Preparation method of modified gallium-adsorbing microporous chelating resin based on polyhedral oligomeric silsesquioxane
The preparation of microporous chelating resins by cage polysilsesquioxane modification solves the problems of unstable resin strength and difficulty in controlling pore structure in the prior art, achieves efficient and long-term adsorption of gallium and improves gallium recovery efficiency and service life of the resin.
Patent Information
- Application Number
- CN202411015948.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The strength of the existing chelating resins is unstable during the gallium recovery process and the pore structure is difficult to control, resulting in a decrease in the adsorption rate and saturation adsorption amount, especially when the pH value is less than 5, which affects the recovery efficiency of gallium.
The microporous chelating resin is prepared by cage polysilsesquioxane (POSS) modification. By modifying the copolymerized porous beads and aminoxime matrices, the strength and pore structure density of the resin are improved, and the adsorption rate of gallium is increased and the adsorption rate of gallium is increased. Saturated adsorption amount.
It significantly improves the adsorption rate and saturated adsorption amount of gallium, ensures efficient and long-term recovery of gallium, and maintains efficient adsorption capacity in low-concentration gallium solutions, extending the service life of the resin.
Smart Images

Figure CN118955996A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a preparation method of a gallium-adsorbing microporous chelating resin modified by cage-type polysilsesquioxane, and belongs to the field of material preparation. Background Art
[0002] As an important rare metal, gallium is widely used in aerospace, electronics, communications, and especially in the current new energy materials and devices. However, gallium can hardly be independently ore-formed, and it is always associated with bauxite. Currently, more than 90% of the gallium metal in the world is extracted from the circulating mother liquor of the Bayer process of bauxite, and almost more than 90% of the gallium metal extraction industry is in China. Among the currently industrialized process methods, the use of acid-based chelating resin to absorb and recover gallium has the advantages of simple process, low requirements for gallium metal concentration in the circulating mother liquor, high recovery rate, and easy large-scale industrial production, and is the most widely used.
[0003] The chelating resins currently used in China are all prepared by a two-step process. First, acrylonitrile (AN) and divinylbenzene (DVB) binary copolymer is used as the skeleton sphere, and then the surface of the sphere is amine-oximinated in the second step to make the surface of the sphere contain oxime groups (~N-OH) and amine groups (-NH2). The amine-oximinated beads use oxime groups (~N-OH) and amine groups (-NH2) to complex the gallium metal in the Bayer process circulating mother liquor and recover the gallium.
[0004] At present, the research on chelating resins is focused on the equipment and process of binary copolymerization of acrylonitrile (AN) and divinylbenzene (DVB). However, the chelating resin prepared by this process not only has unstable bead strength, but also has difficult to control surface pore structure. Uniform pore structure and high bead strength are important factors for improving gallium adsorption rate and saturated adsorption capacity.
[0005] At present, the pore structure of chelating resin is controlled by using only a certain amount of porogen. However, due to its own insufficient strength during use, the bead resin itself is very easy to shrink and deform after repeated use. After 15 adsorption cycles, the saturated adsorption capacity of the resin decreases by more than 50%-70%.
[0006] It is particularly important that bauxite, especially foreign bauxite, contains complex amine organic matter, which can easily cause the decrease of gallium adsorption by chelating resin, especially when the pH value is less than 5, the chelating resin ages quickly, and the root cause of this failure is the failure of the pore structure caused by the collapse of the resin beads. Therefore, seeking a high-strength new microporous chelating resin for efficient and long-term adsorption of gallium in the Bayer process circulating mother liquor has become one of the important research directions of the current gallium recovery industry.
[0007] At present, the strength and pore structure of chelating resin can only be effectively controlled by adjusting the ratio of monomer to porogen during the polymerization process. There is no ideal and controllable method for preparing microporous chelating resin in the prior art.
[0008] POSS is a cage-type polysilsesquioxane, with the general formula (RSiO3 / 2)n, where R is the group connected by the eight corner Si atoms. The inorganic core is composed of a silicon-oxygen skeleton alternately connected by Si-O, and its three-dimensional size is between 1 and 3 nm. The Si atoms as a cage structure not only have excellent acid and alkali resistance, but also the R groups at the eight corners have strong reactivity. There are no reports on the modification of cage-type polysilsesquioxane to improve the strength of chelating resin and its pore structure. Summary of the invention
[0009] The invention provides a preparation method of a microporous chelating resin for adsorbing gallium modified by cage-type polysilsesquioxane, so as to improve the strength of the chelating resin and the adsorption-desorption rate of gallium in a Bayer process circulating mother liquor by the chelating resin without affecting the saturated adsorption amount of gallium by the microporous chelating resin.
