Novel fluorine-containing surfactant, fluorine-containing acrylate polymer and application thereof

Through the development of new fluorine-containing surfactants and acrylate polymers, the problem of PFOS/PFOA fluorocarbon surfactants deteriorate after reducing the length of fluorocarbon chains is solved, and efficient hydrophobic, oil-repellent and inhibitory effects are achieved. Bacterial properties, suitable for emulsifiers and antibacterial agents.

CN118955321APending Publication Date: 2024-11-15SHANGHAI INST OF ORGANIC CHEM CHINESE ACAD OF SCI +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411007599.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

After reducing the length of the fluorocarbon chain, existing PFOS/PFOA fluorocarbon surfactants lead to a decrease in surfactivity, hydrophobic or oil-repellent properties, and are difficult to degrade in nature and organisms, resulting in environmental protection problems.

Method used

Develop a novel fluorine-containing surfactant and fluorine-containing acrylate polymer prepared by neutralization, condensation or quaternization reactions, with excellent hydrophobic, oil-repellent and antibacterial properties, and is used in emulsifiers and polymerization Reaction to form a stable acrylate polymer.

Benefits of technology

Significantly reduce the surface tension of the aqueous solution, improve emulsification performance, have excellent hydrophobic, oil-repellent and antibacterial properties, and are suitable for acrylate monomers and water systems, which can form stable emulsions and be used for golden glutamate and E. coli has a strong antibacterial effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955321A_ABST
    Figure CN118955321A_ABST
Patent Text Reader

Abstract

The invention discloses a novel fluorine-containing surfactant, a fluorine-containing acrylate polymer and application of the fluorine-containing surfactant and the fluorine-containing acrylate polymer. Specifically disclosed is a compound represented by formula I. The compound shown in the formula I can remarkably reduce the surface tension of an aqueous solution, and a product obtained by polymerizing the compound has excellent emulsifying performance and antibacterial performance and has high practical application value and wide market prospects. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of surfactants, and in particular to a novel fluorine-containing surfactant, a fluorine-containing acrylic ester polymer and applications thereof. Background Art

[0002] Fluorocarbon surfactants are surfactants in which all or part of the hydrogen atoms in the hydrocarbon hydrophobic chain are replaced by fluorine atoms. They have been widely used in fire extinguishing agents, surface treatment agents for photosensitive materials, textile finishing agents, cleaning and surface treatment fluids for the semiconductor industry, inert liquids for the aerospace industry, electroplating chrome mist suppressants, industrial and daily cleaning agent additives, coating and paint additives, pesticide additives, cosmetic additives, oil extraction additives, fluorine chemical high-efficiency emulsifiers, etc. The most common fluorocarbon surfactants mainly include: perfluorooctane sulfonates (PFOS) with different hydrophobic chain lengths, perfluorooctanoic acid (PFOA) with different hydrophobic chain lengths, etc. However, due to environmental issues, the production, sale and use of PFOS / PFOA fluorocarbon surfactants have been gradually banned.

[0003] Since the environmental problem of PFOS-type fluorocarbon surfactants is due to the long fluorocarbon chain length, which is difficult to degrade in nature and organisms, the current global PFOS alternative research and development strategy is mainly focused on reducing the toxicity of the fluorocarbon chain, such as reducing the length of the fluorocarbon chain (such as PFHS with a hydrophobic fluorocarbon chain length of 6 carbons and PFBS with a hydrophobic fluorocarbon chain length of 4 carbons), introducing more easily degradable weak sites in the fluorocarbon chain (such as the methylene group in vinylidene fluoride oligomers and the ether bond in hexafluoropropylene oxide oligomers), branching the fluorocarbon chain (such as hexafluoropropylene oligomers), and constructing new fluorocarbon surfactant structures (such as gemini surfactants and hetero-gemini surfactants).

[0004] The increase in the degradability of the fluorocarbon chain actually means a decrease in molecular stability, that is, the reduction of the superior "three highs and two-phobic" properties of fluorocarbon surfactants (high surface activity, high thermal stability and high chemical stability; water-phobic and oil-phobic). Therefore, it is necessary to develop a surfactant that still has superior "three highs and two-phobic" properties while reducing the fluorocarbon chain. Summary of the invention

[0005] The purpose of the present invention is to overcome the defects of the prior art PFOS / PFOA fluorocarbon surfactants in that the surface activity, hydrophobicity or oleophobicity are reduced after the fluorocarbon chain length is reduced, and to provide a new type of fluorinated surfactant, fluorinated acrylic polymer and its application. This type of surfactant can significantly reduce the surface tension of aqueous solution and improve emulsification performance, and the product obtained by polymerization thereof has excellent hydrophobicity, oleophobicity and antibacterial properties.

[0006] The present invention solves the above technical problems through the following technical solutions.

