Photonic crystal film based on lignin nanoparticles and preparation method

The preparation of polyhydroxylignin nanoparticles through non-centrifugal regulation method and hyperbranching reactions solves the problems of high cost and high energy consumption of traditional photonic crystals, and realizes the low-cost and environmentally friendly rainbow-colored photonic crystal film preparation, which enhances the material Stability and optical performance regulation.

CN118955973AActive Publication Date: 2024-11-15SHAANXI UNIV OF SCI & TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411202959.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-15
Estimated Expiration
2044-08-29

AI Technical Summary

Technical Problem

The preparation method of traditional photonic crystals is high cost and complex. In the preparation of lignin-based photonic crystals, monodispersed nanoparticles are difficult to prepare and consume a lot of energy, which limits its flexibility and operability in large-scale production and practical applications. .

Method used

Polyhydroxylignin nanoparticles were prepared through hyperbranching reaction by non-centrifugal regulation, and self-assembly formed a rainbow-colored photonic crystal film by evaporation-induced self-assembly to simplify the process and reduce costs and energy consumption.

Benefits of technology

It has achieved a large-scale production of photonic crystal films with low cost and low energy consumption, enhanced the stability of the material and optical performance regulation capabilities, and provided environmental protection and application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955973A_ABST
    Figure CN118955973A_ABST
Patent Text Reader

Abstract

The preparation method comprises the following steps: adding 2-dimethylolpropionic acid and p-toluenesulfonic acid into a dispersion liquid of the lignin nanoparticles under a protective atmosphere, and carrying out a hyperbranched reaction to obtain a reaction liquid; dialyzing the reaction liquid in deionized water to remove small molecules and homopolymerized 2-dimethylolpropionic acid generated by side reaction, so as to obtain an aqueous dispersion of the modified lignin nanoparticles; and dropwise adding the aqueous dispersion of the modified lignin nanoparticles onto a hard transparent material, and drying by means of electric heating and blast circulation to obtain the photonic crystal film based on the lignin nanoparticles. According to the preparation method disclosed by the invention, H-LNP with polyhydroxy is obtained through hyperbranched reaction, and the polyhydroxy structure endows H-LNPs with good self-assembly tendency, so that the H-LNPs can form a thin film with clear structural color under the condition of evaporation-induced self-assembly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of photonic crystals, and in particular relates to a photonic crystal film based on lignin nanoparticles and a preparation method thereof. Background Art

[0002] Photonic crystal is a material with a periodic structure whose scale is comparable to or smaller than the wavelength of light. Its basic principle is to use the refractive index difference between periodically arranged media or media to realize the diffraction and interference of light. When light passes through a photonic crystal, it will be restricted and scattered by the lattice structure, causing the wavelength of light to be restricted or diffracted in the material, forming a specific photonic band gap. These photonic band gaps prevent light from propagating within a specific frequency range, thereby generating a photonic bandgap, which gives photonic crystals specific optical properties, such as optical isolation, optical waveguide, photon modulation, etc. The design and preparation of photonic crystals can achieve precise control of optical properties by regulating the lattice structure and the refractive index of the material, so it has broad application prospects.

[0003] The preparation of traditional photonic crystals usually uses a combination of high-refractive index and low-refractive index materials to construct a lattice with a periodic structure. Common high-refractive index materials include silicon dioxide, titanium dioxide, etc., while low-refractive index materials include polymers, air, etc. The preparation methods mainly include self-assembly, solvent evaporation, photolithography, etc. In the self-assembly method, the material is usually self-assembled into a periodic structure by physical or chemical means through a template self-assembly method. Although the traditional photonic crystal preparation method has achieved certain success, there are still some challenges and limitations. First, the preparation cost of traditional materials is high, the preparation process is complicated, and special equipment and conditions are required, which limits its application in large-scale production. Secondly, the traditional preparation method has certain restrictions on the selection of materials and the processing process. In addition, the traditional preparation method of photonic crystals often requires a long preparation cycle and high-precision processing technology, which limits its flexibility and operability in some practical applications. Chinese patent CN114507016 discloses a method for preparing photonic crystals, which is prepared by co-assembly of nanoparticles and polymers. The photonic crystals prepared by this method still require a large amount of polymers as components, involving a large amount of synthetic polymers. At the same time, the nanoparticles used are all inorganic nanoparticles, and the precision and requirements of the processing technology are relatively high.

