Preparation method of surface functionalization modified CF / PPS composite material
By electrochemically depositing aminofunctional graphene on the surface of carbon fibers and grafting polyaniline nanofibers to form an amphiphilic interface layer, the problem of insufficient binding force between carbon fiber and PPS resin is solved, and the mechanical and electrical conductivity of the composite material is significantly improved.
Patent Information
- Application Number
- CN202411296174.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-18
- Publication Date
- 2024-11-15
AI Technical Summary
The interface bonding force of carbon fiber with PPS resin in PPS composite materials is insufficient, resulting in the mechanical properties of the composite materials being lower than the theoretical value. The existing surface modification methods may damage carbon fibers or reduce their performance.
Using the amphiphilic molecular structure design, the polyaniline nanofibers are grafted in situ on the surface of the carbon fiber to form the interface layer between graphene and polyaniline to enhance the compatibility and binding force of the carbon fiber with PPS resin. .
The tensile strength, elongation of break and thermal stability of carbon fiber reinforced PPS composite materials are significantly improved, the volume resistivity is reduced, and the overall mechanical and conductive properties are improved.
Smart Images

Figure CN118956154A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of composite materials, and in particular to a method for preparing a surface functionalized modified CF / PPS composite material. Background Art
[0002] Carbon fiber reinforced resin-based composite materials are favored by scientific research and industrial design fields due to their special advantages such as high strength, high modulus, light weight, and recyclability. They have broad application prospects in the fields of automobiles, sports, ships, aerospace, national defense, and wind power generation. Polyphenylene sulfide (PPS) is a special engineering plastic with excellent comprehensive performance. It has excellent crystallinity, heat resistance, chemical resistance, and low water absorption. PPS has become an important resin for carbon fiber reinforced composite materials. Carbon fiber reinforced PPS resin composite materials have been widely used by airlines such as Airbus and Boeing in secondary load-bearing structural components such as tail fins, rudder leading edges, and elevator auxiliaries.
[0003] However, due to the alternating arrangement of benzene rings and sulfur atoms in the main chain structure of PPS, without side chains and reactive groups, and the non-polarity and chemical inertness of the carbon fiber surface, the carbon fiber has poor wetting effect with PPS in the PPS composite material, the thermoplastic PPS resin matrix has weak bonding force with the carbon fiber, and the composite material cannot transfer load, resulting in poor mechanical properties of the composite material, which is far lower than the theoretical value. To this end, it is necessary to improve the wettability and compatibility of carbon fiber and PPS through interface optimization, improve the interfacial bonding force of carbon fiber and PPS resin, and achieve high performance of composite materials by improving the interfacial bonding strength of carbon fiber and PPS resin composite materials. So far, there are many methods for surface modification of carbon fiber, such as oxidation, plasma treatment, sizing and coating, chemical grafting, in-situ self-assembly, vapor deposition, etc. However, chemical treatment of carbon fiber surface will inevitably damage the carbon fiber due to surface "etching", and sizing and excessive increase in the bonding and adhesion between carbon fiber and PPS resin may make the interface phase brittle, resulting in performance degradation. The interface between carbon fiber and polymer resin is a key factor affecting resin composites. In order to further improve the performance of composites and obtain carbon fiber reinforced PPS resin composites with excellent performance to adapt to different product structures and use environments, in-depth research on carbon fiber surface modification and carbon fiber and PPS resin interface strength is very important to improve the performance of composites. Summary of the invention
[0004] The technical problem to be solved by the present invention is: to overcome the shortcomings of the prior art, to provide a method for preparing a surface functionalized modified CF / PPS composite material, to achieve surface functionalization modification of the carbon fiber by designing an amphiphilic molecular structure on the carbon fiber surface, to solve the interface compatibility and bonding strength problems between the carbon fiber and the PPS resin, thereby realizing the high performance of the carbon fiber reinforced PPS composite material.
[0005] The technical solution of the present invention is: The preparation method of the surface functionalized modified CF / PPS composite material comprises the following steps: adding polyphenylene sulfide resin, polyaniline-graphene functionalized surface modified carbon fiber and processing aid into a twin-screw extruder from a main feed port, a side feed port and a main feed port of the twin-screw extruder respectively, and performing melt blending, extrusion, strip drawing, cooling, pelletizing and drying through the twin-screw extruder to obtain the surface functionalized modified CF / PPS composite material.
