Dispersing agent, preparation method thereof and secondary battery
The core-shell structure or agglomerate is formed by polymer stabilizers and small molecule viscosity reducing agents, and combined with coupling agents, the problem of damage to the surface of the positive electrode material by existing dispersants is solved, and the dispersion and performance stability of lithium-ion batteries are improved. , achieving better slurry fluidity and battery performance.
Patent Information
- Application Number
- CN202411343655.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-25
- Publication Date
- 2024-11-15
AI Technical Summary
When used in lithium-ion battery positive electrode materials, the impact force is too strong, destroying the cladding layer on the surface of the positive electrode material and affecting battery performance.
The core-shell structure or agglomerate is formed by polymer stabilizers and small molecule viscosity reducing agents, and the colloid is formed by connecting them through coupling agents, which are preferred to adsorb on the surface of the positive electrode material, providing anchored active sites and steric hindrance to avoid agglomeration. At the same time, it avoids damage to the surface of the positive electrode material.
The dispersion of the positive electrode material and the fluidity of the slurry are improved, the stability of battery performance is maintained, the gelation and aggregation of the slurry is avoided, and the preparation efficiency and performance of lithium-ion batteries are improved.
Smart Images

Figure CN118955786A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of positive electrode materials, and in particular to a dispersant and a preparation method thereof, and a secondary battery. Background Art
[0002] The positive electrode sheet of a lithium-ion battery is composed of positive electrode materials, conductive glue, and a binder. When preparing the positive electrode sheet, the prepared positive electrode slurry needs to be coated on aluminum foil to make the positive electrode sheet. However, the positive electrode material is prone to gelation and agglomeration of active materials during the slurrying process, so the state of the slurry is directly related to the quality of the coating. At present, in order to increase the capacity of lithium batteries, the usual solution is to increase the proportion of positive electrode active materials in the slurry, which will further lead to an excessively high solid content of the slurry, and the slurry will become more viscous, resulting in poor fluidity, affecting the coating effect of the electrode, and further affecting the efficiency of the lithium battery preparation process.
[0003] Therefore, in order to prevent problems such as slurry gelation and active material agglomeration during the preparation of positive electrode material slurry, the prior art usually adds a dispersant during the preparation of positive electrode material slurry to improve the dispersion and uniformity of positive electrode material particles and avoid particle accumulation and agglomeration. However, the impact of the dispersant on the positive electrode material in the prior art is too strong, which will destroy the coating layer on the surface of the positive electrode material, thereby affecting various aspects of the battery performance. Summary of the invention
[0004] The purpose of the present application is to provide a dispersant and a preparation method thereof, and a secondary battery, so as to solve the problem that the existing dispersant impacts the surface of the positive electrode material and causes the battery performance to deteriorate.
[0005] To achieve the purpose of this application, this application provides the following technical solutions:
[0006] In a first aspect, the present invention provides a dispersant, comprising a polymer stabilizer and a small molecule viscosity reducer, wherein the polymer stabilizer and the small molecule viscosity reducer form a core-shell structure or an aggregate.
[0007] In one embodiment, the dispersant further comprises a coupling agent, and the polymer stabilizer is connected to the small molecule viscosity reducer via the coupling agent.
[0008] In one embodiment, the dispersant includes a core, an intermediate layer and an outer shell layer, the intermediate layer is coated on the outer surface of the core, the outer shell layer is coated on the outer surface of the intermediate layer, the core includes the polymer stabilizer, the intermediate layer includes the coupling agent, and the outer shell layer includes the small molecule viscosity reducer.
[0009] In one embodiment, the polymer stabilizer, the coupling agent and the small molecule viscosity reducer form a colloid.
[0010] In one embodiment, the coupling agent includes one or more of a silane coupling agent, a titanate coupling agent, a zirconate coupling agent, an aluminate coupling agent, a bimetallic coupling agent, a rare earth coupling agent, a phosphorus-containing coupling agent, and a boron-containing coupling agent.
[0011] In one embodiment, the mass ratio of the polymer stabilizer, the coupling agent and the small molecule viscosity reducer is (20-40):(2-12):100.
[0012] In one embodiment, the polymer stabilizer includes a first stabilizer and a second stabilizer, the first stabilizer and the second stabilizer are of different types, and the molecular weight of the first stabilizer is greater than the relative molecular weight of the second stabilizer.
[0013] In one embodiment, the ratio of the weight average molecular weight of the first stabilizer to the relative molecular mass of the second stabilizer is (2-500):1.
[0014] In one embodiment, the mass ratio of the first stabilizer to the second stabilizer is 100:(10-30).
[0015] In one embodiment, the polymer stabilizer includes one or more of polyethylene glycol and its derivatives, polyvinyl pyrrolidone and its derivatives, polyester and its derivatives, polyphosphates, and polyacrylates.
[0016] In one embodiment, the small molecule viscosity reducer includes one or more of phthalic anhydride, acetic anhydride, maleic anhydride, carbohydrazide, benzohydrazide, oxalic acid dihydrazide, carboamide, and cyanoacetamide.
[0017] In a second aspect, the present invention provides a method for preparing a dispersant, comprising: adding a polymer stabilizer to a solvent A and stirring the mixture thoroughly; then adding a small molecule viscosity reducer to the solvent A, and obtaining a dispersant after reaction and drying; in the dispersant, the polymer stabilizer and the small molecule viscosity reducer form a core-shell structure or agglomerates.