[0004] With the need for sustainable development and environmental protection, natural biomass has attracted much attention as a material for preparing photonic crystals. Lignin is an important compound in natural biomass, mainly found in plant cell walls, with good mechanical properties and chemical stability. Due to the particularity of its molecular structure, lignin can be used to prepare nanoparticles with stable structure and stable dispersion, which has unique advantages in the preparation of photonic crystals. Using lignin as a raw material for photonic crystals can not only achieve the regulation of optical properties, but also effectively utilize the discarded lignin resources to achieve resource regeneration and recycling. At present, the method for preparing photonic crystals based on lignin is mainly the centrifugal assembly method. The centrifugal assembly method is to disperse monodisperse lignin particles in a solvent, and realize the self-assembly of lignin by controlling parameters such as the concentration of the dispersion and the centrifugal force. However, when preparing photonic crystals based on lignin, it is difficult to prepare monodisperse lignin nanoparticles, and the energy consumption of centrifugal regulation of lignin nanoparticles is too large and the cost is high. Summary of the invention

[0005] In view of the problems existing in the prior art, the present invention provides a photonic crystal film based on lignin nanoparticles and a preparation method thereof. A photonic crystal film with rainbow colors is prepared by a non-centrifugal control method, which is easy to operate, low in cost and low in energy consumption. H-LNP with multiple hydroxyl groups is obtained by a hyperbranching reaction. This multiple hydroxyl structure gives H-LNPs a good self-assembly tendency, so that it can form a film with clear structural color under the condition of evaporation-induced self-assembly.

[0006] The present invention is achieved through the following technical solutions:

[0007] A method for preparing a photonic crystal film based on lignin nanoparticles comprises the following steps:

[0008] S1, under a protective atmosphere, adding 2-dihydroxymethylpropionic acid and p-toluenesulfonic acid to a dispersion of lignin nanoparticles to carry out a hyperbranching reaction, wherein the mass of the 2-dihydroxymethylpropionic acid and the p-toluenesulfonic acid is 5%-20% and 0.1%-10% of the mass of the lignin nanoparticles, respectively, to obtain a reaction solution;

[0009] S2, dialyzing the reaction solution in deionized water to remove small molecules and homopolymerized 2-dihydroxymethylpropionic acid produced by the side reaction, thereby obtaining an aqueous dispersion of modified lignin nanoparticles;

[0010] S3, dropping the water dispersion of modified lignin nanoparticles onto the hard transparent material, and drying it by electric heating and air circulation to obtain a photonic crystal film based on lignin nanoparticles.

[0011] Preferably, the dispersion of lignin nanoparticles described in S1 is obtained by the following process:

[0012] Sodium lignin sulfonate, alkali lignin, ground wood lignin or enzymatic lignin is dissolved in ethylene glycol in an amount of 0.1%-2% by mass, then stirred at room temperature, and then hydrochloric acid with a concentration of 0.01M-0.1M is added to form lignin nanoparticles. The obtained mixed solution is dialyzed in deionized water, and then the lignin nanoparticles therein are replaced with an organic reagent to obtain a dispersion of lignin nanoparticles.

[0013] Furthermore, the addition rate of the hydrochloric acid is 0.01 ml / min-0.2 ml / min, and the volume is 1%-30% of the ethylene glycol.

[0014] Furthermore, the organic reagent is N,N-dimethylformamide.

[0015] Preferably, the hyperbranching reaction described in S1 is carried out at 80°C-180°C for 1 h-10 h.

[0016] Further, when the hyperbranching reaction time is within 2 h, the 2-dihydroxymethylpropionic acid and p-toluenesulfonic acid in S1 are added at one time;

[0017] When the time t of the hyperbranching reaction exceeds 2h, S1 first divides 2-dihydroxymethylpropionic acid and p-toluenesulfonic acid equally into (n1+1) / 2 or n2 / 2 parts according to the amount, n1 is the time number when t only retains integers and is an odd number, and n2 is the time number when t only retains integers and is an even number, and then adds 1 part of 2-dihydroxymethylpropionic acid and 1 part of p-toluenesulfonic acid every 1h.

[0018] Preferably, the hard transparent material described in S3 is a glass slide.

[0019] Preferably, in S3, the mass percentage of the modified lignin nanoparticles in the aqueous dispersion of the modified lignin nanoparticles is adjusted to 0.01%-2%, and then the modified lignin nanoparticles are added dropwise to the hard transparent material, so that a photonic crystal film based on the lignin nanoparticles is formed on the hard transparent material.

[0020] Preferably, the drying method described in S3 is drying in a forced air drying oven at 30°C-150°C for 30 minutes to 12 hours.

[0021] A photonic crystal film based on lignin nanoparticles obtained by any one of the above methods for preparing a photonic crystal film based on lignin nanoparticles.

