Polyurethane wet-process hydrolysis-resistant resin for soft high-peel-off imitation sheepskin leather and preparation method of polyurethane wet-process hydrolysis-resistant resin
By combining polytetrahydrofuran and polypropylene oxide structures and other components in wet hydrolysis-resistant resins, the problem that the prior art cannot achieve the imitation skin feeling and high peel strength at the same time is solved, and the synthetic leather is improved The washing properties and peel strength enhance the application value of the product.
Patent Information
- Application Number
- CN202410953688.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-15
AI Technical Summary
The existing soft imitation skin feeling and high peel wet leather resins cannot take into account both imitation skin feeling and high peel strength properties, resulting in bottlenecks in the application and added value of synthetic leather with imitation sheepskin effect.
Polyurethane wet hydrolysis-resistant resin is used to adjust the viscosity, solid content and reaction conditions of the resin by using polyether polyols, isocyanates, solvents and additives with polytetrahydrofuran structure and polypropylene oxide structure in synthesis to prepare Resin with excellent washing properties and high peel strength.
The high peel strength, washing properties and imitation skin feeling of synthetic leather are achieved, improving the product's hydrolysis resistance and feel, ensuring the realization of the effect of imitation sheepskin and improving the added value.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polyurethane materials, and in particular relates to a polyurethane wet-process hydrolysis-resistant resin for soft high-peelable imitation sheepskin leather, and a preparation method and application thereof. Background Art
[0002] The wet-process hydrolysis-resistant resin for imitation sheepskin leather refers to a synthetic leather that is soft, highly peelable and hydrolysis-resistant, and has an imitation sheepskin feel. The prepared hydrolysis-resistant resin is first applied to a mirror-finished high-F cloth, and then put into water with a scraper of fixed thickness for solidification, washing, and drying. A layer of dry-process protein-like skin-feel resin is then attached to the surface of the wet-process base.
[0003] Currently, there are soft protein-like skin-feel hydrolysis-resistant wet leather resins and soft high-peel hydrolysis-resistant wet leather resins on the market. Soft protein-like skin-feel hydrolysis-resistant wet leather resins are synthetic leathers made by wet-processing imitating sheepskin leather by adding a large amount of protein-like skin-feel additives to the back end of the design formula in order to achieve better protein-like skin-feel performance; the disadvantage of this method is that the synthetic leather with sheepskin-like effect after processing is prone to surface fogging and has significantly low peeling strength. The soft high-peeling hydrolysis-resistant wet leather resin is a synthetic leather made by imitating sheepskin leather using a wet process, in order to achieve high peeling performance, by using a large amount of polyether polyols with a polytetrahydrofuran structure and increasing the solid content of the resin itself. The method has the disadvantage that the synthetic leather feels obviously harder and difficult to wash after processing. The soft protein-like skin-feel hydrolysis-resistant leather resin and the soft high-peeling hydrolysis-resistant leather resin currently sold on the market cannot simultaneously achieve the protein-like skin feel and high peeling strength performance of the product, so that the synthetic leather that cannot achieve the sheepskin-like effect encounters bottlenecks in the back-end application development of various styles, and it is difficult to increase the added value of the products on the market.
[0004] Therefore, it is very necessary to develop a soft high-peelable imitation sheepskin leather polyurethane wet process hydrolysis resistant resin. Summary of the invention
[0005] The existing high-peeling and hydrolysis-resistant synthetic leather is prone to problems such as insufficient base thickness and poor base surface flatness. At the same time, the synthetic leather has unstable product peeling strength due to insufficient water washing, and the use range of back-end application products is limited. The present invention provides a polyurethane wet-process hydrolysis-resistant resin for soft high-peeling imitation sheepskin leather, and a preparation method and application thereof.
[0006] To achieve this object, the present invention adopts the following technical solutions:
[0007] In a first aspect, the present invention provides a polyurethane wet-process hydrolysis-resistant resin for soft high-peelable imitation sheepskin leather, the raw materials for preparation of which include the following components in parts by weight:
[0008] 0.001-0.003 parts of inorganic acid;
[0009] Polyol 205-274 parts;
[0010] Isocyanate 57-77 parts;
[0011] 9-13 parts of small molecule alcohol;
[0012] 14-20 parts of additives;
[0013] 612-816 parts of solvent;
[0014] Preferably, the inorganic acid is concentrated phosphoric acid. In the synthesis of leather resin, a phosphoric acid solution with a concentration of 80%-90% is usually called "concentrated phosphoric acid", and the concentrated phosphoric acid here can be any value within the above concentration range.
