Adhesive with self-repairing function and preparation method thereof
By preparing a mixed adhesive between Shuangbi Microcapsules and Single-wall Microcapsules under low temperature conditions, the self-repair problem of microcracks and electrical branch channels of mica belts is solved, and the rapid repair and insulation performance of mica belts are achieved.
Patent Information
- Application Number
- CN202411301083.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-18
- Publication Date
- 2024-11-15
AI Technical Summary
Existing adhesives cannot automatically repair microcracks or electrical branch channels on mica belts, affecting the insulation performance and safety of electrical equipment.
Using a mixture of Shuangbi microcapsules and single-wall microcapsules, polyurethane or polyurea microcapsules are prepared under low temperature conditions, and core particles are formed by mechanical methods such as spraying, combining isocyanate and aromatic isocyanate monomers to form self-healing. Functional adhesive.
The self-healing function of mica belt is realized, ensuring the rapid release and effective reaction of repair agents, controlling the rate and effect of repair reactions, and improving the cross-linking strength of cured substances and improving insulation performance.
Smart Images

Figure BDA0005047687990000011 
Figure BDA0005047687990000051 
Figure BDA0005047687990000161
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electrical materials, and in particular, relates to an adhesive with a self-repairing function and a preparation method thereof. Background Art
[0002] As an excellent electrical insulation material, mica tape has been widely used in electrical equipment such as motors and transformers. However, during the use of mica tape, microcracks or electrical tree branches may occur in the solidified material of the mica tape due to physical damage or high voltage. Currently, when microcracks or electrical tree branches occur in the mica tape, the existing adhesives generally cannot automatically repair the microcracks or electrical tree branches in the solidified material on the mica tape, which seriously affects the insulation performance and safety of electrical equipment. Summary of the invention
[0003] The purpose of the embodiments of the present invention is to provide an adhesive with a self-repairing function that can automatically repair microcracks or electrical tree channels of a solidified material on a mica tape when the mica tape is physically damaged.
[0004] To achieve the above object, the technical solution adopted by the present invention is: to provide an adhesive with self-repairing function, comprising the following components in parts by weight:
[0005]
[0006] Optionally, the particle size of the two-component single-wall microcapsule A is 20 to 25 μm.
[0007] Optionally, the particle size of the two-component single-wall microcapsule B is 20 to 25 μm.
[0008] Optionally, the particle size of the double-walled microcapsule is 20 to 25 μm.
[0009] Another object of an embodiment of the present invention is to provide a method for preparing an adhesive with a self-repairing function that can automatically repair microcracks or electrical tree channels on a mica tape when the mica tape is physically damaged.
[0010] To achieve the above object, the technical solution adopted by the present invention is: to provide a method for preparing an adhesive with self-repairing function, comprising the following steps:
[0011] Step S01: preparing double-wall microcapsules with a particle size of 20 to 25 μm in a low-temperature dispersion tank at a low temperature of -20 to 5°C;
[0012] Step S02: preparing two-component single-wall microcapsules A with a particle size of 20 to 25 μm under low temperature conditions of -20 to 5° C. in a low temperature dispersion tank;
[0013] Step S03: preparing a two-component single-wall microcapsule B with a particle size of 20 to 25 μm under a low temperature condition of -20 to 5° C. in a low temperature dispersion tank;
[0014] Step S04: Add 4 to 6 parts of double-walled microcapsules, 2 to 4 parts of two-component single-walled microcapsules A and 2 to 3 parts of two-component single-walled microcapsules B into 95 to 100 parts of mica tape adhesive, stir evenly at room temperature, and obtain an adhesive with self-repairing function.
