Polystyrene carrier Ziegler-Natta catalyst with low ash content and high activity and preparation method of polystyrene carrier Ziegler-Natta catalyst

Through the suspension polymerization method and surface modification technology of polystyrene support, low ash and high activity Ziegler-Natta catalysts were prepared, which solved the catalyst morphology and ash problems and improved the activity and application prospects of the catalyst.

CN118955768APending Publication Date: 2024-11-15NORTH HUAJIN CHEM IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411073493.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing Ziegler-Natta catalysts have problems in terms of morphology, particle size distribution and titanium adhesion points. Moreover, due to the use of MgCl2 support, the ash of polymer is difficult to deal with, which limits the application scenarios of polyolefin products, especially in high performance. and precise structural control aspects.

Method used

Polystyrene as a support is used to prepare particulate support by suspension polymerization, and surface modification and active component loading are carried out. Combined with heat treatment and post-treatment steps, low ash, high active Ziegler-Natta catalyst was prepared, using aqueous ethanol solution and coupling. The agent was subjected to surface modification, TiCl4 and fluorene diether were added, and a constant temperature reaction and hot nitrogen treatment were carried out, and a high-active catalyst was obtained by vacuum drying.

Benefits of technology

The good chemical stability and particle size distribution of the catalyst are achieved, the number of active sites supported by titanium is improved, and the ash content of the polymerization product is significantly reduced. It is suitable for polypropylene application scenarios with low ash requirements, such as high-voltage cable coating materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955768A_ABST
    Figure CN118955768A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of catalysts, and in particular discloses a polystyrene carrier Ziegler-Natta catalyst with low ash content and high activity and a preparation method of the polystyrene carrier Ziegler-Natta catalyst. The preparation method comprises the following steps: preparing polystyrene microspheres by using a suspension polymerization method to prepare a carrier, preparing a coupling agent by using an ethanol aqueous solution to carry out surface modification, carrying titanium by using an impregnation method, and carrying out heat treatment and post-treatment on the catalyst to prepare the catalyst. The catalyst can realize good chemical stability and particle size distribution, has a designable pore structure, and can effectively increase the number of titanium-loaded active sites. Through verification, compared with a traditional magnesium chloride carrier, the organic carrier can obviously reduce the ash content of a polymerization product, and has a good application prospect for polypropylene application scenes with low ash content requirements, such as a high-voltage cable coating material and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of catalysts, and specifically discloses a polystyrene carrier low-ash and high-activity Ziegler-Natta catalyst and a preparation method thereof. Background Art

[0002] Ziegler-Natta (ZN) catalysts are widely used in the field of olefin polymerization due to their high efficiency and selectivity in chemical reactions. Up to now, five generations of ZN catalysts have been developed, with good high activity and high directional ability. The prepared catalysts are spherical particles, which can produce spherical polyolefin particles with a diameter of 1 to 5 mm through the polymerization reaction reappearance effect.

[0003] However, it cannot be ignored that due to the limitations of carrier preparation, the current catalysts are still not ideal in solving problems such as morphology, particle size distribution and titanium attachment points. In addition, due to the use of MgCl2 carrier, the ash content of the resulting polymer is also difficult to handle, which to a certain extent limits the application scenarios of polyolefin products. There is a huge obstacle in the transformation of the polyolefin industry from focusing on high activity and high orientation to focusing on product series and high performance, precisely controlling the structure of polymers, producing various special products and then increasing value-added products.

[0004] Therefore, it is necessary to develop a new Ziegler-Natta (ZN) catalyst to solve the above problems in terms of morphology, particle size distribution, titanium attachment points and ash content of the polymerization products. Summary of the invention

[0005] The technical solution adopted by the present invention is as follows:

[0006] In a first aspect, the present invention provides a method for preparing a polystyrene carrier low-ash, high-activity Ziegler-Natta catalyst, comprising the following steps:

[0007] S1 carrier preparation: 0.1-1 parts by mass of benzoyl oxide (BPO) is dissolved in 1-5 parts by volume of styrene to make the BPO concentration be 0.02-1 g / mL; after the BPO is dissolved, 10-20 parts by volume of a polyvinyl alcohol (PVA) solution with a mass concentration of 3-8% is added and mixed to obtain a suspension; the mixed suspension is heated to 70-90°C and kept warm for 90-150 minutes, cooled naturally to room temperature, and then filtered and dried to obtain a polystyrene microparticle carrier;

[0008] S2 surface modification: preparing a coupling agent solution with a mass concentration of 0.1-2% with a 60-80% (v) ethanol aqueous solution, adjusting the pH of the coupling agent solution to 4-5, adding the polystyrene microparticles prepared in step S1 for surface modification to enhance the binding between the polystyrene microparticles and the catalytic active components, and obtaining a surface-modified polystyrene carrier;

[0009] S3 active component loading: adding TiCl4 to the surface-modified polystyrene carrier obtained in step S2, stirring and heating to 80-110°C, then adding fluorene diether, and maintaining a constant temperature to react fully to obtain loaded polystyrene; the concentration ratio of the polystyrene carrier to TiCl4 is not less than 1 g / L; the molar ratio of the added TiCl4 to fluorene diether is 150:1-50:1;

[0010] S4 catalyst heat treatment: heat treating the loaded polystyrene obtained in step S3 with hot nitrogen at 50-80°C;

[0011] S5 catalyst post-treatment: washing to remove the unreacted substances on the surface of the supported ZN catalyst obtained in step S4, and vacuum drying to finally obtain a polystyrene-supported high-activity ZN catalyst.

[0012] Preferably, the coupling agent in step S2 includes any one of methacrylate silane coupling agent, isocyanate silane coupling agent, cyclomethoxy silane coupling agent, α-methyl methacrylate, γ-methyl methacrylate, or a mixture of two or more thereof.

[0013] Preferably, in step S2, acetic acid is used to adjust the solution to a pH of 4 to 5.

[0014] Preferably, in step S3, the isothermal reaction time is 1 to 3 hours.

[0015] Preferably, in step S4, the time for heat treatment with hot nitrogen is not less than 2 hours.

[0016] Preferably, in step S5, the solvent used is hexane.

[0017] Furthermore, in step S5, the vacuum drying temperature is 50-70° C., and the drying time is not less than 3 hours.

[0018] In a second aspect, the present invention provides a polystyrene-supported low-ash, high-activity Ziegler-Natta catalyst, which is prepared by the method described in the first aspect.

[0019] In a third aspect, the present invention provides a use of the polystyrene-supported high-activity ZN catalyst described in the first aspect for catalytic preparation of polypropylene.

[0020] Preferably, the polypropylene is polymerized by a propylene gas phase slurry method, which specifically comprises the following steps: adding hexane as a solvent into a reaction kettle, introducing propylene gas into the kettle to dissolve to saturation, dispersing the prepared ZN catalyst with hexane, and then adding an external electron donor and a co-catalyst of the ZN catalyst to carry out a catalytic reaction.

[0021] Beneficial effects achieved by the present invention:

[0022] The present invention proposes to use polystyrene as a carrier of ZN catalyst. Under the proposed synthesis process, it has been able to achieve good chemical stability and particle size distribution, and it has a designable pore structure, which can effectively increase the number of active sites of titanium. At the same time, it has been verified that compared with the traditional magnesium chloride carrier, the use of an organic carrier can significantly reduce the ash content of the polymer product, and has good application prospects for polypropylene application scenarios with low ash requirements, such as high-voltage cable sheathing materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a flow chart for preparing the polystyrene-supported high-activity ZN catalyst of the present invention;

[0024] Figure 2 The transmission electron microscopy image of the polystyrene microsphere carrier described in the embodiment of the present invention is

[0025] (a) Example 1 (b) Example 2 (c) Example 3;

[0026] Figure 3 Transmission electron microscopy image of the catalyst described in the embodiment of the present invention

[0027] (a) Example 1 (b) Example 2 (c) Example 3 DETAILED DESCRIPTION

[0028] In order to make the purpose, technical solution and advantages of the present invention more clear, the present invention is further described in detail in conjunction with the following examples. It should be noted that the present invention is not limited to the following examples.