[0015] Preferably, the polyether polyol includes polyether polyol and polyester polyol, the polyether polyol is: polyether polyol with polytetrahydrofuran structure (denoted as PE-1), polyether polyol with polypropylene oxide structure (denoted as PE-2), polyether polyol with mixed structure of polypropylene oxide and ethylene oxide (denoted as PE-3), wherein the molar ratio of propylene oxide unit to ethylene oxide unit in PE-3 is 2.8-3:1.8-2; the polyester polyol is polyester polyol of adipic acid-1,4-butanediol system (denoted as PE-4).
[0016] Preferably, the molecular weight range of PE-1 and PE-4 is 1800-2200 in number average molecular weight; the molecular weight range of PE-2 and PE-3 is 3800-4200 in number average molecular weight.
[0017] Preferably, the molecular weights of PE-1 and PE-4 are both 2000; the molecular weights of PE-2 and PE-3 are both 4000.
[0018] Preferably, the isocyanate is one or more of diphenylmethane diisocyanate (MDI), dicyclohexylmethane diisocyanate (HMDI), toluene diisocyanate (TDI), preferably diphenylmethane diisocyanate (MDI).
[0019] Preferably, the small molecule alcohol is one or more of ethylene glycol (EG), diethylene glycol, and monoethanolamine, as a chain extender, preferably ethylene glycol (EG).
[0020] Preferably, the solvent is N,N-dimethylformamide (DMF), and the auxiliary agent is one or more of a water-assisting agent, a stabilizer, a capping agent, and a hindered phenol antioxidant.
[0021] Preferably, the water-assisting agent is a polysiloxane system softener and a polyether polyol, which may be commercially available products.
[0022] Preferably, the stabilizer is benzoic acid.
[0023] Preferably, the capping agent is methanol.
[0024] In a second aspect, the present invention further provides a method for preparing the above-mentioned soft high-peelable imitation sheepskin leather polyurethane wet-process hydrolysis-resistant resin, comprising the following steps:
[0025] First, a polyurethane wet process hydrolysis-resistant resin intermediate is prepared, and the preparation steps are as follows:
[0026] (1) mixing part of the polyether polyol with a polytetrahydrofuran structure, the polyether polyol with a polypropylene oxide structure, the polyester polyol of adipic acid-1,4-butanediol system, part of the small molecule alcohol, part of the hindered phenol antioxidant, the inorganic acid, and part of the solvent, and heating the mixture;
[0027] (2) adding a portion of isocyanate to the mixture after treatment in step (1) and treating at a constant temperature;
[0028] (3) adding part of the isocyanate to the mixture treated in step (2) to react, and maintaining the R value at 0.9-1.1, adding part of the solvent until the viscosity of the reaction liquid is 10-14 Pas / 25 degrees, and the solid content of the reaction liquid is 31%-33%, and then adding the blocking agent, stirring, and cooling;
[0029] (4) adding a stabilizer, a polysiloxane system softener and a water-assistant to the mixture after treatment in step (3) and stirring to obtain the polyurethane wet process hydrolysis-resistant resin intermediate;
[0030] Then, the polyurethane wet process hydrolysis-resistant resin is prepared, and the preparation steps are as follows:
[0031] (a) mixing the remaining polyether polyol with a polytetrahydrofuran structure, the polyether polyol with a mixed structure of polypropylene oxide and ethylene oxide, the remaining small molecule alcohol, the remaining hindered phenol antioxidant, the inorganic acid, and part of the solvent in the polyether polyol, and heating the mixture; (b) adding part of the isocyanate to the mixture after treatment in step (a), and treating the mixture at a constant temperature;
[0032] (c) adding the remaining isocyanate to the mixture after the treatment in step (b) to react, and maintaining the R value at 0.9-1.1, adding the remaining solvent until the viscosity of the reaction liquid is 20-26pas / 25 degrees, and the solid content of the reaction liquid is 31%-33%, and then adding the blocking agent, stirring and cooling; (d) adding a stabilizer, a part of the polyurethane wet process hydrolysis-resistant intermediate, and a polyether polyol water-assistant to the mixture after the treatment in step (c) and stirring to obtain the polyurethane wet process hydrolysis-resistant resin.
[0033] Preferably, the preparation of the polyurethane wet-process hydrolysis-resistant resin is completed in a reaction kettle.
[0034] Preferably, in step (1) and step (a), the temperature treatment condition is to heat the mixture to 40°C-50°C, and after the temperature is raised, the mixture is stirred at a constant temperature for 20-40 minutes. Preferably, based on the total mass of the solvent as 100%, the sum of the added solvents in step (1) and step (a) is 70%-75% (mass percentage) of the total amount of the solvent.