[0006] Preferably, the added amount of polyphenylene sulfide resin is 68-90 parts, the added amount of polyaniline-graphene functionalized surface modified carbon fiber is 10-30 parts, and the added amount of processing aid is 1-1.3 parts.
[0007] Preferably, Figure 1 As shown, the preparation method of polyaniline-graphene functionalized surface modified carbon fiber comprises the following steps: S1 prepared graphene oxide (GO) by improving Hummer method; S2 uses graphene oxide as a precursor to synthesize amino-functionalized reduced graphene (ATRGO); S3 uses an electrochemical electrostatic deposition method to electrostatically deposit amino-functionalized reduced graphene on the surface of carbon fiber to obtain amino-functionalized reduced graphene-coated carbon fiber (CF-ATRGO); S4 in situ grafted polyaniline nanofibers onto the surface of amino-functionalized reduced graphene-coated carbon fibers to obtain polyaniline-graphene functionalized surface-modified carbon fibers (CF-RGO-PANI).
[0008] Preferably, the specific operation of step S1 is: adding concentrated sulfuric acid to graphite powder and sodium nitrate, keeping the temperature below 20°C, adding potassium permanganate with stirring, stirring to obtain a mixture, then adding deionized water, controlling the temperature below 100°C, adding H2O2 solution after the reaction to obtain a graphene oxide suspension, filtering and washing until the filtrate is neutral, and freeze-drying the product under reduced pressure to obtain graphene oxide; the mass volume ratio of graphite powder, sodium nitrate, concentrated sulfuric acid, potassium permanganate and hydrogen peroxide is (3-6g): (1.5-3g): (69-90mL): (9-15g): (15-50mL).
[0009] Preferably, the specific operation of step S2 is: dissolving graphene oxide in dimethylformamide and then sonicating, then adding sodium bicarbonate and stirring, cooling to 0°C, dropwise adding 2,4,6-trichloro-1,3,5-triazine solution and stirring, adding p-phenylenediamine in a nitrogen atmosphere and stirring to react, reflux, cooling to room temperature, filtering, washing, and drying to obtain amino-functionalized reduced graphene.
[0010] Preferably, the molar ratio of the mass of the graphene oxide to the mass of sodium bicarbonate, 2,4,6-trichloro-1,3,5-triazine, and p-phenylenediamine is (380-420 mg): (60-65 mmol): (15-17 mmol): (60-68 mmol).
[0011] Preferably, the specific operation of step S3 is: ultrasonically dispersing the amino-functionalized reduced graphene in deionized water, using carbon fiber as the cathode, the metal steel plate as the anode, the battery voltage as a DC voltage of 10-30V, the electrolyte as a sodium bicarbonate solution with a pH of 10-14, depositing for 5-20 minutes, and then heating at 70-90°C for 20-24 hours to finally obtain amino-functionalized reduced graphene-coated carbon fiber.
[0012] Preferably, the specific operation of step S4 is: ultrasonically uniformly dispersing the amino-functionalized reduced graphene-coated carbon fiber in a 1M HCl solution, cooling to 0°C in an ice-salt bath, adding aniline monomer and stirring sufficiently, then adding ammonium persulfate, reacting at 0°C for 20-24h, then filtering out the carbon fiber after the reaction is completed, and repeatedly washing with deionized water, ethanol, and n-hexane until the filtrate becomes colorless, and drying the obtained product at 70-90°C to constant weight to obtain polyaniline-graphene functionalized surface modified carbon fiber; the mass ratio of amino-functionalized reduced graphene-coated carbon fiber, aniline and ammonium persulfate is (5-15): (0.8-2): (0.1-0.3).
[0013] Preferably, the twin-screw extruder is a co-rotating twin-screw extruder, the screw aspect ratio is (40-52):1, and the extrusion process conditions are: the feeding section temperature is 180-280°C, the plasticizing section temperature is 280-300°C, the homogenizing section temperature is 300-320°C, the head temperature is 310-320°C, the screw speed is 200-600rmp, and the pressure is 6-10MPa.
[0014] Preferably, the processing aid is ethylene bisstearamide, pentaerythritol stearate, antioxidant 1098 and antioxidant 168 in a mass ratio of 1:1:1:1.
