Lanthanum-based MOF crystal material, preparation method and application method in natural gas decarburization
Through the development and application of lanthanum-based MOF crystal materials, the high energy consumption and high cost problems in natural gas decarbonization technology were solved, low energy consumption and low cost CO2 removal and conversion were achieved, and excellent catalytic performance and reaction conditions were demonstrated. Gentleness.
Patent Information
- Application Number
- CN202411007205.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-25
AI Technical Summary
The existing natural gas decarbon dioxide technology has problems of high energy consumption and solvent waste, and the existing catalyst conversion of CO2 into high-value chemical products is high, and the reaction conditions require high pressure and high temperature.
A lanthanum-based MOF crystal material has a three-dimensional porous structure with regular unidirectional hexagonal honeycomb channels and a coordination geometry of La3+ ions. This material is prepared by hydrothermal synthesis method and applied to CO2 and epoxy. In the cycloaddition reaction of chemicals, its catalytic properties are used to achieve the removal and conversion of CO2.
It realizes low-energy consumption and low-cost CO2 removal and conversion, demonstrates excellent catalytic performance, can effectively catalyze the cycloaddition reaction between CO2 and epoxide, and can carry out continuous flow separation of CH4/CO2 under mild conditions. Convert captured CO2 into valuable products.
Smart Images

Figure CN118955923A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of metal organic framework materials, and specifically relates to a lanthanum-based MOF crystal material, a preparation method and an application method in natural gas decarbonization. Background Art
[0002] Natural gas is a high-quality fuel and chemical raw material. The extracted natural gas often contains excessive CO2. Excessive carbon dioxide will reduce the calorific value of natural gas and corrode pipelines and equipment. Natural gas needs to be CO2-removed before it is delivered to users. Currently commonly used removal methods include CO2 amine chemical adsorption, low-temperature distillation, and solvent extraction. These technologies have problems such as high energy consumption and solvent waste. Metal organic framework compounds MOFs have shown broad application prospects in gas storage, adsorption separation, catalysis, etc. due to their highly ordered pore structure and adjustable chemical properties, and are expected to be used in the purification of natural gas with high CO2 content. If the CO2 in the permeate gas is directly discharged, it will inevitably lead to an increase in carbon emissions.
[0003] The cycloaddition reaction of CO2 and epichlorohydrin to prepare propylene chlorocarbonate provides an opportunity to solve environmental problems and utilize resources. Currently, catalysts such as ionic liquids and certain MOF materials have been developed for this reaction. However, the existing catalysts for converting CO2 into high-value chemical products have problems of high energy consumption and solvent waste due to the high pressure and high temperature required for their reaction conditions, and are too expensive. Therefore, the development of MOF materials that combine natural gas purification and CO2 capture and utilization has become a technical problem that needs to be solved urgently. Summary of the invention
[0004] In order to solve the above problems existing in the prior art, the present invention provides a lanthanum-based MOF crystal material, a preparation method and an application method in natural gas decarbonization. The technical problem to be solved by the present invention is achieved by the following technical solutions:
[0005] The embodiment of the present invention provides a lanthanum-based MOF crystal material, the chemical formula of the lanthanum-based MOF crystal material is: (C 54 H 43 La3N3O 22 3- ) n ,1(C2H8N1 1+ ), the organic ligand is 3,3',5'-biphenyltricarboxylic acid;
[0006] The structure of the lanthanum-based MOF crystal material is a three-dimensional porous structure with regular unidirectional hexagonal honeycomb channels, and the three-dimensional porous structure has metal vacancies;
[0007] The lanthanum-based MOF crystal material contains La 3+ Ions have coordination geometry.
[0008] In one embodiment of the present invention, the crystal structure of the lanthanum-based MOF crystal material belongs to the monoclinic system, and the space group is The unit cell parameters are α=90°, β=90°, γ=120°.
