Hydrogel precursor composition capable of 3D printing, double-network hydrogel and preparation method of double-network hydrogel

By introducing carboxymethylcellulose and para-aramid nanofibers into DLP 3D printed hydrogels, combining Fe3+ ions to form a dual network structure, the problem of single mechanical properties and functional properties of the hydrogel is solved, and high strength is achieved. Balance between versatility and shape memory effects.

CN118955806AActive Publication Date: 2024-11-15TSINGHUA UNIVERSITY
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411009004.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-05-10
Filing Date
2024-07-25
Publication Date
2024-11-15
Estimated Expiration
2044-07-25

AI Technical Summary

Technical Problem

The existing DLP 3D printed hydrogels have weak mechanical properties and single functional characteristics, making it difficult to achieve the trade-off between high-precision printing and shape memory effects.

Method used

By introducing carboxymethyl cellulose and para-aramid nanofibers into the hydrogel, a double network structure is formed, and a reversible physical crosslinking network is formed by combining Fe3+ ions to achieve high strength and toughness and shape memory effects, while also having electrical conductivity.

Benefits of technology

It realizes high strength, high toughness and versatility, and can switch single and dual network states under specific conditions. It overcomes the problems of low strength, poor fracture toughness and single functional characteristics of DLP 3D printing hydrogels, and achieves excellent The balance of printability and shape memory effects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955806A_ABST
    Figure CN118955806A_ABST
Patent Text Reader

Abstract

The invention relates to a hydrogel precursor composition capable of 3D printing, double-network hydrogel and a preparation method of the double-network hydrogel. The hydrogel precursor composition of the present invention comprises aramid nanofibers, carboxymethyl cellulose, a monomer, a cross-linking agent, and a water-soluble photoinitiator.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of composite materials, and in particular relates to a 3D printable hydrogel precursor composition, a double network hydrogel and a preparation method thereof. Background Art

[0002] Hydrogel is a kind of soft material composed of long-chain polymer network and water. It has the characteristics of softness, biocompatibility and responsiveness to stimuli. It has a wide range of applications in flexible electronics, biomedicine and other fields. In the past, the preparation of hydrogel mainly adopted the casting method, in which the precursor solution was injected into the mold, and the polymerization was initiated by heating or irradiation with ultraviolet light to obtain a hydrogel of a specified shape. With the continuous development of 3D printing technology, hydrogels with more complex geometric structures can be prepared by 3D printing. According to different printing technologies, it can be divided into: extrusion ink direct writing technology (DIW) and surface projection photocuring digital light processing technology (DLP). Compared with the line scanning printing method of DIW, DLP uses surface projection ultraviolet light to induce polymerization in the specified area and stacking layer by layer, which has higher printing efficiency and precision. It is an ideal hydrogel printing technology. Earlier studies have developed some DLP-based 3D printing hydrogels, such as highly stretchable polyacrylamide hydrogels, self-healing hydrogels containing a large number of hydrogen bonds, and PEGDA hydrogels for cell inoculation. However, the mechanical properties of DLP-based 3D printed hydrogels, such as strength, fracture toughness, and fatigue performance, are generally weak, and their functional characteristics are relatively simple, which limits their scope of application in practice.

[0003] Carboxymethyl cellulose (CMC) is an environmentally friendly hydrophilic anionic polysaccharide obtained by partially replacing the hydroxyl groups of cellulose with carboxymethyl groups. The carboxylic acid groups on the carboxymethyl groups of CMC can provide effective anchoring sites for metal ions, forming a reversible ion coordination cross-linking structure.

[0004] Para-aramid nanofiber (ANF) is a new type of nanofiber prepared from poly(p-phenylene terephthalamide) fiber. Its molecular chain is composed of alternating benzene rings and amide bonds, and the molecular chains interact through hydrogen bonds, π-π stacking and van der Waals forces, and have excellent specific modulus, specific strength and wear resistance. ANF has no active functional groups on the surface, but it is prone to photoaging and breaking under ultraviolet light to form free radicals, which can participate in the photopolymerization reaction of hydrogels, so it can be used as an effective reinforcing phase for composite materials such as photocurable hydrogels.

[0005] At present, the preparation of DLP-based 3D printed hydrogels generally faces a trade-off between high strength, toughness, formability, and functionality. Taking shape memory effect and conductivity as an example, achieving shape memory effect usually requires fewer chemical crosslinking points and loose polymer networks, which is not conducive to the formation of printed structures, and the introduction of conductive ions is usually accompanied by a decrease in mechanical properties and printability; in order to improve the strength and toughness of hydrogels, constructing a double network hydrogel composed of two interpenetrating or semi-interpenetrating polymer networks is an effective strategy, and its precursor solution usually has a high viscosity, which is suitable for extrusion DIW printing but not conducive to DLP 3D printing, so there are few studies on double network DLP printable hydrogels; in order to improve the formability and printability of hydrogels, certain chemical crosslinkers need to be added, which will lead to a significant decrease in the toughness and shape memory ability of hydrogels.

[0006] The trade-off between mechanical properties, printability, and functional characteristics of DLP-based 3D printed hydrogels limits their applications in fields such as biomedicine and flexible electronics. Summary of the invention

[0007] Problem that the invention aims to solve

[0008] Existing DLP 3D printed hydrogels have weak mechanical properties, single functional characteristics, and difficulty in achieving a trade-off between high-precision printing and shape memory effect.

[0009] The purpose of the present invention is to provide a hydrogel precursor composition, which can be made into a hydrogel by 3D printing (such as surface projection microstereolithography technology), and the obtained hydrogel has high strength and toughness, and can also have functional properties such as shape memory effect and conductivity.

[0010] Solutions for solving problems

[0011] In response to the above problems, the inventors have conducted long-term and in-depth research and found that by further introducing carboxymethyl cellulose on the basis of hydrogel, especially aramid nanofiber reinforced hydrogel, to form a second network structure, a double-network hydrogel with high strength and toughness as well as functional properties such as shape memory effect and conductivity can be obtained.

[0012] Specifically, the present invention solves the problem of the present invention through the following solutions.

[0013] [1] A hydrogel precursor composition comprising carboxymethyl cellulose, a monomer, a crosslinking agent and a water-soluble photoinitiator, and optionally further comprising aramid nanofibers and a light absorber.

[0014] [2] The hydrogel precursor composition according to [1], wherein the content of the aramid nanofiber is 0-1 wt%; the content of the carboxymethyl cellulose is 0.001-10 wt%; the content of the monomer is 15-60 wt%; the content of the crosslinking agent is 0.01-5 wt%; the content of the water-soluble photoinitiator is 0.1-1.5 wt%; the content of the light absorber is 0-0.1 wt%;

[0015] Preferably, the weight ratio of the monomer to the cross-linking agent is 100:(0.1-1); the weight ratio of the total weight of the monomer and the cross-linking agent to the water-soluble photoinitiator is (100-40):1.

[0016] [3] The hydrogel precursor composition according to [1] or [2], wherein

[0017] The aramid nanofibers are para-aramid nanofibers with an average diameter of 10 to 500 nm and an aspect ratio of 2000 to 4000;

[0018] The average relative molecular mass of the carboxymethyl cellulose is 10000-1000000, and the degree of carboxymethyl substitution is 0.5-0.9;

[0019] The monomer is one or more selected from (meth)acrylamide monomers and (meth)acrylic acid monomers; preferably, the monomer includes one or more selected from (meth)acrylamide monomers and one or more (meth)acrylic acid monomers, and more preferably, the mass ratio of (meth)acrylamide monomers to (meth)acrylic acid monomers is (1-10):1;

[0020] The crosslinking agent is one or more selected from (meth)acrylic acid and (meth)acrylamide crosslinking agents; wherein the (meth)acrylic acid crosslinking agent is preferably one or more selected from multifunctional (meth)acrylic acid and its salts and multifunctional (meth)acrylates, more preferably polyethylene glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate; the (meth)acrylamide crosslinking agent is preferably N,N-methylenebisacrylamide; the crosslinking agent is preferably polyethylene glycol diacrylate (PEGDA);

[0021] The water-soluble initiator is one or more selected from water-soluble aromatic ketones, condensed aromatic hydrocarbons, polysilanes, acylphosphonates, azos and metal organic complex initiators, preferably water-soluble TPO;

[0022] The light absorber is one or more selected from quinoline yellow, methyl red and brilliant green.

[0023] [4] The method for preparing a hydrogel precursor composition according to any one of [1] to [3], comprising the following steps:

[0024] Dispersing carboxymethyl cellulose in water, or dispersing carboxymethyl cellulose in an aqueous dispersion of aramid nanofibers, to obtain a carboxymethyl cellulose dispersion;

[0025] The carboxymethyl cellulose dispersion is mixed with a monomer, a crosslinking agent and a water-soluble photoinitiator to obtain the hydrogel precursor composition.

[0026] [5] A hydrogel comprising carboxymethyl cellulose and a cross-linked polymer, and optionally further comprising aramid nanofibers, wherein at least a portion of the aramid nanofibers are connected to the cross-linked polymer via covalent bonds.

[0027] [6] A double network hydrogel comprising a first network structure and a second network structure, wherein the first network structure is formed by a cross-linked polymer and optionally aramid nanofibers, at least part of the aramid nanofibers being connected to the cross-linked polymer by covalent bonds; and the second network structure is formed by carboxymethyl cellulose and Fe 3+ form.