[0018] In a third aspect, the present invention provides a secondary battery, comprising a negative electrode plate, an electrolyte and a positive electrode plate, wherein the positive electrode plate comprises a current collector and a positive electrode material layer arranged on the current collector, the positive electrode plate and the negative electrode plate are arranged in the electrolyte, and the electrolyte can be a liquid electrolyte or a solid electrolyte; the positive electrode material comprises the dispersant described in the various embodiments of the first aspect.
[0019] The dispersant provided by the present invention includes a polymer stabilizer and a small molecule viscosity reducer. The small molecule viscosity reducer can be preferentially adsorbed on the surface of the positive electrode material and form anchored active sites on the surface of the positive electrode material, thereby avoiding mutual attraction and agglomeration between the positive electrode materials, thereby improving the dispersibility of the slurry. Due to the molecular weight limitation of the small molecule viscosity reducer, the impact force of the small molecule viscosity reducer on the surface of the positive electrode material is small and will not damage the coating layer on the surface of the positive electrode material, so that the battery performance remains stable; the polymer stabilizer can provide steric hindrance and electrostatic steric hindrance between the positive electrode material and the dispersant, thereby further avoiding the agglomeration of the positive electrode material affecting the slurry coating efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the implementation methods of the present application or the technical solutions in the prior art, the drawings required for use in the implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0021] Figure 1 is a cross-sectional view of a dispersant in one embodiment;
[0022] Figure 2 The present invention is a flow chart of a method for preparing a dispersant in one embodiment. DETAILED DESCRIPTION
[0023] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0024] Unless otherwise defined, all technical and scientific terms used in this application have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used in this application and in the specification are only for the purpose of describing specific embodiments and are not intended to limit this application. The term "and / or" used in this application includes any and all combinations of one or more of the related listed items.
[0025] In conjunction with the accompanying drawings, some embodiments of the present application are described in detail below. In the absence of conflict, the following embodiments and features in the embodiments can be combined with each other.
[0026] The present application provides a dispersant, comprising a polymer stabilizer and a small molecule viscosity reducer, wherein the polymer stabilizer and the small molecule viscosity reducer form a core-shell structure or an aggregate.
[0027] Specifically, the dispersant provided by the present invention is applied to a battery and can be added to the slurry of the positive electrode material. Among them, the types of batteries include but are not limited to lithium ion batteries, sodium ion batteries or potassium ion batteries. The slurry of the positive electrode material includes positive electrode active materials, positive electrode lithium supplement materials and conductive agents. Of course, in other embodiments, the dispersant can also be added to the negative electrode material.
[0028] In one embodiment, the polymer stabilizer includes one or more of polyethylene glycol (PEG) and its derivatives, polyvinyl pyrrolidone (PVP) and its derivatives, polyester and its derivatives, polyphosphate, and polyacrylate. Optionally, polyester and its derivatives specifically include but are not limited to polyethylene adipate and its derivatives and / or polyadipate 1,4-butylene glycol and its derivatives. Optionally, polyacrylate includes but is not limited to one or more of polyacrylic acid sodium salt, polyacrylic acid potassium salt, and polyacrylic acid ammonium salt.
[0029] In one embodiment, the small molecule viscosity reducer includes anhydrides, potassium methyl silicate, hydrazides, and amides, specifically including one or more of phthalic anhydride, acetic anhydride, maleic anhydride, carbohydrazide, benzohydrazide, oxalic acid dihydrazide, carboamide, and cyanoacetamide.
[0030] In one embodiment, the polymer stabilizer and the small molecule viscosity reducer can form a core-shell structure, wherein the small molecule stabilizer is coated on the outer surface of the polymer viscosity reducer. It should be noted that the dispersant provided by the present invention can be solid, and different from the liquid dispersant in the prior art, the solid dispersant provided by the present application can be added to the solvent together with the positive electrode material to form a slurry. The advantage of the solid dispersant is that it is convenient to store and transport, and has little effect on the positive electrode material.
[0031] In one embodiment, the polymer stabilizer and the small molecule viscosity reducer can also be connected to form an agglomerate. It should be noted that the agglomerate is a droplet with a diameter of only a few microns obtained by mixing two colloidal solutions with different charges, wherein a colloid, also known as a colloidal dispersion, is a relatively uniform mixture containing two substances in different states in the colloid, a dispersed phase and another continuous phase. Therefore, the dispersant provided by the present invention can also be liquid, and the polymer stabilizer and the small molecule viscosity reducer are two different colloids, and the two are mixed to form an agglomerate.
[0032] The dispersant provided by the present invention includes a polymer stabilizer and a small molecule viscosity reducer. The small molecule viscosity reducer can be preferentially adsorbed on the surface of the positive electrode material and form anchored active sites on the surface of the positive electrode material, thereby avoiding mutual attraction and agglomeration between the positive electrode materials, thereby improving the dispersibility of the slurry. Due to the molecular weight limitation of the small molecule viscosity reducer, the impact force of the small molecule viscosity reducer on the surface of the positive electrode material is small and will not damage the coating layer on the surface of the positive electrode material, so that the battery performance remains stable; the polymer stabilizer can provide steric hindrance and electrostatic steric hindrance between the positive electrode material and the dispersant, thereby further avoiding the agglomeration of the positive electrode material affecting the slurry coating efficiency.