[0009] In one embodiment of the present invention, there is an asymmetric unit in the three-dimensional porous structure, and the asymmetric unit consists of a La 3+ ion, an organic ligand 3,3',5'-biphenyltricarboxylic acid, a coordinated N,N-dimethylformamide molecule, and one-third μ3-OH - and one third Me2NH2 + Cation composition, the La 3+ The ions are connected to the 3,3',5'-biphenyltricarboxylic acid, the N,N-dimethylformamide molecule, the μ3-OH - Connect respectively, the Me2NH2 + The cation is attracted to the oxygen atom of the 3,3',5'-biphenyltricarboxylic acid by electrostatic forces.
[0010] In one embodiment of the present invention, the three-dimensional porous structure is formed by connecting adjacent trinuclear metal clusters [La3(COO)9(μ3-OH)] along the target direction through the organic ligand; the trinuclear metal cluster [La3(COO)9(μ3-OH)] is composed of three La 3+ The ions pass through μ3-OH - Bond formation; each La 3+ The ionic center presents a nine-coordinate geometric structure, wherein the nine coordinated geometric structures are seven carboxyl oxygen atoms from the organic ligand, one oxygen atom from the N,N-dimethylformamide molecule and one oxygen atom from μ3-OH. - 1 oxygen atom.
[0011] In one embodiment of the present invention, the carboxyl oxygen atom in the organic ligand has three coordination modes: μ3-η 1 :η 2 、μ2-η 1 :η 1 and μ1-η 1 :η 1 .
[0012] Another embodiment of the present invention provides a method for preparing a lanthanum-based MOF crystal material, which is used to prepare the lanthanum-based MOF crystal material as described in the above embodiment, comprising the steps of:
[0013] S1, dissolving 3,3',5'-biphenyltricarboxylic acid and benzoic acid in N,N-dimethylformamide to obtain a first solution, dissolving lanthanum chloride heptahydrate in water to obtain a second solution, and mixing the first solution and the second solution to obtain a mixed solution;
[0014] S2. Using a hydrothermal synthesis method, the mixed solution is subjected to a thermal reaction to obtain a lanthanum-based MOF crystal material.
[0015] In one embodiment of the present invention, the molar ratio of the 3,3',5'-biphenyltricarboxylic acid to the benzoic acid is 1:1;
[0016] The molar ratio of the 3,3',5'-biphenyltricarboxylic acid to the lanthanum chloride heptahydrate is 1:1;
[0017] The ratio of the 3,3',5'-biphenyltricarboxylic acid, the benzoic acid, and the N,N-dimethylformamide is 0.1 mmol: 0.1 mmol: 3 ml;
[0018] The ratio of the lanthanum chloride heptahydrate to the water is 0.1 mmol:2 ml.
[0019] In one embodiment of the present invention, step S2 comprises:
[0020] The mixed solution is heated to 120-180°C at a heating rate of 0.5-1.5°C / min by a hydrothermal synthesis method, and the reaction time is 48-96h at 120-180°C, and then cooled to room temperature at a rate of 0.05-0.15°C / min to obtain the lanthanum-based MOF crystalline material.
[0021] Another embodiment of the present invention provides a method for using a lanthanum-based MOF crystal material in natural gas decarbonization, comprising: placing an epoxide, a catalyst, and a co-catalyst in an environment containing carbon dioxide and heating them, so that the epoxide and the carbon dioxide undergo an addition reaction to remove the carbon dioxide;
[0022] The catalyst uses the lanthanum-based MOF crystal material as described in the above embodiment.