[0007] The present invention provides a compound as shown in formula I:

[0008]

[0009] Wherein, n is 1, 2, 3 or 4;

[0010] R f C substituted with one or more F 1-6 alkyl;

[0011] R1 is -CH2- or -CH(OH)-;

[0012] R2, R3 and R4 are each independently C 1-6 Alkyl or 1 R a Substituted C 1-6 alkyl;

[0013] R a for

[0014] X - is a halogen anion or

[0015] R5 is H or C 1-6 alkyl;

[0016] When R2, R3 and R4 are each independently C 1-6 When X is alkyl, - for

[0017] In one scenario, R f , R2, R3, R4 and R5, the C substituted by one or more F 1-6 Alkyl, the C 1-6 The alkyl group and the a Substituted C 1-6 C in the alkyl group 1-6 The alkyl groups are each independently methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl or tert-butyl; for example methyl or ethyl.

[0018] In one embodiment, the halogen anion is F - , Cl - Br - and I - ; For example, Br - .

[0019] In one embodiment, n is 1.

[0020] In one scenario, Rf It is CF3(CF2)2C(CF3)2-.

[0021] In one embodiment, R1 is -CH2-.

[0022] In one embodiment, R2, R3 and R4 are each independently -CH3, -CH2CH3 or

[0023] In one embodiment, R5 is -CH3.

[0024] In one scenario, X - Br - or

[0025] In one embodiment, the compound of formula I is a compound of formula A or a compound of formula B:

[0026]

[0027] Among them, n, R f , R1, R2, R3, R4, R5 and X - The definitions of are as mentioned above;

[0028] In formula B, R6 is C 1-6 Alkylene;

[0029] In one embodiment, in R6, the C 1-6 Alkylene is independently -CH2-, -CH2CH2-, -CH(CH3)-, -CH(CH3)CH2- or -C(CH3)2-.

[0030] In one embodiment, in Formula B, R6 is -CH2CH2-.

[0031] In one embodiment, in Formula B, X - is a halogen anion, for example, X- is Br - .

[0032] In one embodiment, the compound of formula I is a compound of formula A-1 or a compound of formula B-1;

[0033]

[0034] The present invention provides a method for preparing a compound as shown in Formula I, which is Method 1, Method 2 or Method 3:

[0035] Method 1:

[0036] It includes the following steps:

[0037] In a solvent, a compound represented by formula a and a compound represented by formula d are subjected to a neutralization reaction;

[0038]

[0039] Among them, n, R f , R1, R2, R3, R4 and R5 are defined as above;

[0040] Method 2:

[0041] It includes the following steps:

[0042] In a solvent, the compound represented by formula b and the compound represented by formula e are subjected to condensation reaction;

[0043]

[0044] Among them, n, R f , R1, R2, R3, R5, R6 and X- are as defined above;

[0045] Method 3:

[0046] It includes the following steps:

[0047] In a solvent, a compound represented by formula c and a compound represented by formula f are subjected to a quaternization reaction;

[0048]

[0049] Among them, n, R f , R1, R2, R3, R5, R6 and X - The definitions are as mentioned above.

[0050] The solvent is a conventional solvent for such reactions in the art. In a certain embodiment, the solvent is preferably one or more of an alcohol solvent, a halogenated alkane solvent, an aromatic hydrocarbon solvent, an ether solvent, an amide solvent or a nitrile solvent.

[0051] In one embodiment, the alcohol solvent is preferably one or more of methanol, ethanol and propanol.

[0052] In a certain embodiment, the halogenated alkane solvent is preferably dichloromethane or chloroform.

[0053] In a certain embodiment, the aromatic hydrocarbon solvent is preferably toluene.

[0054] In one embodiment, the ether solvent is preferably diethyl ether or tetrahydrofuran.

[0055] In a certain embodiment, the amide solvent is preferably N,N-dimethylformamide.

[0056] In a certain embodiment, the nitrile solvent is preferably acetonitrile.

[0057] In one embodiment, the solvent is preferably methanol or tetrahydrofuran.

[0058] The amount of the solvent used is the conventional amount used in this type of reaction in the art.

[0059] In one embodiment, in the neutralization reaction, the molar ratio of the compound represented by formula a to the solvent is 0.05 to 1 mol / L, such as 0.1 to 0.2 mol / L.

[0060] In one embodiment, in the condensation reaction, the molar ratio of the compound represented by formula b to the solvent is 0.05 to 1 mol / L, such as 0.1 to 0.2 mol / L.

[0061] In one embodiment, in the quaternization reaction, the molar ratio of the compound represented by formula C to the solvent is 0.05 to 1 mol / L, for example, 0.1 to 0.3 mol / L.

[0062] In one embodiment, in the neutralization reaction, the compound shown in formula d is acrylic acid or methacrylic acid, for example, methacrylic acid.

[0063] In one embodiment, in the neutralization reaction, the molar ratio of the compound represented by formula a to the compound represented by formula d is 1:(0.6-3), preferably 1:(0.8-1.5), for example 1:1.1.