[0010] In order to solve the above problems, a preparation method of a microporous chelating resin for adsorption of gallium modified by cage-type polysilsesquioxane is proposed. The method includes two parts: preparation of modified copolymer porous beads and amine oxime treatment of the beads.
[0011] The raw materials for preparing the modified copolymer porous beads include, by weight, 6-35% of multi-monomers, 1-3% of modified monomers, 5-25% of porogens, 0.5-5% of initiators accounting for the total weight of the multi-monomers, 0.5-10% of dispersants and 25-85% of salt water;
[0012] The multi-monomer comprises a main monomer and a cross-linking monomer. The main monomer is at least one of styrene, acrylic acid, acrylonitrile, methyl methacrylate and hydroxyethyl methacrylate, accounting for 5-25% of the total mass fraction; the cross-linking monomer is at least one of divinylbenzene, butylated acrylamide, N-butoxymethyl acrylamide and hydroxyethyl acrylamide, accounting for 1-10% of the total mass fraction; the modified monomer is at least one of octavinyl silsesquioxane and epoxy polyhedral oligomeric cage-type polysilsesquioxane; the porogen is at least one of toluene, paraffin, xylene and aviation kerosene; the initiator is one of benzoyl peroxide and azobisisobutyronitrile or a combination of two of them; the salt water is one of calcium chloride and sodium chloride aqueous solution or both, and the purity thereof is above 99%; the dispersant is one of gelatin and polyvinyl alcohol or both of them.
[0013] The preparation process of the modified copolymer porous beads specifically includes the following steps:
[0014] Step 1: first, add the modified monomer, salt water and dispersant in a certain proportion into a reaction kettle in order, stir the whole system for 30 minutes to completely dissolve, then evenly mix the main monomer, cross-linking monomer, porogen and initiator in a certain proportion and add them, and then polymerize the whole system by staged temperature increase polymerization;
[0015] Step 2: neutralize the solution after the reaction, separate the polymerized beads from the solution using a sieve, remove the porogen, wash and dry the beads, and then sieve to obtain copolymer porous beads.
[0016] According to the mass percentage, the raw materials for the oximation of beads include 15-35% of copolymer porous beads, 40-65% of reaction medium, 10-25% of oximation auxiliary agent, and 5-10% of cleaning agent.
[0017] The reaction medium is one or both of water and ethanol, the amine oximation auxiliary agent is one or both of hydroxylamine hydrochloride and hydroxylamine sulfate, and the cleaning agent is deionized water or 8% sodium hydroxide aqueous solution.
[0018] The amidoximation process for preparing the modified porous beads comprises the following steps:
[0019] Step 3: Add the modified copolymer porous beads obtained in step 2 to the reaction medium in a certain proportion, slowly stir at 30-40°C for 1-2 hours to fully swell the pore structure of the beads, then increase the stirring speed, heat to 75-80°C, add the oximation reagent, and keep the temperature for 10-12 hours. After the reaction is completed, cool the reaction system to 30-40°C;
[0020] Step 4: Discharge the mixed solution obtained in step 3 under stirring, filter out the solution with a filter, and then wash the obtained product with water for multiple times until the pH value is 7, wherein the product is washed with deionized water, and then filtered to dry the water, and air-dried at low temperature to obtain a cage-type polysilsesquioxane-modified adsorbed gallium chelate microporous bead resin.
[0021] In step 1, the polymerization is carried out by a staged temperature increase polymerization method, wherein the whole system is rapidly heated to 75±2°C and kept warm for 2-3 hours; then heated to 85°C±2°C and kept warm for 2-3 hours; finally heated to 95±2°C and kept warm for 2-3 hours.
[0022] In step 2, the particle size is screened to obtain copolymer porous beads, and the diameter of the beads obtained after screening is less than 50 μm.
[0023] In the above preparation method, the stirring paddle of the reactor used in step 1 should prevent the material from sinking, and salt water should be added first and then the dispersant, and the modifier should be added after the dispersion is uniform.