[0035] Preferably, in step (2) and step (b), the isothermal treatment condition is stirring at 70° C.-75° C. for 1-3 hours; and the sum of the amount of isocyanate added is 90%-95% of the total amount of isocyanate.
[0036] Preferably, in step (3) and step (c), the temperature is controlled at 70° C.-75° C. during the addition of isocyanate.
[0037] In a third aspect, the present invention also provides a synthetic leather, which is prepared using the above-mentioned soft high-peelable imitation sheepskin leather polyurethane wet process hydrolysis-resistant resin, or prepared using the resin prepared by the above-mentioned preparation method of the soft high-peelable imitation sheepskin leather polyurethane wet process hydrolysis-resistant resin.
[0038] Beneficial effects: (1) In the preparation of the polyurethane wet process hydrolysis-resistant resin, the polyether polyol (PE1) with a polytetrahydrofuran structure and the polyether polyol (PE3) with a mixed structure of polypropylene oxide and ethylene oxide are selected through the main synthesis to improve the film-forming property and firmness and thickness of the synthetic leather surface; the water washability and high peel strength of the resin are significantly improved, and it is easier to coordinate the changes in the permeability of the main body to the cloth than using a single-structure polyether polyol; the small molecule alcohol is used as a chain extender to increase the solidification speed of the resin to make the resin more uniform while ensuring the improvement of the firmness, and the increase in the amount of the chain extender to improve the temperature resistance, modulus, solidification speed and gloss of the resin is easier to adjust than using a chain extender containing a side chain; the selection of two additives with different structures not only helps the solidification uniformity but also helps the water washability and improves the gloss of the synthetic leather, and significantly improves the gloss and softness of the synthetic leather surface.
[0039] (2) In the preparation of the polyurethane wet process hydrolysis-resistant resin of the present invention, a polyurethane resin intermediate is synthesized by combining different proportions of a polyether polyol (PE-1) with a polytetrahydrofuran structure, a polyester polyol (PE-4) with a 1,4-butanediol-adipate system, and a polyether polyol (PE-2) with a polypropylene oxide structure, and combining them with a chain extender with good temperature resistance, a polysiloxane softening agent, and the like. The solidification speed, modulus, thickness retention rate, protein-like skin feel, and water washability of the resin are significantly improved, so that when preparing the resin for imitation sheepskin leather, a good combination of water washability and protein-like skin feel can be ensured.
[0040] (3) In the preparation of the polyurethane wet process hydrolysis-resistant resin of the present invention, by selecting a chain extender with strong temperature resistance and a combination ratio between polyether polyol PE-3 (polyether polyol with a mixed structure of polypropylene oxide and ethylene oxide) and PE-1 (polyether polyol with a polytetrahydrofuran structure), good peel strength and water washing performance can be ensured, and 5 years of hydrolysis resistance can also be ensured.
[0041] (4) In the preparation of the polyurethane wet process hydrolysis-resistant resin of the present invention, the main resin accounts for 85% of the total amount of the polyurethane resin synthesized by the same process, and the intermediate resin is added with 15% to improve the 5-year hydrolysis resistance of the resin, thereby achieving the performance of cloth penetration, high peel strength and soft hand feel. It plays a key role in achieving 5-year hydrolysis resistance, soft hand feel and high peel strength for the polyurethane hydrolysis-resistant resin used in the preparation of soft imitation sheepskin leather.