[0064] In one embodiment, the neutralization reaction time is 1 to 6 hours, such as 2 to 4 hours.

[0065] In one embodiment, the neutralization reaction temperature is 10-40°C, preferably 20-40°C, for example 25°C.

[0066] In a certain embodiment, the preparation method of the compound as shown in formula A preferably comprises the following steps: reacting the compound as shown in formula a with the compound as shown in formula d at room temperature in the solvent.

[0067] In a certain embodiment, the method for preparing the compound shown in Formula A preferably further comprises the following post-treatment step after the neutralization reaction is completed: spin-drying the solvent and recrystallizing with an organic solvent. The organic solvent is preferably a ketone solvent, such as acetone.

[0068] The condensation reaction is the condensation reaction of alcohols and acyl chlorides or carboxylic acids conventionally described in the art, and the parameters and conditions of the condensation reaction can be those conventionally used in this field for such reactions.

[0069] The compound shown in formula e is conventionally used in this type of reaction in the art. In a certain embodiment, in the condensation reaction, the compound shown in formula e is preferably a compound containing an acrylic acid functional group or a compound containing an acryloyl chloride functional group, and is further preferably one or more of acrylic acid, methacrylic acid, acryloyl chloride or methacryloyl chloride, such as methacryloyl chloride.

[0070] In a certain embodiment, in the condensation reaction, the molar ratio of the compound represented by formula e to the compound represented by formula b is 1:(0.1-1), preferably 1:(0.3-0.5).

[0071] In one embodiment, the condensation reaction further comprises an organic base, and the organic base is preferably an amine compound, such as triethylamine.

[0072] In a certain embodiment, in the condensation reaction, the molar ratio of the organic base to the compound represented by formula e is preferably 1:(0.8-2), for example 1:1.

[0073] The reaction temperature of the condensation reaction is the temperature conventionally used in this field for such reactions. In the scheme, the temperature of the condensation reaction is preferably 20-40°C, for example 25°C.

[0074] In one embodiment, the condensation reaction time is 6 to 24 hours, for example 12 hours.

[0075] In a certain embodiment, in the condensation reaction, the preparation method of the compound shown in formula B preferably includes the following steps: mixing the compound shown in formula b with the organic base in the solvent, then adding the compound shown in formula e dropwise, and reacting at room temperature.

[0076] In a certain embodiment, in the condensation reaction, the method for preparing the compound shown in Formula B preferably further comprises the following post-treatment steps after the reaction is completed: filtering, removing the solvent under reduced pressure, and separating the mixture by column chromatography to obtain a white solid compound. Among them, the eluent is preferably a mixed solvent of a halogenated alkane solvent and an alcohol solvent, and the volume ratio of the halogenated alkane solvent to the alcohol solvent is preferably (100-10):1; the halogenated alkane solvent is preferably dichloromethane; and the alcohol solvent is preferably methanol.

[0077] The quaternization reaction is the quaternization reaction of a halogenated hydrocarbon with a tertiary amine conventionally described in the art, and the parameters and conditions of the quaternization reaction can be those conventionally used in this type of reaction in the art.

[0078] In one embodiment, the quaternization reaction time is 80 to 140 hours, for example 100 hours.

[0079] The compound shown in formula f is conventionally used in this type of reaction in the art. In a certain scheme, in the quaternization reaction, the compound shown in formula f is preferably one or more of 1-chloromethyl acrylate, 1-bromomethyl acrylate, 1-iodomethyl acrylate, 2-chloroethyl acrylate, 2-bromoethyl acrylate, 2-iodoethyl acrylate, 3-chloropropyl acrylate, 3-bromopropyl acrylate, 3-iodopropyl acrylate, 1-chloromethyl methacrylate, 1-bromomethyl methacrylate, 1-iodomethyl methacrylate, 2-chloroethyl methacrylate, 2-bromoethyl methacrylate, 2-iodoethyl methacrylate, 3-chloropropyl methacrylate, 3-bromopropyl methacrylate or 3-iodopropyl methacrylate, such as 2-bromoethyl methacrylate.

[0080] In one embodiment, in the quaternization reaction, the molar ratio of the compound represented by formula f to the compound represented by formula c is 1:(0.1-1), preferably 1:(0.3-1), for example 1:0.5.

[0081] In one embodiment, the temperature of the quaternization reaction is 40-100°C, more preferably 70-90°C, for example 80°C.

[0082] In a certain embodiment, in the quaternization reaction, the preparation method of the compound represented by formula B preferably comprises the following steps: reacting the compound represented by formula c with the compound represented by formula f at 40 to 100° C. in the solvent.

[0083] In a certain scheme, in the quaternization reaction, the method for preparing the compound shown in Formula B preferably further comprises the following post-treatment steps after the reaction is completed: cooling, removing the solvent under reduced pressure, and separating the mixture by column chromatography to obtain a white solid compound. Among them, the eluent is preferably a mixed solvent of a halogenated alkane solvent and an alcohol solvent, and the volume ratio of the halogenated alkane solvent to the alcohol solvent is preferably (100-10):1; the halogenated alkane solvent is preferably dichloromethane; and the alcohol solvent is preferably methanol.