[0015] Compared with the prior art, the present invention has the following beneficial effects: 1. The preparation method of the surface functionalized modified CF / PPS composite material of the present invention adopts a two-step method to perform surface functionalization modification on the carbon fiber in order to solve the interfacial affinity between the carbon fiber and the PPS resin: first, electrochemically deposit amino-functionalized reduced graphene on the surface of the carbon fiber, and then in situ graft polymerize the intrinsic conductive material polyaniline nanofibers on the surface. The interface layer material graphene grafted polyaniline is amphiphilic. On the one hand, the graphene is connected to the carbon fiber through the carbon plane π-π bond, and on the other hand, the polyaniline and PPS are tightly combined through the intermolecular hydrogen bond interaction force. The polyaniline nanofibers on the surface of the modified carbon fiber increase the wettability and roughness of the carbon fiber surface, and structurally enable the carbon fiber to be anchored to the PPS resin matrix through hydrogen bonds and mechanical locking (such as Figure 2 As shown in the figure, the interface bonding problem between carbon fiber and PPS is solved. At the same time, nano-polyaniline and nano-graphene, as the interface layer between carbon fiber and resin matrix, have a certain interface strength, which ensures the transfer of load between resin and carbon fiber without affecting the performance of the composite material.
[0016] 2. The preparation method of the surface functionalized modified CF / PPS composite material of the present invention uses graphene and intrinsic conductive polyaniline nanofibers as the phase interface layer, and the good interface performance ensures the effective load transfer from the matrix to the filler, which helps to reduce stress concentration and enhance the overall mechanical properties. Compared with the unmodified carbon fiber reinforced PPS composite material, the tensile strength of the surface modified carbon fiber reinforced PPS composite material is increased by up to about 15.6%, the elongation at break is increased by up to about 117%, the HDT is increased by up to about 9°C, and the volume resistivity is reduced by up to one order of magnitude, giving the composite material high mechanical properties, electrical and thermal conductivity, and providing a high-performance composite material for high-demand, multifunctional application environments. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 The present invention is a flow chart of the preparation of the polyaniline-graphene functionalized surface modified carbon fiber.
[0018] Figure 2 It is a schematic diagram of the interlocking anchoring of the interface structure of the surface functionalized modified CF / PPS composite material in the present invention. DETAILED DESCRIPTION
[0019] In order to enable persons skilled in the art to better understand the technical solution of the present invention, the technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention.
[0020] Unless otherwise specified, the raw materials used in the following examples and comparative examples are all commercially available products.
[0021] The carbon fiber before modification used in the following examples and comparative examples is PAN carbon fiber (CH80CP006-PAY, Amos Composite Materials Co., Ltd., South Korea), which was extracted with acetone for 24 hours before use to remove the commercial sizing agent on the surface, and then dried for use.
[0022] Example 1 The preparation method of the surface functionalized modified CF / PPS composite material of this embodiment comprises the following steps: (1) Preparation of CF-RGO-PANI S1 Preparation of GO by improved Hummer method: 3 g of graphite powder and 1.5 g of sodium nitrate were added to a 500 mL three-necked bottle, 69 mL of 98 wt.% sulfuric acid was slowly added under ice bath conditions, the temperature was kept below 20 °C and stirred, 9 g of potassium permanganate was added dropwise, the resulting mixture was stirred at 35 °C for 30 min, 138 mL of deionized water was slowly added, the temperature was controlled below 100 °C, and after reacting for 15 min, 15 mL of 30 wt.% H2O2 solution and 200 mL of deionized water were added to obtain a graphene oxide suspension, which was filtered through a 0.22 μm polytetrafluoroethylene membrane and repeatedly washed with 1 mol / L hydrochloric acid and deionized water to remove excess metal ions until the filtrate was neutral. The product was freeze-dried under reduced pressure for 48 h to obtain GO; S2 Preparation of ATRGO: 400 mg of GO was dissolved in 120 mL of dimethylformamide (DMF) and then sonicated. 