High-thermal-conductivity, high-insulation and high-Tg bio-based epoxy composite material as well as preparation method and application thereof

By reacting epoxy vanillin dimer with epoxy vegetable oil, etc., combined with modified thermally conductive particle fillers and a curing agent containing rigid groups, bio-based epoxy with high thermal conductivity, high insulation and high glass transition temperature were prepared by using epoxy vanillin dimer with epoxy vegetable oil, combined with modified thermally conductive particle fillers and a curing agent containing rigid groups. Composite materials solve the problems of insufficient performance of existing bio-based epoxy resins and the health hazards of bisphenol A epoxy resins, and realize the development of high-performance bio-based epoxy composite materials.

CN118955869AActive Publication Date: 2024-11-15AKM ELECTRONICS INDAL PANYU
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411177473.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-15
Estimated Expiration
2044-08-26

AI Technical Summary

Technical Problem

The existing bio-based epoxy resins have shortcomings in terms of industrial chain integrity and price advantages, and bisphenol A type epoxy resins are harmful to human health and lack high-performance and multifunctional alternative materials.

Method used

Using epoxy vanillin dimer and epoxy vegetable oil, combined with modified thermally conductive particle filler and rigid group-containing curing agent to prepare bio-based epoxy composites with high thermal conductivity, high insulation and high glass transition temperature Materials, avoiding the harm of bisphenol A type epoxy resin.

Benefits of technology

It realizes the high performance characteristics of bio-based epoxy composite materials, has excellent thermal conductivity, insulation and mechanical properties, and is suitable for the field of thermal interface materials, especially in the application of third-generation semiconductor high-power inverters.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_3
    Figure SMS_3
  • Figure FDA0005011108380000011
    Figure FDA0005011108380000011
Patent Text Reader

Abstract

The invention relates to a high-thermal-conductivity, high-insulation and high-Tg bio-based epoxy composite material as well as a preparation method and application thereof. The bio-based epoxy composite material comprises the following raw material components: an epoxy vanillin dimer, epoxy vegetable oil, a curing agent, a modified heat-conducting particle filler and a diluent, and the bio-based epoxy vanillin dimer is adopted to replace bisphenol A epoxy resin, so that the raw materials are wide in source, green and environment-friendly; the rigid epoxy vanillin dimer is matched with the flexible epoxy vegetable oil, and the modified heat-conducting particle filler and the like are further combined, so that the prepared bio-based composite material has high glass-transition temperature and excellent heat-conducting and insulating properties, and has wide application prospects in the field of thermal interface materials; the method is particularly applied to a third-generation semiconductor high-power inverter.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of bio-based composite materials, and specifically relates to a high thermal conductivity, high insulation and high Tg bio-based epoxy composite material and a preparation method and application thereof. Background Art

[0002] Epoxy resins are widely used in various industries due to their excellent mechanical strength, chemical resistance and dimensional stability. Among them, bisphenol A epoxy resins prepared by bisphenol A and epichlorohydrin glycidylation occupy the vast majority of the market share, and E44 and E51 are representative bisphenol A resins. However, the non-renewable raw materials and the harmfulness of bisphenol A structure to human health have forced people to seek epoxy resins from bio-based sources.

[0003] Bio-based epoxy resins synthesized from vegetable oils, starch, cellulose and their derivatives have been widely studied in recent years and have made some progress. However, from the perspective of industrial chain integrity and product application, bio-based epoxy resins currently do not have price advantages. It is of practical significance to develop high-value multifunctional and high-performance bio-based epoxy composite materials. For example, Chinese patent document CN116444462A discloses a bio-based epoxy resin monomer of isovanillin, and the resulting bio-based epoxy resin polymer material has a lower curing process temperature and good heat resistance (initial decomposition temperature ~300.8°C). Summary of the invention

[0004] In view of the above-mentioned deficiencies and problems in the prior art, the present invention is directed to a bio-based epoxy composite material with high thermal conductivity, high insulation and high Tg, and a preparation method and application thereof.

