PVC (polyvinyl chloride) pipe with high organic reagent resistance and preparation method of PVC pipe

By using acrylate-N-(hydroxymethyl)acrylamide copolymer to modify raw materials such as polytetrafluoroethylene and epoxy acrylate in PVC pipes, the corrosion resistance and impact resistance of PVC resin are enhanced, and PVC is solved The problem of swelling of the pipe in organic solvents has achieved better corrosion resistance and impact resistance.

CN118956070APending Publication Date: 2024-11-15NANYANG SENYUAN PLASTIC
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411043144.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

PVC pipes have poor corrosion resistance when they come into contact with organic solvents, which are prone to swelling or dissolution, affecting their impact resistance and toughness.

Method used

Use acrylate-N-(hydroxymethyl)acrylamide copolymer to modify polytetrafluoroethylene, epoxy acrylate, ACR resin, CPE resin, light calcium carbonate, stabilizer, antioxidant and other raw materials to uniformly disperse Reaction with cross-linking enhances the corrosion resistance and impact resistance of PVC resin, and ensures the uniformity and appearance of the finished product by controlling the temperature and rotation speed of the extruder.

Benefits of technology

It significantly improves the corrosion resistance and impact resistance of PVC pipes, enhances their resistance to organic solvents, while maintaining impact strength and toughness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004972862110000071
    Figure BDA0004972862110000071
  • Figure BDA0004972862110000081
    Figure BDA0004972862110000081
Patent Text Reader

Abstract

The invention relates to the technical field of PVC (polyvinyl chloride) pipes, and particularly discloses a PVC pipe with high organic reagent resistance and a preparation method of the PVC pipe. The PVC pipe with strong organic reagent resistance is prepared from the following raw materials: PVC resin, acrylate-N-(hydroxymethyl) acrylamide copolymer modified polytetrafluoroethylene, epoxy acrylate, ACR resin, CPE resin, light calcium carbonate, a stabilizer, a lubricant, a whitening agent and an antioxidant. According to the invention, the corrosion resistance of the matrix resin is enhanced by modifying polytetrafluoroethylene with the acrylate-N-(hydroxymethyl) acrylamide copolymer. Wherein the acrylate-N-(hydroxymethyl) acrylamide copolymer modified polytetrafluoroethylene can be uniformly dispersed into the polyvinyl chloride matrix resin, and the epoxy acrylate and the acrylate-N-(hydroxymethyl) acrylamide copolymer modified polytetrafluoroethylene have a synergistic effect; the crosslinking degree of the acrylate-N-(hydroxymethyl) acrylamide copolymer modified polytetrafluoroethylene and the polyvinyl chloride matrix resin is increased, so that the pipe has excellent corrosion resistance, and the impact strength and toughness of the pipe are not influenced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of PVC pipes, and in particular to a PVC pipe with strong organic reagent resistance and a preparation method thereof. Background Art

[0002] As one of the most in-demand general-purpose plastics in the world, polyvinyl chloride (PVC) resin plays an extremely important role in the fields of construction, food, military industry, aerospace, etc. due to its low cost and excellent processing performance. However, due to the unstable structures such as side chains, double bonds, tertiary chlorine and allyl chloride in PVC resin, PVC materials have defects such as poor thermal stability, easy degradation and poor impact resistance, which limits its further development. Therefore, modifying PVC resin can improve its performance defects and give it excellent comprehensive performance, thereby further broadening its application fields.

[0003] Since PVC is a brittle material at low temperatures, it is easy to form notches or cracks under the impact of stress. By adding impact modifiers, it can absorb impact energy and prevent the development of cracks, thereby improving the impact resistance of PVC pipes. However, the addition of impact modifiers may affect the intermolecular forces of PVC to a certain extent, making its distribution uneven, thus forming local weaknesses. When these local weaknesses come into contact with organic solvents, they are prone to swelling or dissolution, thereby affecting its resistance to organic solvents. Summary of the invention

[0004] In order to improve the problem of poor organic solvent resistance of PVC pipes in the related art, the present application provides a PVC pipe with strong organic solvent resistance and a preparation method thereof.