[0033] In one embodiment, the dispersant further includes a coupling agent, and the polymer stabilizer is connected to the small molecule viscosity reducer through the coupling agent. The coupling agent is used to connect the polymer stabilizer and the small molecule viscosity reducer to improve the stability of the dispersant, which can not only promote the synergistic effect of the polymer stabilizer and the small molecule viscosity reducer, but also firmly fix the polymer stabilizer through the coupling agent to prevent the polymer stabilizer from directly impacting the positive electrode material.
[0034] In addition, the reason for using a coupling agent to connect the two is that, since small molecule viscosity reducers have lower viscosity and higher fluidity, they can penetrate into the gaps between particles, reduce friction and resistance between particles, and improve slurry fluidity and dispersibility, but their stability is poor, so they need to use the steric hindrance or electrostatic hindrance function of the polymer stabilizer to improve their stability, but the connectivity between small molecules and polymers is weak, so they need to use a coupling agent with stronger adhesion to connect the small molecule viscosity reducer and the polymer stabilizer.
[0035] In one embodiment, the coupling agent includes one or more of a silane coupling agent, a titanate coupling agent, a zirconate coupling agent, an aluminate coupling agent, a bimetallic coupling agent (aluminum-zirconate, aluminum-titanium composite coupling agent), a rare earth coupling agent, a phosphorus-containing coupling agent, and a boron-containing coupling agent.
[0036] In a specific embodiment, the silane coupling agent includes one or more of 3-chloropropyltrimethoxysilane, vinyltriethoxysilane, vinyltrimethoxysilane, and vinyltri(β-methoxyethoxy)silane. It is understood that there are many types of silane coupling agents, including monofunctional silanes, difunctional silanes, and multifunctional silanes. Since silane coupling agents are commonly used in battery systems, the reason why silane coupling agents can be preferred is that they have the advantages of high thermal stability, low flammability, non-toxicity, high conductivity, and high decomposition voltage.
[0037] Different coupling agents have different functional groups and reactivity, so the coupling agent can react with the polymer stabilizer and the small molecule viscosity reducer at the same time, and the coupling agent can form a chemical bond with the polymer stabilizer and the small molecule viscosity reducer, and connect the three closely together through strong chemical bonds. Among them, the silane coupling agent is a low-molecular organic silicon compound with a special structure, and its general formula is RSiX3, where R represents an active functional group with affinity or reactivity with the polymer molecule, such as oxy, thiol, vinyl, epoxy, amide, aminopropyl, etc.; X represents an alkoxy group that can be hydrolyzed, such as halogen, alkoxy, acyloxy, etc. These functional groups enable the silane coupling agent to connect with a variety of elements and compounds, react chemically with organic materials or produce strong intermolecular effects, thereby firmly combining two materials with completely different properties.
[0038] In one implementation, please refer to Figure 1 The dispersant includes a core 11, an intermediate layer 12 and an outer shell 13, wherein the intermediate layer 12 is coated on the outer surface of the core 11, and the outer shell 13 is coated on the outer surface of the intermediate layer 12. The core 11 includes a polymer stabilizer, the intermediate layer 12 includes a coupling agent, and the outer shell 13 includes a small molecule viscosity reducer.
[0039] Specifically, the dispersant may be in the form of particles with a core-shell structure, wherein the polymer stabilizer is used as the core 11, the coupling agent is used as the intermediate layer 12 coated on the outer surface of the core 11, and the small molecule viscosity reducer is used as the outer shell layer 13 coated on the outer surface of the intermediate layer 12. It is understood that the small molecule viscosity reducer located in the outermost layer is tightly connected to the polymer stabilizer in the core 11 through the coupling agent, thereby further improving the stability of the positive electrode material slurry, avoiding agglomeration of the positive electrode material, and not affecting the coating efficiency of the slurry.
[0040] It should be explained that, because the coupling agent is a "connector" for connecting the polymer stabilizer and the small molecule viscosity reducer, the coupling agent is arranged in the middle layer 12 to connect the core 11 and the outer shell 13. The reason for arranging the polymer stabilizer in the core 11 is that the molecular weight of the polymer stabilizer is greater than that of the small molecule viscosity reducer. If the polymer stabilizer is located in the outer layer, the viscosity of the slurry will increase, which is not conducive to coating; and the small molecule viscosity reducer located in the outer layer can directly contact the positive electrode material to provide active sites to achieve the effect of dispersing and reducing viscosity.
[0041] In one embodiment, the polymer stabilizer, coupling agent and small molecule viscosity reducer form a colloid. It is understandable that the polymer stabilizer, coupling agent and small molecule viscosity reducer together form a colloid agglomerate, and the specific morphology of the three is not described here, and can refer to the above embodiment.
[0042] In one embodiment, the mass ratio of the polymer stabilizer, the coupling agent and the small molecule viscosity reducer is (20-40): (2-12): 100. Optionally, the mass ratio of the polymer stabilizer, the coupling agent and the small molecule viscosity reducer can be 20: (2-12): 100, 25: (2-12): 100, 30: (2-12): 100, 35: (2-12): 100, 40: (2-12): 100, (20-40): 2: 100, (20-40): 4: 100, (20-40): 6: 100, (20-40): 8: 100, (20-40): 10: 100, (20-40): 12: 100. When the mass ratio of the three is within the above range, the polymer stabilizer, coupling agent and small molecule viscosity reducer can play a synergistic role, and the three are stably and tightly connected, and the dispersant has a higher structural strength.
[0043] In one embodiment, the polymer stabilizer includes a first stabilizer and a second stabilizer, the first stabilizer and the second stabilizer are of different types, and the molecular weight of the first stabilizer is greater than the relative molecular weight of the second stabilizer.