5.46 g (65 mmol) of sodium bicarbonate was added under magnetic stirring. After cooling to 0°C in an ice bath, 3 g (16.26 mmol) of 2,4,6-trichloro-1,3,5-triazine in DMF solution was added dropwise through a reduced pressure dropping funnel and stirred for 4 h. After adding 7.033 g (65.04 mmol) of p-phenylenediamine in a nitrogen atmosphere, the mixture was stirred at room temperature for 4 h. The mixture was heated to 100°C and refluxed in a nitrogen atmosphere for 24 h. The mixture was cooled to room temperature and filtered through a polytetrafluoroethylene membrane with a pore size of 0.22 µm. The mixture was repeatedly washed with acetone, DMF, n-hexane, and deionized water until the filtrate was colorless. The mixture was dried to constant weight in a vacuum drying oven at 50°C to obtain ATRGO. S3 Preparation of CF-ATRGO: 0.6 g of ATRGO was added into 1000 mL of deionized water, and ultrasonicated in a 50 kHz ultrasonic instrument for 1 h to uniformly disperse the ATRGO to obtain an ATRGO dispersion; then, 5 g of carbon fiber was taken and used as the cathode, the metal steel plate as the anode, the battery voltage was a DC voltage of 20 V, the electrolyte was a sodium bicarbonate solution with a pH of 10, and the deposition was performed for 5 min. After that, the carbon fiber on the cathode was taken out and placed in a vacuum oven at 80 ° C for heating for 24 h to finally obtain CF-ATRGO; wherein, ATRGO accounted for 0.1 wt.% of CF-ATRGO; S4 Preparation of CF-RGO-PANI: Add 6g of CF-ATRGO to 1M HCl solution, ultrasonically disperse for 30min, then cool to 0℃ in an ice-salt bath, add 0.816g of aniline monomer and stir thoroughly, then add 0.1g of ammonium persulfate, react at 0℃ for 24h, finally filter out the carbon fiber after the reaction, wash repeatedly with deionized water, ethanol and n-hexane until the filtrate becomes colorless, dry the product in a vacuum oven at 80℃ to constant weight for use, and obtain CF-RGO-PANI; polyaniline accounts for 0.5wt.% of CF-RGO-PANI.
[0023] (2) Preparation of surface functionalized CF / PPS composites 89 parts of PPS resin, 10 parts of CF-RGO-PANI, and 1 part of a processing aid mixed with EBS, PETS, 1098, and 168 in a mass ratio of 1:1:1:1 were added to the twin-screw extruder through a metering scale from the main feed port, side feed port, and main feed port of the twin-screw extruder, respectively. The screw length-diameter ratio was 48:1. The materials were fully melted and mixed under the conveying, shearing, and mixing of the twin screws, and extruded through the head of the twin-screw extruder. The temperature settings of each temperature control zone of the screw extruder are: feeding section temperature 180℃, 240℃, 280℃; plasticizing section temperature 280℃, 290℃, 300℃; homogenizing section temperature 300℃, 310℃, 310℃, 310℃, 310℃, 310℃, head temperature 315℃, screw speed 500rmp, pressure 6MPa; then after drawing, cooling, pelletizing and drying, surface functionalized modified CF / PPS composite materials are obtained.
[0024] Example 2 The preparation method of the surface functionalized modified CF / PPS composite material of this embodiment comprises the following steps: (1) Preparation of CF-RGO-PANI S1 Preparation of GO by improved Hummer method: 6 g of graphite powder and 3 g of sodium nitrate were added to a 500 mL three-necked bottle, 90 mL of 98 wt.% sulfuric acid was slowly added under ice bath conditions, the temperature was kept below 20 °C and stirred, 15 g of potassium permanganate was added dropwise, the resulting mixture was stirred at 35 °C for 30 min, and then 138 mL of deionized water was slowly added, the temperature was controlled below 100 °C, and after reacting for 15 min, 50 mL of 30 wt.% H2O2 solution and 200 mL of deionized water were added to obtain a graphene oxide suspension, which was filtered through a 0.22 μm polytetrafluoroethylene membrane and repeatedly washed with 1 mol / L hydrochloric acid and deionized water to remove excess metal ions until the filtrate was neutral. The product was freeze-dried under reduced pressure for 48 h to obtain GO; S2 Preparation of ATRGO: 420 mg of GO was dissolved in 120 mL of DMF and then ultrasonicated. 5.2 g (62 mmol) of sodium bicarbonate was added under magnetic stirring. After cooling to 0°C in an ice bath, 3.135 g (17 mmol) of 2,4,6-trichloro-1,3,5-triazine in DMF solution was added dropwise through a reduced pressure dropping funnel and stirred for 4 h. After adding 7.344 g (68 mmol) of p-phenylenediamine in a nitrogen atmosphere, the mixture was stirred at room temperature for 4 h. The mixture was heated to 100°C and refluxed in a nitrogen atmosphere for 24 h. The mixture was cooled to room temperature and filtered through a polytetrafluoroethylene membrane with a pore size of 0.22 µm. The mixture was washed repeatedly with acetone, DMF, n-hexane, and deionized water until the filtrate was colorless. The mixture was dried to constant weight in a vacuum drying oven at 50°C to obtain ATRGO. S3 CF-ATRGO was prepared by the same method as step S3 of Example 1; S4 Preparation of CF-RGO-PANI: Add 15g of CF-ATRGO to 1M HCl solution, ultrasonically disperse for 30min, then cool to 0℃ in an ice-salt bath, add 1.981g of aniline monomer and stir thoroughly, then add 0.3g of ammonium persulfate, react at 0℃ for 22h, finally filter out the carbon fiber after the reaction, wash repeatedly with deionized water, ethanol and n-hexane until the filtrate becomes colorless, dry the product in a vacuum oven at 90℃ to constant weight for use, and obtain CF-RGO-PANI; polyaniline accounts for 1wt.% of CF-RGO-PANI.