[0005] In the first aspect, the present application provides a PVC pipe with strong resistance to organic reagents, which adopts the following technical solution: a PVC pipe with strong resistance to organic reagents, comprising the following raw materials by weight: PVC resin 80-100 parts; 5-7 parts of polytetrafluoroethylene modified by acrylate-N-(hydroxymethyl)acrylamide copolymer; Epoxy acrylate 4-6 parts; 6-8 parts of ACR resin; 8-12 parts of CPE resin; Light calcium carbonate 7-10 parts; 3-4 parts of stabilizer; Lubricant 0.4-0.8 parts; Brightener 2.4-2.8 parts; Antioxidant 1.0-1.4 parts.

[0006] By adopting the above technical scheme, the pipe uses polyvinyl chloride as the base resin, ACR resin and CPE resin are used as impact modifiers of the polyvinyl chloride base resin, the corrosion resistance of the base resin is enhanced by modifying polytetrafluoroethylene through acrylate-N-(hydroxymethyl) acrylamide copolymer, light calcium carbonate plays the role of a skeleton, which is helpful to improve the dimensional stability of the PVC pipe, the stabilizer captures the HCl released by the PVC resin or can react with the unstable polyene structure generated by the PVC resin to prevent or reduce the decomposition of the PVC resin, the whitening agent plays a whitening role, and the antioxidant combines with free radicals to form a stable compound, thereby terminating the oxidative degradation reaction of the PVC resin. Among them, acrylate-N-(hydroxymethyl)acrylamide copolymer modified polytetrafluoroethylene can be evenly dispersed in the polyvinyl chloride base resin, and epoxy acrylate and acrylate-N-(hydroxymethyl)acrylamide copolymer modified polytetrafluoroethylene work synergistically to increase the crosslinking degree of acrylate-N-(hydroxymethyl)acrylamide copolymer modified polytetrafluoroethylene and the polyvinyl chloride base resin, so that the pipe has excellent corrosion resistance without affecting the impact strength and toughness of the pipe.

[0007] Preferably, the acrylate-N-(hydroxymethyl)acrylamide copolymer modified polytetrafluoroethylene includes polytetrafluoroethylene, acrylate, N-(hydroxymethyl)acrylamide, a sensitizer and a surfactant, and the weight ratio of the polytetrafluoroethylene, acrylate, N-(hydroxymethyl)acrylamide, sensitizer and surfactant is 6:(2.6-2.8):(1.3-1.4):(0.12-0.14):(0.1-0.2).

[0008] By adopting the above technical scheme, the acrylate-N-(hydroxymethyl) acrylamide copolymer modified polytetrafluoroethylene is prepared by using polytetrafluoroethylene, acrylate, N-(hydroxymethyl) acrylamide, sensitizer and surfactant. Among them, the surfactant forms a thin film on the surface of the liquid to change the molecular arrangement of the liquid surface, thereby reducing the surface tension, the sensitizer can reduce the potential energy of the grafting reaction and promote the grafting reaction, and the acrylate and N-(hydroxymethyl) acrylamide are linked to the polar functional groups by covalent bonds, which enhances the surface polarity of polytetrafluoroethylene and increases the surface energy, and can effectively improve the dispersion performance of polytetrafluoroethylene in the PVC matrix resin. In addition, the grafting of acrylate on polytetrafluoroethylene has a promoting effect on the grafting of N-(hydroxymethyl) acrylamide.

[0009] Preferably, the acrylic acid ester is at least one of hydroxyethyl methacrylate and hydroxypropyl acrylate.