[0024] In the above preparation method, in step 1, the main monomer and the cross-linking monomer must be deblocked with 5-10% sodium hydroxide solution before use.
[0025] Compared with the prior art, the microporous chelating resin prepared by the invention has a saturated adsorption capacity of 12 mg / L-18 mg / L for metal gallium in the Bayer process circulating mother liquor, an effective resolution rate of more than 86%, and a mother liquor with a low concentration of gallium will not affect the saturated adsorption capacity of the microporous chelating resin. The use of the modified monomer polyhedral oligomeric cage-type polysilsesquioxane can not only effectively improve the strength of the spherical resin, but also promote the formation of a dense microporous structure of the sphere. The dense pore structure formed after the cage-type polysilsesquioxane modification can not only greatly improve the strength of the chelating resin beads, but also improve the adsorption rate and adsorption capacity of the chelating resin for gallium in the bauxite Bayer process solution, and effectively improve the resolution efficiency. The social and economic benefits are remarkable, and the invention has important guiding significance and promotion value. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 The microscopic morphology and partial magnification of the porous microspheres modified by octavinyl POSS with amine oxime;
[0027] Figure 2 It is the FT-IR spectrum of the octavinyl POSS modified porous microspheres with amine oxime;
[0028] Figure 3 This is the gallium adsorption performance curve of the porous microspheres modified with octavinyl POSS modified with amine oxime;
[0029] Figure 4 It is the morphology comparison of the amine oxime porous microspheres before and after modification (after 15 cycles of use); DETAILED DESCRIPTION
[0030] In order to make the objectives, technical solutions and advantages of the present invention more clear, the present invention will be further described in detail below in conjunction with the accompanying drawings. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0031] Example 1
[0032] This embodiment is aimed at improving the microporous chelating resin. The specific operation points of the preparation method of the improved microporous chelating resin are as follows: (Steps 1 to 4 are the preparation of modified copolymer porous microspheres, and steps 5 to 6 are the amidoximation of the microspheres, and the microspheres refer to the beads mentioned above)
[0033] Step 1: Add 25 parts of deionized water, 10 parts of CaCl2, 3 parts of NaCl, and then 2 parts of gelatin into the reactor according to mass fraction, slowly stir until the gelatin is fully dissolved, then add 3 parts of glycidyl polyhedral silsesquioxane (epoxy POSS), stir for 30 minutes and heat the reactor to 35-55°C.
[0034] Step 2: Add 25 parts of deionized water, 20 parts of acrylonitrile, 3 parts of divinylbenzene, 2 parts of hydroxyethyl acrylamide, 2.5 parts of toluene, 3.5 parts of aviation kerosene, 0.5 parts of benzoyl peroxide, and 0.5 parts of azobisisobutyronitrile into the batching kettle, and control the temperature at 35-55°C until all materials are fully dissolved.
[0035] Step 3: Pour all the materials in the batching kettle into the reactor, quickly heat the reaction system to 75±2℃, and keep it warm for 2-3 hours; then heat it to 85℃±2℃, and keep it warm for 2-3 hours; finally heat it to 95±2℃, and keep it warm for 2-3 hours.
[0036] Step 4: After the reaction is completed, the material obtained in step 3 is discharged, and then repeatedly washed with 30-40°C warm water, and filtered with a filter with a filter to fully dissolve and remove the porogen. Finally, the beads are dried by air flow and sieved with a dryer at low temperature to obtain copolymer porous microspheres.
[0037] Step 5: Add 30 parts of porous microspheres, 10 parts of ethanol, 5 parts of chloroform, and 20 parts of deionized water to the reactor, and stir at 30°C for 3 hours to fully swell the microspheres; add 15 parts of hydroxylamine sulfate, 5 parts of hydroxylamine hydrochloride, 12 parts of sodium hydroxide, and 3 parts of sodium carbonate under stirring, and heat the reaction system to 50°C for 3 hours, and then heat it to 80°C for 10 hours to complete the reaction. Then cool it to below 30°C before discharging.
[0038] Step 6: After the reaction is completed, the material obtained in step 5 is discharged, and then repeatedly washed with 30-40℃ warm water, and filtered with a filter with a filter to fully dissolve and remove the porogen. Finally, the product is dried by air flow and sieved with a dryer at low temperature to obtain a product of 20-50 mesh, that is, the amine oxime porous microspheres are obtained. The saturated adsorption capacity of the modified gallium adsorption microporous chelating resin for metal gallium in the Bayer process circulating mother liquor reaches 18.02㎎ / L, and the effective resolution rate reaches 81.46%.