[0044] Specifically, the first stabilizer and the second stabilizer may be two of the polymer stabilizers provided in the above embodiments; in a specific embodiment, the first stabilizer may be a mixture of one or more of polyethylene glycol (PEG) and its derivatives, polyvinyl pyrrolidone (PVP) and its derivatives, polyester and its derivatives, and the second stabilizer may be polyphosphate and / or polyacrylate.
[0045] The first stabilizer and the second stabilizer have two different functional stabilizing effects. Among them, the molecular weight of the first stabilizer is greater than the relative molecular mass of the second stabilizer, so that the first stabilizer has a larger spatial steric hindrance, and the second stabilizer has electrostatic steric hindrance. The two form a good synergistic effect, which can further improve the stability of the slurry, effectively reduce the sedimentation of the slurry particles, and improve the stability and use efficiency of the slurry.
[0046] It should be explained that the first stabilizer provides a steric hindrance effect for the dispersant. Since the first stabilizer has a larger molecular weight, the first stabilizer has a larger volume and can be isolated between the positive electrode materials, thereby avoiding the agglomeration of the positive electrode materials. The second stabilizer provides an electrostatic steric hindrance effect for the dispersant. Since the first stabilizer has a smaller molecular weight and can be an organic salt, an ionic bond can be formed on the second stabilizer, so that the second stabilizer can form an electrostatic field force on the positive electrode material to repel it, thereby avoiding the agglomeration between the positive electrode materials.
[0047] In one embodiment, the ratio of the weight average molecular weight of the first stabilizer to the relative molecular weight of the second stabilizer is (2-500): 1. Optionally, the ratio of the weight average molecular weight of the first stabilizer to the relative molecular weight of the second stabilizer can be 2: 1, 5: 1, 10: 1, 20: 1, 50: 1, 100: 1, 200: 1, 500: 1. The ratio of the weight average molecular weight of the first stabilizer to the weight average molecular weight of the second stabilizer is within the above range in order to ensure that the molecular weight of the first stabilizer is greater than the relative molecular weight of the second stabilizer, and that the molecular weights of both stabilizers are within a suitable range, thereby forming a synergistic effect of steric hindrance and electrostatic hindrance.
[0048] In one embodiment, the mass ratio of the first stabilizer to the second stabilizer is 100:(10-30). Optionally, the mass ratio of the first stabilizer to the second stabilizer can be 100:10, 100:12, 100:14, 100:16, 100:18, 100:20, 100:22, 100:24, 100:26, 100:28, 100:30. The mass ratio of the first stabilizer to the second stabilizer is within the above range to ensure that the two stabilizers can provide appropriate steric hindrance effects respectively, avoid the weak effect of either steric hindrance or electrostatic hindrance, thereby ensuring the synergistic effect of the two.
[0049] In one embodiment, the present application also provides a method for preparing a dispersant, which specifically comprises the following steps:
[0050] Step A10, adding a polymer stabilizer into solvent A and stirring thoroughly.
[0051] Step A20, then adding a small molecule viscosity reducer to the solvent A, and obtaining a dispersant after reaction and drying.
[0052] In the dispersant, the polymer stabilizer and the small molecule viscosity reducer form a core-shell structure or an aggregate.
[0053] Wherein, solvent A includes but is not limited to one or more of tetrahydrofuran, methanol, toluene, anisole, N,N-dimethylformamide and the like.
[0054] In one embodiment, the present application also provides a method for preparing a dispersant including a coupling agent, please refer to Figure 2 , specifically including the following steps:
[0055] Step S10, adding a polymer stabilizer into solvent B, and then adding a coupling agent into solvent B, and obtaining a mixture A after reaction and drying.
[0056] Step S20, adding the mixture A into the solvent C, and then adding a small molecule viscosity reducer into the solvent C, and obtaining a dispersant after reaction and drying.
[0057] Optionally, in step S10, the polymer stabilizer is added to the solvent B, specifically, the polymer stabilizer is added to the solvent B at 50° C. to 100° C. The solvent B includes, but is not limited to, one or more of tetrahydrofuran, methanol, toluene, anisole, N,N-dimethylformamide, and the like.
[0058] Optionally, in step S10, after adding the coupling agent to the solvent B, the reaction can be carried out at a constant temperature for 1 hour to 24 hours under an inert atmosphere, and then filtered and dried to obtain a mixture A, wherein the mixture A includes an inner core and an intermediate layer, the inner core includes a polymer stabilizer, and the intermediate layer includes a coupling agent.
[0059] Optionally, in step S20, the mixture A is added to the solvent C, specifically, the mixture A is added to the solvent C at 60° C. to 90° C. The solvent B includes, but is not limited to, one or more of tetrahydrofuran, methanol, toluene, anisole, N,N-dimethylformamide, and the like.
[0060] Optionally, in step S20, after adding a small molecule viscosity reducer to solvent C, the mixture may be stirred for 2 to 4 hours under an inert atmosphere, and then the solvent C may be removed by vacuum distillation, and the product may be transferred to a drying oven for drying to obtain a dispersant. The dispersant includes a core, an intermediate layer, and an outer shell layer, and the outer shell layer includes a small molecule stabilizer.
[0061] It is understandable that in step S10, since the organic functional groups in the coupling agent, such as vinyl, ethoxy, amino, epoxy, methacryloxy, thiol, etc., can react chemically with the organic material or produce strong intermolecular effects, firmly combining two materials with completely different properties, the polymer stabilizer is combined with the coupling agent in step S10. In step S20, the other end of the coupling agent is combined with the small molecule viscosity reducer to finally form a core-shell structured dispersant.