[0010] By adopting the above technical solution, both hydroxyethyl methacrylate and hydroxypropyl acrylate molecules contain hydroxyl groups, and polar monomers exist in the molecular weight of polytetrafluoroethylene. These polar monomers can increase the interaction between molecules and promote the uniform dispersion of polytetrafluoroethylene. At the same time, polytetrafluoroethylene with a high grafting rate carries more charges. When the distance between particles increases, the charge repulsion rate can balance the gravity of the particles, so it has the effect of uniform dispersion.

[0011] Preferably, the epoxy acrylate is at least one of bisphenol A epoxy acrylate and bisphenol S epoxy acrylate.

[0012] By adopting the above technical scheme, the epoxy acrylate molecule contains epoxy groups and unsaturated double bonds, and the unsaturated double bonds in the epoxy acrylate ester-N-(hydroxymethyl) acrylamide copolymer modified polytetrafluoroethylene are combined with the unsaturated double bonds in the acrylate ester-N-(hydroxymethyl) acrylamide copolymer modified polytetrafluoroethylene. Through synergistic effect, the epoxy groups can undergo a ring-opening reaction to produce a planar adsorption effect, and cross-link to form a tight three-dimensional network structure, thereby improving the cross-linking degree between the acrylate ester-N-(hydroxymethyl) acrylamide copolymer modified polytetrafluoroethylene and the PVC resin, and further improving the corrosion resistance.

[0013] Preferably, the stabilizer comprises a combination of zinc stearate and calcium stearate, and the weight ratio of zinc stearate to calcium stearate is 1:(1-1.2).

[0014] By adopting the above technical scheme, the active and unstable chlorine atoms in the molecule can be replaced, the HC1 released during the processing can be absorbed or neutralized, the dehydrochlorination reaction can be inhibited, and the double bond addition reaction with the polyolefin structure can be carried out to capture free radicals and adsorb ionic impurities, thereby eliminating or slowing down the discoloration of PVC resin.

[0015] Preferably, the lubricant is at least one of polyethylene wax and stearic acid.

[0016] By adopting the above technical solution, the lubricant plays a lubricating role, reducing the friction between the polymer and the equipment, and the internal friction between the polymer molecular chains.

[0017] Preferably, the whitening agent is titanium dioxide with a particle size of 0.15-0.30 μm.

[0018] By adopting the above technical solution, the reflection and scattering of light by titanium dioxide particles will affect their whiteness value, and titanium dioxide within a certain particle size range has a higher whiteness value, obtaining a blue base phase, which has a shielding effect on yellowing resin.

[0019] Preferably, the antioxidant is a composition of bisphenol A and triphenyl phosphite, and the weight ratio of bisphenol A to triphenyl phosphite is 1:(1-1.5).

[0020] By adopting the above technical solution, bisphenol A is the main antioxidant and triphenyl phosphite is the auxiliary antioxidant. The main antioxidant acts as a chain breaker or eliminates free radicals. Its reaction mechanism is to combine with free radicals to form stable compounds to terminate the chain reaction. The main and auxiliary antioxidants can play a synergistic role.

[0021] In the second aspect, the present application provides a method for preparing a PVC pipe with strong resistance to organic reagents, which adopts the following technical solution: A method for preparing a PVC pipe with strong organic reagent resistance comprises the following steps: S1. PVC resin, acrylate-N-(hydroxymethyl) acrylamide copolymer modified polytetrafluoroethylene, epoxy acrylate, ACR resin, CPE resin, light calcium carbonate, stabilizer, polyethylene wax, stearic acid, titanium dioxide, antioxidant are mixed at high speed to 100-120°C, then mixed at low speed, cooled to 40-50°C and discharged for standby use; S2. The material is heated and extruded, and finally vacuum cooled and shaped to obtain a PVC pipe; The temperature range of the extrusion zone in S2 is 170-195°C, the speed of the extruder is 35-40r / min, and the feeding speed is 55-60r / min.

[0022] By adopting the above technical solution, the mixing speed and the temperature and rotation speed of the extruder are controlled during the preparation process, which is conducive to obtaining a PVC pipe with uniformity and good finished product appearance.