[0023] In one embodiment of the present invention, the epoxide includes epichlorohydrin, and the co-catalyst includes tetrabutylammonium bromide; the ratio of the epoxide, the catalyst, and the co-catalyst is: 21 mmol: 70 mg: 0.21 mmol;
[0024] The reaction temperature of the addition reaction is 50-70° C., and the reaction time is 32-60 h.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] The lanthanum-based MOF crystal material of the present invention is a three-dimensional porous structure with regular unidirectional hexagonal honeycomb channels, and the three-dimensional porous structure has metal vacancies. 3+ The ions have a coordination geometry to form La 3+ Ionic metal sites, metal vacancies, La 3+ Ionic metal sites, Me2NH2 + The combination of the lanthanum-based MOF crystal material with a three-dimensional porous structure with regular unidirectional hexagonal honeycomb channels gives it excellent adsorption capacity, and can be used as a catalyst to catalyze the cycloaddition reaction of CO2 and epoxides. It exhibits good catalytic performance for the carbon dioxide cycloaddition reaction of epoxides, and the reaction conditions are mild, with low energy consumption and low cost, thus achieving the purpose of continuous flow separation of CH4 / CO2 and converting captured CO2 into valuable final products. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 A schematic diagram of a three-dimensional porous framework of a lanthanum-based MOF crystal material mentioned in an embodiment of the present invention;
[0028] Figure 2 A schematic diagram of the structure of an organic ligand mentioned in an embodiment of the present invention;
[0029] Figure 3 A schematic diagram of an asymmetric unit of a lanthanum-based MOF crystal material provided in an embodiment of the present invention;
[0030] Figure 4 A schematic diagram of a trinuclear metal cluster [La3(COO)9(μ3-OH)] provided in an embodiment of the present invention;
[0031] Figure 5 A schematic diagram of a synthesis process of a lanthanum-based MOF crystal material provided in an embodiment of the present invention;
[0032] Figure 6 BET test curve diagram of La-MOF provided by an embodiment of the present invention;
[0033] Figure 7 A pore size distribution diagram of La-MOF provided in an embodiment of the present invention;
[0034] Figure 8 FT-IR characterization diagram of La-MOF provided in an embodiment of the present invention;
[0035] Fig. 9 The XRD diagram of La-MOF provided in the embodiment of the present invention;
[0036] Fig.10 A morphology diagram of La-MOF provided in an embodiment of the present invention;
[0037] Fig.11 A particle size distribution diagram of La-MOF provided in an embodiment of the present invention;
[0038] Fig.12 Schematic diagram of the mechanism of La-MOF catalytic conversion of CO2 provided in an embodiment of the present invention;
[0039] Fig.13 The adsorption isotherm of La-MOF provided in the embodiment of the present invention;
[0040] Fig.14 Adsorption selectivity diagram of La-MOF provided by an embodiment of the present invention;
[0041] Fig.15 This is a comparison chart of the yields of different catalytic systems provided in the embodiments of the present invention. DETAILED DESCRIPTION
[0042] The present invention is further described in detail below with reference to specific embodiments, but the embodiments of the present invention are not limited thereto.
[0043] Embodiment 1
[0044] See also Figure 1 , Figure 1 A schematic diagram of a three-dimensional porous framework of a lanthanum-based MOF crystal material mentioned in an embodiment of the present invention.
[0045] The chemical formula of the lanthanum-based MOF (La-MOF) crystal material provided in this embodiment is: 54 H 43 La3N3O 22 3- ) n ,1(C2H8N1 1+ ), the organic ligand is 3,3',5'-biphenyltricarboxylic acid, named FMU-101.
[0046] See also Figure 2 , Figure 2 This is a schematic diagram of the structure of an organic ligand mentioned in an embodiment of the present invention.
[0047] The structure of the lanthanum-based MOF crystal material is a three-dimensional porous structure with regular unidirectional hexagonal honeycomb channels, and there are metal vacancies in the three-dimensional porous structure.
[0048] Specifically, metal vacancies refer to a defect structure in a crystal, that is, one or more atoms are missing from the atomic position in the crystal, forming a vacancy or hole. In the crystal structure, metal atoms usually exist in the vacant positions of the crystal lattice, and metal vacancies are the unoccupied positions in these vacancies.
[0049] La in lanthanum-based MOF crystal materials 3+ The ions have a coordination geometry that forms metal sites.
[0050] Specifically, the metal site refers to the central atom in the coordination compound formed by the metal ion and one or more coordination groups. 3+ The ion has a coordination geometry, forming La 3+ Ionic metal sites.