[0022] Compared with the prior art, the present invention has the following beneficial technical effects:

[0023] The invention discloses a method for preparing a photonic crystal film based on lignin nanoparticles. By reasonably controlling the dosage of 2-dihydroxymethylpropionic acid and p-toluenesulfonic acid, the hyperbranching reaction between the 2-dihydroxymethylpropionic acid and the lignin nanoparticles can be facilitated. The small molecules and homopolymerized 2-dihydroxymethylpropionic acid generated by the side reaction can be removed by dialysis in deionized water to prepare polyhydroxy lignin nanoparticles with good dispersibility. The drying speed can be reasonably controlled by dripping and subsequent electric heating and air circulation drying, which is conducive to the regular movement of the polyhydroxy lignin nanoparticles under the conditions of evaporation-induced self-assembly, forming a tree-like morphology, and finally obtaining a film with clear structural color. The invention prepares a rainbow-colored photonic crystal film by a non-centrifugal control method, avoiding a high-cost and high-energy consumption centrifugal process. The hyperbranching reaction simplifies the process, improves the preparation efficiency, and makes large-scale production more economical and environmentally friendly. This structure not only enhances the stability of the photonic crystal, but also realizes the precise control of the optical properties. The invention does not require complex conditions and expensive equipment, and does not require the lignin nanoparticles to be graded. In the self-assembly process, there is no need for excessive external force. Only through hyperbranching modification, the directional aggregation of lignin particles of different sizes can be achieved through spontaneous induced self-assembly, thus presenting a colorful rainbow film. H-LNPs have a good tendency to self-assemble. Under the method of evaporation-induced self-assembly, the H-LNPs film produces a clear structural color, thus presenting a colorful rainbow film. The present invention reveals an important progress in lignin-based photonic crystal materials, which can achieve large-scale, low-cost, and environmentally friendly preparation of photonic crystal films without expensive equipment and complex conditions, and has significant environmental benefits and application prospects.

[0024] Furthermore, the present invention utilizes sodium lignin sulfonate, alkali lignin, ground wood lignin or enzymatic lignin to obtain lignin nanoparticles, effectively utilizing waste lignin resources and converting them into high value-added photonic crystal materials, which is conducive to resource regeneration and recycling.

[0025] The rainbow-colored light spots produced by the photonic crystal film of the present invention are caused by reflecting visible light, and the generated color distribution is relatively wide, including most standard colors, providing new ideas and technical support for the application of photonic crystal materials in the fields of optical isolation, optical waveguide, photon modulation, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1a This is the X-ray photoelectron spectrum of pure sodium lignin sulfonate.

[0027] Figure 1b This is the X-ray photoelectron spectrum of the lignin nanoparticles after the reaction in Example 1.

[0028] Figure 2This is a digital photo of the photonic crystal based on lignin nanoparticles prepared in Example 4.

[0029] Figure 3a This is the reflection spectrum of the photonic crystal based on lignin nanoparticles prepared in Example 3 within the visible light wavelength range.

[0030] Figure 3b This is a distribution diagram of the color generated by the photonic crystal based on lignin nanoparticles prepared in Example 3 in the CIE1931 standard color space.

[0031] Figure 4a This is a surface microscopic morphology of the red-orange region of the photonic crystal based on lignin nanoparticles prepared in Example 4.

[0032] Figure 4b This is a microscopic morphology of the surface of the yellow-green region of the photonic crystal based on lignin nanoparticles prepared in Example 4.

[0033] Figure 4c This is a microscopic image of the surface morphology of the cyan region of the photonic crystal based on lignin nanoparticles prepared in Example 4.

[0034] Figure 5a This is a photo of the photonic crystal obtained in Comparative Example 1.

[0035] Figure 5b This is the SEM image of the photonic crystal obtained in Comparative Example 1.

[0036] Figure 6a This is a photo of the photonic crystal obtained in Comparative Example 2.

[0037] Figure 6b This is the SEM image of the photonic crystal obtained in Comparative Example 2.

[0038] Figure 7a This is a scanning electron microscope image of the oriented aggregation of lignin nanoparticles in the photonic crystal film obtained in Example 1.

[0039] Figure 7b This is a scanning electron microscope image of the oriented aggregation of lignin nanoparticles in the photonic crystal film obtained in Example 2.

[0040] Figure 7c This is a scanning electron microscope image of the oriented aggregation of lignin nanoparticles in the photonic crystal film obtained in Example 3.

[0041] Figure 7d This is a scanning electron microscope image of the oriented aggregation of lignin nanoparticles in the photonic crystal film obtained in Example 4.

[0042] Figure 8a for Figure 7aEnlarged view in the rectangular box.

[0043] Figure 8b for Figure 7b Enlarged view in the rectangular box.

[0044] Figure 8c for Figure 7c Enlarged view in the rectangular box.

[0045] Figure 8d for Figure 7d Enlarged view in the rectangular box.

[0046] Figure 9a This is a graph showing the surface electrostatic potential results of the grafted polyhydroxylated lignin nanoparticles obtained in an example of the present invention.

[0047] Figure 9b This is an adsorption model diagram of the grafted polyhydroxy lignin nanoparticles obtained in an embodiment of the present invention.