[0023] Preferably, the method for preparing the acrylate-N-(hydroxymethyl)acrylamide copolymer modified polytetrafluoroethylene comprises the following steps: Adding a surfactant to deionized water, stirring evenly, then adding polytetrafluoroethylene, stirring evenly to obtain a suspension, introducing nitrogen, then adding acrylate, N-(hydroxymethyl)acrylamide and a sensitizer to the suspension, heating to 60-70° C., stirring for 3-4 hours to obtain a modified solution, separating a precipitate from the modified solution, and drying to obtain acrylate-N-(hydroxymethyl)acrylamide copolymer modified polytetrafluoroethylene; The surfactant is benzalkonium chloride, and the sensitizer is concentrated sulfuric acid.

[0024] By adopting the above technical solution, benzalkonium chloride can effectively reduce the surface tension of water, and concentrated sulfuric acid can reduce the potential energy of the grafting reaction, thereby promoting the grafting reaction.

[0025] In summary, this application at least includes the following beneficial technical effects: In the present application, the pipe uses polyvinyl chloride as the base resin, ACR resin and CPE resin are used together as impact modifiers of the polyvinyl chloride base resin, the corrosion resistance of the base resin is enhanced by modifying polytetrafluoroethylene through acrylate-N-(hydroxymethyl)acrylamide copolymer, light calcium carbonate plays the role of a skeleton, which helps to improve the dimensional stability of the PVC pipe, the stabilizer captures the HCl released by the PVC resin or can react with the unstable polyene structure produced by the PVC resin to prevent or reduce the decomposition of the PVC resin, the whitening agent plays a whitening role, and the antioxidant combines with free radicals to form a stable compound, thereby terminating the oxidative degradation reaction of the PVC resin. Among them, acrylate-N-(hydroxymethyl)acrylamide copolymer modified polytetrafluoroethylene can be evenly dispersed in the polyvinyl chloride base resin, and epoxy acrylate and acrylate-N-(hydroxymethyl)acrylamide copolymer modified polytetrafluoroethylene work synergistically to increase the crosslinking degree of acrylate-N-(hydroxymethyl)acrylamide copolymer modified polytetrafluoroethylene and the polyvinyl chloride base resin, so that the pipe has excellent corrosion resistance without affecting the impact strength and toughness of the pipe. DETAILED DESCRIPTION

[0026] Preparation Example Preparation Example 1 Preparation of acrylate-N-(hydroxymethyl)acrylamide copolymer modified polytetrafluoroethylene: 0.1 kg of benzalkonium chloride was added to 100 kg of deionized water, and 6 kg of polytetrafluoroethylene was added after stirring, and nitrogen was introduced. 2.6 kg of acrylate, 1.3 kg of N-(hydroxymethyl)acrylamide and 0.12 kg of concentrated sulfuric acid were added to the suspension, and the mixture was heated to 60° C. and stirred for reaction for 3 hours to obtain a modified solution. A precipitate was separated from the modified solution, and the precipitate was dried to obtain acrylate-N-(hydroxymethyl)acrylamide copolymer modified polytetrafluoroethylene.

[0027] Preparation Example 2 Preparation of acrylate-N-(hydroxymethyl)acrylamide copolymer modified polytetrafluoroethylene: 0.2 kg of benzalkonium chloride was added to 100 kg of deionized water, and 6 kg of polytetrafluoroethylene was added after stirring, and nitrogen was introduced. 2.7 kg of acrylate, 1.4 kg of N-(hydroxymethyl)acrylamide and 0.13 kg of concentrated sulfuric acid were added to the suspension, and the mixture was heated to 65° C. and stirred for reaction for 3.5 hours to obtain a modified solution. A precipitate was separated from the modified solution, and the precipitate was dried to obtain acrylate-N-(hydroxymethyl)acrylamide copolymer modified polytetrafluoroethylene.