[0025] (2) Preparation of surface functionalized modified CF / PPS composite material: A surface functionalized modified CF / PPS composite material was prepared by the same method as step (2) of Example 1.
[0026] Example 3 The preparation method of the surface functionalized modified CF / PPS composite material of this embodiment comprises the following steps: (1) Preparation of CF-RGO-PANI S1 Preparation of GO by improved Hummer method: 4 g of graphite powder and 2 g of sodium nitrate were added to a 500 mL three-necked bottle, 80 mL of 98 wt.% sulfuric acid was slowly added under ice bath conditions, the temperature was kept below 20 °C and stirred, 12 g of potassium permanganate was added dropwise, the resulting mixture was stirred at 35 °C for 30 min, 138 mL of deionized water was slowly added, the temperature was controlled below 100 °C, after reacting for 15 min, 30 mL of 30 wt.% H2O2 solution and 200 mL of deionized water were added to obtain a graphene oxide suspension, filtered through a 0.22 μm polytetrafluoroethylene membrane and repeatedly washed with 1 mol / L hydrochloric acid and deionized water to remove excess metal ions until the filtrate was neutral, and the product was freeze-dried under reduced pressure for 48 h to obtain GO; S2 ATRGO was prepared by the same method as step S2 of Example 1; S3 Preparation of CF-ATRGO: Take 1g of ATRGO, add it into 1000mL of deionized water, and ultrasonicate it in a 50kHz ultrasonic instrument for 1h to evenly disperse the ATRGO to obtain an ATRGO dispersion; then, take 5g of carbon fiber, and use the carbon fiber as the cathode, the metal steel plate as the anode, the battery voltage is a DC voltage of 10V, the electrolyte is a sodium bicarbonate solution with a pH of 13.5, and deposit for 10min. After that, take out the carbon fiber on the cathode, place it in a vacuum oven at 90℃ and heat it for 20h, and finally obtain CF-ATRGO; wherein, ATRGO accounts for 0.2wt.% of CF-ATRGO; S4 Preparation of CF-RGO-PANI: Add 5g of CF-ATRGO to 1M HCl solution, ultrasonically disperse for 30min, then cool to 0℃ in an ice-salt bath, add 1.212g of aniline monomer and stir thoroughly, then add 0.2g of ammonium persulfate, react at 0℃ for 20h, finally filter out the carbon fiber after the reaction, wash repeatedly with deionized water, ethanol and n-hexane until the filtrate becomes colorless, dry the product in a vacuum oven at 70℃ to constant weight for use, and obtain CF-RGO-PANI; polyaniline accounts for 0.5wt.% of CF-RGO-PANI.