[0062] In one embodiment, the present application also provides a method for preparing a dispersant, wherein the dispersant includes a first stabilizer and a second stabilizer, please refer to Figure 2 , specifically including the following steps:
[0063] Step S00, adding the first stabilizer and the second stabilizer into the solvent D, filtering and drying after sufficient dispersion reaction, to obtain a polymer stabilizer.
[0064] Step S10, adding a polymer stabilizer into solvent B, and then adding a coupling agent into solvent B, and obtaining a mixture A after reaction and drying.
[0065] Step S20, adding the mixture A into the solvent C, and then adding a small molecule viscosity reducer into the solvent C, and obtaining a dispersant after reaction and drying.
[0066] Optionally, in step S00, the first stabilizer and the second stabilizer are added to the solvent D, specifically, the first stabilizer and the second stabilizer are added to the solvent D at 60° C. to 80° C. The solvent D includes, but is not limited to, one or more of tetrahydrofuran, methanol, toluene, anisole, N,N-dimethylformamide, and the like.
[0067] Optionally, in step S00, after dispersing the first stabilizer and the second stabilizer, the two can be reacted for 1 hour to 4 hours under an inert atmosphere, and then filtered and dried to obtain a polymer stabilizer. The polymer stabilizer includes the first stabilizer and the second stabilizer.
[0068] The preparation method of the dispersant provided by the present invention is used to prepare the dispersant provided in the above-mentioned embodiment, and the preparation method process is simple, and a solid dispersant can be obtained, wherein the solvent can be recycled and reused, and the coupling agent in the dispersant is used to connect the polymer stabilizer and the small molecule viscosity reducer, so as to improve the stability of the dispersant, so that the polymer stabilizer and the small molecule viscosity reducer can play a synergistic role. In addition, in the prepared dispersant, the small molecule viscosity reducer will be preferentially adsorbed on the carbon surface outside the positive electrode material, that is, adsorbed on the positive electrode material surface by intermolecular forces and van der Waals forces, and the silane coupling agent connecting the small molecule viscosity reducer and the polymer stabilizer will slowly stretch, forming a solvation segment in the slurry (solvation is the process of interaction between the solute molecules and the solvent molecules, resulting in the phenomenon that the solute is stable in the solution), preventing the positive electrode materials from attracting and agglomerating each other, thereby improving the stability of the positive electrode slurry.
[0069] In one embodiment, the present invention also provides a secondary battery, which can be a commonly used composition system in the prior art, for example, including a negative electrode plate, an electrolyte, a separator and a positive electrode plate, the electrolyte can be a solid electrolyte or a liquid electrolyte, and the use of the separator can be adaptively selected when a solid electrolyte is selected; the positive electrode plate includes a current collector and a positive electrode material layer arranged on the current collector, and the positive electrode material layer includes the dispersant provided above. The secondary battery includes a positive electrode material and a dispersant as provided in the above embodiment. Specifically, the positive electrode material may include a positive electrode active material and a positive electrode lithium supplement material. Optionally, the positive electrode active material may be a phosphate positive electrode active material and a ternary positive electrode active material. In a specific embodiment, it includes one or more of lithium iron phosphate, lithium cobalt oxide, lithium manganese oxide, lithium manganese iron phosphate, lithium vanadium phosphate, lithium vanadium oxyphosphate, fluorolithium vanadium phosphate, lithium titanate, lithium nickel cobalt manganese oxide, and lithium nickel cobalt aluminum oxide.
[0070] The technical solution of the present invention is described in detail below through specific embodiments.
[0071] Example 1
[0072] This embodiment provides a dispersant, which includes a core, an intermediate layer and an outer shell layer, wherein the core includes polyurethane (MW=91965) and sodium tripolyphosphate (367.86), the intermediate layer includes vinyl trimethoxysilane, and the outer shell layer includes phthalic anhydride.
[0073] The weight average molecular weight ratio of polyurethane to sodium tripolyphosphate is 250:1, the mass ratio of polyurethane to sodium tripolyphosphate is 100:20, and the mass ratio of polymer stabilizer (the sum of polyurethane and sodium tripolyphosphate), vinyl trimethoxysilane and small molecular viscosity reducer phthalic anhydride is 20:2:100.
[0074] The preparation method of the dispersant provided in this embodiment is as follows:
[0075] (1) Preparation of polymer stabilizer core: polyurethane and sodium tripolyphosphate are added to methanol at 70° C. and fully dispersed; then reacted for 2 h under an inert gas atmosphere; filtered and dried to obtain a polymer stabilizer core.
[0076] (2) Preparation of coupling agent intermediate layer: Add the polymer stabilizer core into DMF at 80° C., then add vinyltrimethoxysilane thereto, react at constant temperature for 12 h under an inert atmosphere, and obtain the core with the intermediate layer after filtering and drying.
[0077] (3) Preparation of a small molecule viscosity reducer shell layer: Add the inner core with the middle layer to a DMF organic solution at 80°C, then add the small molecule viscosity reducer, stir and disperse, and stir thoroughly for 3 hours under an inert atmosphere; remove the solvent by vacuum distillation, and transfer the product to a drying oven to obtain a dispersant.
[0078] Example 2
[0079] This embodiment provides a dispersant, which includes a core, an intermediate layer and an outer shell layer, wherein the core includes polyurethane (MW=1000) and sodium tripolyphosphate (367.86), the intermediate layer includes vinyl trimethoxysilane, and the outer shell layer includes phthalic anhydride.