[0084] The present invention also provides the use of the compound shown in formula I as described above as an emulsifier;

[0085] The emulsifier is preferably used as an emulsifier for acrylic ester monomers and water systems.

[0086] The compound as shown in formula I is preferably used together with allyloxy nonylphenol polyoxyethylene ether ammonium sulfate (DNS-86) to form a composite emulsifier as an emulsifier for the acrylic ester monomer and water system.

[0087] The present invention further provides an acrylic acid ester polymer, which is prepared by the following polymerization reaction:

[0088] In the presence of an emulsifier, the compound represented by formula I and the compound represented by formula II are polymerized to obtain an acrylic acid ester polymer;

[0089]

[0090] In Formula II, R7 and R8 are independently C 1-6 alkyl.

[0091] In one embodiment, the compound as shown in formula II is one or more of butyl methacrylate (BMA), methyl methacrylate (MMA) or 2-ethylbutyl acrylate, such as BMA and / or MMA.

[0092] In one embodiment, the emulsifier is allyloxy nonylphenol polyoxyethylene ether ammonium sulfate (DNS-86).

[0093] In a certain embodiment, the compound shown in formula I is the compound shown in formula A-1 as described above or the compound shown in formula B-1, preferably the compound shown in formula B-1.

[0094] In a certain embodiment, the weight proportion of the compound represented by formula II is 0.1 to 10 parts, preferably 0.1 to 4 parts.

[0095] In a certain embodiment, the weight proportion of the emulsifier is 0.01 to 0.1 parts, preferably 0.02 to 0.08 parts, for example 0.06 parts.

[0096] In a certain embodiment, the weight proportion of the compound as shown in Formula I is 0.01 to 0.1 parts, preferably 0.01 to 0.05 parts, for example 0.02 parts.

[0097] In a certain embodiment, the weight proportion of BMA is 0.1 to 5 parts, preferably 0.1 to 2 parts, for example 1.232 parts.

[0098] In a certain embodiment, the weight proportion of the MMA is 0.01 to 1 part, preferably 0.01 to 0.5 part, for example 0.328 part.

[0099] In one embodiment, the acrylic polymer is prepared by the following polymerization reaction: 1.232 parts of the BMA, 0.328 parts of the MMA and 0.02 parts of the compound represented by formula B-1 are polymerized in the presence of 0.06 parts of DNS-86 to obtain the acrylic polymer.

[0100] In one embodiment, the acrylic acid ester polymer as described above is prepared by polymerization reaction as follows:

[0101] Step 1: In the presence of the emulsifier, the compound of formula I, the compound of formula II and a solvent are mixed to obtain a pre-emulsion;

[0102] Step 2: In the presence of an initiator, the pre-emulsion in step 1, the emulsifier and the solvent are mixed and a reaction is initiated to obtain a reaction solution;

[0103] Step 3: Mix the pre-emulsion in step 1, the initiator and the reaction solution in step 2 and perform polymerization reaction to obtain the acrylic polymer.

[0104] In one embodiment, the solvent is water, such as distilled water.

[0105] In one embodiment, in step 2 and step 3, the initiator is ammonium persulfate (APS); preferably, the APS is used in the form of an aqueous solution of APS; the total weight fraction of the initiator in step 2 and step 3 is preferably 0.01 to 0.05 parts, for example 0.0267 parts.

[0106] In one embodiment, the weight proportion of the solvent is 0.5 to 10 parts, such as 1 to 6 parts.

[0107] In one embodiment, the total weight of the pre-emulsion is 1 to 10 parts, for example 3.1 parts, wherein the total weight of the pre-emulsion refers to the weight of the pre-emulsion obtained in step 1.

[0108] In one embodiment, in step 1, the weight proportions of the monomers are as described above, wherein the weight proportion of the emulsifier is 0.01 to 0.05 parts, for example, 0.02 parts.

[0109] In one embodiment, in step 2, the weight portion of the emulsifier is 0.02 to 0.06 parts, for example, 0.04 parts.

[0110] In one embodiment, in step 2, the weight ratio of the initiator to the total weight of the initiators is 1:3.

[0111] In one embodiment, in step 2, the weight ratio of the pre-emulsion to the total weight of the pre-emulsion is 1:3.

[0112] In one embodiment, in step 1, the mixing temperature is 10-40°C, for example, 25°C.

[0113] In one embodiment, in step 2, the mixing temperature is 30-90°C, for example, 60°C.

[0114] In one embodiment, in step 3, the polymerization reaction time is 0.5 to 5 hours.

[0115] In one embodiment, in step 3, the polymerization reaction temperature is 50-100°C, for example, 70°C.