[0051] Furthermore, from the perspective of framework connection construction, the crystal structure of lanthanum-based MOF crystal materials belongs to the monoclinic system, and the space group is The unit cell parameters are α=90°, β=90°, γ=120°.
[0052] See also Figure 3 , Figure 3 A schematic diagram of an asymmetric unit of a lanthanum-based MOF crystal material provided in an embodiment of the present invention.
[0053] Lanthanum-based MOF crystal material FMU-101 is a three-dimensional porous structure with regular unidirectional hexagonal honeycomb channels. There is an asymmetric unit in the three-dimensional framework of FMU-101. The asymmetric unit consists of a La 3+ ion, an organic ligand 3,3',5'-biphenyltricarboxylic acid (C 15 H 10 O6), a coordinated N,N-dimethylformamide (DMF) molecule, one-third of μ3-OH - and one third Me2NH2 + Cation composition. Among them, La 3+ The ion is connected to 3,3',5'-biphenyltricarboxylic acid, N,N-dimethylformamide molecule, μ3-OH-, Me2NH2 through oxygen atoms. + The cation is attracted to the oxygen atom of 3,3',5'-biphenyltricarboxylic acid by electrostatic forces.
[0054] In the above asymmetric unit, the dimethylamine cation (Me2NH2 + ) is composed of DMF in the solvent and free ions in the solution, and the structure of the dimethylamine cation and the negatively charged unsaturated site is attracted by electrostatic attraction. Furthermore, the asymmetric unit is not a planar structure, but a distorted structure.
[0055] See also Figure 4 , Figure 4 A schematic diagram of a trinuclear metal cluster [La3(COO)9(μ3-OH)] provided in an embodiment of the present invention.
[0056] In FMU-101, the three-dimensional porous structure is formed by adjacent trinuclear metal clusters [La3(COO)9(μ3-OH)] connected along the target direction through organic ligands; the trinuclear metal cluster [La3(COO)9(μ3-OH)] consists of three La 3+ The ions pass through μ3-OH - Bonding is formed. The target direction may be the c-axis (the a-axis is along the horizontal direction, the b-axis is along the vertical direction, and the c-axis is perpendicular to the paper surface).
[0057] Specifically, three La 3+ ions, two adjacent La 3+ The ion is μ3-OH - Bonded together, the three La 3+ The ion is replaced by a μ3-OH - Bonding to form a trinuclear metal cluster [La3(COO)9(μ3-OH)]. Adjacent trinuclear metal clusters are connected along the c-axis by organic ligands to form a three-dimensional porous structure with regular unidirectional hexagonal honeycomb channels, such as Figure 1 It can be understood that since the asymmetric unit is a non-planar twisted structure, the asymmetric unit of the twisted structure further extends in all directions in a repetitive manner of the space group to form a three-dimensional porous structure of regular unidirectional hexagonal honeycomb channels.
[0058] Furthermore, each La 3+ The ionic center presents a nine-coordinated geometric structure, which includes seven carboxyl oxygen atoms from organic ligands, one oxygen atom from the N,N-dimethylformamide molecule, and one oxygen atom from μ3-OH-.
[0059] Furthermore, in the three-dimensional organic framework of FMU-101, the carboxylic acid groups in the ligands exhibit three coordination modes: μ3-η 1 :η 2 ,μ2-η 1 :η 1 and μ1-η 1 :η 1 Among them, η n The n in μ represents the number of atoms coordinated with the metal atom. Generally speaking, these coordinated atoms are directly connected. n For bridging ligands, the subscript n indicates that one ligand is connected to several metals. Generally speaking, if n = 2, it can be omitted.