[0080] The difference between this embodiment and embodiment 1 is that the weight average molecular weight ratio of polyurethane to sodium tripolyphosphate is 2.7:1.
[0081] The steps for preparing the dispersant provided in this embodiment are the same as those in Example 1.
[0082] Example 3
[0083] This embodiment provides a dispersant, which includes a core, an intermediate layer and an outer shell layer. The core includes polyurethane (MW=183930) and sodium tripolyphosphate (367.86), the intermediate layer includes vinyl trimethoxysilane, and the outer shell layer includes phthalic anhydride.
[0084] The difference between this embodiment and embodiment 1 is that the weight average molecular weight ratio of polyurethane to sodium tripolyphosphate is 500:1.
[0085] The steps for preparing the dispersant provided in this embodiment are the same as those in Example 1.
[0086] Example 4
[0087] This embodiment provides a dispersant, which includes a core, an intermediate layer and an outer shell layer. The core includes polyurethane and sodium tripolyphosphate, the intermediate layer includes vinyl trimethoxy silane, and the outer shell layer includes phthalic anhydride.
[0088] The difference between this embodiment and embodiment 1 is that the mass ratio of polyurethane to sodium tripolyphosphate is 100:30.
[0089] The steps for preparing the dispersant provided in this embodiment are the same as those in Example 1.
[0090] Example 5
[0091] This embodiment provides a dispersant, which includes a core, an intermediate layer and an outer shell layer. The core includes polyurethane and sodium tripolyphosphate, the intermediate layer includes vinyl trimethoxy silane, and the outer shell layer includes phthalic anhydride.
[0092] The difference between this embodiment and embodiment 1 is that the mass ratio of polyurethane to sodium tripolyphosphate is 100:10.
[0093] The steps for preparing the dispersant provided in this embodiment are the same as those in Example 1.
[0094] Example 6
[0095] This embodiment provides a dispersant, which includes a core, an intermediate layer and an outer shell layer. The core includes polyurethane and sodium tripolyphosphate, the intermediate layer includes vinyl trimethoxy silane, and the outer shell layer includes phthalic anhydride.
[0096] The difference between this embodiment and embodiment 1 is that the mass ratio of the polymer stabilizer (the sum of polyurethane and sodium tripolyphosphate), vinyl trimethoxysilane and small molecule viscosity reducer is 30:3:100.
[0097] The steps for preparing the dispersant provided in this embodiment are the same as those in Example 1.
[0098] Example 7
[0099] This embodiment provides a dispersant, which includes a core, an intermediate layer and an outer shell layer. The core includes polyurethane and sodium tripolyphosphate, the intermediate layer includes vinyl trimethoxy silane, and the outer shell layer includes phthalic anhydride.
[0100] The difference between this embodiment and embodiment 1 is that the mass ratio of the polymer stabilizer (the sum of polyurethane and sodium tripolyphosphate), vinyl trimethoxysilane and small molecule viscosity reducer is 40:12:100.
[0101] The steps for preparing the dispersant provided in this embodiment are the same as those in Example 1.
[0102] Example 8
[0103] This embodiment provides a dispersant, which includes a core, an intermediate layer and an outer shell layer. The core includes polyurethane, the intermediate layer includes vinyltrimethoxysilane, and the outer shell layer includes phthalic anhydride.
[0104] The difference between this embodiment and embodiment 1 is that it only includes polyurethane.
[0105] The steps for preparing the dispersant provided in this embodiment are the same as those in Example 1.
[0106] Example 9
[0107] This embodiment provides a dispersant, which includes a core, an intermediate layer and an outer shell layer. The core includes sodium tripolyphosphate, the intermediate layer includes vinyl trimethoxysilane, and the outer shell layer includes phthalic anhydride.
[0108] The difference between this embodiment and embodiment 1 is that only sodium tripolyphosphate is included.
[0109] The steps for preparing the dispersant provided in this embodiment are the same as those in Example 1.
[0110] Example 10
[0111] This embodiment provides a dispersant, which includes a core, an intermediate layer and an outer shell layer. The core includes polyvinyl pyrrolidone K30 and sodium tripolyphosphate, the intermediate layer includes vinyl trimethoxy silane, and the outer shell layer includes oxalyl dihydrazide.
[0112] The difference between this embodiment and embodiment 1 is that the inner core includes polyvinyl pyrrolidone K30 and sodium tripolyphosphate, and the outer shell includes oxalyl dihydrazide.
[0113] The steps for preparing the dispersant provided in this embodiment are the same as those in Example 1.
[0114] Embodiment 11
[0115] This embodiment provides a dispersant, which includes a core, an intermediate layer and an outer shell layer. The core includes polyurethane and ammonium polyacrylate, the intermediate layer includes vinyltrimethoxysilane, and the outer shell layer includes carbonamide.
[0116] The difference between this embodiment and embodiment 1 is that the inner core includes polyurethane and ammonium polyacrylate.
[0117] The steps for preparing the dispersant provided in this embodiment are the same as those in Example 1.
[0118] Example 12
[0119] This embodiment provides a dispersant, which includes a core, an intermediate layer and an outer shell layer. The core includes polyurethane and polyphosphate, the intermediate layer includes 3-chloropropyltrimethoxysilane, and the outer shell layer includes phthalic anhydride.
[0120] The difference between this embodiment and embodiment 1 is that the intermediate layer includes 3-chloropropyltrimethoxysilane.