[0116] The present invention provides an antibacterial agent, which comprises the acrylic ester polymer as described above. The antibacterial agent is preferably used for inhibiting Staphylococcus aureus and / or Escherichia coli.

[0117] The present invention provides an emulsion, which comprises the acrylic acid ester polymer as described above.

[0118] The present invention further provides a compound as shown in formula a;

[0119]

[0120] Among them, n, R f , R1, R2, R3 and R4 are defined as above.

[0121] In a certain embodiment, the compound shown in formula a is preferably the following compound:

[0122]

[0123] The present invention further provides a compound as shown in formula b;

[0124]

[0125] Among them, n, R f , R1, R2, R3, R6 and X- are defined as above.

[0126] In a certain embodiment, the compound shown in formula b is preferably the following compound:

[0127]

[0128] Without violating the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention.

[0129] The reagents and raw materials used in the present invention are commercially available.

[0130] The positive and progressive effects of the present invention are:

[0131] 1. The fluorocarbon surfactant of the present invention is a white powder or a paste-like solid, and is an amphoteric fluorocarbon surfactant. After reducing the length of the fluorocarbon chain, it can also significantly reduce the surface tension of the aqueous solution.

[0132] 2. The fluorocarbon surfactant of the present invention can be used as an emulsifier for acrylic ester monomers and water systems, has excellent emulsifying properties, can form a stable emulsion, and can also form a compound emulsifier together with DNS-86.

[0133] 3. The product obtained by polymerization of the fluorocarbon surfactant of the present invention has excellent water-repellent, oil-repellent and antibacterial properties. The contact angle WCA of the product to water is 85.42°, the contact angle HCA to cyclohexane is 10.13°, and the antibacterial effect on Staphylococcus aureus and Escherichia coli is strong. BRIEF DESCRIPTION OF THE DRAWINGS

[0134] Figure 1 The surface tension of the aqueous solution of the compound prepared in Examples 1 to 3 varies with concentration, wherein surface tension refers to the surface tension, log C / mol·L -1 is the logarithmic value of the concentration.

[0135] Figure 2 These are the emulsion morphology diagrams of emulsion 1 and emulsion 2.

[0136] Figure 3 Water contact angle diagrams of the coatings of emulsion 1 and emulsion 2.

[0137] Figure 4 Cyclohexane contact angle diagrams of the coatings of emulsion 1 and emulsion 2.

[0138] Figure 5 This is the antibacterial performance diagram of the coating of emulsion 1, where None means no inhibitory effect on Aspergillus niger.

[0139] Figure 6 This is the antibacterial performance diagram of the coating of emulsion 2, where None means no inhibitory effect on Aspergillus niger. DETAILED DESCRIPTION

[0140] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.

[0141] Unless otherwise specified, the room temperature in the following embodiments refers to 20-40°C. The synthesis method of compound 1 can be found in CN109851529B, (Synthesis and combined properties of novel fluorinated cationicsurfactants derived from hexafluoropropylene dimer, DOI: 10.1016 / j.cclet.2018.04.017), (Synthesis and combined properties of novel branched fluorocarbon surfactants, DOI: 10.6023 / cjoc201806014).

[0142] Example 1

[0143] This embodiment provides a method for synthesizing an amphoteric fluorocarbon surfactant, which specifically comprises the following steps:

[0144] (1) 0.63 g (1.2 mmol, 1.0 equiv) of compound 1, 0.37 g (2.4 mmol, 2.0 equiv) of iodoethane and 7.0 mL of anhydrous tetrahydrofuran were reacted at 80°C in a 50 mL sealed tube under argon protection. The reaction progress was monitored by TLC and the reaction was completed after 12 h. The system was cooled to room temperature and the solvent was removed under reduced pressure. The solid was washed with acetone, filtered, and then dissolved in methanol. After removing the solvent, a white solid compound 2 was obtained.

[0145] (2) Add 5.10 g (7.35 mmol, 1.0 equiv) of compound 2, 30.0 g of 717 strong base ion exchange resin and 50 mL of anhydrous methanol into a 150 mL round-bottom flask and stir at room temperature for 12 hours. Filter the reaction system, collect the filtrate, add 0.69 mL (8.1 mmol, 1.1 equiv) of methacrylic acid to the filtrate, and stir at room temperature for 2 hours. Directly spin dry the solvent, and recrystallize from acetone solution to obtain white solid compound 3.