[0005] The first object of the present invention is to provide a bio-based epoxy composite material with high thermal conductivity, high insulation and high Tg, which is mainly composed of the following raw materials: epoxy vanillin dimer, epoxy vegetable oil, curing agent, modified thermal conductive particle filler and diluent, wherein the curing agent is a curing agent containing a rigid group, and the structural formula of the epoxy vanillin dimer is

[0006]

[0007] The scheme of the present invention utilizes epoxy vanillin dimer and epoxy vegetable oil which are similar in structure to bisphenol A epoxy resin to prepare bio-based epoxy composite material, thus avoiding the harm of bisphenol A epoxy resin and promoting the development of bio-based epoxy resin.

[0008] The epoxy vanillin dimer in the scheme of the present invention is obtained by using vanillin as a raw material, and then further glycidylating the dimer after obtaining the dimer through coupling reaction. Specifically, vanillin, ferrous sulfate, and sodium persulfate are used as raw materials, and a coupling reaction is performed at 80° C. to prepare the dimer; then the dimer is mixed with epichlorohydrin and TBAB (tetrabutylammonium bromide) at 80° C. for polymerization reaction, and then a sodium hydroxide aqueous solution and TBAB are added at room temperature for ring-closing reaction to obtain the epoxy vanillin dimer. In a specific embodiment, 6 g of vanillin (39.5 mmol), 0.2 g of FeSO4·7H2O (0.72 mmol) and 5 g of Na2S2O8 (21.0 mmol, 0.53 equiv) were mixed in 400 mL of water, stirred at 80° C. for 30 min, the precipitate was collected after filtration, washed three times with 80° C. hot water and dried to obtain vanillin dimer; then 4 g of vanillin dimer (13.2 mmol), 24.5 g of epichlorohydrin (0.265 mol) and 0.4 g of TBAB (tetrabutylammonium bromide, 1.2 mmol) were stirred at 80° C. for 2 h, then an aqueous sodium hydroxide solution (5 M, 10.6 mL) and 0.4 g of TBAB (1.2 mmol) were added to the reaction solution at room temperature and the reaction was continued for 1 h to close the ring, and finally the solvent was removed by freeze drying, and the epoxy vanillin dimer was obtained by washing with deionized water for several times and drying.

[0009] In some embodiments, the raw material components of the epoxy bio-based composite material include 30-50 parts of epoxy vanillin dimer, 0-20 parts of epoxy vegetable oil, 5-30 parts of curing agent, 10-80 parts of modified thermally conductive particle filler and 10-30 parts of diluent in parts by weight; preferably, it includes 40-50 parts of epoxy vanillin dimer, 10-20 parts of epoxy vegetable oil, 5-30 parts of curing agent, 10-50 parts of modified thermally conductive particle filler and 10-30 parts of diluent.

[0010] In some embodiments, the epoxidized vegetable oil is at least one or more of epoxidized soybean oil, epoxidized castor oil, epoxidized tung oil, epoxidized linseed oil and epoxidized palm oil.

[0011] In some embodiments, the curing agent is at least one or more of a phenolic epoxy resin curing agent, anhydride curing agent, polyamine curing agent, and polyamide curing agent containing a rigid group, such as a phenolic epoxy resin curing agent; anhydride curing agent, polyamine curing agent, or polyamide curing agent containing a rigid aliphatic ring or benzene ring structure.

[0012] In some embodiments, the diluent is at least one or more of acetone, butanone, toluene, dichloromethane, N,N-dimethylformamide and N,N-dimethylacetamide.

[0013] In some embodiments, the modified thermally conductive particle filler in the solution of the present invention is a thermally conductive particle filler modified by a silane coupling agent. Specifically, the thermally conductive particles are added to a silane coupling agent solution for hydrolysis modification, and then washed and dried.

[0014] In some embodiments, the silane coupling agent is at least one or more of KH-550, KH-560 and KH-580.

[0015] In some embodiments, the thermally conductive particles are at least one or more of boron nitride, aluminum nitride, aluminum oxide, silicon carbide, or artificial diamond.

[0016] Another object of the present invention is to provide a method for preparing the above-mentioned high thermal conductivity, high insulation and high Tg bio-based epoxy composite material, which, in some embodiments, comprises the following steps:

[0017] (1) weighing epoxy vanillin dimer, epoxy vegetable oil, curing agent, modified thermal conductive particle filler and diluent; stirring and mixing evenly and degassing to obtain a bio-based epoxy resin solution;

[0018] (2) The bio-based epoxy resin solution is poured into a mold and pre-cured at 50-90°C for 0.5-2h to volatilize the diluent, and then cured at 120-160°C for 12-36h to obtain a bio-based epoxy composite material. Specifically, it can be adjusted according to the type and amount of the diluent, such as pre-curing at 50°C, 60°C, 70°C, 80°C, or 90°C for 0.5h, 1h, 1.5h, 2h, etc.; and then cured at 120°C, 130°C, 140°C, 150°C, or 160°C for 12h, 18h, 24h, 30h, 36h, etc.