[0028] Preparation Example 3 Preparation of acrylate-N-(hydroxymethyl)acrylamide copolymer modified polytetrafluoroethylene: 0.2 kg of benzalkonium chloride was added to 100 kg of deionized water, and 6 kg of polytetrafluoroethylene was added after stirring, and a suspension was obtained. Nitrogen was introduced, and 2.8 kg of acrylate, 1.4 kg of N-(hydroxymethyl)acrylamide and 0.14 kg of concentrated sulfuric acid were added to the suspension. The suspension was heated to 70° C. and stirred for reaction for 4 hours to obtain a modified solution. A precipitate was separated from the modified solution, and the precipitate was dried to obtain acrylate-N-(hydroxymethyl)acrylamide copolymer modified polytetrafluoroethylene. Example

[0029] Example 1 A PVC pipe with strong resistance to organic reagents, comprising 80kg PVC resin (Huasu SG-5 type), 5kg acrylate-N-(hydroxymethyl) acrylamide copolymer modified polytetrafluoroethylene (acrylate-N-(hydroxymethyl) acrylamide copolymer modified polytetrafluoroethylene prepared in Preparation Example 1), 4kg bisphenol A epoxy acrylate (Hubei Yamade 71281-65-7), 6kg ACR resin (Messer New Material 630), 8kg CPE resin (Liaoyang Petrochemical L0555PX), 7kg light calcium carbonate, 1.5kg zinc stearate, 1.5kg calcium stearate, 0.4kg polyethylene wax, 2.4kg titanium dioxide (particle size 0.15μm), 0.5kg bisphenol A, and 0.5kg triphenyl phosphite.

[0030] The method for preparing the PVC pipe with strong resistance to organic reagents in this embodiment comprises the following steps: S1. PVC resin, acrylate-N-(hydroxymethyl) acrylamide copolymer modified polytetrafluoroethylene, epoxy acrylate, ACR resin, CPE resin, light calcium carbonate, zinc stearate and calcium stearate, polyethylene wax, titanium dioxide, bisphenol A and triphenyl phosphite are mixed at high speed to 100°C, then mixed at low speed, cooled to 40°C and discharged for use; S2. The material is heated and extruded to form, and finally vacuum cooled and formed to obtain a PVC pipe.

[0031] Among them, the temperature of the extruder barrel zone 1 is 185°C, the temperature of zone 2 is 190°C, the temperature of zone 3 is 180°C, and the temperature of zone 4 is 175°C. The temperature of the mold zone 1 is 175°C, the temperature of zone 2 is 180°C, the temperature of zone 3 is 190°C, and the temperature of zone 4 is 195°C. The extruder speed is 35.7r / min, and the feeding speed is 58r / min.

[0032] Example 2 A PVC pipe with strong resistance to organic reagents, comprising 90kg PVC resin (Huasu SG-5 type), 6kg acrylate-N-(hydroxymethyl) acrylamide copolymer modified polytetrafluoroethylene (acrylate-N-(hydroxymethyl) acrylamide copolymer modified polytetrafluoroethylene obtained in Preparation Example 2), 5kg bisphenol S epoxy acrylate (Wuhan Kemik KMK-1869), 7kg ACR resin (Messer New Material 630), 10kg CPE resin (Liaoyang Petrochemical L0555PX), 8kg light calcium carbonate, 1.4kg zinc stearate, 1.6kg calcium stearate, 0.5kg stearic acid, 2.6kg titanium dioxide (particle size 0.20μm), 0.5kg bisphenol A, and 0.7kg triphenyl phosphite.

[0033] The method for preparing the PVC pipe with strong resistance to organic reagents in this embodiment comprises the following steps: S1. PVC resin, acrylate-N-(hydroxymethyl) acrylamide copolymer modified polytetrafluoroethylene, epoxy acrylate, ACR resin, CPE resin, light calcium carbonate, zinc stearate and calcium stearate, stearic acid, titanium dioxide, bisphenol A and triphenyl phosphite are mixed at high speed to 110°C, then mixed at low speed, cooled to 45°C and discharged for standby use; S2. The material is heated and extruded to form, and finally vacuum cooled and formed to obtain a PVC pipe.