[0028] [7] The hydrogel according to [5] or [6], wherein the aramid nanofibers are para-aramid nanofibers having an average diameter of 10 to 500 nm and an aspect ratio of 2000 to 4000; and the content of the aramid nanofibers is 0 to 1 wt%;

[0029] The content of the carboxymethyl cellulose is 0.001-10wt%;

[0030] The content of the cross-linked polymer is 15 to 65 wt %; the cross-linked polymer comprises structural units derived from one or more monomers selected from (meth)acrylamide monomers and (meth)acrylic acid monomers; preferably, the cross-linked polymer is formed by polymerizing a raw material composition comprising a monomer and a cross-linking agent, the monomer being one or more selected from (meth)acrylamide monomers and (meth)acrylic acid; the cross-linking agent is one or more selected from (meth)acrylic acid and (meth)acrylamide cross-linking agents; the weight ratio of the monomer to the cross-linking agent is 100:(0.1 to 1); the polymerization is preferably photoinitiated polymerization.

[0031] [8] The method for preparing a hydrogel according to [5], comprising the step of irradiating the hydrogel precursor composition according to any one of [1] to [3] with light;

[0032] Preferably, the hydrogel precursor composition is poured into a mold and then the light irradiation is performed; or the light irradiation is performed while the hydrogel precursor composition is 3D printed;

[0033] Preferably, the light irradiation is performed using light with a wavelength of 365 to 405 nm;

[0034] Preferably, the light irradiation is performed by digital light processing (DLP) technology of surface projection photocuring.

[0035] [9] The method for preparing the double network hydrogel according to [6], comprising: mixing the hydrogel according to [5] with a Fe 3+ a step of contacting an aqueous solution;

[0036] Preferably, the contact time is 1 to 100 minutes, preferably 5 to 80 minutes, more preferably 10 to 60 minutes;

[0037] Preferably, the contacting is carried out by immersing the hydrogel described in [5] in a liquid containing Fe 3+ in an aqueous solution;

[0038] Preferably, the Fe 3+ Fe in aqueous solution 3+ The concentration is 0.01~2mol / L;

[0039] Preferably, the Fe 3+ The aqueous solution is an aqueous solution of a water-soluble iron salt, and the water-soluble iron salt is one or more selected from ferric nitrate, ferric chloride, and ferric sulfate.

[0040]

[10] The method for preparing the double network hydrogel according to [9] further comprises: 3+ The step of immersing the hydrogel in water after contact with the aqueous solution, preferably, the immersion time in water is 1 to 24 hours, preferably 6 to 18 hours, more preferably the time for the hydrogel to reach swelling equilibrium.

[0041]

[11] Use of the hydrogel according to [5] or the double network hydrogel according to [6] for drug delivery or pressure sensor.

[0042]

[12] A drug capsule comprising a shell having a cavity therein and a drug contained in the cavity, wherein the shell is composed of the double-network hydrogel according to [6].

[0043]

[13] The drug capsule according to

[12] , wherein the shell forms an opening when in contact with an acid or a chelating agent, so that the drug contained in the cavity can be released to the outside of the drug capsule through the opening;

[0044] Preferably, the chelating agent is EDTA·2Na.

[0045]

[14] The method for preparing the pharmaceutical capsule according to

[12] or

[13] , comprising the following steps:

[0046] Using the hydrogel precursor composition described in any one of [1] to [3], a shell precursor having an opening is obtained by using digital light processing (DLP) technology of surface projection photocuring;

[0047] filling the shell precursor with a drug through the opening on the shell precursor;

[0048] The opening of the shell precursor is closed under the action of external force to form a shell having a closed structure and containing a drug in the internal cavity;

[0049] Then with Fe 3+ to obtain drug capsules.

[0050]

[15] A pressure sensor device comprising the double network hydrogel described in [6] and a packaging body covering the double network hydrogel, wherein the packaging body is used to prevent water loss from the hydrogel;

[0051] The encapsulant is preferably electrically insulating, more preferably comprises polysiloxane, and further preferably comprises polydimethylsiloxane.

[0052]

[16] A pressure detection device, comprising the pressure sensor device described in

[15] .

[0053]

[17] The pressure detection device according to

[16] also includes a power supply and a circuit board with a resistance detection module, and optionally includes one or more components selected from a housing for accommodating various components, a display screen for outputting information, and an adjustment button.

[0054] Effects of the Invention

[0055] Compared with the prior art, the present invention can achieve the following beneficial effects:

[0056] In addition to the chemically cross-linked network formed by the monomer and the cross-linking agent, the single network hydrogel of the present invention can form a double network hydrogel with shape memory effect under specific conditions due to the inclusion of carboxymethyl cellulose. The double network hydrogel of the present invention has a second network formed by physical cross-linking of carboxymethyl cellulose and iron ions, so it has the mechanical properties of high strength and high toughness, and can be transformed into a single network hydrogel under specific conditions.

[0057] For the high-strength and tough hydrogel composite material reinforced by para-aramid nanofibers and carboxymethyl cellulose in the preferred embodiment of the present invention, the para-aramid nanofibers are prone to photoaging and breakage to form free radicals under ultraviolet light irradiation, and the strength and toughness of the hydrogel can be improved through covalent crosslinking points, hydrogen bonds and long-chain entanglements. Carboxymethyl cellulose can form coordination crosslinks with metal ions through post-treatment to form the second layer network of the hydrogel, significantly improving the strength and toughness of the hydrogel.

[0058] The single network hydrogel and the double network hydrogel of the present invention can be switched to achieve the shape memory effect. The first layer of network (permanent covalent cross-linking network) determines the initial shape of the hydrogel (i.e., permanent shape), and the second layer of network (reversible physical cross-linking network) determines the temporary shape of the hydrogel. The reversible physical cross-linking can be removed by a chelating agent or a low pH environment to achieve shape recovery. In addition, due to the presence of metal ions, the double network hydrogel also has functional properties such as conductivity.

[0059] The hydrogel composite material of the present invention can be used to manufacture complex three-dimensional structures based on DLP 3D printing, and the prepared structure has excellent mechanical properties or functional characteristics such as high strength, shape memory effect, conductivity, high resolution, etc. This overcomes the problems of low strength, poor fracture toughness, and single functional characteristics of hydrogels currently printed by DLP 3D, and achieves a balance between excellent printability and effective shape memory effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0060] Figure 1 The stress-strain curves of four single-network hydrogel composite materials with different aramid fiber contents prepared in Example 1;

[0061] Figure 2 The stress-strain curves of the double-network hydrogel composite materials with four different aramid fiber contents prepared in Example 1;

[0062] Figure 3 The fracture energy diagrams of the double network hydrogel composite materials with four different aramid fiber contents prepared in Example 1;

[0063] Figure 4 Fatigue threshold diagrams of four double network hydrogel composite materials with different aramid fiber contents prepared in Example 1;

[0064] Figure 5 This is a photo of the three-dimensional structure hydrogel composite material printed by DLP 3D in Example 2;

[0065] Figure 6 The photographs and schematic diagrams of the shape fixing and recovery process of the shape memory hydrogel in Example 3;

[0066] Figure 7Schematic diagram of the cross-linking mechanism of a 3D printable hydrogel precursor composition according to one embodiment of the present invention;

[0067] Figure 8 are photos of the hydrogel sheet, drug capsule and the hydrogel sheet restored to the original shape obtained in Example 4;

[0068] Fig. 9 The single network gel, double network hydrogel, integrated pressure detection device and the test photos using the integrated pressure detection device obtained in Example 5 are shown. DETAILED DESCRIPTION

[0069] The following is a detailed description of the present invention. The technical features described below are described based on representative embodiments and specific examples of the present invention, but the present invention is not limited to these embodiments and specific examples.

[0070] <Terms and Definitions>

[0071] In the present specification, the term "alkyl group" includes a linear, branched or cyclic alkyl group, unless otherwise specifically stated.

[0072] In the present specification, the term "monomer" refers to a compound capable of undergoing a polymerization reaction, and has a molecular weight of 500 or less, for example 400 or less, for example 300 or less, more preferably 200 or less, or 100 or less.

[0073] In this specification, the numerical range expressed using "a numerical value A to a numerical value B" means a range including the endpoints numerical values ​​A and B.

[0074] In the present specification, a numerical range expressed using "above" or "below" means a numerical range including the number.

[0075] In this specification, the word "may" means both performing a certain process and not performing a certain process.

[0076] In this specification, the use of "optionally" or "optional" indicates that certain substances, components, execution steps, application conditions and other factors are used or not used.

[0077] In this specification, the unit names used are all international standard unit names, and unless otherwise stated, the "%" used indicates weight or mass percentage.

[0078] In this specification, the references to "preferred embodiments", "embodiments", etc., mean that the specific elements (e.g., features, structures, properties and / or characteristics) described in connection with the embodiments are included in at least one embodiment described herein, and may or may not exist in other embodiments. In addition, it should be understood that the elements may be combined in various embodiments in any suitable manner.

[0079] <Hydrogel Precursor Composition>

[0080] One of the objects of the present invention is to provide a hydrogel precursor composition, which comprises carboxymethyl cellulose, a monomer, a crosslinking agent and a water-soluble photoinitiator, and optionally comprises aramid nanofibers and a light absorber.

[0081] The hydrogel precursor composition of the present invention contains a water-soluble photoinitiator, so it can be cured by light irradiation, so that a complex three-dimensional structure can be manufactured by using technologies such as 3D printing. In addition, when aramid nanofibers are included, during the light irradiation process, the amide bonds on the surface of the aramid nanofibers are broken to form free radicals, which can form covalent bonds with the cross-linked polymer formed by the monomer and the cross-linking agent, thereby obtaining a more excellent toughening effect.