[0121] The steps for preparing the dispersant provided in this embodiment are the same as those in Example 1.
[0122] Embodiment 13
[0123] This embodiment provides a dispersant, which includes polyurethane, sodium tripolyphosphate, vinyl trimethoxysilane and phthalic anhydride.
[0124] The difference between this embodiment and embodiment 1 is that the dispersant is not a core-shell structure.
[0125] The preparation method of the dispersant provided in this embodiment differs from that in Embodiment 1 in that:
[0126] (1) Polyurethane, sodium tripolyphosphate, vinyl trimethoxysilane and phthalic anhydride are simply ground and mixed in a mass ratio of 20:2:2:100 to obtain a dispersant.
[0127] Comparative Example 1
[0128] This comparative example provides a mixture of polyurethane and sodium tripolyphosphate.
[0129] Comparative Example 2
[0130] This comparative example provides vinyltrimethoxysilane.
[0131] Comparative Example 3
[0132] This comparative example provides phthalic anhydride.
[0133] The dispersant parameters provided by Examples 1 to 13 and Comparative Examples 1 to 3 are shown in Table 1:
[0134] Table 1 Dispersant parameters provided in Examples and Comparative Examples
[0135]
[0136]
[0137] The dispersants provided in the above-mentioned Examples 1 to 13 and Comparative Examples 1 to 3 were added to the positive electrode slurry of lithium iron phosphate battery and named as Verification Example B1 to Verification Example B13 and Verification Comparative Example B1 to Verification Comparative Example B3, respectively. And the positive electrode slurry was prepared according to the following method:
[0138] The positive electrode slurry of lithium iron phosphate battery is mixed with solid dry material and N-methylpyrrolidone (wherein the weight of N-methylpyrrolidone is 41.75wt% of the total weight of the positive electrode slurry). Taking the total weight as 100wt%: the solid dry material in the positive electrode slurry includes 96.5wt% of lithium iron phosphate, 1.3wt% of Super P and 2.2wt% of polyvinylidene fluoride. Among them, the outer surface of the positive electrode active material (lithium iron phosphate) has a carbon coating layer, and the thickness of the carbon coating layer is 5nm to 10nm. Stir polyvinylidene fluoride and Super P in N-methylpyrrolidone at 400 rpm for 20 minutes, add lithium iron phosphate and stir at 200 rpm for 10 minutes, then add dispersant and stir at 2000 rpm for 70 minutes to obtain a positive electrode slurry. The amount of dispersant added is 0.1%, that is, the amount of dispersant added is 0.1% of the mass of the positive electrode active material.
[0139] Viscosity test: Verification Example B1-Verification Example B13, Verification Comparative Example B1-Verification Comparative Example B3, test the viscosity of the slurry at discharge and 24h, respectively, and the test results are shown in Table 2. Select a suitable rotor, fix the viscometer rotor, place the glue under the viscometer rotor, and the glue just submerges the scale line of the rotor. Instrument model: Shanghai Fangrui NDJ-5S, rotor: 64#, speed: 15-30r / min, test temperature: 25℃, test humidity: 20RH%~30RH%, test time: 1min, wait for the display to stabilize and read the data.
[0140] The positive electrode slurry provided in the above verification examples B1-B13 and verification comparative examples B1-B3 was coated on the current collector to make a positive electrode sheet, and the positive electrode sheet was assembled into a secondary battery, and the electrochemical performance of the positive electrode sheet and the secondary battery was tested. Among them, the resistivity of the electrode sheet was tested using a four-probe resistance tester. The lower the resistivity, the better the dispersant and stability in the slurry, and the stronger the conductivity of the electrode sheet. The test results are shown in Table 2.
[0141] Table 2 Test results of verification examples and verification comparison examples
[0142]
[0143]
[0144] From the test results of the verification example and the comparative example in Table 2, it can be seen that the dispersant provided by the present invention is added to the slurry, and the viscosity of the slurry after discharge and after being set aside for 24 hours is lower than that of the verification comparative example, indicating that the slurry of the verification example has good fluidity and coatability; and the pole piece and battery containing the dispersant prepared by the present invention have excellent performance, the pole piece resistivity of the verification example is lower than that of the verification comparative example, and the charge and discharge capacity and efficiency of the battery are higher than that of the verification comparative example. In contrast, the dispersant used in the verification comparative example contains only a single substance or does not have a core-shell structure, so its slurry performance, pole piece performance, and battery electrochemical performance are relatively poor.
[0145] From the test results of Verification Examples B1-B3 in Table 2, it can be seen that the difference between Verification Examples B1-B3 lies in the different weight-average molecular weights of the first stabilizer in the inner core. In Verification Examples B2 and B3, since the weight-average molecular weights of the first stabilizer are too large or too small, it is difficult to fully exert the steric hindrance stabilization mechanism, and the slurry stability is poor, and the slurry increase is much greater than that of Verification Example B1. During the coating process, the slurry viscosity of Verification Examples B2 and B3 increases too fast, and the conductive carbon in the slurry is unevenly distributed, resulting in the resistivity of the prepared positive electrode sheet being larger than that of Verification Example B1. Since the conductivity of the positive electrode sheet in the battery is low, its electrochemical performance is also reduced.