[0048] Fig.10 Schematic diagram of the microscopic mechanism by which the H-LNPs film obtained in the present invention produces photonic crystal properties. DETAILED DESCRIPTION

[0049] The following will be combined with the drawings, process steps, specific implementation conditions and materials in the embodiments of the present invention to clearly and completely describe the technical solution of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0050] The present invention provides a method for preparing a photonic crystal film based on lignin nanoparticles, comprising the following steps:

[0051] Step 1, dissolving a certain amount of sodium lignin sulfonate, alkali lignin, ground wood lignin or enzymatic lignin in ethylene glycol, the mass percentage is 0.1%-2%, stirring at room temperature, adding hydrochloric acid with a concentration of 0.01M-0.1M, the volume is 1%-30% of ethylene glycol, and the addition speed is controlled to be 0.01ml / min-0.2ml / min. LNPs with good dispersibility are prepared by adjusting the pH value, and the obtained mixed solution is dialyzed in deionized water.

[0052] Step 2, replacing the lignin nanoparticles in the aqueous dispersion of lignin nanoparticles (LNPs) obtained in step 1) with N,N-dimethylformamide, using a three-necked flask as a reaction container, introducing argon as a protective gas, adding 2-dihydroxymethylpropionic acid and p-toluenesulfonic acid thereto, the addition amounts of which are 5%-20% and 0.1%-10% of the mass of the lignin nanoparticles, respectively, and performing a hyperbranching reaction at 80° C.-180° C. for 1 h-10 h. When the hyperbranching reaction time is within 2 h, 2-dihydroxymethylpropionic acid and p-toluenesulfonic acid are All-at-once addition; when the time t of the hyperbranching reaction exceeds 2h, firstly divide 2-dihydroxymethylpropionic acid and p-toluenesulfonic acid equally into (n1+1) / 2 or n2 / 2 parts according to the amount, n1 is the time number of t only retaining integers and being odd numbers, n2 is the time number of t only retaining integers and being even numbers, and then add 1 part of 2-dihydroxymethylpropionic acid and 1 part of p-toluenesulfonic acid every 1h, and start timing after the addition. After the reaction is completed, dialyze the obtained reaction solution in deionized water to remove small molecules produced by side reactions and homopolymerized 2-dihydroxymethylpropionic acid.

[0053] Step 3, adjusting the mass percentage of the modified lignin nanoparticles (polyhydroxy lignin nanoparticles, H-LNPs) dispersion obtained by dialysis to 0.01%-2%, dropping it on a hard transparent material and drying it at 30°C-150°C for 30min-12h. The drying method is to dry it in a forced air drying oven to cause evaporation-induced self-assembly. The obtained film is a photonic crystal material based on lignin nanoparticles.

[0054] In the following examples, sodium lignin sulfonate is used as a raw material to illustrate the present invention.

[0055] Example 1

[0056] Sodium lignin sulfonate was first dissolved in ethylene glycol to a mass percentage of 0.56%, stirred at room temperature for 2 hours, then 0.025M hydrochloric acid was added, the volume of which was 15% of the volume of ethylene glycol, and the dripping rate was controlled to be 0.04 ml / min. The resulting mixed solution was dialyzed in deionized water.

[0057] The lignin nanoparticles in the lignin nanoparticle aqueous dispersion were replaced with N,N-dimethylformamide, a three-necked flask was used as a reaction container, argon was introduced as a protective gas, 2-dihydroxymethylpropionic acid equivalent to 14.2% of the mass of the lignin nanoparticles and 4.1% of p-toluenesulfonic acid were added thereto, the reaction was carried out at 140°C for 1 hour, and the reaction solution was dialyzed in deionized water.

[0058] The dispersion obtained by dialysis (lignin nanoparticles after the reaction were recorded as H1-LNPs) was adjusted to 0.8% by mass, dropped on a glass slide and air-dried, and then dried in a forced air oven at 60° C. for 30 min to obtain a photonic crystal.

[0059] Example 2

[0060] Sodium lignin sulfonate was first dissolved in ethylene glycol to a mass percentage of 0.56%, stirred at room temperature for 2 hours, then 0.025M hydrochloric acid was added, the volume of which was 15% of the volume of ethylene glycol, and the dripping rate was controlled to be 0.04 ml / min. The resulting mixed solution was dialyzed in deionized water.

[0061] The lignin nanoparticles in the lignin nanoparticle water dispersion are replaced into N,N-dimethylformamide, a three-necked flask is used as a reaction container, argon is introduced as a protective gas, 2-dihydroxymethylpropionic acid and 4.1% p-toluenesulfonic acid equivalent to 14.2% of the mass of the lignin nanoparticles are added, and the reaction is carried out at 140° C. for 2 hours, wherein 1 part of 2-dihydroxymethylpropionic acid and p-toluenesulfonic acid is added every 1 hour, and the reaction solution is dialyzed in deionized water.

[0062] The mass percentage of the dialyzed dispersion (lignin nanoparticles after the reaction were recorded as H2-LNPs) was adjusted to 0.8%, dropped on a glass slide and air-dried, and then dried in a forced air oven at 60° C. for 30 min to obtain a photonic crystal.