[0027] (2) Preparation of surface functionalized CF / PPS composites 78.8 parts of PPS resin, 20 parts of CF-RGO-PANI, and 1.2 parts of a processing aid mixed with EBS, PETS, 1098, and 168 in a mass ratio of 1:1:1:1 were added to the twin-screw extruder through a metering scale from the main feed port, side feed port, and main feed port of the twin-screw extruder, respectively. The screw aspect ratio was 48:1. The materials were fully melted and mixed under the conveying, shearing, and mixing of the twin screws, and extruded through the head of the twin-screw extruder. The temperature settings of each temperature control zone of the twin-screw extruder are: feeding section temperature 180℃, 240℃, 280℃; plasticizing section temperature 280℃, 290℃, 300℃; homogenizing section temperature 300℃, 310℃, 310℃, 310℃, 310℃, 320℃, head temperature 320℃, screw speed 600rmp, pressure 10MPa; then after drawing, cooling, pelletizing and drying, the surface functionalized modified CF / PPS composite material is obtained.
[0028] Example 4 The preparation method of the surface functionalized modified CF / PPS composite material of this embodiment comprises the following steps: (1) Preparation of CF-RGO-PANI S1 GO was prepared by the same method as step S1 of Example 1; S2 Preparation of ATRGO: 380 mg of GO was dissolved in 120 mL of DMF and then ultrasonicated. 5.04 g (60 mmol) of sodium bicarbonate was added under magnetic stirring. After cooling to 0°C in an ice bath, 2.766 g (15 mmol) of 2,4,6-trichloro-1,3,5-triazine in DMF solution was added dropwise through a reduced pressure dropping funnel and stirred for 4 h. After adding 6.48 g (60 mmol) of p-phenylenediamine in a nitrogen atmosphere, the mixture was stirred at room temperature for 4 h. The mixture was heated to 100°C and refluxed in a nitrogen atmosphere for 24 h. The mixture was cooled to room temperature and filtered through a polytetrafluoroethylene membrane with a pore size of 0.22 µm. The mixture was washed repeatedly with acetone, DMF, n-hexane, and deionized water until the filtrate was colorless. The mixture was dried to constant weight in a vacuum drying oven at 50°C to obtain ATRGO. S3 was prepared by the same method as step S3 of Example 3; S4 CF-RGO-PANI was prepared by the same method as step S4 of Example 2.
[0029] (2) Preparation of surface functionalized modified CF / PPS composite material: A surface functionalized modified CF / PPS composite material was prepared by the same method as step (2) of Example 3.
[0030] Example 5 The preparation method of the surface functionalized modified CF / PPS composite material of this embodiment comprises the following steps: (1) Preparation of CF-RGO-PANI S1 GO is prepared by the same method as step S1 of Example 2; S2 ATRGO was prepared by the same method as step S2 of Example 1; S3 Preparation of CF-ATRGO: 1.5 g of ATRGO was added into 1000 mL of deionized water, and ultrasonicated in a 50 kHz ultrasonic instrument for 1 h to uniformly disperse the ATRGO to obtain an ATRGO dispersion; then, 5 g of carbon fiber was taken and used as the cathode, the metal steel plate as the anode, the battery voltage was a DC voltage of 30 V, the electrolyte was a sodium bicarbonate solution with a pH of 14, and the deposition was performed for 20 min. After that, the carbon fiber on the cathode was taken out and placed in a vacuum oven at 70 ° C for heating for 22 h to finally obtain CF-ATRGO; wherein, ATRGO accounted for 0.3 wt.% of CF-ATRGO; S4 CF-RGO-PANI was prepared by the same method as step S4 of Example 1.
[0031] (2) Preparation of surface functionalized CF / PPS composites 68.7 parts of PPS resin, 30 parts of CF-RGO-PANI, and 1.3 parts of a processing aid mixed with EBS, PETS, 1098, and 168 in a mass ratio of 1:1:1:1 were added to the twin-screw extruder through a metering scale from the main feed port, side feed port, and main feed port of the twin-screw extruder, respectively. The screw length-diameter ratio was 48:1. The materials were fully melted and mixed under the conveying, shearing, and mixing of the twin screws, and extruded through the head of the twin-screw extruder. The temperature settings of each temperature control zone of the twin-screw extruder are: feeding section temperature 180℃, 240℃, 280℃; plasticizing section temperature 280℃, 290℃, 300℃; homogenizing section temperature 300℃, 310℃, 310℃, 310℃, 310℃, 310℃, head temperature 310℃, screw speed 200rmp, pressure 8MPa; then after drawing, cooling, pelletizing and drying, the surface functionalized modified CF / PPS composite material is obtained.