[0146] 1 H NMR (400MHz, CD3OD) δ7.86 (d, J = 8.3 Hz, 2H), 7.48 (d, J = 8.1 Hz, 2H), 5.72 (d, J = 1.5 Hz, 1H), 5.20 (dd, J = 2.3, 1.4 Hz, 1H), 3.84 (t, J = 6.8 Hz, 2H), 3.77 (s, 2H), 3.60–3.45 (m, 4H), 3.17 (s, 6H), 1.90 (s, 3H), 1.42 (t, J = 7.1 Hz, 3H). The synthetic route is as follows:

[0147]

[0148] Example 2

[0149] This embodiment provides a method for synthesizing an amphoteric fluorocarbon surfactant, which specifically comprises the following steps:

[0150] (1) 5.24 g (10.0 mmol, 1.0 equiv) of compound 1, 2.50 g (20 mmol, 2.0 equiv) of bromoethanol and 60.0 mL of anhydrous tetrahydrofuran were reacted in a 200 mL three-necked flask under argon protection at 80°C. The reaction progress was monitored by TLC and the reaction was completed after 60 h. The system was cooled to room temperature, 2.53 g (25 mmol, 2.5 equiv) of triethylamine was added, and 2.61 g (25 mmol, 2.5 equiv) of methacryloyl chloride was added dropwise under an ice-water bath. The system was gradually restored to room temperature and stirred for 12 h. The mixture was filtered and the solvent was removed under reduced pressure. Finally, the mixture was separated by column chromatography (dichloromethane: methanol = 20:1) to obtain a white solid compound 5.

[0151] 1 H NMR (400MHz, DMSO-d6) δ9.22 (t, J = 5.3Hz, 1H), 7.89 (d, J = 8.4Hz, 2H), 7.42 (d, J = 8.1Hz, 2H), 6.06 (t, 1H), 5.72 (t, 1H), 4.54 (s, 2H), 3.88–3.73 (m, 4H), 3.65 (dt, J = 27.3, 5.9Hz, 4H), 3.20 (s, 6H), 1.87 (s, 3H). Its synthesis route is as follows:

[0152]

[0153] Example 3

[0154] This embodiment provides a method for synthesizing an amphoteric fluorocarbon surfactant, which specifically comprises the following steps:

[0155] (1) 5.24 g (10.0 mmol, 1.0 equiv) of compound 1, 3.86 g (20 mmol, 2.0 equiv) of 2-bromoethyl methacrylate and 60.0 mL of anhydrous tetrahydrofuran were reacted at 80°C in a 200 mL three-necked flask under argon protection. The reaction progress was monitored by TLC, and the reaction was completed after 100 h. The system was cooled to room temperature, and the solvent was removed under reduced pressure. Finally, the mixture was separated by column chromatography (dichloromethane:methanol=20:1) to obtain white solid compound 5. 1H NMR (400MHz, DMSO-d6) δ9.22(t,J=5.3Hz,1H),7.89(d,J=8.4Hz,2H),7.42(d,J=8.1Hz,2H),6.06(t,1H ),5.72(t,1H),4.54(s,2H),3.88–3.73(m,4H),3.65(dt,J=27.3,5.9Hz,4H),3.20(s,6H),1.87(s,3H).

[0156] Its synthetic route is as follows:

[0157]

[0158] Effect Example 1 Surface tension test of aqueous solutions of compound 3 and compound 5

[0159] At 25°C, the surface tension of aqueous solutions of various compounds at different concentrations was measured using a German Kruss fully automatic surface tension meter K100 plate method to obtain the data in Table 1.

[0160] Table 1. Surface tension values ​​of aqueous solutions of compounds at different concentrations

[0161]

[0162] The surface tension of the aqueous solutions of the compounds 3 and 5 prepared in Examples 1 to 3 varies with concentration, wherein surface tension refers to the surface tension, log C / mol*L -1 is the logarithmic value of the concentration (see Figure 1 ).

[0163] Among them, compound 3: CMC (mol / L) is 1.15×10 -3 ; γ cmc (mN / m) is 19.02. Compound 5: CMC (mol / L) is 6.58×10 -4 ; γ cmc (mN / m) is 23.24. (γ cmc CMC is the critical micelle concentration, which is the lowest concentration of surfactants in the solvent when they associate to form micelles. When this concentration is reached, the surface tension of the solvent no longer decreases with increasing concentration.

[0164] At the same time, as a comparison, the present invention and the commercially available product Dupont TM 1157, 3M TM The relevant values ​​of compound 4a in FC 4430 and CN109851529B are shown in Table 2 below, where Dupont TM 1157 and 3MTM The data of FC 4430 are respectively derived from the product manuals published by American Como Chemicals (formerly DuPont Performance Chemicals Division) and American 3M Company.

[0165]

[0166] Table 2 Comparison of surface tension values ​​of aqueous solutions

[0167]

[0168] As can be seen from the table, the surface activity of compound 3 is similar to that of the commercially available product 3M TM The surface activity of FC 4430 is comparable, and the surface activity of compound 5 is better than that of the commercial product 3M TM The surface activity of FC 4430 is comparable to that of compound 4a in CN109851529B, and is comparable to that of the commercially available product Dupont TM 1157 have comparable surface activity.