[0034] The temperature of the extruder barrel zone 1 is 170°C, the temperature of zone 2 is 180°C, the temperature of zone 3 is 175°C, and the temperature of zone 4 is 180°C. The temperature of the mold zone 1 is 175°C, the temperature of zone 2 is 180°C, the temperature of zone 3 is 185°C, and the temperature of zone 4 is 190°C. The extruder speed is 35r / min, and the feeding speed is 60r / min.

[0035] Example 3 A PVC pipe with strong resistance to organic reagents, comprising 100kg PVC resin (Huasu SG-5 type), 7kg acrylate-N-(hydroxymethyl) acrylamide copolymer modified polytetrafluoroethylene (acrylate-N-(hydroxymethyl) acrylamide copolymer modified polytetrafluoroethylene prepared in Preparation Example 3), 6kg bisphenol A epoxy acrylate (Hubei Yamade 71281-65-7), 8kg ACR resin (Messer New Material 630), 12kg CPE resin (Liaoyang Petrochemical L0555PX), 10kg light calcium carbonate, 1.3kg zinc stearate, 1.7kg calcium stearate, 0.8kg polyethylene wax, 2.8kg titanium dioxide (particle size 0.30μm), 0.6kg bisphenol A, and 0.8kg triphenyl phosphite.

[0036] The method for preparing the PVC pipe with strong resistance to organic reagents in this embodiment comprises the following steps: S1. PVC resin, acrylate-N-(hydroxymethyl) acrylamide copolymer modified polytetrafluoroethylene, epoxy acrylate, ACR resin, CPE resin, light calcium carbonate, zinc stearate and calcium stearate, polyethylene wax, titanium dioxide, bisphenol A and triphenyl phosphite are mixed at high speed to 120°C, then mixed at low speed, cooled to 50°C and discharged for standby use; S2. The material is heated and extruded to form, and finally vacuum cooled and formed to obtain a PVC pipe.

[0037] Among them, the temperature of the extruder barrel zone 1 is 175°C, the temperature of zone 2 is 185°C, the temperature of zone 3 is 1180°C, and the temperature of zone 4 is 185°C. The temperature of the mold zone 1 is 180°C, the temperature of zone 2 is 185°C, the temperature of zone 3 is 190°C, and the temperature of zone 4 is 195°C. The extruder speed is 40r / min, and the feeding speed is 55r / min.

[0038] Comparative Example Comparative Example 1 A PVC pipe with strong resistance to organic reagents, which differs from Example 1 in that the acrylate-N-(hydroxymethyl)acrylamide copolymer modified polytetrafluoroethylene is replaced by an equal amount of polytetrafluoroethylene.

[0039] Comparative Example 2 A PVC pipe with strong resistance to organic reagents, which differs from Example 1 in that hydroxyethyl methacrylate is used alone to modify polytetrafluoroethylene.

[0040] Comparative Example 3 A PVC pipe with strong resistance to organic reagents, which differs from Example 1 in that N-(hydroxymethyl)acrylamide is used alone to modify polytetrafluoroethylene.

[0041] Comparative Example 4 A PVC pipe with strong resistance to organic reagents, which differs from Example 1 in that the acrylate in the acrylate-N-(hydroxymethyl)acrylamide copolymer uses an equal amount of isooctyl acrylate instead of hydroxyethyl methacrylate.

[0042] Comparative Example 5 A PVC pipe with strong resistance to organic reagents, which differs from Example 1 in that bisphenol A epoxy acrylate is not added.

[0043] Performance testing 1. Organic solvent resistance test: Soak the samples in ethanol, acetone and tetrahydrofuran respectively, and observe whether the samples have any corrosion phenomenon.