[0039] The numbers of parts mentioned in the above steps are all by mass.
[0040] Embodiment 2:
[0041] Step 1: Add 25 parts of deionized water, 10 parts of CaCl2, 3 parts of NaCl, and then 2 parts of gelatin into the reactor by mass fraction, slowly stir until the gelatin is fully dissolved, add 3 parts of octavinyl cage-type polysilsesquioxane (octavinyl POSS), stir for 30 minutes, and then heat the reactor to 35-55°C.
[0042] Step 2: Add 25 parts of deionized water, 20 parts of acrylonitrile, 3 parts of divinylbenzene, 1 part of hydroxyethyl acrylamide, 1 part of butylated acrylamide, 2.5 parts of toluene, 3.5 parts of aviation kerosene, 0.5 parts of benzoyl peroxide, and 0.5 parts of azobisisobutyronitrile into the batching kettle, and control the temperature at 35-55°C until all materials are fully dissolved.
[0043] Step 3: Pour all the materials in the batching kettle into the reactor, quickly heat the reaction system to 75±2℃, and keep it warm for 2-3 hours; then heat it to 85℃±2℃, and keep it warm for 2-3 hours; finally heat it to 95±2℃, and keep it warm for 2-3 hours.
[0044] Step 4: After the reaction is completed, the material obtained in step 3 is discharged, and then repeatedly washed with 30-40°C warm water, and filtered with a filter with a filter to fully dissolve and remove the porogen. Finally, the beads are dried by air flow and sieved with a dryer at low temperature to obtain copolymer porous microspheres.
[0045] Step 5: Add 35 parts of porous microspheres, 10 parts of ethanol, and 20 parts of deionized water to the reactor, and stir at 30°C for 3 hours to fully swell the microspheres; add 15 parts of hydroxylamine sulfate, 5 parts of hydroxylamine hydrochloride, 10 parts of sodium hydroxide, and 3 parts of sodium carbonate under stirring, and heat the reaction system to 50°C for 3 hours, and then heat to 80°C for 10 hours to complete the reaction. Then cool to below 30°C before discharging.
[0046] Step 6: After the reaction is completed, the material obtained in step 5 is discharged, and then repeatedly washed with 30-40°C warm water, and filtered with a filter with a filter to fully dissolve and remove the porogen. Finally, the product is dried by air flow and sieved at low temperature in a dryer to obtain a 20-50 mesh product, and the amine oxime porous microspheres are obtained. The surface of the modified gallium adsorption microporous chelating resin obtained has a dense microporous structure ( Figure 1 ), the microsphere surface is rich in amine oxime groups ( Figure 2 ) can effectively complex and adsorb gallium in the solution. The resin has a fast adsorption rate for gallium, and the adsorption rate in 20 minutes is close to 80% ( Figure 3), after 60 minutes, the adsorption equilibrium was basically reached, and the adsorption rate was 86.34%; the saturated adsorption of metal gallium in the Bayer process circulating mother liquor reached 17.78 mg / L, and the effective resolution rate reached 86.12%. The strength of the porous microspheres was significantly improved after octavinyl POSS modification. After 15 cycles of use, the original microsphere morphology was still basically maintained, while the unmodified porous microspheres had completely collapsed ( Figure 4 ).
[0047] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a gallium-adsorbing microporous chelating resin modified by cage-type polysilsesquioxane, characterized in that: The method comprises two parts: preparation of modified copolymer porous beads and amine oxime treatment of the beads.
2. A method for preparing a gallium adsorbing microporous chelating resin modified by cage-type polysilsesquioxane according to claim 1, characterized in that: The raw materials for preparing the modified copolymer porous beads include 6-35% of multi-monomers, 1-3% of modified monomers, 5-25% of porogens, 0.5-5% of initiators accounting for the total weight of the multi-monomers, 0.5-10% of dispersants, 8-15% of salts and 40-60% of deionized water.