[0169] Example 4 (Compound used as polymerizable emulsifier in emulsion polymerization):

[0170] Emulsion 1: 1.232g BMA, 0.328g MMA, 0.04g DNS-86 and 1.5g distilled water were placed in a container and stirred vigorously for 0.5 hours to form a pre-emulsified pre-emulsion. 0.04g DNS-86, 1 / 3 APS aqueous solution (0.04g APS dissolved in 3mL distilled water), 1 / 3 pre-emulsified emulsion and 1.5mL distilled water were added to a 20mL three-necked flask, and stirred at 250rpm for 20 minutes at 60°C. The system was successfully initiated and a blue phase appeared. The temperature was gradually raised to 70°C, and the remaining 2 / 3 pre-emulsified pre-emulsion and 1 / 3 APS aqueous solution were slowly added dropwise for 90 minutes. After the addition was completed, the system continued to stir and react for 2 hours. Emulsion 1 was prepared.

[0171] Emulsion 2: 1.232g BMA, 0.328g MMA, 0.02g DNS-86, 0.02g compound 5 and 1.5g distilled water were placed in a container and stirred vigorously for 0.5 hours to form a pre-emulsified pre-emulsion. 0.04g DNS-86, 1 / 3 APS aqueous solution (0.04g APS dissolved in 3mL distilled water), 1 / 3 pre-emulsified emulsion and 1.5mL distilled water were added to a 20mL three-necked flask, and stirred at 250rpm for 20 minutes at 60°C. The system was successfully initiated and a blue phase appeared. The temperature was gradually raised to 70°C, and the remaining 2 / 3 pre-emulsified pre-emulsion and 1 / 3 APS aqueous solution were slowly added dropwise for 90 minutes. After the addition was completed, the system continued to stir and react for 2 hours. Emulsion 2 was prepared.

[0172] During the preparation of emulsion 2, 0.02 g of compound 5 and 0.02 g of DNS-86 can form a stable pre-emulsion, which is applied to the emulsion polymerization to synthesize acrylic polymer emulsion. The emulsion morphology is shown in FIG. Figure 2 .

[0173] Example 5 (Comparison of properties of different acrylic polymer coatings):

[0174] Preparation of emulsion coating: 0.2 g of emulsion 1 or emulsion 2 was taken, diluted to 1 mL with distilled water, and the coating was prepared on a clean glass surface by spraying, and then placed in an oven at 100°C for 2 hours for curing. Pure water and analytical grade cyclohexane were used to test the contact angle of the coating with water and cyclohexane.

[0175] from Figure 3 and Figure 4 It can be seen that compared with the coating formed by emulsion 1, the hydrophobic property of the coating formed by emulsion 2 has no significant change, but the oleophobicity (anti-cyclohexane) ability of the coating is significantly improved.

[0176] Example 6 (antibacterial properties of coating):

[0177] from Figure 5 and Figure 6 It can be seen that compared with the coating formed by emulsion 1, the antibacterial performance of the coating formed by emulsion 2 is significantly improved, and the inhibition zone after 96 hours in the Staphylococcus aureus and Escherichia coli culture dishes is still 2.1 cm and 1.6 cm, respectively.

Claims

1. A compound as shown in formula I, characterized in that, Wherein, n is 1, 2, 3 or 4; R f C substituted with one or more F 1-6 alkyl; R1 is -CH2- or -CH(OH)-; R2, R3 and R4 are each independently C 1-6 Alkyl or 1 R a Substituted C 1-6 alkyl; R a for X- is a halogen anion or R5 is H or C 1-6 alkyl; When R2, R3 and R4 are each independently C 1-6 When X is alkyl, - for 2. The compound as shown in formula I according to claim 1, characterized in that It meets one or more of the following conditions; (1) n is 1; (2)R f CF3(CF2)2C(CF3)2-; (3) R1 is -CH2-; (4) R2, R3 and R4 are each independently -CH3, -CH2CH3 or (5) R5 is -CH3; (6)X - Br - or 3. The compound as shown in formula I according to claim 1 or 2, characterized in that, The compound shown in formula I is a compound shown in formula A or a compound shown in formula B: Among them, n, R f , R1, R2, R3, R4, R5 and X- are as defined in claim 1 or 2; In formula B, R6 is C 1-6 Alkylene; Preferably, in formula B, R6 is -CH2CH2-; Preferably, in formula B, X- is a halogen anion, such as X - Br - .

4. The compound as shown in formula I according to claim 1, characterized in that The compound of formula I is a compound of formula A-1 or a compound of formula B-1; 5. A method for preparing the compound of formula I as claimed in any one of claims 1 to 4, characterized in that: It is either Method 1, Method 2 or Method 3: Method 1: It includes the following steps: In a solvent, a compound represented by formula a and a compound represented by formula d are subjected to a neutralization reaction; Among them, n, R f , R1, R2, R3, R4 and R5 are defined as any one of claims 1 to 4; Method 2: It includes the following steps: In a solvent, the compound represented by formula b and the compound represented by formula e are subjected to condensation reaction; Among them, n, R f , R1, R2, R3, R5, R6 and X- are defined as any one of claims 1 to 4; Method 3: It includes the following steps: In a solvent, a compound represented by formula c and a compound represented by formula f are subjected to a quaternization reaction; Among them, n, R f , R1, R2, R3, R5, R6 and X- are defined as in any one of claims 1 to 4.