[0019] Another object of the present invention is to provide application of the above-mentioned high thermal conductivity, high insulation and high Tg bio-based epoxy composite material in the field of thermal interface materials.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] The present invention uses bio-based epoxy vanillin dimer to replace bisphenol A epoxy resin, and the raw materials are widely available, green and environmentally friendly, and in line with the concept of sustainable development. Rigid epoxy vanillin dimer is matched with flexible epoxy vegetable oil, and further combined with modified thermal conductive particle filler, etc., to prepare a bio-based composite material with high glass transition temperature, excellent thermal conductivity and insulation properties, and has broad application prospects in the field of thermal interface materials, especially in the application of third-generation semiconductor high-power inverters. DETAILED DESCRIPTION

[0022] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to relevant embodiments. Preferred embodiments of the present invention are given in the embodiments. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.

[0023] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0024] The reagents used in the following examples, unless otherwise specified, can be obtained from commercial channels; the methods used in the following examples, unless otherwise specified, can be achieved by conventional methods.

[0025] The structural formula of the epoxy vanillin dimer used in the following examples and comparative examples is as follows:

[0026] It is made from vanillin as raw material, and the dimer is obtained through coupling reaction and then further glycidylated.

[0027] Specifically, 6 g of vanillin (39.5 mmol), 0.2 g of FeSO4·7H2O (0.72 mmol) and 5 g of Na2S2O8 (21.0 mmol, 0.53 equiv) were mixed in 400 mL of water, stirred at 80 °C for 30 min, the precipitate was collected after filtration, washed three times with 80 °C hot water and dried to obtain vanillin dimer;

[0028] Then 4 g of vanillin dimer (13.2 mmol), 24.5 g of epichlorohydrin (0.265 mol) and 0.4 g of TBAB (1.2 mmol) were stirred at 80 ° C for 2 h, and then sodium hydroxide aqueous solution (5 M, 10.6 mL) and 0.4 g of TBAB (1.2 mmol) were added to the reaction solution at room temperature and the reaction was continued for 1 h to close the ring. Finally, the solvent was removed by freeze drying, and the mixture was washed with deionized water several times and then dried to obtain epoxy vanillin dimer.

[0029] Example 1

[0030] An epoxy bio-based composite material, the preparation method of which comprises the following steps:

[0031] Step 1: Take 50 parts of epoxy vanillin dimer, 10 parts of flexible epoxy castor oil, 30 parts of phenolic modified amine curing agent, 50 parts of KH-560 modified boron nitride filler and 20 parts of acetone according to weight parts, stir and mix them evenly with a stirrer and degas, to obtain a bio-based epoxy resin solution;

[0032] Step 2: Pour the above bio-based epoxy resin solution into a mold and pre-cure it at 50° C. for 1 h to volatilize the diluent, and then cure it at 120° C. for 24 h to obtain a bio-based epoxy composite material.

[0033] Example 2

[0034] An epoxy bio-based composite material, the preparation method of which comprises the following steps:

[0035] Step 1: Take 50 parts of rigid epoxy vanillin dimer, 10 parts of flexible epoxy castor oil, 30 parts of phenolic modified amine curing agent, 50 parts of KH-560 modified aluminum nitride filler and 20 parts of acetone according to weight parts, stir and mix them evenly with a stirrer and degas, to obtain a bio-based epoxy resin solution;

[0036] Step 2: Pour the above bio-based epoxy resin solution into a mold and pre-cure it at 50° C. for 1 h to volatilize the diluent, and then cure it at 120° C. for 24 h to obtain a bio-based epoxy composite material.

[0037] Example 3

[0038] An epoxy bio-based composite material, the preparation method of which comprises the following steps:

[0039] Step 1: Take 50 parts of rigid epoxy vanillin dimer, 10 parts of flexible epoxy castor oil, 30 parts of phenolic modified amine curing agent, 50 parts of KH-560 modified alumina filler and 20 parts of acetone according to weight parts, stir and mix them evenly with a stirrer and degas, to obtain a bio-based epoxy resin solution;

[0040] Step 2: Pour the above bio-based epoxy resin solution into a mold and pre-cure it at 50° C. for 1 h to volatilize the diluent, and then cure it at 120° C. for 24 h to obtain a bio-based epoxy composite material.