[0042] (5) In the preparation of the polyurethane wet process hydrolysis-resistant resin of the present invention, the water washing performance and the softness of the resin are improved by adding a polysiloxane softener as an auxiliary agent when the synthesis of the intermediate resin is terminated, and then the water washing performance is improved by adding a polyether polyol when the synthesis of the main resin is terminated. The two are matched with each other to achieve water washing and softness, and at the same time, the amount of polysiloxane softener used is reduced to ensure the effect of the polysiloxane softener on the peel strength (the compatibility of the polysiloxane softener with the polyurethane resin is poor). DETAILED DESCRIPTION
[0044] The raw materials used in the examples and comparative examples of the present invention are as follows:
[0045] PE-1 (polyether polyol with polytetrahydrofuran structure): molecular weight 2000 (Hyosung Group (Jiaxing) Co., Ltd., model: PTMG-2000);
[0046] PE-17 (polyether polyol with polytetrahydrofuran structure): molecular weight 1000 (Hyosung Group (Jiaxing) Co., Ltd., model: PTMG-1000);
[0047] PE-2 (polyether polyol with polypropylene oxide structure): molecular weight 4000 (Shandong Bluestar Dongda Co., Ltd., model: DP-4000D);
[0048] PE-3 (polyether polyol with mixed structure of polypropylene oxide and ethylene oxide): molecular weight is 4000 (Shandong Bluestar Dongda Co., Ltd., model: ED-28), the molar ratio of propylene oxide unit to ethylene oxide unit in PE-3 is about 3:2;
[0049] PE-4 (polyester polyol of adipic acid-1,4-butanediol system): molecular weight is 2000;
[0050] PE-5 (polyester polyol of adipic acid-1,4-butanediol-ethylene glycol system): molecular weight is 2000;
[0051] Hindered phenol antioxidant: ROX-13TP (Double Bond Chemical Co., Ltd., Taiwan, China, model: antioxidant 1330);
[0052] Water-assisting detergent polysiloxane softener: XP-300 (Guangzhou Siluoke Polymer Co., Ltd., model: 8818F2) and polyether polyol: XP-600 (Shandong Bluestar Dongda Co., Ltd., model: EP-3600).
[0053] Among the raw materials used in the present invention, PE-4 and PE-5 are both homemade in the laboratory (using a batch process), and the others are commercially available products.
[0054] Example 1
[0055] A polyurethane wet-process hydrolysis-resistant resin for soft high-peelable sheepskin-like leather, the preparation raw materials of which include the following components:
[0056] PE-1: 102g, PE-2: 9g, PE-3: 93g, PE-4: 5g, hindered phenol antioxidant ROX-13TP: 0.2g, concentrated phosphoric acid: 0.002g, ethylene glycol: 10g, DMF: 613g, MDI: 58g, methanol: 0.45g, benzoic acid: 0.45g, polysiloxane softener XP-300: 2g, polyether polyol XP-600: 13g.
[0057] The preparation method of the above-mentioned polyurethane wet process hydrolysis-resistant resin is as follows.
[0058] First, prepare a polyurethane wet process hydrolysis-resistant resin intermediate, and the preparation steps are as follows:
[0059] (1) According to the above mass, 9% (mass percentage, the same below) of the total amount of polyether polyol (PE-1) with polytetrahydrofuran structure, polyether polyol (PE-2) with polypropylene oxide structure, polyester polyol (PE-4) with adipic acid-1,4-butanediol system, 20% of the total amount of ethylene glycol (EG), half of the amount of hindered phenol antioxidant ROX-23TP, concentrated phosphoric acid, and 9% of the total amount of DMF were added to the reactor, the temperature was raised to 40° C., the temperature was maintained constant, and stirred for 30 minutes;
[0060] (2) adding 12% of MDI to the mixture after treatment in step (1), and stirring at 70° C. for 2 hours;
[0061] (3) adding 0.2% of MDI to the mixture after treatment in step (2) to carry out reaction, keeping the R value at 1, maintaining 70° C., adding 5% of DMF to the total amount of DMF until the viscosity of the reaction liquid is 12 Pas / 25 degrees, and the solid content of the reaction liquid is 32%, and then adding methanol capping agent, stirring for 30 minutes and cooling to 60° C.;
[0062] (4) Add benzoic acid stabilizer and polysiloxane softener XP-300 water-aid detergent to the mixture after treatment in step (3), and stir for 1.5 hours to obtain a polyurethane wet process hydrolysis-resistant resin intermediate.
[0063] Then, the polyurethane wet process hydrolysis resistant resin is prepared, and the preparation steps are as follows:
[0064] (a) adding PE-1 accounting for 91% of the total amount of polyether polyol PE-1 having a polytetrahydrofuran structure, polyether polyol PE-3 having a mixed structure of polypropylene oxide and ethylene oxide, the remaining ethylene glycol, the remaining hindered phenol antioxidant ROX-23TP, concentrated phosphoric acid, and DMF accounting for 64% of the total amount of DMF into a reaction kettle, heating to 40° C., maintaining a constant temperature, and stirring for 30 minutes;
[0065] (b) adding 80% of the total amount of MDI to the mixture after treatment in step (a), maintaining stirring at 70° C. for 2 hours;
[0066] (c) adding 7.8% of the total amount of MDI to the mixture after treatment in step (b) to carry out reaction, keeping the R value at 1, maintaining the temperature at 70° C., adding the remaining 22% of DMF until the viscosity of the reaction solution is 24 Pas / 25 degrees, and the solid content of the reaction solution is 32%, and then adding methanol capping agent, stirring for 30 minutes and cooling to 60° C.;
[0067] (d) adding benzoic acid stabilizer, polyurethane wet process hydrolysis resistant intermediate, and polyether polyol XP-600 water-assistant detergent to the mixture after treatment in step (c), stirring for 1.5 hours to obtain polyurethane wet process hydrolysis resistant resin. In the polyurethane wet process hydrolysis resistant resin, the mass of the added polyurethane wet process hydrolysis resistant intermediate accounts for 15% of the total mass of the obtained polyurethane wet process hydrolysis resistant resin.