[0029] Example 1

[0030] A novel polystyrene-supported high-activity ZN catalyst, the preparation process is as follows Figure 1 As shown, the specific steps include:

[0031] S1. Preparation of polystyrene carrier

[0032] Prepare polystyrene microparticles by suspension polymerization. Take 0.3g of benzoyl peroxide (BPO) and 3mL of styrene in a conical flask, shake until the solid is dissolved, then add 15mL of 5% polyvinyl alcohol (PVA) solution, shake and stir, rinse the conical flask three times with 30mL of deionized water, and pour the liquid in the conical flask after rinsing into a three-necked flask, adjust the stirring speed to 400rpm, and stir at room temperature for 50min. Heat to 80℃, keep warm for 90min, cool naturally to room temperature, and then filter and dry. The transmission electron microscope image is as follows Figure 2 a;

[0033] S2. Surface modification

[0034] 100 mL of a 0.2% mass fraction of γ-methyl methacrylate solution was prepared with an ethanol-water solution in a volume ratio of 3:1, the pH of the mixed solution was adjusted to 5 with acetic acid, and 5 g of polystyrene particles prepared by S1 were added for surface modification.

[0035] S3. Active component loading

[0036] Titanium was loaded by impregnation. 100 mL of titanium tetrachloride was added to the surface-modified polystyrene carrier prepared by 0.5 g S2, and then stirred and heated to 90 °C, and then fluorene diether was added (the molar ratio of TiCl4 to fluorene diether was 100:1), and the reaction was kept at a constant temperature for 2 h;

[0037] S4. Catalyst heat treatment

[0038] Hot nitrogen at 70°C was blown into the catalyst obtained in S3 for 2 h.

[0039] S5. Catalyst post-treatment

[0040] The catalyst obtained from S4 was washed four times with white oil (200 mL each time) to remove the unreacted substances on its surface, and then vacuum dried at 60°C to finally obtain an active ZN catalyst, the transmission electron microscopy image of which is shown in FIG. Figure 3 a.

[0041] S6. Propylene gas phase slurry polymerization: Add 700 mL of purified hexane as solvent into the reactor, introduce propylene gas into the reactor until it dissolves to saturation, weigh 0.01 g of the ZN catalyst prepared in S5, disperse it with hexane, add 0.5 mL of methoxysilane and 1 mL of triethylaluminum (0.1 M, hexane as solvent), and react at 70°C and 0.7 MPa for 4 hours.

[0042] The product PP was subjected to five voltage breakdown tests, and the test results are shown in Table 1 (test standard: GB / T1408-2006; test method: AC test; voltage rise rate: 0.5 kV / s; test method: breakdown test; humidity 30%; temperature 23°C), and the catalyst activity is shown in Table 2 (calculation method: mass kg of PP obtained by polymerization after sufficient drying / mass g of catalyst added in polymerization, the same below).

[0043] Example 2

[0044] Preparation of novel polystyrene-supported high-activity ZN catalyst:

[0045] S1. Preparation of polystyrene carrier

[0046] Prepare polystyrene microparticles by suspension polymerization. Take 0.3g of benzoyl peroxide (BPO) and 5mL of styrene in a conical flask, shake until the solid is dissolved, then add 18mL of 5% polyvinyl alcohol (PVA) solution, shake and stir, rinse the conical flask three times with 30mL of deionized water, and pour the liquid in the conical flask into a three-necked flask to adjust the stirring speed, stir at room temperature for 50min. Start heating to 80℃, keep warm for 90min, cool naturally to room temperature, filter and dry, and its transmission electron microscope picture is as follows Figure 2 b;

[0047] S2. Surface modification

[0048] Use ethanol water solution with a volume ratio of 3:1 to prepare 0.2% methacrylate silane coupling agent

[0049] solution, adjusting the pH of the mixed solution to 5 with acetic acid, and adding the polystyrene microparticles prepared in S1 for surface modification.