[0082] In one embodiment, the aramid nanofiber is a para-aramid nanofiber. The para-aramid nanofiber is composed of poly(p-phenylene terephthalamide) having liquid crystal properties, and its molecular chains are arranged more regularly and have higher strength, so it is preferred.

[0083] In one embodiment, the average diameter of the aramid nanofiber is 10 to 500 nm, preferably 10 to 300 nm, more preferably 10 to 100 nm, and the aspect ratio of the aramid nanofiber is 2000 to 4000, preferably 3000 to 4000. The length of the aramid nanofiber is 20 to 1200 μm, preferably 30 to 800 μm, more preferably 30 to 500 μm. By using aramid nanofibers with an average diameter and aspect ratio within the above range, better toughening effect can be obtained. Moreover, the longer the length of the aramid nanofiber and the smaller the diameter, the better the toughening effect on the hydrogel.

[0084] In one embodiment, in the hydrogel precursor composition of the present invention, the content of the aramid nanofiber is 0.001 to 1 wt%, preferably 0.002 to 0.9 wt%, more preferably 0.003 to 0.8 wt%, further preferably 0.004 to 0.75 wt%, and further preferably 0.005 to 0.7 wt%, 0.006 to 0.65 wt%, 0.007 to 0.6 wt%, 0.008 to 0.55 wt%, 0.009 to 0.5 wt%, 0.01 to 0.45 wt%, 0.015 to 0. 4wt%, 0.02-0.375wt%, for example, 0.03wt%, 0.04wt%, 0.05wt%, 0.06wt%, 0.07wt%, 0.08wt%, 0.09wt%, 0.1wt%, 0.12wt%, 0.14wt%, 0.16wt%, 0.18wt%, 0.20wt%, 0.22wt%, 0.24wt%, 0.26wt%, 0.28wt%, 0.30wt%, 0.32wt%, 0.34wt%, 0.36wt%. By making the content of aramid nanofiber within the above range, excellent toughening effect can be obtained, and at the same time, the hydrogel precursor composition can be ensured to have a suitable viscosity for 3D printing processing. If the content of aramid nanofibers is too high, the viscosity of the hydrogel precursor composition will be too high, affecting its application in 3D printing; if the content of aramid nanofibers is too low, sufficient strengthening effect cannot be obtained, and the strength of the hydrogel is not enough to meet the needs.

[0085] In a specific embodiment, the aramid nanofibers can be commercially obtained through conventional channels, including but not limited to the para-aramid nanofibers from Shandong Jufang New Materials Co., Ltd. used in the examples below.

[0086] In one embodiment, in the hydrogel precursor composition of the present invention, the content of the carboxymethyl cellulose is 0.001 to 10 wt%, preferably 0.005 to 9 wt%, more preferably 0.01 to 8 wt%, further preferably 0.02 to 7.5 wt%, further preferably 0.03 to 7 wt%, 0.04 to 6.5 wt%, 0.05 to 6 wt%, 0.06 to 5.5 wt%, 0.07 to 5 wt%, 0.08 to 4.5 wt%, 0.09 to 4 wt%, 0.1 to 3.5 wt%, for example 0. 15wt%, 0.2wt%, 0.25wt%, 0.03wt%, 0.35wt%, 0.4wt%, 0.45wt%, 0.5wt%, 0.55wt%, 0.6wt%, 0.65wt%, 0.7wt%, 0.7 5wt%, 0.8wt%, 0.85wt%, 0.9wt%, 0.95wt%, 1wt%, 1.05wt%, 1.1wt%, 1.15wt%, 1.2wt%, 1.25wt%, 1.3wt%, 1.35wt% , 1.4wt%, 1.45wt%, 1.5wt%, 1.55wt%, 1.6wt%, 1.65wt%, 1.7wt%, 1.75wt%, 1.8wt%, 1.85wt%, 1.9wt%, 2wt%, 2.05 wt%, 2.1wt%, 2.15wt%, 2.2wt%, 2.25wt%, 2.3wt%, 2.35wt%, 2.4wt%, 2.45wt%, 2.5wt%, 2.55wt%, 2.6wt%, 2.65wt %, 2.7wt%, 2.75wt%, 2.8wt%, 2.85wt%, 2.9wt%, 2.95wt%, 3wt%, 3.1wt%, 3.2wt%, 3.25wt%, 3.3wt%, 3.35wt%, 3.4 wt%, 3.45wt%, 3.5wt%, 3.55wt%, 3.6wt%, 3.65wt%, 3.7wt%, 3.75wt%, 3.8wt%, 3.85wt%, 3.9wt%, 3.95wt%, 4wt%.

[0087] In one embodiment, the molecular weight of the carboxymethyl cellulose is an average relative molecular mass of 10,000 to 1,000,000, preferably 15,000 to 900,000, more preferably 20,000 to 800,000, and further preferably 25,000 to 700,000, 30,000 to 600,000, 35,000 to 500,000, 40,000 to 400,000, 45,000 to 300,000, 50,000 to 200,000, 55,000 to 180,000, 60,000 to 160,000, 65,000 to 140,000, 70,000 to 120,000, 75,000 to 110,000, and 80,000 to 100,000.

[0088] In one embodiment, the carboxymethyl cellulose has a degree of carboxymethyl substitution of 0.5 to 0.9, preferably 0.55 to 0.85, 0.6 to 0.8, or 0.65 to 0.75.

[0089] In one embodiment, in the hydrogel precursor composition of the present invention, the monomer content is 15-60wt%, preferably 21-59wt%, 22-58wt%, 23-57wt%, 24-56wt%, 25-55wt%, 26-54wt%, 27-53wt%, 28-52wt%, 29-51wt%, 30-50wt%, 31-49wt%, 32-48wt%, 33-47wt%, 34-46wt%, 35-45wt%, 36-44wt%, 37-43wt%, 38-42wt%, 39-41wt%, and for example 16wt%, 17wt%, 18wt%, 19wt%, 20wt%.

[0090] The monomer is one or more monomers selected from (meth)acrylamide monomers and (meth)acrylic acid.

[0091] In this specification, (meth)acrylamide monomers refer to monomers having (meth)acrylamide groups, including acrylamide monomers and methacrylamide monomers. Specific examples of (meth)acrylamide monomers include, but are not limited to, acrylamide, methacrylamide, N,N-dimethylacrylamide, N,N-diethylacrylamide, N-isopropylacrylamide, and the like.

[0092] In the present specification, (meth)acrylic monomers refer to monomers having a (meth)acryloyloxy group, wherein the (meth)acryloyloxy group includes an acryloyloxy group and a methacryloyloxy group. (Meth)acrylic monomers include (meth)acrylic acid and its salts and (meth)acrylic acid ester monomers (e.g., (meth)acrylic acid C1-5 alkyl esters). Specific examples of (meth)acrylic monomers include, but are not limited to, (meth)acrylic acid and its alkali metal or alkaline earth metal salts (e.g., sodium acrylate, potassium acrylate, sodium methacrylate, potassium methacrylate), polyethylene glycol mono(meth)acrylate, hydroxyethyl (meth)acrylate, 3-[[2-(methacryloyloxy)ethyl]dimethylammonium]propionate, 2-methacryloyloxyethyl phosphorylcholine (MPA), and the like.

[0093] Preferably, the monomers include one or more selected from (meth)acrylamide monomers and one or more selected from (meth)acrylic acid monomers. More preferably, the monomers include acrylamide and acrylic acid.

[0094] The content of the (meth)acrylamide monomer is 14-50wt%, preferably 15-48wt%, 17-45wt%, 20-40wt%, 25-35wt%, 26-34wt%, 27-33wt%, 28-32wt%, 29-31wt%, for example 30wt%. The content of the (meth)acrylic acid monomer is 1-15wt%, preferably 2-14wt%, 3-13wt%, 4-12wt%, 5-11wt%, 6-10wt%, 7-9wt%, for example 1.2wt%, 1.4wt%, 1.6wt%, 1.8wt%, 2wt%, 2.2wt%, 2.4wt%, 8wt%.

[0095] In one embodiment, the mass ratio of (meth)acrylamide monomer to (meth)acrylic acid monomer is (1-20):1, preferably (1-18):1, (1-16):1, (1-14):1, (1-13):1, (1-10):1, preferably (1.5-9):1, (2-8):1, (2.5-7):1, (2.8-6):1, (3-5):1.

[0096] In one embodiment, in the hydrogel precursor composition of the present invention, the crosslinking agent is one or more selected from (meth) acrylic acid and (meth) acrylamide crosslinking agents. The (meth) acrylic acid crosslinking agent is one or more selected from multifunctional (meth) acrylic acid and its salts and multifunctional (meth) acrylates, and specific examples thereof include but are not limited to polyethylene glycol di(meth) acrylate, pentaerythritol di(meth) acrylate, pentaerythritol tri(meth) acrylate, pentaerythritol tetra(meth) acrylate. The (meth) acrylamide crosslinking agent is, for example, N,N-methylenebisacrylamide.

[0097] Preferably, the crosslinking agent is polyethylene glycol diacrylate (PEGDA), and the number average molecular weight of PEGDA is 300-3000, preferably 400-2000, more preferably 500-1000, and further preferably 600-900.

[0098] In one embodiment, the total content of the monomer and the cross-linking agent is 15 to 65 wt %, preferably 20 to 60 wt %, and more preferably 30 to 50 wt %. By making the total content of the monomer and the cross-linking agent within the above range, the obtained hydrogel can have excellent mechanical properties while maintaining a sufficient amount of water.