[0146] From the test results of Verification Examples B1, B4 and B5 in Table 2, it can be seen that the mass ratio of the first stabilizer to the second stabilizer also has an impact on the performance of the dispersant. In Verification Examples B4 and B5, since the mass ratio of the first stabilizer to the second stabilizer is close to imbalance, the viscosity value of the discharge material and the viscosity value of the slurry after 24 hours of storage are significantly larger than those of Verification Example B1, which will affect the coatability of the slurry, but the performance of the battery obtained in the end is less affected, and there is no serious deterioration trend in the resistivity of the electrode sheet and the electrochemical performance of the battery.
[0147] From the test results of Verification Example B1, Verification Example B6 and Verification Example B7 in Table 2, it can be seen that in Verification Example B6 and Verification Example B7, because the ratio of the polymer stabilizer (core), coupling agent and shell small molecule viscosity reducer is too large or too small, the viscosity reduction and stabilization performance of the core-shell structure dispersant formed is lower than that of Verification Example B1.
[0148] From the test results of Verification Examples B1, B8 and B9 in Table 2, it can be seen that since the polymer stabilizer of the inner core in Verification Examples B8 and B9 only contains one stabilizer, the stability of the inner core material will also decrease compared to Verification Example B1.
[0149] From the test results of Verification Example B1, Verification Example B10, Verification Example B11 and Verification Example B12 in Table 2, it can be seen that the differences between Verification Example B10, Verification Example B11 and Verification Example B12 and Verification Example B1 are that the type of the first stabilizer in the polymer core, the type of the coupling agent in the middle layer, and the type of small molecule viscosity reduction have changed. However, since Verification Example B10, Verification Example B11 and Verification Example B12 adopt the core-shell dispersant prepared by the technical solution of the invention of the present application, the slurry still has good viscosity reduction and viscosity stabilization performance.
[0150] From the test results of verification examples B1 and B13 in Table 2, it can be seen that the added dispersant in verification example B13 does not adopt a core-shell structure, but the dispersant supports the agglomerates. Therefore, the viscosity reduction and stabilization performance of the slurry is lower than that of other verification examples, and the obtained electrode and battery performance are also reduced.
[0151] In the description of the embodiments of the present application, it should be noted that the orientation or positional relationship of terms such as "center", "up", "down", "left", "right", "vertical", "horizontal", "inside" and "outside" are based on the orientation or positional relationship described in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present application.
[0152] What is disclosed above is only a preferred embodiment of the present application, and it certainly cannot be used to limit the scope of rights of the present application. Ordinary technicians in this field can understand that all or part of the processes of implementing the above embodiment and equivalent changes made according to the claims of the present application are still within the scope covered by the present application.
Claims
1. A dispersant, characterized in that: The invention comprises a polymer stabilizer and a small molecule viscosity reducer, wherein the polymer stabilizer and the small molecule viscosity reducer form a core-shell structure or an aggregate.
2. The dispersant according to claim 1, characterized in that The dispersant further comprises a coupling agent, and the polymer stabilizer is connected to the small molecule viscosity reducing agent via the coupling agent.
3. The dispersant according to claim 2, characterized in that The dispersant includes an inner core, an intermediate layer and an outer shell layer, wherein the intermediate layer is coated on the outer surface of the inner core, and the outer shell layer is coated on the outer surface of the intermediate layer. The inner core includes the polymer stabilizer, the intermediate layer includes the coupling agent, and the outer shell layer includes the small molecule viscosity reducer, or the polymer stabilizer, the coupling agent and the small molecule viscosity reducer form a colloid.
4. The dispersant according to claim 2, characterized in that The coupling agent includes one or more of a silane coupling agent, a titanate coupling agent, a zirconate coupling agent, an aluminate coupling agent, a bimetallic coupling agent, a rare earth coupling agent, a phosphorus-containing coupling agent, and a boron-containing coupling agent.
5. The dispersant according to claim 2, characterized in that The mass ratio of the polymer stabilizer, the coupling agent and the small molecule viscosity reducer is (20-40):(2-12):
100.
6. The dispersant according to any one of claims 1 to 5, characterized in that The polymer stabilizer includes a first stabilizer and a second stabilizer, the first stabilizer and the second stabilizer are of different types, and the molecular weight of the first stabilizer is greater than the relative molecular weight of the second stabilizer.
7. The dispersant according to claim 6, characterized in that The ratio of the weight average molecular weight of the first stabilizer to the relative molecular mass of the second stabilizer is (2-500):1; and / or the mass ratio of the first stabilizer to the second stabilizer is 100:(10-30).
8. The dispersant according to any one of claims 1 to 5, characterized in that The polymer stabilizer includes one or more of polyethylene glycol and its derivatives, polyvinyl pyrrolidone and its derivatives, polyester and its derivatives, polyphosphate, and polyacrylate; and / or the small molecule viscosity reducer includes one or more of phthalic anhydride, acetic anhydride, maleic anhydride, carbohydrazide, benzohydrazide, oxalic acid dihydrazide, carbamide, and cyanoacetamide.
9. A method for preparing a dispersant, characterized in that: include: Add the polymer stabilizer into solvent A and stir thoroughly; Then, a small molecule viscosity reducer is added to the solvent A, and a dispersant is obtained after reaction and drying; In the dispersant, the polymer stabilizer and the small molecule viscosity reducer form a core-shell structure or an aggregate.
10. A secondary battery, characterized in that: It comprises a negative electrode sheet, an electrolyte and a positive electrode sheet, wherein the positive electrode sheet comprises a current collector and a positive electrode material layer arranged on the current collector, the positive electrode sheet and the negative electrode sheet are arranged in the electrolyte, and the positive electrode material layer comprises a dispersant as described in any one of claims 1 to 8.