[0050] S3. Active component loading

[0051] Titanium was loaded by impregnation method. 100 mL of titanium tetrachloride was added to the surface-modified polystyrene carrier prepared with 0.5 g of S2, and after stirring and heating to 90°C, fluorene diether was added (the molar ratio of TiCl4 to fluorene diether was 100:1), and the reaction was kept at constant temperature for 2 h.

[0052] S4. Catalyst heat treatment

[0053] Hot nitrogen at 70°C was blown into the catalyst obtained in S3 for 2 h.

[0054] S5. Catalyst post-treatment

[0055] The catalyst obtained in step S4 was washed four times with white oil (200 mL each time) to remove the unreacted substances on its surface, and then vacuum dried at 60° C. to finally obtain an active ZN catalyst, the transmission electron microscopy image of which is shown in FIG. Figure 3 b.

[0056] S6, propylene gas phase slurry polymerization: 700 mL of purified hexane was added to the reactor as solvent, propylene gas was introduced into the reactor, and the solution reached saturation. 0.01 g of the ZN catalyst prepared in S5 was weighed, dispersed in hexane, and then 0.5 mL of methoxysilane and 1 mL of triethylaluminum (0.1 M, hexane as solvent) were added, and the reaction was carried out at 70°C and 0.7 MPa for 4 hours. The product PP was subjected to five voltage breakdown tests, and the test results are shown in Table 1, and the catalyst activity is shown in Table 2.

[0057] Example 3

[0058] S1. Preparation of polystyrene carrier

[0059] Prepare polystyrene microparticles by suspension polymerization. Take 0.3g of benzoyl peroxide (BPO) and 7mL of styrene in a conical flask, shake until the solid is dissolved, then add 20mL of 5% polyvinyl alcohol (PVA) solution, shake and stir, rinse the conical flask three times with 30mL of deionized water, and pour the rinsed liquid into a three-necked flask to adjust the stirring speed and stir at room temperature for 50min. Start heating to 80℃, keep warm for 90min, cool naturally to room temperature, and then filter and dry. The transmission electron microscope image is as follows Figure 2 c;

[0060] S2. Surface modification

[0061] A 0.2% mass fraction cyclomethoxysilane coupling agent solution was prepared with an ethanol-water solution in a volume ratio of 3:1, the pH of the mixed solution was adjusted to 5 with acetic acid, and the polystyrene particles prepared by S1 were added for surface modification.

[0062] S3. Active component loading

[0063] Titanium was loaded by impregnation method. 100 mL of titanium tetrachloride was added to the surface-modified polystyrene carrier prepared with 0.5 g of S2, and after stirring and heating to 90°C, fluorene diether was added (the molar ratio of TiCl4 to fluorene diether was 100:1), and the reaction was kept at constant temperature for 2 h.

[0064] S4. Catalyst heat treatment

[0065] Hot nitrogen at 70°C was blown into the catalyst obtained in S3 for 2 h.

[0066] S5. Catalyst post-treatment

[0067] The catalyst obtained in step S4 was washed four times with white oil (200 mL each time) to remove the unreacted substances on its surface, and then vacuum dried at 60° C. to finally obtain an active ZN catalyst, the transmission electron microscopy image of which is shown in FIG. Figure 3 c.

[0068] S6, propylene gas phase slurry polymerization: 700 mL of purified hexane was added to the reactor as solvent, propylene gas was introduced into the reactor, and the solution reached saturation. 0.01 g of the ZN catalyst prepared in S5 was weighed, dispersed in hexane, and then 0.5 mL of methoxysilane and 1 mL of diethylaluminum monochloride (0.1 M, hexane as solvent) were added, and the reaction was carried out at 70°C and 0.7 MPa for 4 h. The product PP was subjected to five voltage breakdown tests, and the test results are shown in Table 1, and the catalyst activity is shown in Table 2.

[0069] Table 1 Test results of PP voltage breakdown test of products obtained in Examples 1, 2 and 3

[0070]

[0071]

[0072] Table 2 Catalyst activities of Examples 1, 2, and 3

[0073]

[0074] Using the test method GB / T 9345.1-2008 Method A and a test temperature of 850° C., the ash contents of the products PP obtained in Examples 1, 2, and 3 were 42 ppm, 38 ppm, and 33 ppm, respectively.