[0015] Furthermore, the step S01 includes the following steps:
[0016] Step S011: adding isocyanate, HDI adduct and IPDI adduct in a mass ratio of 5:3:2 into a sealed dispersion tank, dispersing at a temperature of 93 to 96° C. and a dispersion rate of 400 to 420 rpm for 10 to 15 minutes to obtain an -NCO-containing core material resin material;
[0017] Step S012: introducing dry high-pressure air into the sealed dispersion tank so that the pressure in the sealed dispersion tank is maintained at 1.8 to 2.2 times the atmospheric pressure, and spraying the liquid in the sealed dispersion tank intermittently into the methyl acetate solvent in the low-temperature dispersion tank by an airless sprayer, wherein the temperature in the low-temperature dispersion tank is controlled at -20°C, to obtain core material particles C containing -NCO;
[0018] Step S013: uniformly mixing a trifunctional terminal secondary amino polyether, a polyamide resin and methyl acetate in a mass ratio of 2:2:1 to form an amino resin E; after the temperature in the low-temperature dispersion tank is raised to -5°C, dripping the amino resin E into the low-temperature dispersion tank at a rate of 0.2 to 0.3 g / min, and simultaneously raising the temperature in the low-temperature dispersion tank to 5°C at a rate of 4 min / °C; the total reaction time is 1.5 h; after the reaction is completed, uniformly lowering the temperature in the low-temperature dispersion tank to -5°C to form a polyurea inner capsule wall layer on the outer shell of the core material particles under low temperature conditions;
[0019] Step S014: a trifunctional terminal secondary amino polyether, a polyamide resin and methyl acetate in a mass ratio of 8:1:1 are uniformly mixed to form an amino resin F. After the temperature in the low-temperature dispersion tank is raised to -5°C, the amino resin F is evenly divided into 3 portions, each portion of the amino resin F is dripped into the low-temperature dispersion tank at a rate of 3 to 3.5 g / min. After the dripping of each portion of the amino resin F is completed, 1 portion of the MDI monomer solution is added until all 3 portions of the amino resin F are dripped into the low-temperature dispersion tank, and the temperature in the low-temperature dispersion tank is uniformly reduced to -10 to -15°C, so as to drip -NH n The resin forms an outer core material on the outer shell of the core material particle C;
[0020] Step S015: dripping the isocyanate solution into the low-temperature dispersion tank at a rate of 1.8-2.1 g / min, and raising the temperature to 5°C at a rate of 1.8-2.1 min / °C, with a total reaction time of not less than 2 hours, so as to add an excess of low-molecular-weight isocyanate resin to the outer shell of the core particle C under low temperature conditions to form an outer capsule wall layer;
[0021] Step S016: Pass the prepared capsule particles through a 500-mesh sieve, place the sieved microcapsules in a sealed reaction tank, add 0.1 parts of deionized water, maintain the reaction temperature at 25°C, and the dispersion rate at 150 rpm. React for 1 hour to obtain double-wall microcapsules with a particle size range of 20 to 25 μm.
[0022] Furthermore, the step S02 includes the following steps:
[0023] Step S021: adding isocyanate, HDI adduct and IPDI adduct in a mass ratio of 5:3:2 into a sealed dispersion tank, dispersing at a temperature of 93 to 96° C. and a dispersion rate of 400 to 420 rpm for 10 to 15 minutes to obtain an -NCO-containing core material resin material;
[0024] Step S022: introducing dry high-pressure air into the sealed dispersion tank so that the pressure in the sealed dispersion tank is maintained at 1.8 to 2.2 times the atmospheric pressure, and spraying the liquid in the sealed dispersion tank intermittently into the methyl acetate solvent in the low-temperature dispersion tank by an airless sprayer, wherein the temperature in the low-temperature dispersion tank is controlled at -20°C, to obtain core material particles C containing -NCO;
[0025] Step S023: uniformly mixing a trifunctional terminal secondary amino polyether, a polyamide resin and methyl acetate in a mass ratio of 1:9:5 to form an amino resin G; after the temperature in the low-temperature dispersion tank is raised to -5°C, dripping the amino resin G into the low-temperature dispersion tank at a rate of 0.2-0.3 g / min, and simultaneously raising the temperature in the low-temperature dispersion tank to 5°C at a rate of 4 min / °C; the total reaction time is 1.5 h; after the reaction is completed, uniformly lowering the temperature in the low-temperature dispersion tank to -5°C to form a polyurea capsule wall layer on the outer shell of the core particle C under low temperature conditions;
[0026] Step S024: Pass the prepared capsule particles through a 500-mesh sieve, place the sieved microcapsules in a sealed reaction tank, add 0.02 parts of epoxy resin, maintain the reaction temperature at 25°C, and the dispersion rate at 150 rpm. React for 1 hour to obtain two-component single-wall microcapsules A with a particle size in the range of 20 to 25 μm.