3. A method for preparing a gallium adsorbing microporous chelating resin modified by cage-type polysilsesquioxane according to claim 2, characterized in that: The multi-monomer comprises a main monomer and a cross-linking monomer. The main monomer is at least one of styrene, acrylic acid, acrylonitrile, methyl methacrylate and hydroxyethyl methacrylate, accounting for 5-25% of the total mass fraction; the cross-linking monomer is at least one of divinylbenzene, butylated acrylamide, N-butoxymethyl acrylamide and hydroxyethyl acrylamide, accounting for 1-10% of the total mass fraction; the modified monomer is at least one of octavinyl silsesquioxane and epoxy polyhedral oligomeric cage-type polysilsesquioxane; the porogen is at least one of toluene, paraffin, xylene and aviation kerosene; the initiator is one of benzoyl peroxide and azobisisobutyronitrile or a combination of two of them; the salt water is one of calcium chloride and sodium chloride aqueous solution or both, and the purity thereof is above 99%; the dispersant is one of gelatin and polyvinyl alcohol or both of them.
4. A method for preparing a gallium adsorbing microporous chelating resin modified by cage-type polysilsesquioxane according to claim 1, characterized in that: The preparation process of the modified copolymer porous beads specifically includes the following steps: Step 1: first, add the modified monomer, salt water and dispersant in a certain proportion into a reaction kettle in order, stir the whole system for 30 minutes to completely dissolve, then evenly mix the main monomer, cross-linking monomer, porogen and initiator in a certain proportion and add them, and then polymerize the whole system by staged temperature increase polymerization; Step 2: neutralize the solution after the reaction, separate the polymerized beads from the solution using a sieve, remove the porogen, wash and dry the beads, and then sieve to obtain copolymer porous beads.
5. A method for preparing a gallium-adsorbing microporous chelating resin modified by cage-type polysilsesquioxane according to claim 4, characterized in that: In step 1, the polymerization is carried out by a staged temperature increase polymerization method, wherein the whole system is rapidly heated to 75±2°C and kept warm for 2-3 hours; then heated to 85°C±2°C and kept warm for 2-3 hours; finally heated to 95±2°C and kept warm for 2-3 hours.
6. A method for preparing a gallium-adsorbing microporous chelating resin modified by cage-type polysilsesquioxane according to claim 4, characterized in that: In step 2, the particle size is screened to obtain copolymer porous beads, and the diameter of the beads obtained after screening is less than 50 μm.
7. A method for preparing a gallium-adsorbing microporous chelating resin modified by cage-type polysilsesquioxane according to claim 1, characterized in that: In the above preparation method, the stirring paddle of the reactor used in step 1 should prevent the material from sinking, and salt water should be added first and then the dispersant. After uniform dispersion, the modifier, main monomer and cross-linking monomer are added and used after deblocking with 5-10% sodium hydroxide solution.
8. A method for preparing a gallium-adsorbing microporous chelating resin modified by cage-type polysilsesquioxane according to claim 1, characterized in that: By weight, the raw materials for the oximation of beads include 15-35% of copolymeric porous beads, 40-65% of reaction medium, 10-25% of oximation auxiliary agent, and 5-10% of cleaning agent.
9. A method for preparing a gallium-adsorbing microporous chelating resin modified by cage-type polysilsesquioxane according to claim 5, characterized in that: The reaction medium is one or both of water and ethanol, the amine oximation auxiliary agent is one or both of hydroxylamine hydrochloride and hydroxylamine sulfate, and the cleaning agent is deionized water or 8% sodium hydroxide aqueous solution.
10. A method for preparing a gallium-adsorbing microporous chelating resin modified by cage-type polysilsesquioxane according to claim 1, characterized in that: The amidoximation process for preparing the modified porous beads comprises the following steps: Step 3: Add the modified copolymer porous beads obtained in step 2 to the reaction medium in a certain proportion, slowly stir at 30-40°C for 1-2 hours to fully swell the pore structure of the beads, then increase the stirring speed, heat to 75-80°C, add the oximation reagent, and keep the temperature for 10-12 hours. After the reaction is completed, cool the reaction system to 30-40°C; Step 4: Discharge the mixed solution obtained in step 3 under stirring, filter out the solution with a filter, and then wash the obtained product with water for multiple times until the pH value is 7, and then filter and dry the water, and air-dry at low temperature to obtain a cage-type polysilsesquioxane-modified gallium-adsorbing chelating microporous bead resin.
Citation Information
Cited By
Method for separating gallium and germanium from zinc slag and purifying gallium
CN120350254A