[0041] Example 4

[0042] An epoxy bio-based composite material, the preparation method of which comprises the following steps:

[0043] Step 1: Take 50 parts of rigid epoxy vanillin dimer, 10 parts of flexible epoxy castor oil, 30 parts of phenolic modified amine curing agent, 50 parts of KH-560 modified artificial diamond filler and 20 parts of acetone according to weight parts, stir and mix them evenly with a stirrer and degas to obtain a bio-based epoxy resin solution;

[0044] Step 2: Pour the above bio-based epoxy resin solution into a mold and pre-cure it at 50° C. for 1 h to volatilize the diluent, and then cure it at 120° C. for 24 h to obtain a bio-based epoxy composite material.

[0045] Example 5

[0046] An epoxy bio-based composite material, the preparation method of which comprises the following steps:

[0047] Step 1: Take 50 parts of rigid epoxy vanillin dimer, 10 parts of flexible epoxy castor oil, 30 parts of phenolic modified amine curing agent, 50 parts of KH-560 modified silicon carbide filler and 20 parts of acetone according to weight parts, stir and mix them evenly with a stirrer and degas, to obtain a bio-based epoxy resin solution;

[0048] Step 2: Pour the above bio-based epoxy resin solution into a mold and pre-cure it at 50° C. for 1 h to volatilize the diluent, and then cure it at 120° C. for 24 h to obtain a bio-based epoxy composite material.

[0049] Comparative Example 1

[0050] An epoxy composite material, the preparation method of which comprises the following steps:

[0051] Step 1: Take 50 parts of epoxy E44 resin, 10 parts of flexible epoxy castor oil, 30 parts of phenolic modified amine curing agent, 50 parts of KH-560 modified boron nitride filler and 20 parts of acetone according to weight parts, stir and mix them evenly with a stirrer and degas to obtain an epoxy resin solution;

[0052] Step 2: Pour the above epoxy resin solution into a mold and pre-cure it at 50°C for 1 hour to volatilize the diluent, and then cure it at 120°C for 24 hours to obtain a bio-based epoxy composite material.

[0053] Comparative Example 2

[0054] An epoxy bio-based composite material, the preparation method of which comprises the following steps:

[0055] Step 1: Take 50 parts of rigid epoxy vanillin dimer, 10 parts of flexible epoxy castor oil, 30 parts of phenolic modified amine curing agent, 50 parts of unmodified boron nitride filler and 20 parts of acetone according to weight parts, stir and mix them evenly with a stirrer and degas, to obtain a bio-based epoxy resin solution;

[0056] Step 2: Pour the above bio-based epoxy resin solution into a mold and pre-cure it at 50° C. for 1 h to volatilize the diluent, and then cure it at 120° C. for 24 h to obtain a bio-based epoxy composite material.

[0057] Performance Test:

[0058] Thermal conductivity: The thermal diffusion coefficient α, m of the implementation case and the comparison case was tested using the LFA467 laser scattering thermal conductivity instrument from NETZSCH, Germany. 2 / s, using the drainage method, using an electronic balance to test the bulk density of the material, ρ, g / cm 3 According to the formula

[0059] λ=α×ρ×Cp

[0060] Calculate the thermal conductivity λ of the composite material, W / (m·K).

[0061] Dielectric strength: The insulation strength of the implementation case and the comparison case was tested using Taiwan Chroma 19073.

[0062] Glass transition temperature: A TA-Q200 differential scanning calorimeter produced by TA Instruments, Inc., USA, was used to study and analyze different samples.

[0063] Mechanical properties: The samples were tested using the UTM 5000 universal testing machine from Shenzhen Sansi Company. Based on ASTM D638-03, each sample was tested five times.

[0064] The test results are shown in Table 1.