[0060] The lanthanum-based MOF crystal material of this embodiment is a three-dimensional porous structure with regular unidirectional hexagonal honeycomb channels, and there are metal vacancies in the three-dimensional porous structure. 3+ The ions have a coordination geometry to form La 3+Ionic metal sites, metal vacancies, La 3+ Ionic metal sites, Me2NH2 + The combination of the lanthanum-based MOF crystal material with a three-dimensional porous structure with regular unidirectional hexagonal honeycomb channels gives it excellent adsorption capacity, and can be used as a catalyst to catalyze the cycloaddition reaction of CO2 and epoxides. It exhibits good catalytic performance for the carbon dioxide cycloaddition reaction of epoxides, and the reaction conditions are mild, with low energy consumption and low cost, thus achieving the purpose of continuous flow separation of CH4 / CO2 and converting captured CO2 into valuable final products.
[0061] Embodiment 2
[0062] On the basis of Example 1, this example provides a method for preparing a lanthanum-based MOF crystal material, which is used to prepare the lanthanum-based MOF crystal material of Example 1.
[0063] See also Figure 5 , Figure 5 A schematic diagram of a synthesis process of a lanthanum-based MOF crystal material provided in an embodiment of the present invention, the synthesis process comprising:
[0064] S1. Dissolve 3,3',5'-biphenyltricarboxylic acid and benzoic acid in N,N-dimethylformamide to obtain a first solution, dissolve lanthanum chloride heptahydrate in water to obtain a second solution, and mix the first solution and the second solution to obtain a mixed solution.
[0065] Specifically, the organic ligand 3,3',5'-biphenyltricarboxylic acid and the auxiliary ligand benzoic acid are simultaneously dissolved in N,N dimethylformamide (DMF) to form a first solution, and lanthanum chloride heptahydrate (LaCl3·7H2O) is dissolved in H2O to form a second solution. After the first solution and the second solution are completely dissolved under ultrasonic conditions, the dissolved solutions are mixed uniformly to form a mixed solution.
[0066] Specifically, the molar ratio of the organic ligand 3,3',5'-biphenyltricarboxylic acid to the auxiliary ligand benzoic acid is 1:1, and the molar ratio of the organic ligand 3,3',5'-biphenyltricarboxylic acid to lanthanum chloride heptahydrate is 1:1. The amount of DMF added is 3 ml of DMF for every 0.1 mmol of 3,3',5'-biphenyltricarboxylic acid and every 0.1 mmol of benzoic acid, that is, the ratio of 3,3',5'-biphenyltricarboxylic acid, benzoic acid, and N,N-dimethylformamide is 0.1 mmol: 0.1 mmol: 3 ml. The amount of H2O added is 2 ml of H2O for every 0.1 mmol of lanthanum chloride heptahydrate, that is, the ratio of lanthanum chloride heptahydrate to water is 0.1 mmol: 2 ml.
[0067] S2. Using a hydrothermal synthesis method, a lanthanum-based MOF crystal material is obtained by subjecting the mixed solution to a thermal reaction.
[0068] Specifically, the mixed solution is sealed and placed in an oven, and a lanthanum-based MOF crystalline material is obtained after a solvothermal reaction. Further, a hydrothermal synthesis method is used, and after the mixed solution is sealed and placed in an oven, the mixed solution is heated to 120-180°C at a heating rate of 0.5-1.5°C / min, and the reaction time is 48-96h at 120-180°C, and then cooled to room temperature at a rate of 0.05-0.15°C / min, and then the product is washed and dried to obtain a lanthanum-based MOF crystalline material. Exemplarily, the mixed solution is heated to 150°C at a heating rate of 1°C / min, and the reaction time is 72h at 150°C, and then cooled to room temperature at a rate of 0.1°C / min.
[0069] On the basis of the above preparation method, this example adopts a hydrothermal synthesis method to prepare La-MOF and tests the performance of La-MOF.
[0070] The hydrothermal synthesis method for preparing La-MOF mainly includes the following experimental contents:
[0071] Take 3,3',5'-biphenyltricarboxylic acid (0.1mmol, 28.6mg) and benzoic acid (0.1mmol, 12.2mg) and dissolve them in 3mL DMF, and take LaCl3·7H2O (0.1mmol, 37.1mg) and dissolve it in 2mL H2O. The two solutions are ultrasonically treated until the solid is dissolved. After mixing the two solutions, transfer them to a stainless steel reactor lined with polytetrafluoroethylene, heat to 150℃ within 2 hours, keep at 150℃ for 72 hours, and then cool to room temperature at a rate of 0.1℃ / min. Collect the hexagonal crystals and wash them with DMF several times, then immerse them in DMF, decant and replenish DMF 3 times a day for 3 consecutive days, and finally dry them under vacuum at room temperature for 6 hours to obtain La-MOF.