[0099] In one embodiment, the weight ratio of the monomer to the cross-linking agent is 100: (0.1-1), preferably 100: (0.2-0.9), more preferably 100: (0.3-0.8), 100: (0.4-0.7), 100: (0.5-0.6). Alternatively, based on 100 parts by weight of the monomer, the weight content of the cross-linking agent is 0.1-1 parts by weight, preferably 0.2-0.9 parts by weight, more preferably 0.3-0.8 parts by weight, 0.4-0.7 parts by weight, 0.5-0.6 parts by weight. By making the weight ratio (or weight) of the monomer to the cross-linking agent within the above range, the cross-linked polymer obtained by polymerization can have a suitable degree of cross-linking, so that the strength and elongation at break of the hydrogel can be taken into account.

[0100] The present invention has no particular restrictions on water-soluble photoinitiators. Generally, water-soluble photoinitiators include photoinitiators obtained by adding a hydrophilic surfactant to a non-water-soluble photoinitiator or introducing functional groups such as ammonium salts or sulfonates to make it water-soluble. By using a water-soluble photoinitiator, it is possible to avoid the suspended particles in the hydrogel precursor composition from scattering and diffracting light while initiating a free radical polymerization reaction by light, thereby affecting the processing of the hydrogel precursor composition by 3D printing technologies such as digital light processing technology (DLP) of surface projection photocuring.

[0101] In one embodiment, the water-soluble photoinitiator is one or more selected from water-soluble aromatic ketones, condensed aromatic hydrocarbons, polysilanes, acylphosphonates, azos and metal organic complexes, such as the photoinitiator Irgacure 2959 commercially available from BASF, and the water-soluble 2,4,6 (trimethylbenzoyl) diphenylphosphine oxide (TPO) commercially available from Sigma-Aldrich with product number 906808.

[0102] In a specific embodiment, the water-soluble photoinitiator is a commercially available water-soluble TPO nanoparticle photoinitiator, including but not limited to the water-soluble TPO based nanoparticle photoinitiator (Product No.: 906808) produced by Sigma-Aldrich Company mentioned above.

[0103] In one embodiment, the weight ratio of the total weight of the monomer and the crosslinking agent to the weight of the water-soluble photoinitiator is (100-40): 1. Alternatively, based on 1 part by weight of the photoinitiator, the total weight of the monomer and the crosslinking agent is 100-40 parts by weight, preferably 95-45 parts by weight, 90-50 parts by weight, 85-55 parts by weight, 80-60 parts by weight, 75-62 parts by weight, 70-64 parts by weight. By making the weight ratio (or weight) of the total weight of the monomer and the crosslinking agent to the water-soluble photoinitiator within the above range, the polymerization reaction can be carried out sequentially under appropriate light exposure.

[0104] In one embodiment, the hydrogel precursor composition of the present invention may further comprise one or more other components selected from light absorbers, dyes, pigments, polymerization inhibitors, other polymerization initiators, light stabilizers, heat stabilizers, etc. In a preferred embodiment, the hydrogel precursor composition of the present invention further comprises a light absorber, preferably a water-soluble light absorber, and the light absorber may be one or more selected from quinoline yellow, methyl red, and brilliant green.

[0105] In one embodiment, in the hydrogel precursor composition of the present invention, the content of the light absorber is 0-0.1 wt%, preferably 0.001-0.5 wt%, 0.005-0.1 wt%, 0.008-0.015 wt%, 0.01-0.012 wt%.

[0106] In one embodiment, based on the total mass of the hydrogel composition, the content of other components is 0.001 wt% to 1 wt%, for example, 0.003 wt% to 0.5 wt%, and for example, 0.005 wt% to 0.1 wt%.

[0107] One of the objects of the present invention is to provide a method for preparing the hydrogel precursor composition of the present invention, which comprises the following steps:

[0108] Dispersing carboxymethyl cellulose in water, or dispersing carboxymethyl cellulose in an aqueous dispersion of aramid nanofibers, to obtain a carboxymethyl cellulose dispersion;

[0109] The carboxymethyl cellulose dispersion is mixed with a monomer, a crosslinking agent and a water-soluble photoinitiator to obtain the hydrogel precursor composition.

[0110] Preferably, carboxymethyl cellulose is dispersed in the aqueous dispersion of aramid nanofibers to obtain a carboxymethyl cellulose dispersion. In this embodiment, the method for preparing the hydrogel precursor composition of the present invention further comprises the following steps: mixing aramid nanofibers with water and stirring to obtain an aqueous dispersion of aramid nanofibers.

[0111] In one embodiment, water or an aqueous dispersion of aramid nanofibers is mixed with carboxymethyl cellulose and stirred to obtain a carboxymethyl cellulose dispersion. The stirring time is preferably 1 hour or more, 2 hours or more, 3 hours or more, 4 hours or more, 5 hours or more, or 6 hours or more.

[0112] In one embodiment, the content of aramid nanofibers in the aqueous dispersion of aramid nanofibers is 0.001-1 wt %, preferably so that the obtained hydrogel precursor composition meets the range of aramid nanofiber content described above for the hydrogel precursor composition.

[0113] The present invention has no particular limitation on the water used in preparing the aqueous dispersion of aramid nanofibers or the dispersion of carboxymethyl cellulose. From the perspective of avoiding the introduction of impurities into the hydrogel, deionized water or distilled water is preferably used.

[0114] In the aqueous dispersion of aramid nanofibers obtained by the preparation method of the present invention, the aramid nanofibers are uniformly dispersed, and no obvious stratification occurs in the aqueous dispersion after being left to stand for 30 days.

[0115] In one embodiment, the carboxymethyl cellulose dispersion is mixed with a monomer, a crosslinking agent and a water-soluble photoinitiator, and stirred to obtain the hydrogel precursor composition. The stirring time is preferably 10 minutes or more, 20 minutes or more, 30 minutes or more, 40 minutes or more, 50 minutes or more, or 60 minutes or more.

[0116] The stirring in the preparation method of the present invention can be carried out by any stirring method known in the art, including but not limited to mechanical stirring, magnetic stirring and ultrasonic dispersion, among which magnetic stirring is preferred. The stirring is preferably carried out under light-proof conditions to prevent the aramid nanofibers from aging under light.

[0117] For the aramid nanofibers, monomers, crosslinking agents, initiators, etc. used in the preparation method of the present invention, refer to the corresponding description of the hydrogel precursor composition above.

[0118] The present invention also accordingly relates to a hydrogel precursor composition obtained by the preparation method of the present invention.

[0119] <Single Network Hydrogel>

[0120] One of the objects of the present invention is to provide a single network hydrogel comprising carboxymethyl cellulose and a cross-linked polymer, and optionally further comprising aramid nanofibers, wherein at least part of the aramid nanofibers are connected to the cross-linked polymer via covalent bonds.

[0121] In the present invention, at least part of the aramid nanofibers are connected to the cross-linked polymer via covalent bonds, so that an excellent toughening effect can be obtained with a relatively small amount of aramid nanofibers added.

[0122] The hydrogel of the present invention can be a photocurable hydrogel. In this case, covalent bonds between the aramid nanofibers and the cross-linked polymer can be formed during the photocuring process. When irradiated during the photocuring process, the aramid nanofibers undergo photoaging and break to form free radicals. These free radicals react with free radicals on the polymer chain during the polymerization process, thereby forming covalent bonds between the aramid nanofibers and the cross-linked polymer.

[0123] It should be noted that the above-described method of forming covalent bonds between aramid nanofibers and cross-linked polymers by irradiating light is only exemplary, and does not exclude other possible methods of forming covalent bonds between aramid nanofibers and cross-linked polymers.

[0124] In one embodiment, in the hydrogel of the present invention, the content of the aramid nanofibers is the same as the range described above for the hydrogel precursor composition. The above description of the aramid nanofibers also applies to this embodiment.

[0125] In one embodiment, in the hydrogel of the present invention, the content of the carboxymethyl cellulose is the same as the range described above for the hydrogel precursor composition. The above description of carboxymethyl cellulose is also applicable to this embodiment.

[0126] In one embodiment, in the hydrogel of the present invention, the content of the cross-linked polymer is 15-65wt%, preferably 22-62wt%, 24-60wt%, 26-58wt%, 28-56wt%, 30-54wt%, 32-56wt%, 34-54wt%, 36-52wt%, 38-50wt%, 40-48wt%, 42-46wt%, 44-45wt%, and for example 16wt%, 17wt%, 18wt%, 19wt%, 20wt%, 21wt%. By making the content of the cross-linked polymer within the above range, the hydrogel can have excellent mechanical properties while maintaining a sufficient amount of water.

[0127] In the present invention, the cross-linked polymer refers to a polymer having a three-dimensional network structure. It can be obtained by methods known in the art, for example, by polymerizing a monomer and a cross-linking agent, or by further cross-linking a chain polymer with a cross-linking agent, or by cross-linking molecular chains of a chain polymer using an initiator.

[0128] In one embodiment, the crosslinked polymer is formed by polymerization of a raw material composition comprising monomers and a crosslinking agent, preferably by photoinitiated polymerization. Regarding the types and amount ratios of the monomers and crosslinking agent, as well as the initiator, see the description of the hydrogel precursor composition above.

[0129] In one embodiment, the cross-linked polymer comprises structural units derived from one or more monomers selected from (meth)acrylamide monomers and (meth)acrylic acid monomers; preferably, the cross-linked polymer is formed by polymerizing a raw material composition comprising monomers and a cross-linking agent, wherein the monomers are one or more selected from (meth)acrylamide monomers and (meth)acrylic acid; and the cross-linking agent is one or more multifunctional (meth)acrylate cross-linking agents.

[0130] In one embodiment, the water content in the hydrogel of the present invention is 50 to 85 wt %, preferably 60 to 75 wt %.