[0032] Example 6 The preparation method of the surface functionalized modified CF / PPS composite material of this embodiment comprises the following steps: (1) Preparation of CF-RGO-PANI S1 GO was prepared by the same method as step S1 of Example 3; S2 ATRGO was prepared by the same method as step S2 of Example 1; S3 CF-ATRGO was prepared by the same method as step S3 of Example 5; S4 CF-RGO-PANI was prepared by the same method as step S4 of Example 2.
[0033] (2) Preparation of surface functionalized modified CF / PPS composite material: A surface functionalized modified CF / PPS composite material was prepared by the same method as step (2) of Example 5.
[0034] Comparative Example 1 The difference from Example 1 is that step (1) is not performed, and an equal amount of CH80CP006-PAY carbon fiber is used to replace the CF-RGO-PANI in step (2).
[0035] Comparative Example 2 The difference from Example 5 is that step (1) is not performed, and an equal amount of CH80CP006-PAY carbon fiber is used to replace the CF-RGO-PANI in step (2).
[0036] Comparative Example 3 The difference from Example 1 is that in step (1), step S4 is not performed, and CF-ATRGO is prepared.
[0037] Comparative Example 4 The difference from Example 1 is that step (1) includes the following steps: S1 GO was prepared by the same method as step S1 of Example 1; S2 prepares graphene oxide-coated carbon fiber material (CF-GO) by electrochemical deposition method: take 0.2g of GO, add it into 1000mL of deionized water, and ultrasonicate it in a 50kHz ultrasonic instrument for 1h to disperse the GO evenly and obtain a GO dispersion; then, take 5g of carbon fiber, and use the carbon fiber as the anode, the metal steel plate as the cathode, the battery voltage is a DC voltage of 20V, the electrolyte is a sodium bicarbonate solution with a pH of 14, and deposit for 10min. After that, take out the carbon fiber on the anode, place it in a vacuum oven at 80℃ and heat it for 24h to finally obtain CF-GO; among them, GO accounts for 0.1wt.% of CF-GO.
[0038] The proportions of components in Examples 1-6 and Comparative Examples 1-4 are shown in Table 1: Table 1 Component ratios in Examples 1-6 and Comparative Examples 1-4
[0039] The surface functionalized modified CF / PPS composite materials prepared in Examples 1-6 and Comparative Examples 1-4 were tested for performance, and the test methods and test standards were as follows: tensile strength and elongation at break were tested according to the American Society for Testing and Materials test standard ASTMD638; melting temperature and crystallization temperature were tested by differential scanning calorimetry (DSC); volume resistivity was tested according to the International Electrotechnical Commission standard IEC 60093. The test results are shown in Table 2: Table 2 Performance test results of surface functionalized modified CF / PPS composites prepared in Examples 1-6 and Comparative Examples 1-4
[0040] As can be seen from Table 2, the present invention introduces graphene and polyaniline nanomaterials on the surface of carbon fiber to perform functionalized surface modification on carbon fiber, and adopts the method of melt blending and extrusion to obtain a high-performance PPS composite material with excellent comprehensive properties such as mechanical properties, thermal properties, and electrical properties. Compared with the surface functionalized CF / PPS composite material directly modified by surface functionalization and the surface functionalized CF / PPS composite material modified by the existing modification method, the comprehensive properties such as strength, toughness, and heat resistance of the PPS composite material of the present invention are greatly improved. The surface modification method of carbon fiber of the present invention provides the possibility for the development of high-performance and functionalized composite materials and opens up a wide range of application space.
Claims
1. A method for preparing a surface functionalized modified CF / PPS composite material, characterized in that: Polyphenylene sulfide resin, polyaniline-graphene functionalized surface modified carbon fiber and processing aids are added into the twin-screw extruder from the main feed port, side feed port and main feed port of the twin-screw extruder respectively, and the surface functionalized modified CF / PPS composite material is obtained by melt blending, extrusion, drawing, cooling, pelletizing and drying through the twin-screw extruder.
2. The method for preparing the surface functionalized modified CF / PPS composite material according to claim 1, characterized in that: The added amount of polyphenylene sulfide resin is 68-90 parts, the added amount of polyaniline-graphene functionalized surface modified carbon fiber is 10-30 parts, and the added amount of processing aid is 1-1.3 parts.