6. Use of the compound of formula I as claimed in any one of claims 1 to 4 as an emulsifier; The emulsifier is preferably used as an emulsifier for acrylic ester monomers and water systems; The compound as shown in formula I is preferably used together with DNS-86 to form a composite emulsifier as an emulsifier for the acrylic ester monomer and water system.

7. An acrylic acid ester polymer, characterized in that: It is prepared by the following polymerization reaction: In the presence of an emulsifier, polymerizing the compound represented by formula I according to any one of claims 1 to 4 and the compound represented by formula II to obtain an acrylic acid ester polymer; In Formula II, R7 and R8 are independently C 1-6 alkyl.

8. The acrylic polymer according to claim 7, characterized in that It meets one or more of the following conditions: (1) The compound represented by formula II is one or more of BMA, MMA or 2-ethylbutyl acrylate, such as BMA and / or MMA; (2) The emulsifier is DNS-86; (3) The compound of formula I is the compound of formula A-1 or the compound of formula B-1 as claimed in claim 4, preferably the compound of formula B-1; (4) The weight proportion of the compound represented by formula II is 0.1 to 10 parts, preferably 0.1 to 4 parts; (5) The weight percentage of the emulsifier is 0.01 to 0.1 parts, preferably 0.02 to 0.08 parts, for example 0.06 parts; (6) The weight proportion of the compound of formula I is 0.01 to 0.1 parts, preferably 0.01 to 0.05 parts, for example 0.02 parts.

9. The acrylic polymer according to claim 8, characterized in that It meets one or both of the following conditions: (1) The weight proportion of BMA is 0.1 to 5 parts, preferably 0.1 to 2 parts, for example 1.232 parts; (2) The weight proportion of the MMA is 0.01 to 1 part, preferably 0.01 to 0.5 part, for example 0.328 part.

10. The acrylic polymer according to claim 9, characterized in that The acrylic polymer is prepared by the following polymerization reaction: in the presence of 0.06 parts of DNS-86, 1.232 parts of the BMA, 0.328 parts of the MMA and 0.02 parts of the compound represented by formula B-1 are polymerized to obtain the acrylic polymer.

11. The acrylic acid ester polymer according to any one of claims 7 to 10, wherein The acrylic acid ester polymer is prepared by polymerization reaction as follows: Step 1: In the presence of the emulsifier, the compound of formula I, the compound of formula II and a solvent are mixed to obtain a pre-emulsion; Step 2: In the presence of an initiator, the pre-emulsion in step 1, the emulsifier and the solvent are mixed and a reaction is initiated to obtain a reaction solution; Step 3: mixing the pre-emulsion in step 1, the initiator and the reaction solution in step 2 and subjecting them to polymerization reaction to obtain the acrylic polymer; The solvent is preferably water, such as distilled water; In the step 2 and the step 3, the initiator is preferably APS; further preferably, the APS is used in the form of an aqueous solution of APS; the total weight fraction of the initiator in the step 2 and the step 3 is preferably 0.01 to 0.05 parts, for example 0.0267 parts; The weight proportion of the solvent is preferably 0.5 to 10 parts, such as 1 to 6 parts; The total weight of the pre-emulsion is preferably 1 to 10 parts, for example 3.1 parts; In the step 1, the weight portion of the emulsifier is preferably 0.01 to 0.05 parts, for example 0.02 parts; In the step 2, the weight portion of the emulsifier is preferably 0.02 to 0.06 parts, for example 0.04 parts; In the step 2, the weight ratio of the initiator to the total weight of the initiators is preferably 1:3; In the step 2, the weight ratio of the pre-emulsion to the total weight of the pre-emulsion is preferably 1:3; In the step 1, the mixing temperature is preferably 10-40°C, for example 25°C; In the step 2, the mixing temperature is preferably 30 to 90°C, for example 60°C; In the step 3, the polymerization reaction temperature is preferably 50-100°C, for example 70°C.

12. An antibacterial agent, characterized in that It comprises the acrylic acid ester polymer according to any one of claims 7 to 11, The antibacterial agent is preferably used to inhibit Staphylococcus aureus and / or Escherichia coli.

13. An emulsion, characterized in that It comprises the acrylic ester polymer according to any one of claims 7 to 11.

14. A compound represented by formula a or a compound represented by formula b: in, n、R f , R1, R2, R3, R4, R6 and X - The definitions are as described in any one of claims 1 to 4; Preferably, the compound represented by formula a is the following compound: Preferably, the compound shown in formula b is the following compound:

Citation Information

Cited By

  • Bio-based surfactant, fluorinated acrylate polymer and preparation method

    CN119874841B