[0131] The present invention also correspondingly provides a method for preparing the single-network hydrogel of the present invention, which comprises the step of irradiating the hydrogel precursor composition of the present invention with light.

[0132] In one embodiment, the light irradiation is performed using ultraviolet light with a wavelength of 365 to 405 nm. The specific wavelength can be selected according to the specific photoinitiator.

[0133] In one embodiment, the hydrogel precursor composition of the present invention is poured into a mold, and then the light irradiation is performed. The size, shape and material of the mold are not particularly limited in the present invention, and those skilled in the art can make specific selections according to actual needs.

[0134] In one embodiment, the hydrogel of the present invention is prepared from the hydrogel precursor composition of the present invention using 3D printing technology such as digital light processing technology of surface projection photocuring.

[0135] The digital light processing technology of surface projection photocuring uses a high-precision ultraviolet light projection system to slice the three-dimensional model to be printed layer by layer and project it onto the surface of the hydrogel precursor liquid. The three-dimensional sample can be directly processed from the digital model by stacking them layer by layer.

[0136] The present invention accordingly relates to the hydrogel obtained by the preparation method of the present invention.

[0137] In the case of containing aramid nanofibers, the single network hydrogel of the present invention (hereinafter also referred to as aramid nanofiber-toughened hydrogel) has excellent mechanical properties.

[0138] In one embodiment, the tensile strength of the aramid nanofiber toughened hydrogel of the present invention is 20 kPa or more, preferably 30 kPa or more, more preferably 40 kPa or more, further preferably 50 kPa or more, and even more preferably 60 kPa or more. There is no particular restriction on the upper limit of the tensile strength, which is usually 500 kPa or less, or 400 kPa or less, or 300 kPa, or 200 kPa or less. The tensile strength of the aramid nanofiber toughened hydrogel of the present invention is 1.1 to 30 times that of the original hydrogel, for example, 1.3 to 20 times, for example, 1.4 to 15 times, and for example, 1.5 to 12 times, 1.6 to 10 times, 1.7 to 8 times, 1.8 to 6 times, 2 to 4 times, 2.2 to 3.6 times, 1.3 to 3.4 times, 2.4 to 3.2 times, 2.6 to 3 times.

[0139] Here, the "original hydrogel" refers to a hydrogel having the same composition and content as the aramid nanofiber toughened hydrogel of the present invention, except that the aramid nanofiber dispersion is replaced with the same content of water during preparation.

[0140] <Double network hydrogel>

[0141] Another object of the present invention is to provide a double network hydrogel comprising a first network structure and a second network structure, wherein the first network structure is formed by a cross-linked polymer and optional aramid nanofibers, at least part of the aramid nanofibers being connected to the cross-linked polymer by covalent bonds; and the second network structure is formed by carboxymethyl cellulose and Fe 3+ form.

[0142] In one embodiment, the first network structure and the second network structure are interpenetrating network structures.

[0143] Figure 7 The crosslinking mechanism of the hydrogel precursor composition or the double network hydrogel of the present invention in the preferred embodiment of the present invention is shown. The first network is a P (AAm-co-AAc) copolymer network that is permanently covalently crosslinked by ultraviolet light. Additional covalent crosslinking points and long chain entanglements are generated between the para-aramid fiber and the hydrogel polymer chain to form a mixed network. Subsequently, the introduction of iron ions causes the carboxyl groups on the carboxymethyl cellulose and acrylic acid to form a strong metal ion coordination with the iron ions. This coordination is a reversible physical crosslinking effect. Therefore, the double network hydrogel composite material is composed of a permanently covalently crosslinked P (AAm-co-AAc) network and a reversible physically crosslinked CMC-Fe 3+The network forms an interpenetrating double network. The permanent covalent cross-linking network determines the initial shape of the hydrogel (i.e., the permanent shape), and the physical cross-linking network determines the temporary shape of the hydrogel. The reversible physical cross-linking can be removed by a chelating agent (e.g., EDTA·2Na) or a low pH value (e.g., pH=0-3) environment, thereby achieving shape recovery.

[0144] The above description of the components and contents of the single network hydrogel is also applicable to the double network hydrogel of the present invention.

[0145] In one embodiment, the double network hydrogel of the present invention is prepared by combining a single network hydrogel with a Fe 3+ obtained by contacting with an aqueous solution.

[0146] One object of the present invention is to provide a method for preparing a double network hydrogel, which comprises the steps of: 3+ The step of contacting an aqueous solution.

[0147] Preferably, the contact time is 1 to 100 minutes, preferably 5 to 80 minutes, more preferably 10 to 60 minutes.

[0148] Preferably, the contacting is carried out by immersing the single network hydrogel in a liquid containing Fe 3+ is carried out in an aqueous solution.

[0149] Preferably, the Fe 3+ Fe in aqueous solution 3+ The concentration is 0.01-2 mol / L, preferably 0.05-1.8 mol / L, 0.1-1.6 mol / L, 0.2-1.5 mol / L, 0.3-1.4 mol / L, 0.4-1.3 mol / L, 0.5-1.2 mol / L, 0.6-1.1 mol / L, 0.7-1 mol / L, 0.8-0.9 mol / L.

[0150] Preferably, the Fe 3+ The aqueous solution is an aqueous solution of a water-soluble iron salt, and the water-soluble iron salt is one or more selected from ferric nitrate, ferric chloride, and ferric sulfate.

[0151] In one embodiment, the preparation method of the double network hydrogel further comprises: 3+ The step of immersing the hydrogel in water after contacting with the aqueous solution.

[0152] Preferably, the immersion time in water is 1 to 24 hours, preferably 6 to 18 hours, more preferably a time for the hydrogel to reach swelling equilibrium.

[0153] The present invention also correspondingly relates to the double network hydrogel obtained by the preparation method of the present invention.

[0154] The double network hydrogel of the invention has excellent mechanical properties.

[0155] In one embodiment, the tensile strength of the double network hydrogel of the present invention is 1500 kPa or more, preferably 1600 kPa or more, more preferably 1700 kPa or more, further preferably 1800 kPa or more, and even more preferably 1900 kPa or more. There is no particular restriction on the upper limit of the tensile strength, which is usually 5000 kPa or less, or 4500 kPa or less, or 4200 kPa, or 4000 kPa or less.

[0156] The tensile strength of the double network hydrogel of the present invention is 3+ The hydrogel has a monolayer structure having the same composition as that of a single network hydrogel, for example, 5 to 50 times, for example, 8 to 45 times, for example, 9 to 40 times, for example, 10 to 35 times, 11 to 33 times, 12 to 32 times, 13 to 31 times, 14 to 30 times, 15 to 29 times.

[0157] In one embodiment, the fracture energy of the double network hydrogel of the present invention is 1000 J / m 2 Above, preferably 1500 J / m 2 More preferably 2000 J / m 2 More preferably, 2500 J / m 2 More preferably, 3000 J / m 2 There is no particular limit on the upper limit of the fracture energy, which is usually 5000 J / m 2 Below, or 4500J / m 2 Below, or 4200J / m 2 Below, or 4000J / m 2 the following.

[0158] For the double network hydrogel of the present invention, the fracture energy when containing aramid nanofibers is 1.5 to 15 times, for example, 1.6 to 12 times, for example, 1.7 to 10 times, 1.8 to 8 times, 1.9 to 6 times, 2 to 4 times, 2.1 to 3 times, 2.2 to 2.8 times, 2.3 to 2.7 times, 2.4 to 2.5 times, of the case where other conditions are the same but aramid nanofibers are not included.

[0159] In one embodiment, the fatigue threshold of the double network hydrogel of the present invention is 10 J / m 2 Above, preferably 15 J / m 2 More preferably, 20 J / m 2 More preferably, 25 J / m 2 More than 30 J / m2 Above, 35J / m 2 There is no particular limit on the upper limit of the fatigue threshold, which is usually 200 J / m 2 Below, or 150J / m 2 Below, or 100J / m 2 For the double network hydrogel of the present invention, the fatigue threshold when the aramid nanofiber is included is 1.5 to 15 times, for example, 1.6 to 12 times, for example, 1.7 to 10 times, for example, 1.8 to 8 times, 1.9 to 6 times, 2.0 to 5 times, 2.1 to 4 times, 2.2 to 3 times, of the case where other conditions are the same but the aramid nanofiber is not included.

[0160] The present invention also relates to the use of the hydrogel of the present invention in the fields of flexible electronic devices and biomedical engineering.

[0161] <Drug delivery and drug capsules>

[0162] In one embodiment, the present invention aims to provide use of the hydrogel or double network hydrogel of the present invention for drug delivery.

[0163] In one embodiment, the present invention provides a drug capsule, comprising a shell having a cavity therein and a drug contained in the cavity, wherein the shell is composed of the double-network hydrogel of the present invention.

[0164] The present invention also provides a method for preparing the pharmaceutical capsule of the present invention, which comprises the following steps:

[0165] Using the hydrogel precursor composition of the present invention to obtain a shell precursor with an opening through digital light processing (DLP) technology of surface projection photocuring;

[0166] filling the shell precursor with a drug through the opening on the shell precursor;

[0167] The opening of the shell precursor is closed under the action of external force to form a shell having a closed structure and containing a drug in the internal cavity;

[0168] Then with Fe 3+ to obtain drug capsules.

[0169] The various features and preferred embodiments described above for the hydrogel precursor composition, single-network hydrogel, double-network hydrogel and preparation methods thereof of the present invention are also applicable to the pharmaceutical capsule and preparation method thereof of the present invention.