3. The method for preparing the surface functionalized modified CF / PPS composite material according to claim 1, characterized in that: The preparation method of polyaniline-graphene functionalized surface modified carbon fiber comprises the following steps: S1 prepared graphene oxide by improving Hummer method; S2 uses graphene oxide as a precursor to synthesize amino-functionalized reduced graphene; S3 uses an electrochemical electrostatic deposition method to electrostatically deposit amino-functionalized reduced graphene on the surface of the carbon fiber to obtain amino-functionalized reduced graphene-coated carbon fiber; S4 in situ grafted polyaniline nanofibers are grown on the surface of amino-functionalized reduced graphene-coated carbon fibers to obtain polyaniline-graphene functionalized surface-modified carbon fibers.
4. The method for preparing the surface functionalized modified CF / PPS composite material according to claim 3, characterized in that: The specific operation of step S1 is: adding concentrated sulfuric acid to graphite powder and sodium nitrate, keeping the temperature below 20°C, adding potassium permanganate with stirring, stirring to obtain a mixture, then adding deionized water, controlling the temperature below 100°C, adding H2O2 solution after the reaction to obtain a graphene oxide suspension, filtering and washing until the filtrate is neutral, and freeze-drying the product under reduced pressure to obtain graphene oxide; the mass volume ratio of graphite powder, sodium nitrate, concentrated sulfuric acid, potassium permanganate and hydrogen peroxide is (3-6g): (1.5-3g): (69-90mL): (9-15g): (15-50mL).
5. The method for preparing the surface functionalized modified CF / PPS composite material according to claim 3, characterized in that: The specific operation of step S2 is: dissolving graphene oxide in dimethylformamide and then sonicating, then adding sodium bicarbonate and stirring, cooling to 0°C, dropwise adding 2,4,6-trichloro-1,3,5-triazine solution and stirring, adding p-phenylenediamine in a nitrogen atmosphere and stirring to react, reflux, cooling to room temperature, filtering, washing, and drying to obtain amino-functionalized reduced graphene.
6. The method for preparing the surface functionalized modified CF / PPS composite material according to claim 5, characterized in that: The molar ratio of the mass of graphene oxide to that of sodium bicarbonate, 2,4,6-trichloro-1,3,5-triazine, and p-phenylenediamine is (380-420 mg): (60-65 mmol): (15-17 mmol): (60-68 mmol).
7. The method for preparing the surface functionalized modified CF / PPS composite material according to claim 3, characterized in that: The specific operation of step S3 is: ultrasonically disperse the amino-functionalized reduced graphene in deionized water, use carbon fiber as cathode, metal steel plate as anode, battery voltage is DC voltage 10-30V, electrolyte is sodium bicarbonate solution with pH 10-14, deposit for 5-20min, then heat at 70-90°C for 20-24h, and finally obtain amino-functionalized reduced graphene-coated carbon fiber.
8. The method for preparing the surface functionalized modified CF / PPS composite material according to claim 3, characterized in that: The specific operation of step S4 is: ultrasonically uniformly dispersing the amino-functionalized reduced graphene-coated carbon fiber in a 1M HCl solution, cooling to 0°C in an ice-salt bath, adding aniline monomer and stirring thoroughly, then adding ammonium persulfate, reacting at 0°C for 20-24h, then filtering out the carbon fiber after the reaction is completed, and repeatedly washing with deionized water, ethanol, and n-hexane until the filtrate becomes colorless, and drying the obtained product at 70-90°C to constant weight to obtain polyaniline-graphene functionalized surface modified carbon fiber; the mass ratio of amino-functionalized reduced graphene-coated carbon fiber, aniline and ammonium persulfate is (5-15): (0.8-2): (0.1-0.3).
9. The method for preparing the surface functionalized modified CF / PPS composite material according to claim 1, characterized in that: The twin-screw extruder is a co-rotating twin-screw extruder with a screw length-diameter ratio of (40-52):1, a feeding section temperature of 180-280°C, a plasticizing section temperature of 280-300°C, a homogenizing section temperature of 300-320°C, a die head temperature of 310-320°C, a screw speed of 200-600rmp, and a pressure of 6-10MPa.
10. The method for preparing the surface functionalized modified CF / PPS composite material according to claim 1, characterized in that: The processing aids are ethylene bisstearamide, pentaerythritol stearate, antioxidant 1098 and antioxidant 168 in a mass ratio of 1:1:1:1.