement ratio is 0.45, the CR emulsion content is 6%, and the rubber particle content is 8%. This mix ratio not only meets the requirements of mechanical properties and volume stability, but also has excellent fluidity and vertical expansion rate, which can better meet the various performance requirements of prefabricated concrete wall panel structure joint materials.
[0093] Comparative Example 9 (Mortar before modification)
[0094] 660 parts of P·Ⅱ52.5 silicate cement, 360 parts of limestone powder through a 300-mesh sieve, 76.8 parts of calcium oxide expansion agent, 264 parts of water, 400 parts of quartz sand with a particle size of -16 mesh to +30 mesh, 500 parts of quartz sand with a particle size of -30 mesh to +50 mesh, 2.3 parts of high-performance polycarboxylic acid water-reducing agent, 0.24 parts of rubber foaming agent, and 1.0 parts of tributyl phosphate defoaming agent.
[0095] The preparation method is the same as Example 1.
[0096] The performance test results of Example 1 and Comparative Example 9 (mortar before modification) are shown in Table 6.
[0097] Table 6 Comparison of mortar properties before and after modification
[0098]
[0099]
[0100] It can be seen that the modified grouting mortar can meet various performance requirements of grouting materials.
[0101] First, the modified grouting mortar has good fluidity and can maintain a high degree of fluidity even after 30 minutes, which greatly improves the operability of the construction. From the vertical expansion rate index, the modified grouting mortar can continue to expand and deform during the plastic hardening process, meeting the requirements of fully filling gaps in joints and other parts and compensating for plastic deformation during the shrinkage hardening stage, ensuring the quality of grouting. However, the baseline grouting material before modification shrinks slightly during the hardening process and has poor expansion performance.
[0102] From the perspective of mechanical properties, the modified grouting mortar meets the strength requirements of the specified age, has a high flexural strength, and exhibits strong toughness. This is mainly due to the increase in water-cement ratio and the addition of polymer emulsion and rubber particle-emulsified asphalt. Although these factors also lead to a decrease in its compressive strength and bonding strength, the flexural strength remains basically unchanged or even increases, significantly improving the toughness of the mortar.
[0103] In addition, the ratio of the bond strength to the compressive strength of the modified mortar also increased by 8.6%, indicating that its bonding performance has been significantly improved compared to before modification. Although there is no specific bond strength standard for grouting mortar, compared with cement-based materials used in ceramic tile adhesives, the bond strength of the modified mortar has greatly exceeded the requirements of relevant specifications and can meet the bonding performance requirements of joint grouting.
[0104] In terms of shrinkage performance, the modified grouting mortar did not shrink or deform under dry and closed conditions for 28 days, but maintained a certain amount of micro-expansion. This not only meets the shrinkage requirements of the "Sleeve Grouting Material for Steel Bar Connection" for grouting materials, but also complies with the provisions of the "Technical Specifications for the Application of Concrete Admixtures" for limiting the expansion rate of joint filling concrete.
[0105] In summary, the modified grouting mortar has comprehensive properties such as high fluidity, micro-expansion during hardening, high adhesion and high toughness, which can well meet the structural joint performance requirements and construction quality requirements of PC wall panels.
[0106] Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the present invention will not be limited to the embodiments shown herein, but will conform to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A modified cement-based micro-expansion mortar for vertical joints, characterized in that: It includes the following components by weight: 650-670 parts of cement; 355-365 parts of limestone powder; 277-285 parts of water; Sand 859-877 parts; 53 to 53.8 parts of expansion agent; Water reducing agent 3.56-3.64 parts; 0.29-0.31 parts of foaming agent; 1.78-1.82 parts of defoaming agent; 39-40 parts of polymer emulsion; 9.43-9.63 parts of rubber particles; 1.42 to 1.46 parts of emulsified asphalt.
2. The modified cement-based slightly expansive mortar for vertical joints according to claim 1, characterized in that: The cement is silicate cement.
3. The modified cement-based micro-expansion mortar for vertical joints according to claim 1, characterized in that: The particle size of the limestone powder is -300 mesh.
4. The modified cement-based slightly expansive mortar for vertical joints according to claim 1, characterized in that: The sand is quartz sand; the sand includes coarse sand with a particle size of -16 mesh to +30 mesh and fine sand with a particle size of -30 mesh to +50 mesh.
5. The modified cement-based slightly expansive mortar for vertical joints according to claim 4, characterized in that: The mass of the coarse sand is 364 to 372 parts; the mass of the fine sand is 495 to 505 parts.
6. The modified cement-based slightly expansive mortar for vertical joints according to claim 1, characterized in that: The expansion agent is a calcium oxide expansion agent.
7. The modified cement-based slightly expansive mortar for vertical joints according to claim 1, characterized in that: The water reducer is a polycarboxylate water reducer; The foaming agent is a rubber foaming agent; The defoamer is tributyl phosphate defoamer; The polymer emulsion is anionic chloroprene rubber latex; The rubber particles are waste tire rubber particles; The emulsified asphalt is anionic emulsified asphalt.
8. The modified cement-based slightly expansive mortar for vertical joints according to claim 7, characterized in that: The particle size of the rubber particles is -20 mesh.
9. The method for preparing a modified cement-based micro-expansion mortar for vertical joints according to claims 1 to 8, characterized in that: The cement, limestone powder, sand, expansion agent, water reducing agent, foaming agent, defoaming agent and rubber particles are mixed, and then materials containing water, polymer emulsion and emulsified asphalt are added and mixed to obtain the product.
Citation Information
Patent Citations
A cement-emulsified asphalt self-penetrating grouting material for semi-flexible pavements
CN102276199A
Polymer cement mortar for slab ballastless track of high-speed railway
CN104030644A
Water-resistance-excellent cement emulsified asphalt mortar used for plate-type ballastless track
CN104211349A
Cement-based grouting material and preparation method thereof
CN106186932A
Joint repairing material and repairing method for wide joint of CRTS II type track plate
CN111333385A