[0170] The present invention has no particular limitation on the shape of the shell precursor, which may be any suitable shape, such as a sheet, a sphere, a cylinder, and a common capsule shape, etc. For a sheet, it may be a triangle or a polygon that can form a closed structure (such as a tetrahedron, a cube, a cuboid, etc.).

[0171] When the shell of the drug capsule of the present invention comes into contact with an acid (such as hydrochloric acid) or a chelating agent (such as EDTA·2Na), the reversibly physically cross-linked CMC-Fe 3+ The network is destroyed, and the shell recovers from a closed structure toward the sheet, thereby forming an opening on the shell (restoring the shape of the shell precursor), so that the drug contained in the cavity can be released to the outside of the drug capsule through the opening.

[0172] The present invention has no particular limitation on the acid capable of releasing the drug, such as hydrochloric acid.

[0173] The present invention has no particular limitation on the drug in the drug capsule, which can be a drug for treating or preventing various diseases, such as a drug for treating or preventing various functional diseases and organic diseases, as needed. More specifically, it can be a drug for treating or preventing various respiratory diseases, digestive system diseases, cardiovascular and cerebrovascular system diseases, urogenital system diseases, and endocrine and metabolic system diseases.

[0174] The drug capsule of the present invention can be used for drug transportation (delivery) and drug capture.

[0175] <Pressure sensor device and pressure detection device>

[0176] In one embodiment, the purpose of the present invention is to provide a use of the double network hydrogel of the present invention for a pressure sensor. 3+ ions, and therefore have conductivity, and their conductivity changes with applied pressure, so they can be used in pressure sensors.

[0177] In one embodiment, the present invention provides a pressure sensor device, which includes the double network hydrogel of the present invention and a packaging body covering the double network hydrogel, wherein the packaging body is used to prevent water loss of the hydrogel.

[0178] Preferably, the package body is electrically insulating, for example, made of an electrically insulating polymer material.

[0179] Preferably, the encapsulant comprises polysiloxane, and more preferably comprises polydimethylsiloxane.

[0180] In one embodiment, the present invention provides a method for preparing the pressure sensor device of the present invention, which comprises: a step of preparing the double network hydrogel of the present invention as described above, and a step of encapsulating the obtained double network hydrogel.

[0181] The encapsulation method is not particularly limited in the present invention and can be carried out by any known suitable method, for example, by an impregnation method. Specifically, the double network hydrogel can be impregnated in a composition containing an encapsulation body. The impregnation time can be 2 to 20 hours, preferably 4 to 16 hours. The temperature during the impregnation is 15 to 80 degrees Celsius, preferably 20 to 70 degrees Celsius.

[0182] The composition forming the package body may be, for example, a composition containing polydimethylsiloxane and a curing agent. Specifically, various commercially available potting compounds may be used, including but not limited to 194(Shenzhen Osbon Co., Ltd.), DOWSIL TM 184 (Dow Corning DC184), Momentive RTV615 PDMS, etc.

[0183] More specifically, polydimethylsiloxane optical potting glue (containing two components of glue and curing agent, uniformly mixed in a mass ratio of 10:1) can be used, poured into a container containing a double network hydrogel, and allowed to stand at room temperature for 8 to 20 hours (or heated at 60°C for more than 2 hours) to obtain a packaging body composed of polydimethylsiloxane elastomer covering the double network hydrogel.

[0184] In one embodiment, the present invention provides a pressure detection device, which includes the pressure sensor device of the present invention.

[0185] In one embodiment, the pressure detection device of the present invention further includes a power supply and a circuit board having a resistance detection module.

[0186] Preferably, the power source includes a secondary battery (rechargeable battery), such as a lithium secondary battery, a lithium ion secondary battery, or the like.

[0187] Preferably, the pressure detection device of the present invention further comprises a housing for accommodating various components.

[0188] Preferably, the pressure detection device of the present invention further comprises a display screen for outputting information (eg, displaying measurement results).

[0189] Preferably, the pressure detection device of the present invention further comprises an adjustable button, and the adjustable button can realize one or more functions of power on / off, detection mode switching, unit switching and sensor calibration.

[0190] Preferably, the pressure detection device of the present invention has one or more of the following detection modes: real-time mass detection mode, real-time force detection mode, force change history curve mode and impact load mode. Among them, the real-time mass detection mode and the real-time force detection mode can reflect the mass of the object or the magnitude of the external force applied to the pressure sensor in real time; the force change history curve mode can record the change trend of the magnitude of the external force applied to the pressure sensor over time and draw a force-time change history curve; the impact load mode can record the maximum value of the external force acting on the pressure sensor within a period of time.

[0191] Example

[0192] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the following is a further detailed description of the embodiments of the present invention in conjunction with the accompanying drawings and examples. It should be understood that the detailed description and drawings of the following embodiments are used to illustrate the principles of the present invention by way of example and are not intended to limit the scope of the present invention. In addition, the embodiments of the present invention described below and the features in the embodiments may be combined with each other without conflict.

[0193] The descriptions of the raw materials and instruments used in the following examples are as follows:

[0194] Para-aramid nanofibers: purchased from Shandong Jufang New Materials Co., Ltd., with a diameter of 10 to 100 nm and a length of 30 to 300 μm;

[0195] Carboxymethyl cellulose: purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., brand number C104983, average molecular weight of 90,000, carboxymethyl substitution degree of 0.7;

[0196] Water-soluble TPO nanoparticles: purchased from Sigma-Aldrich, brand number 906808;

[0197] PEGDA: purchased from Shanghai Keraman Reagent Co., Ltd., brand name KLM211227, average molecular weight 700;

[0198] Fiber detangling machine: The manufacturer is Dongguan Hengke Automation Equipment Co., Ltd.

[0199] Example 1

[0200] (1) Taking different contents of para-aramid nanofibers, dispersing them in water by a fiber detangler, and obtaining uniform dispersions with para-aramid fiber mass concentrations of 0.125wt%, 0.25wt% and 0.375wt%, respectively.

[0201] (2) 6.4 g of deionized water and 6.4 g of the uniform dispersions prepared in step (1) with mass concentrations of 0.125 wt%, 0.25 wt% and 0.375 wt% were taken respectively, 0.2 g of carboxymethyl cellulose was added to the deionized water and the three solutions, and the mixtures were stirred with a magnetic stirrer for more than 6 hours in a light-proof environment to form a uniform dispersion.

[0202] (3) 3 g acrylamide, 0.24 g acrylic acid, 0.01875 g PEGDA, and 0.05 g water-soluble TPO nanoparticles were added to the four dispersions prepared in step (2), and the final mass was titrated to 10 g with deionized water. The mixture was stirred with a magnetic stirrer for more than 1 hour in a light-proof environment to form a uniform hydrogel precursor solution. The aramid fiber content in the final precursor was 0 wt%, 0.08 wt%, 0.16 wt%, and 0.24 wt%, respectively.

[0203] (4) The four hydrogel precursor solutions prepared in step (3) are filled into a polytetrafluoroethylene mold that conforms to the type 4 dumbbell-shaped specimen in GB / T528-2009, covered with a transparent acrylic plate and placed in a UV light box, and irradiated with 405 nm UV light for 5 min to obtain four single-network hydrogel composite materials with different aramid fiber contents.

[0204] (5) The four hydrogel precursor solutions prepared in step (3) were filled into a rectangular mold with a size of 25 mm × 20 mm × 0.8 mm, covered with a transparent acrylic plate and placed in a UV light box, and irradiated with 405 nm UV light for 4 min to obtain four single-network hydrogel composite materials with different aramid fiber contents.

[0205] (6) The single network hydrogel composite material obtained by curing in steps (4) and (5) was immersed in a 0.1M ferric nitrate solution for 30 minutes, and then immersed in deionized water for more than 12 hours to achieve swelling equilibrium, and finally four double network hydrogel composite materials with different aramid fiber contents were obtained. The dumbbell-shaped specimen can be used for uniaxial tensile test, and the rectangular specimen can be used for Rivlin-Thomas fracture test and fatigue cyclic loading test.

[0206] Figure 1 The stress-strain curves of four single network hydrogel composites with different aramid fiber contents are shown. Figure 1 It can be seen that the strength of the single network hydrogel composites with 0.08wt%, 0.16wt% and 0.24wt% aramid fiber content is increased by 59%, 142% and 270% respectively compared with the hydrogel without aramid fiber.

[0207] Figure 2The stress-strain curves of four double network hydrogel composites with different aramid fiber contents after treatment with iron ions are shown. Figure 2 It can be seen that the strength of the double-network hydrogel composites with 0.08wt%, 0.16wt% and 0.24wt% aramid fiber content is increased by 25%, 53% and 79% respectively compared with the hydrogel without aramid fiber.

[0208] Will Figure 1 and Figure 2 By comparison, the strength of the double network hydrogel composites with four aramid fiber contents (2.0 MPa, 2.5 MPa, 3.1 MPa, and 3.6 MPa) increased to 28.5, 22.3, 18.0, and 13.8 times that of the original single network hydrogel composites, respectively. 3+ The formed second layer network significantly improved the strength of the hydrogel, and the increase in strength was not accompanied by a decrease in elongation at break.

[0209] Figure 3 The fracture energy variation curves of four double network hydrogel composite materials are shown. The fracture energy test method is consistent with the literature Nature, 2012, 489(7414): 133-136. Figure 3 It can be seen that the fracture energy of the double network hydrogel composites with 0.08wt%, 0.16wt% and 0.24wt% aramid fiber content is 3675J / m 2 、3935J / m 2 、4008J / m 2 ) compared to the fracture energy of the hydrogel without aramid fiber (1600 J / m 2 ) increased by 130%, 146% and 150% respectively.