[0072] See also Figure 6 , Figure 6 This is a BET test curve of La-MOF provided in the embodiment of the present invention. After calculation, it can be obtained that the specific surface area (Brunauer-Emmett-Teller, BET) of La-MOF is 236.16m 2 g-1.
[0073] See also Figure 7 , Figure 7 The pore size distribution diagram of La-MOF provided in the embodiment of the present invention. The pore size distribution span of La-MOF is about This facilitates the unimpeded passage of gas molecules; data analysis demonstrates the successful design of MOF materials with persistent porosity.
[0074] See also Figure 8 , Figure 8 FT-IR characterization diagram of La-MOF provided in the embodiment of the present invention. 780cm -1 The adsorption band at 1400 cm represents the partial distribution of COO- groups in [1,1'-biphenyl]-3,3',5-tricarboxylic acid. -1 (COO-symmetric vibration) and 1600cm -1 The adsorption band at 3410 cm (COO- asymmetric vibration) highlights the presence of CH and COO- groups in La-MOF. -1 (NH stretching vibration) and 1360cm -1 The single band of (CN stretching vibration) provides evidence for the presence of dimethylamine cation in the structure.
[0075] See also Fig. 9 , Fig. 9 The XRD diagram of La-MOF provided in the embodiment of the present invention. Fig. 9 The diffraction peaks of La-MOF observed in the experiment are consistent with those of single crystal simulations, confirming the material's continued crystallinity and unchanged structure under different pH conditions, highlighting its chemical stability.
[0076] See also Fig.10 , Fig.10 This is a morphology diagram of the La-MOF provided in an embodiment of the present invention. Fig.10 It shows that La-MOF presents a uniformly dispersed hexagonal prism structure.
[0077] See also Fig.11 , Fig.11 The particle size distribution diagram of La-MOF provided in the embodiment of the present invention. As can be seen from the figure, the particle size of La-MOF is about 480nm.
[0078] In this example, organic ligand 3,3',5'-biphenyltricarboxylic acid and metallic lanthanum are selected to prepare lanthanum-based MOF crystal materials by solvothermal method. The preparation method is simple and easy to implement. The obtained lanthanum-based MOF structure contains metal vacancies. Metal vacancies, La 3+ Ionic metal sites, Me2NH2 + The combination of a three-dimensional porous structure with regular unidirectional hexagonal honeycomb channels gives the lanthanum-based MOF crystal material excellent adsorption capacity, which can adsorb carbon dioxide from natural gas.
[0079] Embodiment 3
[0080] Based on Example 1 and Example 2, this example provides a method for applying a lanthanum-based MOF crystal material in natural gas decarbonization. Specifically, the lanthanum-based MOF crystal material FMU-101 can be used as a catalyst in the carbon dioxide cycloaddition catalytic reaction of epoxides, that is, the epoxide, the catalyst and the co-catalyst are placed in an environment containing carbon dioxide and heated, so that the epoxide and carbon dioxide undergo an addition reaction to remove carbon dioxide; wherein the catalyst uses the lanthanum-based MOF crystal material FMU 101 of Example 1.
[0081] Specifically, the epoxide includes epichlorohydrin, the cocatalyst includes tetrabutylammonium bromide (TBAB), the ratio of the epoxide, the catalyst, and the cocatalyst is 21 mmol: 70 mg: 0.21 mmol, the reaction temperature of the addition reaction is 50-70° C., and the reaction time is 32-60 hours. Exemplarily, the reaction temperature of the addition reaction is 60° C., and the reaction time is 48 hours.