[0044] 2. Acid and alkali resistance test: Use 10% hydrochloric acid and 40% sodium hydroxide to test the acid and alkali resistance of the samples.

[0045] 3. Impact resistance test: refer to the international standard GB / T 1843-2008 "Determination of plastic cantilever beam impact strength" method for measurement. Before the test, the sample is placed at a temperature of 23°C and a relative humidity of 50% for 20 hours. Notch type: Type A, 6 parallel groups, take the average value.

[0046] 4. Tensile properties test: refer to the national standard GB / T 5836.1-2018 "Rigid polyvinyl chloride (PVC-U) pipes for building drainage" and GB / T1040.2-2022 "Determination of tensile properties of plastics Part 2: Test conditions for molded and extruded plastics" method for testing; the test specimen is a 1A dumbbell type with a thickness of 4mm and a test speed of 50mm / min. Before the test, the sample is regulated at a constant temperature of 23°C and a relative humidity of 50% for 24 hours, and 6 parallel groups are tested to take the average value.

[0047] Table 1 According to the comparison between Example 1 and Comparative Example 1 and the data in Table 1, it can be seen that when polytetrafluoroethylene is directly added to the raw material without modification, the dispersion performance of polytetrafluoroethylene in the PVC matrix resin is poor, thereby forming local weaknesses of the PVC pipe, and the phenomenon of local swelling corrosion occurs, resulting in a significant decrease in the corrosion resistance of the PVC pipe, and causing a significant decrease in the impact resistance and tensile properties of the pipe.

[0048] According to the comparison between Example 1 and Comparative Examples 2-3 and the data in Table 1, when hydroxyethyl methacrylate is used alone to modify polytetrafluoroethylene, the peroxy radicals of polytetrafluoroethylene will produce free hydroxyl radicals and chain transfer reactions when hydroxyethyl methacrylate is grafted on the surface of polytetrafluoroethylene, which will cause homopolymerization, consume the grafted monomers in the reaction solution, increase the viscosity of the solution, and make it difficult for the active sites on the surface of polytetrafluoroethylene to diffuse. When N-(hydroxymethyl)acrylamide is used alone to modify polytetrafluoroethylene, N-(hydroxymethyl)acrylamide has poor compatibility with non-polar polytetrafluoroethylene and cannot fully contact, resulting in a low grafting rate of polytetrafluoroethylene. Only by using hydroxyethyl methacrylate and N-(hydroxymethyl)acrylamide to modify polytetrafluoroethylene at the same time, and making hydroxyethyl methacrylate and N-(hydroxymethyl)acrylamide form a copolymer and graft it on the surface of polytetrafluoroethylene, can the effect of uniform dispersion be achieved. In addition, hydroxyethyl methacrylate has a promoting effect on the grafting of N-(hydroxymethyl)acrylamide, which is beneficial to increase the grafting rate.

[0049] According to the comparison between Example 1 and Comparative Example 4 and the data in Table 1, it can be seen that the acrylate in the acrylate-N-(hydroxymethyl)acrylamide copolymer is affected by the number of alkyl carbon atoms. As the number of carbon atoms increases, the shielding effect on other polar groups increases, thereby weakening the intermolecular force, resulting in a decrease in the dispersion performance of polytetrafluoroethylene, forming a local weakness of the PVC pipe, and reducing the pipe's resistance to organic reagents.

[0050] According to the comparison between Example 1 and Comparative Example 5 and the data in Table 1, it can be seen that the synergistic effect of epoxy acrylate and acrylate-N-(hydroxymethyl) acrylamide copolymer can increase the crosslinking degree of polytetrafluoroethylene and PVC resin, and further improve the corrosion resistance of PVC pipes.