[0065] Table 1 Performance comparison of embodiments and comparative examples

[0066]

[0067] As shown in the test results of Table 1, bio-based rigid epoxy vanillin dimer has better mechanical properties, glass transition temperature, thermal conductivity and insulation properties than traditional petroleum-based bisphenol A epoxy resin. Epoxy vanillin dimer is a biphenyl structure, and the hydroxyl groups on the benzene ring are more likely to form intermolecular hydrogen bonds. During the curing process, the hard segments of the polymer network are aggregated, and it is easier to form regular molecular segments, so the mechanical properties are excellent. The difference in thermal conductivity is determined by the performance of the thermally conductive particles themselves. Comparative Example 1 and Comparative Example 2 can be seen that the particles modified by the silane coupling agent KH-560 are more evenly dispersed in the resin, and a continuous thermal conductive network is formed after curing, so the thermally conductive particles after filling and modification are more excellent than the unmodified particles. At the same time, the more regular molecular segments will reduce the scattering of phonons, so after comparing Example 1 and Comparative Example 1, it is found that the thermal conductivity of the bio-based epoxy composite material is more excellent, with significant improvement, and other properties are also improved.

[0068] In summary, the bio-based epoxy composite material with high thermal conductivity, high insulation and high Tg of the present invention has broad application prospects in thermal interface materials, especially in the field of semiconductor packaging.

[0069] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0070] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A high thermal conductivity, high insulation and high Tg bio-based epoxy composite material, characterized in that: The raw material components of the bio-based epoxy composite material include epoxy vanillin dimer, epoxy vegetable oil, a curing agent, a modified thermal conductive particle filler and a diluent. The curing agent is a curing agent containing a rigid group. The structural formula of the epoxy vanillin dimer is 2. The bio-based epoxy composite material according to claim 1, characterized in that: In terms of weight, the raw material components include 30-50 parts of epoxy vanillin dimer, 0-20 parts of epoxy vegetable oil, 5-30 parts of curing agent, 10-80 parts of modified thermal conductive particle filler and 10-30 parts of diluent.

3. The bio-based epoxy composite material according to claim 1, characterized in that: The epoxidized vegetable oil is at least one or more of epoxidized soybean oil, epoxidized castor oil, epoxidized tung oil, epoxidized linseed oil and epoxidized palm oil.

4. The bio-based epoxy composite material according to claim 1, characterized in that: The curing agent is at least one or more of a phenolic epoxy resin curing agent, an acid anhydride curing agent, a polyamine curing agent and a polyamide curing agent containing a rigid group.

5. The bio-based epoxy composite material according to claim 1, characterized in that: The diluent is at least one or more of acetone, butanone, toluene, dichloromethane, N,N-dimethylformamide and N,N-dimethylacetamide.

6. The bio-based epoxy composite material according to any one of claims 1 to 5, characterized in that: The modified thermally conductive particle filler is a thermally conductive particle filler modified by a silane coupling agent.

7. The bio-based epoxy composite material according to claim 6, characterized in that: The silane coupling agent is at least one or more of KH-550, KH-560 and KH-580.

8. The bio-based epoxy composite material according to claim 6, characterized in that: The thermally conductive particles are at least one or more of boron nitride, aluminum nitride, aluminum oxide, silicon carbide or artificial diamond.

9. A method for preparing a bio-based epoxy composite material with high thermal conductivity, high insulation and high Tg as claimed in any one of claims 1 to 8, characterized in that: The following steps are involved: (1) weighing epoxy vanillin dimer, epoxy vegetable oil, curing agent, modified thermal conductive particle filler and diluent; stirring and mixing evenly and degassing to obtain a bio-based epoxy resin solution; (2) The bio-based epoxy resin solution is poured into a mold and pre-cured at 50-90° C. for 0.5-2 h to volatilize the diluent, and then cured at 120-160° C. for 12-36 h to obtain the bio-based epoxy composite material.

10. Application of the high thermal conductivity, high insulation and high Tg bio-based epoxy composite material according to any one of claims 1 to 9 in the field of thermal interface materials.

Citation Information

Patent Citations

  • Halogen-free flame-retardant epoxy resin precursor, halogen-free flame-retardant epoxy resin composition, molding compound product, preparation method and application

    CN111793091A

  • Bio-based resin matrix material, carbon fiber bio-based resin composite material and preparation method thereof

    CN113897026A

  • Modified epoxy resin and preparation method thereof

    CN115028965A

  • Difunctional biphenyl compounds, preparation, and uses

    US20200399419A1

  • Epoxy resin derived from vanillin and thermosets therefrom

    WO2016172353A1