[0210] Figure 4 The fatigue threshold test results of four double network hydrogel composites are shown. The fatigue threshold test method is consistent with the literature Extreme Mechanics Letters, 2017, 15: 91-96. Figure 4 It can be seen that the fatigue thresholds of the double network hydrogel composites with 0.08wt%, 0.16wt% and 0.24wt% aramid fiber content are 48.59J / m 2 、63.03J / m 2 、79.88J / m 2 , respectively, to the fatigue threshold of the hydrogel without aramid fiber (25.34 J / m 2 ) are 1.9, 2.5, and 3.2 times as high.

[0211] Example 2

[0212] (1) The para-aramid nanofibers were dispersed in water using a fiber deflaying machine to obtain a uniform dispersion having a para-aramid fiber mass concentration of 0.125 wt %.

[0213] (2) Take 25.6 g of the aramid fiber uniform dispersion prepared in step (1), add 0.8 g of carboxymethyl cellulose thereto, and stir with a magnetic stirrer for more than 6 hours in a light-proof environment to make the above mixture into a uniform dispersion.

[0214] (3) Add 12 g acrylamide, 0.96 g acrylic acid, 0.075 g PEGDA, 0.2 g water-soluble TPO nanoparticles, and 12 mg quinoline yellow to the dispersion prepared in step (2), and titrate the mixture to a final mass of 40 g with deionized water. Stir with a magnetic stirrer for more than 1 hour in a light-proof environment to form a uniform hydrogel precursor solution.

[0215] (4) The hydrogel precursor solution prepared in step (3) was transferred to the liquid tank of the DLP 3D printer, and the slice thickness was set to 40 μm, the UV wavelength to 405 nm, and the UV intensity to 58 mW / cm 2 The exposure time of the bottom layer is 8s, and the exposure time of the remaining layers is 6s, and a high-resolution hydrogel structure is printed.

[0216] (5) The high-resolution hydrogel structure printed in step (4) was immersed in a 0.1 M ferric nitrate solution for 30 min, and then immersed in deionized water for more than 12 hours to achieve swelling equilibrium, thereby finally obtaining a high-strength, high-resolution hydrogel structure.

[0217] Figure 5 The high-resolution hydrogel three-dimensional lattice structure printed by DLP 3D is displayed. The upper and lower rows of each structure are actual photos before and after immersion in ferric nitrate solution.

[0218] Example 3

[0219] (1) The para-aramid nanofibers were dispersed in water using a fiber deflaying machine to obtain a uniform dispersion having a para-aramid fiber mass concentration of 0.125 wt %.

[0220] (2) Take 6.4 g of the aramid fiber uniform dispersion prepared in step (1), add 0.2 g of carboxymethyl cellulose thereto, and stir with a magnetic stirrer for more than 6 hours in a light-proof environment to make the above mixture into a uniform dispersion.

[0221] (3) Add 3 g acrylamide, 0.24 g acrylic acid, 0.01875 g PEGDA, and 0.05 g water-soluble TPO nanoparticles to the dispersion prepared in step (2), and titrate the mixture to a final mass of 10 g with deionized water. Stir the mixture with a magnetic stirrer for more than 1 hour in a light-proof environment to form a uniform hydrogel precursor solution.

[0222] (4) The hydrogel precursor solution prepared in step (3) was filled into a rectangular parallelepiped mold with a size of 25 mm×2 mm×1 mm, covered with a transparent acrylic plate and placed in a UV light box, and irradiated with 405 nm UV light for 5 min to obtain a single network hydrogel composite material.

[0223] (5) applying an external force to the single-network hydrogel composite material obtained by curing in step (4), bending it 180° and soaking it in a 0.8 M ferric nitrate solution for 5 min, then transferring it to deionized water and soaking it for 5 min to remove excess ferric nitrate solution, and removing the external force to obtain a double-network hydrogel composite material with a fixed shape.

[0224] (6) The double network hydrogel with fixed shape in step (5) is immersed in an acidic environment with pH = 0, and the hydrogel can gradually recover to the initial shape after curing in step (4), and the recovery time is within 3 minutes.

[0225] (7) The double network hydrogel with fixed shape in step (5) is immersed in a 0.1 M chelating agent EDTA·2Na solution. The hydrogel can also gradually recover to the initial shape after curing in step (4), and the recovery time is within 30 minutes.

[0226] (8) Steps (5) and (6) or steps (5) and (7) can be repeated multiple times.

[0227] Figure 6 The shape memory effect of fiber-reinforced hydrogel composites was demonstrated, which can achieve shape fixation induced by metal ions and shape recovery induced by pH or chelating agents.

[0228] Figure 7 The cross-linking mechanism of the fiber-reinforced hydrogel composite material was demonstrated. The first layer of the network was a P(AAm-co-AAc) copolymer network that was permanently covalently cross-linked by UV light. Additional covalent cross-linking points and long-chain entanglements were generated between the para-aramid fibers and the hydrogel polymer chains to form a mixed network. Subsequently, the introduction of iron ions allowed the carboxyl groups on carboxymethyl cellulose and acrylic acid to form a strong metal ion coordination with the iron ions. This coordination was a reversible physical cross-linking effect. Therefore, the double-network hydrogel composite material was composed of a permanently covalently cross-linked P(AAm-co-AAc) network and a reversible physically cross-linked CMC-Fe 3+The network forms an interpenetrating double network. The permanent covalent cross-linking network determines the initial shape of the hydrogel (i.e., the permanent shape), and the physical cross-linking network determines the temporary shape of the hydrogel. The reversible physical cross-linking can be removed by the chelating agent EDTA·2Na or a low pH environment, thereby achieving shape recovery.

[0229] Embodiment 4:

[0230] (1) The para-aramid nanofibers were dispersed in water using a fiber deflaying machine to obtain a uniform dispersion having a para-aramid fiber mass concentration of 0.125 wt %.

[0231] (2) Take 25.6 g of the aramid fiber uniform dispersion prepared in step (1), add 0.8 g of carboxymethyl cellulose thereto, and stir with a magnetic stirrer for more than 6 hours in a light-proof environment to make the above mixture into a uniform dispersion.

[0232] (3) Add 12 g acrylamide, 0.96 g acrylic acid, 0.075 g PEGDA, and 0.2 g water-soluble TPO nanoparticles to the dispersion prepared in step (2), and titrate the final mass to 40 g with deionized water. Stir with a magnetic stirrer for more than 1 hour in a light-proof environment to form a uniform hydrogel precursor solution.

[0233] (4) The hydrogel precursor solution prepared in step (3) was transferred to the liquid tank of the DLP 3D printer, and the slice thickness was set to 40 μm, the UV wavelength to 405 nm, and the UV intensity to 58 mW / cm 2 The exposure time of the bottom layer is 8s, and the exposure time of the remaining layers is 6s, and a three-dimensional structured hydrogel sheet is printed.

[0234] (5) applying external force to the hydrogel sheet obtained by printing in step (4), filling the hydrogel sheet with drugs and fixing it into a temporary shape with a closed structure, and then soaking it in a 0.8M ferric nitrate solution for 5 minutes, and then soaking it in deionized water for 5 minutes to remove excess ferric nitrate solution. After removing the external force, a drug capsule encapsulating the drug with a fixed shape can be obtained.

[0235] (6) The capsule containing the drug with a fixed shape in step (5) is immersed in an acidic environment with pH = 0, and the hydrogel can gradually return to its original shape after printing in step (4).

[0236] (7) The capsule containing the drug with a fixed shape in step (5) is immersed in a 0.1 M chelating agent EDTA·2Na solution, and the hydrogel can also gradually return to the original shape after printing in step (4).

[0237] (8) Repeat steps (5) and (6) or steps (5) and (7) multiple times.

[0238] Figure 8 The hydrogel sheet printed by DLP 3D in step (4), the drug capsule encapsulating the drug with a fixed shape in step (5), and the hydrogel sheet restored to its original shape in step (6) are shown. Figure 8 It can be seen that the drug capsule of the present invention can achieve effective shape fixation and shape recovery induced by pH value or chelating agent to achieve the function of drug delivery or grasping.

[0239] Embodiment 5:

[0240] (1) The para-aramid nanofibers were dispersed in water using a fiber deflaying machine to obtain a uniform dispersion having a para-aramid fiber mass concentration of 0.125 wt %.

[0241] (2) Take 25.6 g of the aramid fiber uniform dispersion prepared in step (1), add 0.8 g of carboxymethyl cellulose thereto, and stir with a magnetic stirrer for more than 6 hours in a light-proof environment to make the above mixture into a uniform dispersion.

[0242] (3) Add 12 g acrylamide, 0.96 g acrylic acid, 0.075 g PEGDA, and 0.2 g water-soluble TPO nanoparticles to the dispersion prepared in step (2), and titrate the final mass to 40 g with deionized water. Stir with a magnetic stirrer for more than 1 hour in a light-proof environment to form a uniform hydrogel precursor solution.

[0243] (4) The hydrogel precursor solution prepared in step (3) was transferred to the liquid tank of the DLP 3D printer, and the slice thickness was set to 40 μm, the UV wavelength to 405 nm, and the UV intensity to 58 mW / cm 2 The exposure time of the bottom layer is 8s, and the exposure time of the remaining layers is 6s, and a high-resolution three-dimensional structure hydrogel is printed.

[0244] (5) Soaking the hydrogel printed in step (4) in a 0.1 M ferric nitrate solution for 30 min, and then soaking it in deionized water for more than 12 hours to achieve swelling equilibrium, thereby finally obtaining a high-strength, high-resolution, conductive double-network hydrogel with pressure sensing performance.