[0082] See also Fig.12 , Fig.12 Schematic diagram of the process of La-MOF catalytic conversion of CO2 provided in an embodiment of the present invention. Specifically, the reaction equation of epichlorohydrin and CO2 is:
[0083]
[0084] Specifically, after La-MOF is prepared, the corresponding separation performance test is performed by the following method:
[0085] 21mmol of epoxide, 70mg of catalyst and 0.21mmol of co-catalyst were placed in a 10ml flask with a magnetic stirrer. CO2 gas was introduced into the flask for 30 minutes, and the pure CO2 gas was completely replaced into the reaction flask. After the gas replacement was completed, a balloon filled with CO2 gas was connected to ensure sufficient CO2 supply during the reaction. Finally, the reaction flask was placed in a 60℃ water bath for 48 hours, and then the reaction was continued for 24 hours. 1 The product structure was analyzed by HNMR (deuterated DMSO).
[0086] See also Fig.13 , Fig.13 The adsorption isotherm of La-MOF provided in the embodiment of the present invention shows that FMU-101 is adsorbed on CO2 (109.5 cm 3 g -1 ) showed excellent adsorption performance, and its adsorption capacity was CH4 (11.4cm 3 g -1 ) is 9.6 times.
[0087] See also Fig.14 , Fig.14This is a diagram of the adsorption selectivity of La-MOF provided in an embodiment of the present invention. Fig.14 The selectivity of La-MOF for CO2 / CH4 mixtures at 273 K and 298 K was demonstrated. For equimolar CO2 / CH4 mixtures, the selectivity of FMU-101 at 1 atm was 1.6, indicating the high selectivity of FMU-101a for CO2 adsorption.
[0088] See also Fig.15 , Fig.15 The yield comparison diagram of different catalytic systems provided in the embodiments of the present invention is shown in FIG. Fig.15 As shown, the catalytic efficiency of La-MOF exhibits significantly higher levels when juxtaposed with metal salts and ligands.
[0089] In this embodiment, the lanthanum-based MOF can be used as a catalyst to catalyze the cycloaddition reaction of CO2 and epichlorohydrin to prepare propylene chlorocarbonate, and exhibits good catalytic performance for the carbon dioxide cycloaddition reaction of epoxides. In addition, the reaction conditions are mild, the energy consumption is low, and the amount of solvent used is small. The continuous flow separation of CH4 / CO2 and the conversion of captured CO2 into valuable final products are achieved, providing opportunities for solving environmental problems and resource utilization.
[0090] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the protection scope of the present invention.
Claims
1. A lanthanum-based MOF crystal material, characterized in that: The chemical formula of the lanthanum-based MOF crystal material is: 54 H 43 La3N3O 22 3- ) n ,1(C2H8N1 1+ ), the organic ligand is 3,3',5'-biphenyltricarboxylic acid; The structure of the lanthanum-based MOF crystal material is a three-dimensional porous structure with regular unidirectional hexagonal honeycomb channels, and the three-dimensional porous structure has metal vacancies; The lanthanum-based MOF crystal material contains La 3+ Ions have coordination geometry.
2. The lanthanum-based MOF crystalline material according to claim 1, characterized in that The crystal structure of the lanthanum-based MOF crystal material belongs to the monoclinic system, and the space group is The unit cell parameters are α=90°, β=90°, γ=120°.
3. The lanthanum-based MOF crystalline material according to claim 1, characterized in that: There is an asymmetric unit in the three-dimensional porous structure, and the asymmetric unit consists of a La 3+ ion, an organic ligand 3,3',5'-biphenyltricarboxylic acid, a coordinated N,N-dimethylformamide molecule, and one-third μ3-OH - and one third Me2NH2 + Cation composition, the La 3+ The ions are connected to the 3,3',5'-biphenyltricarboxylic acid, the N,N-dimethylformamide molecule, the μ3-OH - Connect respectively, the Me2NH2 + The cation is attracted to the oxygen atom of the 3,3',5'-biphenyltricarboxylic acid by electrostatic forces.