[0068] Example 2
[0069] A polyurethane wet-process hydrolysis-resistant resin for soft high-peelable sheepskin-like leather, the preparation raw materials of which include the following components:
[0070] PE-1: 92g, PE-2: 9g, PE-3: 103g, PE-4: 5g, hindered phenol antioxidant ROX-13TP: 0.2g, concentrated phosphoric acid: 0.002g, ethylene glycol: 10g, DMF: 613g, MDI: 58g, methanol: 0.45g, benzoic acid: 0.45g, polysiloxane softener XP-300: 2g, polyether polyol XP-600: 13g.
[0071] The preparation method of the above-mentioned polyurethane wet process hydrolysis-resistant resin is as follows.
[0072] First, prepare a polyurethane wet process hydrolysis-resistant resin intermediate, and the preparation steps are as follows:
[0073] (1) According to the above mass, 9% of the total amount of polyether polyol PE-1 with polytetrahydrofuran structure, polyether polyol (PE-2) with polypropylene oxide structure, polyester polyol (PE-4) with adipic acid-1,4-butanediol system, 20% of the total amount of ethylene glycol, half of the amount of hindered phenol antioxidant ROX-23TP, concentrated phosphoric acid, and 9% of the total amount of DMF were added to the reactor, the temperature was raised to 40° C., the temperature was maintained constant, and the reaction was stirred for 30 minutes;
[0074] (2) adding 12% of MDI to the mixture after treatment in step (1), and maintaining the mixture at a constant temperature of 70° C. with stirring for 2 hours;
[0075] (3) adding 0.2% of MDI to the mixture after treatment in step (2) to carry out reaction, keeping the R value at 1, maintaining 70° C., adding 5% of DMF to the total amount of DMF until the viscosity of the reaction liquid is 12 Pas / 25 degrees, and the solid content of the reaction liquid is 32%, and then adding methanol capping agent, stirring for 30 minutes and cooling to 60° C.;
[0076] (4) Add benzoic acid stabilizer and polysiloxane softener XP-300 water-aid detergent to the mixture after treatment in step (3), and stir for 1.5 hours to obtain a polyurethane wet process hydrolysis-resistant resin intermediate.
[0077] Then, the polyurethane wet process hydrolysis resistant resin is prepared, and the preparation steps are as follows:
[0078] (a) adding 91% of the total amount of polyether polyol PE-1 having a polytetrahydrofuran structure, polyether polyol PE-3 having a mixed structure of polypropylene oxide and ethylene oxide, the remaining ethylene glycol, the remaining hindered phenol antioxidant ROX-23TP, concentrated phosphoric acid, and DMF accounting for 64% of the total amount of DMF into a reaction kettle, heating to 40° C., maintaining a constant temperature, and stirring for 30 minutes;
[0079] (b) adding 80% of the total amount of MDI to the mixture after treatment in step (a), maintaining stirring at 70° C. for 2 hours;
[0080] (c) adding 7.8% of the total amount of MDI to the mixture after treatment in step (b) to carry out reaction, keeping the R value at 1, maintaining the temperature at 70° C., adding the remaining 22% of DMF until the viscosity of the reaction solution is 24 Pas / 25 degrees, and the solid content of the reaction solution is 32%, and then adding methanol capping agent, stirring for 30 minutes and cooling to 60° C.;
[0081] (d) adding benzoic acid stabilizer, polyurethane wet process hydrolysis resistant intermediate, and polyether polyol XP-600 water-assistant detergent to the mixture after treatment in step (c), stirring for 1.5 hours to obtain polyurethane wet process hydrolysis resistant resin. In the polyurethane wet process hydrolysis resistant resin, the mass of the added polyurethane wet process hydrolysis resistant intermediate accounts for 15% of the total mass of the obtained polyurethane wet process hydrolysis resistant resin.