[0245] (6) Preparation of polydimethylsiloxane optical potting glue ( 194, the two components of the adhesive and the curing agent are uniformly mixed in a mass ratio of 10:1), poured into a rectangular cavity mold containing the double network hydrogel obtained in step (5), and allowed to stand at room temperature for more than 12 hours to obtain a PDMS elastomer-encapsulated pressure sensor device that can effectively prevent the hydrogel from losing water.

[0246] (7) The pressure sensor device obtained in step (6) is connected to a circuit board including a resistance detection module, calibrated and marked, and assembled together with a rechargeable battery into a customized instrument box to obtain an integrated pressure detection device.

[0247] Fig. 9 The three-dimensional structure of the single network gel obtained by DLP 3D printing in step (4), the double network hydrogel obtained in step (5), and the physical picture of the integrated pressure detection device assembled in step (7) are shown, as well as photos of various modes of testing using the integrated pressure detection device. The integrated pressure detection device of the present invention has a digital screen with accurate display, a calibration system that can be calibrated according to different hydrogel characteristics, an adjustable button and a charging module, and can realize four modes of detection: real-time mass detection mode, real-time force detection mode, force change history curve mode over time, and impact load (maximum value) mode.

[0248] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principle of the present invention should be included in the scope of the claims of the present invention.

[0249] Industrial Applicability

[0250] The hydrogel precursor composition of the present invention can be used as a resin material for commercial DLP printing companies to print hydrogel soft materials with excellent mechanical properties and multifunctionality. The hydrogel of the present invention has good electrical conductivity, and its resistance can change with applied strain, and can be widely used in the field of flexible electronic devices. Unlike traditional sensors, the present invention can prepare conductive hydrogel materials with specific geometric shapes through 3D printing to adapt to different application scenarios.

Claims

1. A hydrogel precursor composition, characterized in that The invention comprises carboxymethyl cellulose, a monomer, a cross-linking agent and a water-soluble photoinitiator, and optionally further comprises aramid nanofibers and a light absorber.

2. The hydrogel precursor composition according to claim 1, characterized in that The content of the aramid nanofiber is 0-1wt%; the content of the carboxymethyl cellulose is 0.001-10wt%; the content of the monomer is 15-60wt%; the content of the crosslinking agent is 0.01-5wt%; the content of the water-soluble photoinitiator is 0.1-1.5wt%; the content of the light absorber is 0-0.1wt%; Preferably, the weight ratio of the monomer to the cross-linking agent is 100:(0.1-1); the weight ratio of the total weight of the monomer and the cross-linking agent to the water-soluble photoinitiator is (100-40):

1.

3. The hydrogel precursor composition according to claim 1 or 2, characterized in that: The aramid nanofibers are para-aramid nanofibers with an average diameter of 10 to 500 nm and an aspect ratio of 2000 to 4000; The average relative molecular mass of the carboxymethyl cellulose is 10000-1000000, and the degree of carboxymethyl substitution is 0.5-0.9; The monomer is one or more selected from (meth)acrylamide monomers and (meth)acrylic acid monomers; preferably, the monomer includes one or more selected from (meth)acrylamide monomers and one or more (meth)acrylic acid monomers, and more preferably, the mass ratio of (meth)acrylamide monomers to (meth)acrylic acid monomers is (1-20):1; The crosslinking agent is one or more selected from (meth)acrylic acid and (meth)acrylamide crosslinking agents; wherein the (meth)acrylic acid crosslinking agent is preferably one or more selected from multifunctional (meth)acrylic acid and its salts and multifunctional (meth)acrylates, more preferably polyethylene glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate; the (meth)acrylamide crosslinking agent is preferably N,N-methylenebisacrylamide; the crosslinking agent is preferably polyethylene glycol diacrylate (PEGDA); The water-soluble initiator is one or more selected from water-soluble aromatic ketones, condensed aromatic hydrocarbons, polysilanes, acylphosphonates, azos and metal organic complex initiators, preferably water-soluble TPO; The light absorber is one or more selected from quinoline yellow, methyl red and brilliant green.

4. The method for preparing a hydrogel precursor composition according to any one of claims 1 to 3, characterized in that: The following steps are involved: Dispersing carboxymethyl cellulose in water, or dispersing carboxymethyl cellulose in an aqueous dispersion of aramid nanofibers, to obtain a carboxymethyl cellulose dispersion; The carboxymethyl cellulose dispersion is mixed with a monomer, a crosslinking agent and a water-soluble photoinitiator to obtain the hydrogel precursor composition.

5. A hydrogel, characterized in that: The invention comprises carboxymethyl cellulose and a cross-linked polymer, and optionally further comprises aramid nanofibers, wherein at least a part of the aramid nanofibers are connected to the cross-linked polymer via covalent bonds.

6. A double network hydrogel, characterized in that: The invention comprises a first network structure and a second network structure, wherein the first network structure is formed by a cross-linked polymer and optional aramid nanofibers, at least part of the aramid nanofibers are connected to the cross-linked polymer by covalent bonds; and the second network structure is formed by carboxymethyl cellulose and Fe 3+ form.

7. The hydrogel according to claim 5 or 6, characterized in that The aramid nanofiber is a para-aramid nanofiber with an average diameter of 10 to 500 nm and an aspect ratio of 2000 to 4000; the content of the aramid nanofiber is 0 to 1 wt%; The content of the carboxymethyl cellulose is 0.001-10wt%; The content of the cross-linked polymer is 15 to 65 wt %; the cross-linked polymer comprises structural units derived from one or more monomers selected from (meth)acrylamide monomers and (meth)acrylic acid monomers; preferably, the cross-linked polymer is formed by polymerizing a raw material composition comprising a monomer and a cross-linking agent, the monomer being one or more selected from (meth)acrylamide monomers and (meth)acrylic acid; the cross-linking agent is one or more selected from (meth)acrylic acid and (meth)acrylamide cross-linking agents; the weight ratio of the monomer to the cross-linking agent is 100:(0.1 to 1); the polymerization is preferably photoinitiated polymerization.

8. The method for preparing the hydrogel according to claim 5, characterized in that: The method comprises the step of irradiating the hydrogel precursor composition according to any one of claims 1 to 3 with light; Preferably, the hydrogel precursor composition is poured into a mold and then the light irradiation is performed; or the light irradiation is performed while the hydrogel precursor composition is 3D printed; Preferably, the light irradiation is performed using light with a wavelength of 365 to 405 nm; Preferably, the light irradiation is performed by digital light processing (DLP) technology of surface projection photocuring.

9. The method for preparing the double network hydrogel according to claim 6, characterized in that: The hydrogel according to claim 5 is mixed with Fe 3+ a step of contacting an aqueous solution; Preferably, the contact time is 1 to 100 minutes, preferably 5 to 80 minutes, more preferably 10 to 60 minutes; Preferably, the contacting is carried out by immersing the hydrogel according to claim 5 in a liquid containing Fe 3+ in an aqueous solution; Preferably, the Fe 3+ Fe in aqueous solution 3+ The concentration is 0.01~2mol / L; Preferably, the Fe 3+ The aqueous solution is an aqueous solution of a water-soluble iron salt, and the water-soluble iron salt is one or more selected from ferric nitrate, ferric chloride, and ferric sulfate.

10. The method for preparing the double network hydrogel according to claim 9, characterized in that: It also includes the 3+ The step of immersing the hydrogel in water after contact with the aqueous solution, preferably, the immersion time in water is 1 to 24 hours, preferably 6 to 18 hours, more preferably the time for the hydrogel to reach swelling equilibrium.

11. Use of the hydrogel according to claim 5 or the double network hydrogel according to claim 6 for drug delivery or pressure sensor.

12. A drug capsule, characterized in that: It comprises a shell having a cavity inside and a drug contained in the cavity, wherein the shell is composed of the double-network hydrogel according to claim 6.

13. The drug capsule according to claim 12, characterized in that: The shell forms an opening when in contact with an acid or a chelating agent, so that the drug contained in the cavity can be released to the outside of the drug capsule through the opening; Preferably, the chelating agent is EDTA·2Na.

14. The method for preparing the drug capsule according to claim 12 or 13, characterized in that: The following steps are involved: A shell precursor having an opening is obtained by using the hydrogel precursor composition according to any one of claims 1 to 3 through digital light processing (DLP) technology of surface projection photocuring; filling the shell precursor with a drug through the opening on the shell precursor; The opening of the shell precursor is closed under the action of external force to form a shell having a closed structure and containing a drug in the internal cavity; Then with Fe 3+ to obtain drug capsules.

15. A pressure sensor device, characterized in that: It comprises the double network hydrogel according to claim 6 and a packaging body covering the double network hydrogel, wherein the packaging body is used to prevent water loss of the hydrogel; The encapsulant is preferably electrically insulating, more preferably comprises polysiloxane, and further preferably comprises polydimethylsiloxane.

16. A pressure detection device, characterized in that: Includes the pressure sensor device as claimed in claim 15.

17. The pressure detection device according to claim 16, characterized in that: It also includes a power supply and a circuit board with a resistance detection module, and optionally includes one or more components selected from a housing for accommodating various components, a display screen for outputting information, and an adjustment button.

Citation Information

Patent Citations

  • Ion-covalent double-network hydrogel and preparation method thereof

    CN105461945A

  • Carboxymethyl cellulose / aramid nano fiber composite membrane as well as preparation method and application thereof

    CN112920467A

  • Aramid nanofiber strengthening and toughening hydrogel and preparation method thereof

    CN114437372A

  • Hydrogel composite comprising nanocellulose and fabrication method thereof

    KR1020160085152A