4. The lanthanum-based MOF crystalline material according to claim 1, characterized in that: The three-dimensional porous structure is formed by connecting adjacent trinuclear metal clusters [La3(COO)9(μ3-OH)] along a target direction through the organic ligands; the trinuclear metal cluster [La3(COO)9(μ3-OH)] is composed of three La 3+ The ions pass through μ3-OH - Bond formation; each La 3+ The ionic center presents a nine-coordinate geometric structure, wherein the nine coordinated geometric structures are seven carboxyl oxygen atoms from the organic ligand, one oxygen atom from the N,N-dimethylformamide molecule and one oxygen atom from μ3-OH. - 1 oxygen atom.
5. The lanthanum-based MOF crystalline material according to claim 4, characterized in that: The carboxyl oxygen atom in the organic ligand has three coordination modes: μ3-η 1 :η 2 、μ2-η 1 :η 1 and μ1-η 1 :η 1 .
6. A method for preparing a lanthanum-based MOF crystal material, characterized in that: For preparing the lanthanum-based MOF crystalline material according to any one of claims 1 to 5, comprising the steps of: S1, dissolving 3,3',5'-biphenyltricarboxylic acid and benzoic acid in N,N-dimethylformamide to obtain a first solution, dissolving lanthanum chloride heptahydrate in water to obtain a second solution, and mixing the first solution and the second solution to obtain a mixed solution; S2. Using a hydrothermal synthesis method, the mixed solution is subjected to a thermal reaction to obtain a lanthanum-based MOF crystal material.
7. The method for preparing the lanthanum-based MOF crystal material according to claim 6, characterized in that: The molar ratio of the 3,3',5'-biphenyltricarboxylic acid to the benzoic acid is 1:1; The molar ratio of the 3,3',5'-biphenyltricarboxylic acid to the lanthanum chloride heptahydrate is 1:1; The ratio of the 3,3',5'-biphenyltricarboxylic acid, the benzoic acid, and the N,N-dimethylformamide is 0.1 mmol: 0.1 mmol: 3 ml; The ratio of the lanthanum chloride heptahydrate to the water is 0.1 mmol:2 ml.
8. The method for preparing the lanthanum-based MOF crystal material according to claim 6, characterized in that: Step S2 includes: The mixed solution is heated to 120-180°C at a heating rate of 0.5-1.5°C / min by a hydrothermal synthesis method, and the reaction time is 48-96h at 120-180°C, and then cooled to room temperature at a rate of 0.05-0.15°C / min to obtain the lanthanum-based MOF crystalline material.
9. A method for applying a lanthanum-based MOF crystal material in natural gas decarbonization, characterized in that: include: placing an epoxide, a catalyst and a co-catalyst in an environment containing carbon dioxide and heating them so that the epoxide and the carbon dioxide undergo an addition reaction to remove the carbon dioxide; The catalyst adopts the lanthanum-based MOF crystal material as described in any one of claims 1-5.
10. The method for using the lanthanum-based MOF crystal material in natural gas decarbonization according to claim 9, characterized in that: The epoxide includes epichlorohydrin, and the co-catalyst includes tetrabutylammonium bromide; the ratio of the epoxide, the catalyst, and the co-catalyst is: 21 mmol: 70 mg: 0.21 mmol; The reaction temperature of the addition reaction is 50-70° C., and the reaction time is 32-60 h.
Citation Information
Patent Citations
La-MOF material with dual ligands and preparation method
CN107674213A
Dual-emission lanthanide europium metal-organic framework material and preparation and application methods thereof
CN108329485A
Terbium coordination polymer for separating propyne / propylene gas mixture and preparation method thereof
CN110698686A
Diaphragm, electronic device comprising diaphragm and preparation method of diaphragm
CN114006131A
Gas adsorption material containing active metal sites as well as preparation method and application of gas adsorption material
CN114471470A
Cited By
Scandium-based MOF (Metal Organic Framework) crystal material as well as preparation method and application thereof
CN119823406A