[0051] This specific implementation manner is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make non-creative modifications to the specific implementation manner as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A PVC pipe with strong resistance to organic reagents, characterized in that: By weight, it contains the following raw materials: PVC resin 80-100 parts; 5-7 parts of polytetrafluoroethylene modified by acrylate-N-(hydroxymethyl)acrylamide copolymer; Epoxy acrylate 4-6 parts; 6-8 parts of ACR resin; 8-12 parts of CPE resin; Light calcium carbonate 7-10 parts; 3-4 parts of stabilizer; Lubricant 0.4-0.8 parts; Brightener 2.4-2.8 parts; Antioxidant 1.0-1.4 parts.

2. The PVC pipe with strong resistance to organic reagents according to claim 1, characterized in that: The acrylate-N-(hydroxymethyl)acrylamide copolymer modified polytetrafluoroethylene comprises polytetrafluoroethylene, acrylate, N-(hydroxymethyl)acrylamide, a sensitizer and a surfactant, and the weight ratio of the polytetrafluoroethylene, acrylate, N-(hydroxymethyl)acrylamide, the sensitizer and the surfactant is 6: (2.6-2.8): (1.3-1.4): (0.12-0.14): (0.1-0.2).

3. The PVC pipe with strong resistance to organic reagents according to claim 1, characterized in that: The acrylic acid ester is at least one of hydroxyethyl methacrylate and hydroxypropyl acrylate.

4. The PVC pipe with strong resistance to organic reagents according to claim 1, characterized in that: The epoxy acrylate is at least one of bisphenol A epoxy acrylate and bisphenol S epoxy acrylate.

5. The PVC pipe with strong resistance to organic reagents according to claim 1, characterized in that: The stabilizer comprises a composition of zinc stearate and calcium stearate, wherein the weight ratio of the zinc stearate to the calcium stearate is 1:(1-1.2).

6. The PVC pipe with strong resistance to organic reagents according to claim 1, characterized in that: The lubricant is at least one of polyethylene wax and stearic acid.

7. The PVC pipe with strong resistance to organic reagents according to claim 1, characterized in that: The whitening agent is titanium dioxide with a particle size of 0.15-0.30 μm.

8. The PVC pipe with strong resistance to organic reagents according to claim 1, characterized in that: The antioxidant is a composition of bisphenol A and triphenyl phosphite, and the weight ratio of bisphenol A to triphenyl phosphite is 1:(1-1.5).

9. The method for preparing a PVC pipe with strong organic reagent resistance according to any one of claims 1 to 8, characterized in that: The following steps are involved: S1. PVC resin, acrylate-N-(hydroxymethyl) acrylamide copolymer modified polytetrafluoroethylene, epoxy acrylate, ACR resin, CPE resin, light calcium carbonate, stabilizer, polyethylene wax, stearic acid, titanium dioxide, antioxidant are mixed at high speed to 100-120°C, then mixed at low speed, cooled to 40-50°C and discharged for use; S2. The material is heated and extruded, and finally vacuum cooled and shaped to obtain a PVC pipe; The temperature range of the extrusion zone in S2 is 170-195°C, the speed of the extruder is 35-40r / min, and the feeding speed is 55-60r / min.

10. A PVC pipe with strong resistance to organic reagents according to any one of claim 9, characterized in that: The preparation method of the acrylate-N-(hydroxymethyl)acrylamide copolymer modified polytetrafluoroethylene comprises the following steps: Add surfactant to deionized water, stir evenly, then add polytetrafluoroethylene, stir evenly to obtain a suspension, introduce nitrogen, then add acrylate, N-(hydroxymethyl)acrylamide and sensitizer to the suspension, heat to 60-70°C, stir and react for 3-4 hours to obtain a modified solution, separate a precipitate from the modified solution, and dry to obtain acrylate-N-(hydroxymethyl)acrylamide copolymer modified polytetrafluoroethylene; The surfactant is benzalkonium chloride, and the sensitizer is concentrated sulfuric acid.

Citation Information

Cited By

  • Corrosion-resistant PVC-U drain pipe and preparation method thereof

    CN120349605A