[0063] Example 3

[0064] Sodium lignin sulfonate was first dissolved in ethylene glycol to a mass percentage of 0.56%, stirred at room temperature for 2 hours, then 0.025M hydrochloric acid was added, the volume of which was 15% of the volume of ethylene glycol, and the dripping rate was controlled to be 0.04 ml / min. The resulting solution was dialyzed in deionized water.

[0065] The lignin nanoparticles in the lignin nanoparticle water dispersion are replaced into N,N-dimethylformamide, a three-necked flask is used as a reaction container, argon is introduced as a protective gas, 2-dihydroxymethylpropionic acid and 4.1% p-toluenesulfonic acid equivalent to 14.2% of the mass of the lignin nanoparticles are added, and the reaction is carried out at 140°C for 3 hours, wherein 1 part of 2-dihydroxymethylpropionic acid and p-toluenesulfonic acid is added every 1 hour, and the reaction solution is dialyzed in deionized water.

[0066] The mass percentage of the dialyzed dispersion (lignin nanoparticles after the reaction were recorded as H3-LNPs) was adjusted to 0.8%, dropped on a glass slide and air-dried, and then dried in a forced air oven at 60° C. for 30 min to obtain a photonic crystal.

[0067] Example 4

[0068] Sodium lignin sulfonate was first dissolved in ethylene glycol to a mass percentage of 0.56%, stirred at room temperature for 2 hours, then 0.025M hydrochloric acid was added, the volume of which was 15% of the volume of ethylene glycol, and the dripping rate was controlled to be 0.04 ml / min. The resulting solution was dialyzed in deionized water.

[0069] The lignin nanoparticles in the lignin nanoparticle water dispersion are replaced with N,N-dimethylformamide, a three-necked flask is used as a reaction container, argon is introduced as a protective gas, 2-dihydroxymethylpropionic acid and 4.1% p-toluenesulfonic acid equivalent to 14.2% of the mass of the lignin nanoparticles are added, and the reaction is carried out at 140°C for 4 hours, wherein 1 part of 2-dihydroxymethylpropionic acid and p-toluenesulfonic acid is added every 1 hour, and the reaction solution is dialyzed in deionized water.

[0070] The mass percentage of the dialyzed dispersion (lignin nanoparticles after the reaction were recorded as H4-LNPs) was adjusted to 0.8%, dropped on a glass slide and air-dried, and then dried in a forced air oven at 60° C. for 30 min to obtain a photonic crystal.

[0071] from Figure 7a and Figure 8a It can be clearly seen that H1-LNPs have a tendency to self-assemble close to each other. Figure 7b and Figure 8b It can be clearly seen that the assembly trend of H2-LNPs is further obvious, and the spherical particles are assembled in a fixed direction, showing a radial arrangement trend. Figure 7c and Figure 8c The morphology of H3-LNPs can be clearly seen in the figure. With the increase of the degree of hyperbranching, the assembly between the small balls shows a tree-like morphology. Figure 7d and Figure 8d The morphology of H4-LNPs can be clearly seen in the figure. After four hyperbranching reactions, the self-assembly behavior between the small balls is more obvious, and obvious tree-like morphology accumulation appears. The diameter of the assembled tree-like structure can reach 30μm.

[0072] Comparative Example 1

[0073] Sodium lignin sulfonate was first dissolved in ethylene glycol to a mass percentage of 0.56%, stirred at room temperature for 2 hours, then 0.025M hydrochloric acid was added, the volume of which was 15% of the volume of ethylene glycol, and the dripping rate was controlled to be 0.04 ml / min. The resulting solution was dialyzed in deionized water.

[0074] The lignin nanoparticles in the lignin nanoparticle water dispersion are replaced with N,N-dimethylformamide, a three-necked flask is used as a reaction container, argon is introduced as a protective gas, 2-dihydroxymethylpropionic acid and 4.1% p-toluenesulfonic acid equivalent to 14.2% of the mass of the lignin nanoparticles are added, and the reaction is carried out at 140°C for 4 hours, wherein 1 part of 2-dihydroxymethylpropionic acid and p-toluenesulfonic acid is added every 1 hour, and the reaction solution is dialyzed in deionized water.

[0075] The mass percentage of the dialyzed dispersion was adjusted to 0.8%, dropped on a glass slide and air-dried, and dried in a vacuum oven at 60° C. for 30 min to obtain a photonic crystal.

[0076] Comparative Example 2

[0077] Sodium lignin sulfonate was first dissolved in ethylene glycol to a mass percentage of 0.56%, stirred at room temperature for 2 hours, then 0.025M hydrochloric acid was added, the volume of which was 15% of the volume of ethylene glycol, and the dripping rate was controlled to be 0.04 ml / min. The resulting solution was dialyzed in deionized water.