[0082] Example 3
[0083] A polyurethane wet-process hydrolysis-resistant resin for soft high-peelable sheepskin-like leather, the preparation raw materials of which include the following components:
[0084] PE-1: 102g, PE-2: 19g, PE-3: 83g, PE-4: 5g, hindered phenol antioxidant ROX-13TP: 0.2g, concentrated phosphoric acid: 0.002g, ethylene glycol: 10g, DMF: 613g, MDI: 58g, methanol: 0.45g, benzoic acid: 0.45g, polysiloxane softener XP-300: 2g, polyether polyol XP-600: 13g.
[0085] The preparation method of the above-mentioned polyurethane wet process hydrolysis-resistant resin is as follows.
[0086] First, prepare a polyurethane wet process hydrolysis-resistant resin intermediate, and the preparation steps are as follows:
[0087] (1) According to the above mass, 9% of the total amount of polyether polyol PE-1 with polytetrahydrofuran structure, polyether polyol (PE-2) with polypropylene oxide structure, polyester polyol (PE-4) with adipic acid-1,4-butanediol system, 20% of the total amount of ethylene glycol, half of the amount of hindered phenol antioxidant ROX-23TP, concentrated phosphoric acid, and 9% of the total amount of DMF were added to the reactor, the temperature was raised to 40° C., the temperature was maintained constant, and the reaction was stirred for 30 minutes;
[0088] (2) adding 12% of MDI to the mixture after treatment in step (1), and stirring at 70° C. for 2 hours;
[0089] (3) adding 0.2% of MDI to the mixture after treatment in step (2) to carry out reaction, keeping the R value at 1, maintaining 70° C., adding 5% of DMF to the total amount of DMF until the viscosity of the reaction liquid is 12 Pas / 25 degrees, and the solid content of the reaction liquid is 32%, and then adding methanol capping agent, stirring for 30 minutes and cooling to 60° C.;
[0090] (4) Add benzoic acid stabilizer and polysiloxane softener XP-300 water-aid detergent to the mixture after treatment in step (3), and stir for 1.5 hours to obtain a polyurethane wet process hydrolysis-resistant resin intermediate.
[0091] Then, the polyurethane wet process hydrolysis resistant resin is prepared, and the preparation steps are as follows:
[0092] (a) adding 91% of the total amount of polyether polyol PE-1 having a polytetrahydrofuran structure, polyether polyol PE-3 having a mixed structure of polypropylene oxide and ethylene oxide, the remaining ethylene glycol, the remaining hindered phenol antioxidant ROX-23TP, concentrated phosphoric acid, and DMF accounting for 64% of the total amount of DMF into a reaction kettle, heating to 40° C., maintaining a constant temperature, and stirring for 30 minutes;
[0093] (b) adding 80% of the total amount of MDI to the mixture after treatment in step (a), maintaining stirring at 70° C. for 2 hours;
[0094] (c) adding 7.8% of the total amount of MDI to the mixture after treatment in step (b) to carry out reaction, keeping the R value at 1, maintaining the temperature at 70° C., adding the remaining 22% of DMF until the viscosity of the reaction solution is 24 Pas / 25 degrees, and the solid content of the reaction solution is 32%, and then adding methanol capping agent, stirring for 30 minutes and cooling to 60° C.;
[0095] (d) adding benzoic acid stabilizer, polyurethane wet process hydrolysis resistant intermediate, and polyether polyol XP-600 water-assistant detergent to the mixture after treatment in step (c), stirring for 1.5 hours to obtain polyurethane wet process hydrolysis resistant resin. In the polyurethane wet process hydrolysis resistant resin, the mass of the added polyurethane wet process hydrolysis resistant intermediate accounts for 15% of the total mass of the obtained polyurethane wet process hydrolysis resistant resin.
[0096] Comparative Example 1
[0097] The preparation process is basically the same as that of Example 1, except that 14.5 g of 1,4-butanediol (BDO) is used as the chain extender instead of 10 g of ethylene glycol.
[0098] Comparative Example 2
[0099] The preparation process is basically the same as that in Example 1, except that 14.5 g of 2-methyl-1,3-propanediol (MPO) is used as the chain extender instead of 10 g of ethylene glycol.
[0100] Comparative Example 3
[0101] The preparation process is basically the same as that of Example 1, except that a polyester polyol (PE-5) of adipic acid-1,4-butanediol-ethylene glycol system is used instead of a polyester polyol (PE-4) of adipic acid-1,4-butanediol system.
[0102] Comparative Example 4
[0103] The preparation process is basically the same as that of Example 1, except that a polyether polyol with a molecular weight of 1000 (denoted as PE-17) is used in the polyether polyol with a polytetrahydrofuran structure instead of a polyether polyol with a molecular weight of 2000 (PE-1).