[0075] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a polystyrene-supported low-ash, high-activity Ziegler-Natta catalyst, It is characterized in that The following steps are involved: S1 carrier preparation: 0.1-1 parts by mass of benzoyl oxide (BPO) is dissolved in 1-5 parts by volume of styrene to make the BPO concentration be 0.02-1 g / mL; after the BPO is dissolved, 10-20 parts by volume of a polyvinyl alcohol (PVA) solution with a mass concentration of 3-8% is added and mixed to obtain a suspension; the mixed suspension is heated to 70-90°C and kept warm for 90-150 minutes, cooled naturally to room temperature, and then filtered and dried to obtain a polystyrene microparticle carrier; S2 surface modification: preparing a coupling agent solution with a mass concentration of 0.1-2% with a 60-80% (v) ethanol aqueous solution, adjusting the pH of the coupling agent solution to 4-5, adding the polystyrene microparticles prepared in step S1 for surface modification to enhance the binding between the polystyrene microparticles and the catalytic active components, and obtaining a surface-modified polystyrene carrier; S3 Active component loading: Take the surface-modified polystyrene carrier prepared in step S2 and add TiCl 4 , stirring and heating to 80-110°C, then adding fluorene diether, and maintaining constant temperature to react fully to obtain loaded polystyrene; polystyrene carrier and TiCl 4 The concentration ratio is not less than 1g / L; adding TiCl 4 The molar ratio of the fluorene diether is 150:1 to 50:1; S4 catalyst heat treatment: heat treating the loaded polystyrene obtained in step S3 with hot nitrogen at 50-80°C; S5 catalyst post-treatment: washing to remove the unreacted substances on the surface of the supported ZN catalyst obtained in step S4, and vacuum drying to finally obtain a polystyrene-supported high-activity ZN catalyst.

2. The polystyrene-supported low-ash, high-activity Ziegler-Natta catalyst according to claim 1, It is characterized in that The coupling agent in step S2 includes any one of methacrylate silane coupling agent, isocyanate silane coupling agent, cyclomethoxy silane coupling agent, α-methyl methacrylate, and γ-methyl methacrylate, or a mixture of two or more thereof.

3. The polystyrene-supported low-ash, high-activity Ziegler-Natta catalyst according to claim 1, It is characterized in that In the step S2, acetic acid is used to adjust the solution to a pH of 4 to 5.

4. The polystyrene-supported low-ash, high-activity Ziegler-Natta catalyst according to claim 1, It is characterized in that In step S3, the isothermal reaction time is 1 to 3 hours.

5. The polystyrene-supported low-ash, high-activity Ziegler-Natta catalyst according to claim 1, It is characterized in that In step S4, the heat treatment time of hot nitrogen is not less than 2 hours.

6. The polystyrene-supported low-ash, high-activity Ziegler-Natta catalyst according to claim 1, It is characterized in that In the step S5, the solvent used is hexane.

7. The polystyrene-supported low-ash, high-activity Ziegler-Natta catalyst according to claim 6, It is characterized in that In step S5, the vacuum drying temperature is 50-70° C., and the drying time is not less than 3 hours.

8. A polystyrene-supported low-ash, high-activity Ziegler-Natta catalyst prepared by the method of any one of claims 1 to 6.

9. Use of the polystyrene-supported low-ash, high-activity Ziegler-Natta catalyst as claimed in claim 8 in preparing polypropylene.

10. Use of the polystyrene-supported low-ash, high-activity Ziegler-Natta catalyst according to claim 9 for catalytic preparation of polypropylene, It is characterized in that The polypropylene is polymerized by a propylene gas phase slurry method, which specifically includes the following steps: adding hexane as a solvent into a reaction kettle, introducing propylene gas into the kettle to dissolve to saturation, dispersing the prepared ZN catalyst with hexane, and then adding an external electron donor and a co-catalyst of the ZN catalyst to carry out a catalytic reaction.