[0078] The lignin nanoparticles in the lignin nanoparticle water dispersion are replaced with N,N-dimethylformamide, a three-necked flask is used as a reaction container, argon is introduced as a protective gas, 2-dihydroxymethylpropionic acid and 4.1% p-toluenesulfonic acid equivalent to 14.2% of the mass of the lignin nanoparticles are added, and the reaction is carried out at 140°C for 4 hours, wherein 1 part of 2-dihydroxymethylpropionic acid and p-toluenesulfonic acid is added every 1 hour, and the reaction solution is dialyzed in deionized water.

[0079] The mass percentage of the dialyzed dispersion was adjusted to 0.8%, dropped on a glass slide and air-dried, and the photonic crystal was obtained after drying at room temperature for 24 hours.

[0080] from Figure 5a It can be seen that at a vacuum drying speed of 60 °C, the H-LNPs film did not produce any color due to the excessively fast drying speed.

[0081] from Figure 5b It can be seen that too fast drying speed will cause H-LNPs to assemble quickly and then wrinkle and crack, and it will be impossible to form a microscopic morphology with photonic crystal characteristics.

[0082] from Figure 6a It can be seen that natural drying at room temperature does produce the properties of photonic crystals ( Figure 6b It can also be seen from a microscopic perspective that H-LNPs naturally dried at room temperature can form a concave structure that meets the characteristics of photonic crystals), but because the drying speed is too slow and the drying interface advances too slowly, the movement of H-LNPs is irregular, which ultimately leads to a disorderly arrangement of colors.

[0083] Example 5

[0084] Sodium lignin sulfonate was first dissolved in ethylene glycol to a mass percentage of 0.56%, stirred at room temperature for 2 hours, then 0.025M hydrochloric acid was added, the volume of which was 15% of the volume of ethylene glycol, and the dripping rate was controlled to be 0.04 ml / min. The resulting solution was dialyzed in deionized water.

[0085] The lignin nanoparticles in the lignin nanoparticle water dispersion are replaced into N,N-dimethylformamide, a three-necked flask is used as a reaction container, argon is introduced as a protective gas, 2-dihydroxymethylpropionic acid and 4.1% p-toluenesulfonic acid equivalent to 14.2% of the mass of the lignin nanoparticles are added, and the reaction is carried out at 140° C. for 5 hours, wherein 1 part of 2-dihydroxymethylpropionic acid and p-toluenesulfonic acid is added every 1 hour, and the reaction solution is dialyzed in deionized water.

[0086] The mass percentage of the dialyzed dispersion was adjusted to 0.8%, dropped on a glass slide and air-dried, and then dried in a forced air oven at 60° C. for 30 min to obtain a photonic crystal.

[0087] Example 6

[0088] Sodium lignin sulfonate was first dissolved in ethylene glycol to a mass percentage of 0.56%, stirred at room temperature for 2 hours, then 0.025M hydrochloric acid was added, the volume of which was 15% of the volume of ethylene glycol, and the dripping rate was controlled to be 0.04 ml / min. The resulting solution was dialyzed in deionized water.

[0089] The lignin nanoparticles in the lignin nanoparticle water dispersion are replaced with N,N-dimethylformamide, a three-necked flask is used as a reaction container, argon is introduced as a protective gas, 2-dihydroxymethylpropionic acid and 4.1% p-toluenesulfonic acid equivalent to 14.2% of the mass of the lignin nanoparticles are added, and the reaction is carried out at 140°C for 4 hours, wherein 1 part of 2-dihydroxymethylpropionic acid and p-toluenesulfonic acid is added every 1 hour, and the reaction solution is dialyzed in deionized water.

[0090] The mass percentage of the dialyzed dispersion was adjusted to 0.01%, dropped on a glass slide and air-dried, and then dried in a forced air oven at 60° C. for 30 min to obtain a photonic crystal.

[0091] Example 7

[0092] Sodium lignin sulfonate was first dissolved in ethylene glycol to a mass percentage of 0.56%, stirred at room temperature for 2 hours, then 0.025M hydrochloric acid was added, the volume of which was 15% of the volume of ethylene glycol, and the dripping rate was controlled to be 0.04 ml / min. The resulting solution was dialyzed in deionized water.

[0093] The lignin nanoparticles in the lignin nanoparticle water dispersion are replaced with N,N-dimethylformamide, a three-necked flask is used as a reaction container, argon is introduced as a protective gas, 2-dihydroxymethylpropionic acid and 4.1% p-toluenesulfonic acid equivalent to 14.2% of the mass of the lignin nanoparticles are added, and the reaction is carried out at 140°C for 4 hours, wherein 1 part of 2-dihydroxymethylpropionic acid and p-toluenesulfonic acid is added every 1 hour, and the reaction solution is dialyzed in deionized water.

[0094] The mass percentage of the dialyzed dispersion was adjusted to 0.1%, dropped on a glass slide and air-dried, and then dried in a forced air oven at 60° C. for 30 min to obtain a photonic crystal.