[0104] The raw materials and contents of the polyurethane wet-process hydrolysis-resistant resins of Examples 1-3 and Comparative Examples 1-4 are shown in Table 1, unit: g.
[0105] Table 1
[0106]
[0107]
[0108] The polyurethane wet process hydrolysis-resistant resins of the above-mentioned examples 1-3 and comparative examples 1-4 were respectively prepared into imitation sheepskin synthetic leather according to the following steps: 100 g of the above-mentioned synthesized polyurethane resin was added into a plastic bottle, 10 g of calcium carbonate, 10 g of wood powder, 1 g of oily special black pulp and 70 g of solvent DMF were added thereto, and the mixture was heated at 3000 r·min. -1The mixture is dispersed evenly at a high speed under a stirring speed of , and then allowed to stand for degassing for standby use. The leather base cloth is soaked in a 50% DMF aqueous solution to remove impurities on its surface, and then the water is pressed with a water press, and then the cloth is ironed with an iron until it is half dry, and then a 0.2mm thick feeler gauge is placed on the back of the base cloth. A small amount of the slurry to be used is poured on the front of the mirror high F cloth and scraped, and then placed in water for sufficient solidification, and then washed and dried to make a wet-method bass, and then a 15-thread-thick dry-method protein-like skin-feel fabric is attached to obtain the imitation sheepskin synthetic leather of Examples 1-3 and the imitation sheepskin synthetic leather of Comparative Examples 1-4.
[0109] The following performance tests were performed on the imitation sheepskin synthetic leathers of Examples 1-3 and Comparative Examples 1-4, respectively, and the test evaluation standards are as follows:
[0110] Thickness: After the resin coating is spread according to the fixed caliper 100 wires, the thickness of 0.3mm or more is excellent, and less than 0.1mm is poor.
[0111] Peel strength: After drying at 110°C, the peel strength reaches 5KG, which is excellent; if it does not reach 5KG, it is poor.
[0112] Feel: If the flesh feels thick and rebounds well after high-temperature drying at 110℃, it is excellent; if the flesh feels thick and rebounds poorly, it is poor.
[0113] 5-year hydrolysis resistance: After soaking in 10% NaOH aqueous solution for 24 hours, wash off the NaOH and dry, the peel strength before and after soaking remains unchanged, which is excellent; if the peel strength before and after soaking decreases significantly, it is poor.
[0114] Water washing: After 15 times of squeezing with a water washing roller, the surface is flat, which is good; if the surface is uneven, it is poor. The results are shown in Table 2.
[0115] Table 2
[0116]
[0117]
[0118] As can be seen from Table 2, Example 1 has 5-year hydrolysis resistance, moderate thickness, high peel strength, thick feel, good elasticity, outstanding water washing performance, and excellent comprehensive performance.
[0119] By comparing Example 1 and Comparative Example 3, it can be seen that the combination of two polyurethane resins with different properties produced by the same process can improve the thickness retention rate and thickness feeling of the product, especially the water washing performance, compared with the production of polyurethane resin by only a single process.
[0120] By comparing Example 1 with Example 3, it can be seen that by selecting a polyether polyol with a specific molecular weight of 4000 of a mixed structure of polypropylene oxide and ethylene oxide, the synthetic leather product can obtain better resilience and significantly improve peel strength, and it also helps with water washing. By comparing Example 1 with Comparative Example 4, it can be seen that by selecting a polyether polyol with a specific molecular weight of 2000, the film-forming property and water washability of the synthetic leather base surface can be improved.
[0121] The above-mentioned technologies not specifically mentioned are all referred to the prior art.
[0122] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.
Claims
1. A polyurethane wet process hydrolysis resistant resin for soft high peeling imitation sheepskin leather, It is characterized in that The raw materials for preparation include the following components in parts by weight: 0.001-0.003 parts of inorganic acid; Polyol 205-274 parts; Isocyanate 57-77 parts; 9-13 parts of small molecule alcohol; 14-20 parts of additives; Solvent 612-816 parts.
2. The polyurethane wet-process hydrolysis-resistant resin for soft high-peelable imitation sheepskin leather according to claim 1, It is characterized in that The inorganic acid is concentrated phosphoric acid.
3. The polyurethane wet-process hydrolysis-resistant resin for soft high-peelable imitation sheepskin leather according to claim 1, It is characterized in that The polyols include polyether polyols and polyester polyols. The polyether polyols are: polyether polyols with a polytetrahydrofuran structure, polyether polyols with a mixed structure of polypropylene oxide and ethylene oxide, and polyether polyols with a polypropylene oxide structure; wherein the molar ratio of propylene oxide units to ethylene oxide units in the polyether polyols with a mixed structure of polypropylene oxide and ethylene oxide is 2.8-3:1.8-2; and the polyester polyols are: polyester polyols of adipic acid-1,4-butanediol system.
4. The polyurethane wet-process hydrolysis-resistant resin for soft high-peelable imitation sheepskin leather according to claim 3, It is characterized in that The molecular weights of the polyether polyol with polytetrahydrofuran structure and the polyester polyol with adipic acid-1,4-butanediol system are both 1800-2200, and the molecular weights of the polyether polyol with a mixed structure of polypropylene oxide and ethylene oxide and the polyether polyol with polypropylene oxide structure are 3800-4200.
5. The polyurethane wet-process hydrolysis-resistant resin for soft high-peelable imitation sheepskin leather according to claim 1, It is characterized in that The isocyanate is one or more of diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate and toluene diisocyanate.
6. The polyurethane wet-process hydrolysis-resistant resin for soft high-peelable imitation sheepskin leather according to claim 1, It is characterized in that The small molecule alcohol is one or more of ethylene glycol, diethylene glycol, and monoethanolamine.
7. The polyurethane wet-process hydrolysis-resistant resin for soft high-peelable imitation sheepskin leather according to claim 1, It is characterized in that The solvent is N,N-dimethylformamide, and the auxiliary agent is one or more of a water-assisting agent, a stabilizer, a capping agent, and a hindered phenol antioxidant.
8. The polyurethane wet-process hydrolysis-resistant resin for soft high-peelable imitation sheepskin leather according to claim 7, It is characterized in that The water-assisting detergent is a polyether polyol and a polysiloxane system softener, the stabilizer is benzoic acid, and the end-capping agent is methanol.
9. The method for preparing the polyurethane wet-process hydrolysis-resistant resin for soft high-peelable imitation sheepskin leather according to any one of claims 1 to 8, It is characterized in that The steps include: First, a polyurethane wet process hydrolysis-resistant resin intermediate is prepared, and the preparation steps are as follows: (1) mixing part of the polyether polyol with a polytetrahydrofuran structure, the polyether polyol with a polypropylene oxide structure, the polyester polyol of adipic acid-1,4-butanediol system, part of the small molecule alcohol, part of the hindered phenol antioxidant, the inorganic acid, and part of the solvent, and heating the mixture; (2) adding a portion of isocyanate to the mixture after treatment in step (1) and treating at a constant temperature; (3) adding part of the isocyanate to the mixture treated in step (2) to react, and maintaining the R value at 0.9-1.1, adding part of the solvent until the viscosity of the reaction liquid is 10-14 Pas / 25 degrees, and the solid content of the reaction liquid is 31%-33%, and then adding the blocking agent, stirring, and cooling; (4) adding a stabilizer, a polysiloxane system softener and a water-assistant to the mixture after treatment in step (3) and stirring to obtain the polyurethane wet process hydrolysis-resistant resin intermediate; Then, the polyurethane wet process hydrolysis-resistant resin is prepared, and the preparation steps are as follows: (a) mixing the remaining polytetrahydrofuran structure polyether polyol, the polyether polyol of a mixed structure of polypropylene oxide and ethylene oxide, the remaining small molecule alcohol, the remaining hindered phenol antioxidant, the inorganic acid, and part of the solvent in the polyether polyol, and heating the mixture; (b) adding a portion of isocyanate to the mixture after treatment in step (a), and treating at a constant temperature; (c) adding the remaining isocyanate to the mixture after treatment in step (b) to react, and maintaining the R value at 0.9-1.1, adding the remaining solvent until the viscosity of the reaction solution is 20-26pas / 25 degrees, and the solid content of the reaction solution is 31%-33%, and then adding the blocking agent, stirring, and cooling; (d) adding a stabilizer, a portion of the polyurethane wet process hydrolysis resistant intermediate, and a polyether polyol water-assistant to the mixture after treatment in step (c), and stirring to obtain the polyurethane wet process hydrolysis resistant resin.
10. A synthetic leather, It is characterized in that It is prepared using the soft high-peelable sheepskin-like leather polyurethane wet process hydrolysis-resistant resin described in any one of claims 1-8, or is prepared using the resin prepared by the preparation method of the soft high-peelable sheepskin-like leather polyurethane wet process hydrolysis-resistant resin described in claim 9.