[0095] Example 8

[0096] Sodium lignin sulfonate was first dissolved in ethylene glycol to a mass percentage of 0.56%, stirred at room temperature for 2 hours, then 0.025M hydrochloric acid was added, the volume of which was 15% of the volume of ethylene glycol, and the dripping rate was controlled to be 0.04 ml / min. The resulting solution was dialyzed in deionized water.

[0097] The lignin nanoparticles in the lignin nanoparticle water dispersion are replaced with N,N-dimethylformamide, a three-necked flask is used as a reaction container, argon is introduced as a protective gas, 2-dihydroxymethylpropionic acid and 4.1% p-toluenesulfonic acid equivalent to 14.2% of the mass of the lignin nanoparticles are added, and the reaction is carried out at 140°C for 4 hours, wherein 1 part of 2-dihydroxymethylpropionic acid and p-toluenesulfonic acid is added every 1 hour, and the reaction solution is dialyzed in deionized water.

[0098] The mass percentage of the dialyzed dispersion was adjusted to 1%, dropped on a glass slide and air-dried, and then dried in a forced air oven at 60° C. for 30 min to obtain a photonic crystal.

[0099] Example 9

[0100] Sodium lignin sulfonate was first dissolved in ethylene glycol to a mass percentage of 0.56%, stirred at room temperature for 2 hours, then 0.025M hydrochloric acid was added, the volume of which was 15% of the volume of ethylene glycol, and the dripping rate was controlled to be 0.04 ml / min. The resulting solution was dialyzed in deionized water.

[0101] The lignin nanoparticles in the lignin nanoparticle water dispersion are replaced with N,N-dimethylformamide, a three-necked flask is used as a reaction container, argon is introduced as a protective gas, 2-dihydroxymethylpropionic acid and 4.1% p-toluenesulfonic acid equivalent to 14.2% of the mass of the lignin nanoparticles are added, and the reaction is carried out at 140°C for 4 hours, wherein 1 part of 2-dihydroxymethylpropionic acid and p-toluenesulfonic acid is added every 1 hour, and the reaction solution is dialyzed in deionized water.

[0102] The mass percentage of the dialyzed dispersion was adjusted to 1.5%, dropped on a glass slide and air-dried, and then dried in a forced air oven at 60° C. for 30 min to obtain a photonic crystal.

[0103] Figure 1a This is the X-ray photoelectron spectrum of pure sodium lignin sulfonate LS. Figure 1b This is the X-ray photoelectron spectrum of the lignin nanoparticles H1-LNPs after the reaction. By comparison, it can be seen that after the reaction, an obvious C=O peak appears at 288.33 eV, indicating that the reaction successfully prepared H1-LNPs.

[0104] Figure 2 This is a digital photo of the photonic crystal based on lignin nanoparticles prepared in Example 4. The prepared material has a typical photonic crystal structural color. It should be noted that the red circle part located on the outside is the lignin particles that have not formed a photonic crystal arrangement, which is the result of disordered arrangement during drying, caused by too low concentration in the outer circle or insufficient surface tension.

[0105] Figure 3a This is the reflection spectrum within the visible light wavelength range of the photonic crystal based on lignin nanoparticles prepared in Example 3. It can be seen from the figure that obvious reflection peaks appear at 428nm to 628nm, indicating that the rainbow-colored light spots produced by the photonic crystal are caused by the reflection of visible light. The pictures above the curve represent the standard colors in different visible light bands as a comparison. Figure 3b This is the distribution of colors generated by photonic crystals in the CIE1931 standard color space. The generated color distribution is relatively wide and includes most standard colors.

[0106] Figure 4a The microscopic morphology of the red-orange region of the photonic crystal based on lignin nanoparticles prepared in Example 4 is shown in FIG. Figure 4b The picture shows the microscopic morphology of the yellow-green area. Figure 4c The picture shows the microscopic morphology of the blue area, which was obtained by observing and photographing the sample at a voltage of 10kV after gold was sprayed on it using an environmental scanning electron microscope. Figure 4a , Figure 4b and Figure 4c It can be seen that a uniformly distributed concave structure appears on the surface of the prepared photonic crystal. This self-assembled inverse opal structure forms a periodically symmetric photonic band gap, which makes the H-LNPs film have typical photonic crystal properties.

[0107] The present invention uses the method of molecular surface electrostatic potential to reveal the mechanism of self-assembly of H-LNPs. Figure 9a As shown in Figure 2, the maximum electrostatic potential energy (ESP Max) of L-LNPS grafting was significantly reduced, but Figure 9aThe maximum value marked by the arrow is located at the hydrogen atoms of the four hydroxyl ends after the grafted small molecule (the picture has a symmetrical structure, and one of the arrows is blocked). The grafted sodium lignin sulfonate has four symmetrical grafting sites, so it is easier to form Figure 9b The adsorption model, in which the electrostatic potential energy is 2.151eV, indicates that the grafting reaction will occur here.

[0108] like Fig.10 As shown in the figure, due to the mutual attraction and assembly of H-LNPs and the surface tension of different components during evaporation, holes of different diameters will appear on the surface of the H-LNPs film at the end of self-assembly. This self-assembled inverse opal structure forms a periodically symmetrical photonic band gap, which makes the H-LNPs film have typical photonic crystal properties. When the incident light is irradiated on the large pore area formed by the aggregation of small-sized H-LNPs, the pore diameter is close to the wavelength corresponding to red and orange, so the reflected light appears orange and red; when the incident light is irradiated on the small pore area formed by the aggregation of large-sized H-LNPs, the pore diameter is close to the wavelength corresponding to blue and purple, and the reflected light appears blue and purple.

Claims

1. A method for preparing a photonic crystal film based on lignin nanoparticles, characterized in that: The steps include: S1, under a protective atmosphere, adding 2-dihydroxymethylpropionic acid and p-toluenesulfonic acid to a dispersion of lignin nanoparticles to carry out a hyperbranching reaction, wherein the mass of the 2-dihydroxymethylpropionic acid and the p-toluenesulfonic acid is 5%-20% and 0.1%-10% of the mass of the lignin nanoparticles, respectively, to obtain a reaction solution; S2, dialyzing the reaction solution in deionized water to obtain an aqueous dispersion of modified lignin nanoparticles; S3, dropping the water dispersion of modified lignin nanoparticles onto the hard transparent material, and drying it by electric heating and air circulation to obtain a photonic crystal film based on lignin nanoparticles.

2. The method for preparing a photonic crystal film based on lignin nanoparticles according to claim 1, characterized in that: The dispersion of lignin nanoparticles described in S1 is obtained by the following process: Sodium lignin sulfonate, alkali lignin, ground wood lignin or enzymatic lignin is dissolved in ethylene glycol in an amount of 0.1%-2% by mass, then stirred at room temperature, and then hydrochloric acid with a concentration of 0.01M-0.1M is added to form lignin nanoparticles. The obtained mixed solution is dialyzed in deionized water, and then the lignin nanoparticles therein are replaced with an organic reagent to obtain a dispersion of lignin nanoparticles.

3. The method for preparing a photonic crystal film based on lignin nanoparticles according to claim 2, characterized in that: The addition rate of the hydrochloric acid is 0.01 ml / min-0.2 ml / min, and the volume is 1%-30% of the ethylene glycol.

4. The method for preparing a photonic crystal film based on lignin nanoparticles according to claim 2, characterized in that: The organic reagent is N,N-dimethylformamide.

5. The method for preparing a photonic crystal film based on lignin nanoparticles according to claim 1, characterized in that: The hyperbranching reaction described in S1 is carried out at 80°C-180°C for 1 h-10 h.

6. The method for preparing a photonic crystal film based on lignin nanoparticles according to claim 5, characterized in that: When the hyperbranching reaction time is within 2 h, the 2-dihydroxymethylpropionic acid and p-toluenesulfonic acid in S1 are added at one time; When the time t of the hyperbranching reaction exceeds 2h, S1 first divides 2-dihydroxymethylpropionic acid and p-toluenesulfonic acid equally into (n1+1) / 2 or n2 / 2 parts according to the amount, n1 is the time number when t only retains integers and is an odd number, and n2 is the time number when t only retains integers and is an even number, and then adds 1 part of 2-dihydroxymethylpropionic acid and 1 part of p-toluenesulfonic acid every 1h.

7. The method for preparing a photonic crystal film based on lignin nanoparticles according to claim 1, characterized in that: The hard transparent material described in S3 is a glass slide.

8. The method for preparing a photonic crystal film based on lignin nanoparticles according to claim 1, characterized in that: S3: adjusting the mass percentage of the modified lignin nanoparticles in the aqueous dispersion of the modified lignin nanoparticles to 0.01%-2%, and then dripping the modified lignin nanoparticles onto the hard transparent material, so that a photonic crystal film based on the lignin nanoparticles is formed on the hard transparent material.

9. The method for preparing a photonic crystal film based on lignin nanoparticles according to claim 8, characterized in that: The drying method described in S3 is drying in a forced air drying oven at 30°C-150°C for 30 minutes-12 hours.

10. A photonic crystal film based on lignin nanoparticles obtained by the preparation method of the photonic crystal film based on lignin nanoparticles according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Method for preparing photonic crystal material through ordered self-assembly of emulsion

    CN111363189A

  • Preparation method of responsive structural color optically variable anti-counterfeiting coating

    CN112126322A

  • Photonic crystal structural color material based on natural polymer material and preparation method thereof

    CN118444413A

  • Corn-based plastics reinforced by lignin and cellulose nanofibrils

    US20230340235A1

  • Transparent and homogenous cellulose nanocrystal-lignin UV protection films

    WO2019183166A1