[0027] Furthermore, the step S03 includes the following steps:
[0028] Step S031: uniformly mixing a trifunctional secondary amino-terminated polyether, a polyamide resin, an MDI monomer and methyl acetate in a mass ratio of 5:3:2 to form an amino resin H, and adding the amino resin H into a sealed dispersion tank;
[0029] Step S032: Dry high-pressure air is introduced into the sealed dispersion tank to maintain the pressure in the sealed dispersion tank at 1.8 to 2.2 times the atmospheric pressure, and the liquid material in the sealed dispersion tank is sprayed intermittently into the methyl acetate solvent in the low-temperature dispersion tank by an airless sprayer, and the temperature in the low-temperature dispersion tank is controlled at -20°C to obtain a -NH n Core material particles D;
[0030] Step S033: dripping the isocyanate solution into the low-temperature dispersion tank at a rate of 1.8-2.1 g / min, and raising the temperature to 5°C at a rate of 1.8-2.1 min / °C, with a total reaction time of not less than 2 hours, so as to form a polyurea capsule wall layer on the outer shell of the core particle D under low temperature conditions;
[0031] Step S034: Pass the prepared capsule particles through a 500-mesh sieve, place the sieved microcapsules in a sealed reaction tank, add 0.1 parts of deionized water, maintain the reaction temperature at 25°C, and the dispersion rate at 150 rpm. React for 1 hour to obtain dual-component single-wall microcapsules B with a particle size in the range of 20 to 25 μm.
[0032] Furthermore, the amine value of the trifunctional secondary amino-terminated polyether is 400 mg / KOH / g, and the amine value of the polyamide resin is 420 mg / KOH / g.
[0033] Furthermore, the NCO content of the isocyanate is 16%.
[0034] Compared with the prior art, the one or more technical solutions in the embodiments of the present invention have at least one of the following beneficial effects:
[0035] The adhesive with self-repairing function in the embodiment of the present invention, by mixing double-wall microcapsules and single-wall microcapsules, can not only automatically repair microcracks or electrical tree channels on the mica tape when the mica tape is physically damaged, but also ensure the rapid release and effective reaction of the repair agent. In addition, since double-wall microcapsules and single-wall microcapsules are mixed, the rate and effect of the repair reaction can be controlled by adjusting the ratio of double-wall microcapsules to single-wall microcapsules. The method for preparing an adhesive with self-repairing function in the present invention uses low temperature conditions to prepare polyurethane and / or polyurea double-wall microcapsules and two-component single-wall microcapsules. Since the viscosity of the polymer liquid resin material increases with decreasing temperature, and then solidifies into a solid core resin material, it is possible to form core material particles by mechanical methods such as spraying without adding an emulsifier, and the shape of the core material particles can be well maintained under stirring and dispersing conditions, which can effectively reduce the requirements for the viscosity of the core material resin. At the same time, under low temperature conditions, the reaction of -NCO and -NH is controlled within a certain range of the core particle shell, which not only provides a guarantee for the formation of double-wall microcapsules and two-component single-wall microcapsule particles with relatively stable size, shape and composition, but also effectively controls the reaction rate without excessive restrictions on the type and quantity of functional groups (-NCO) in the core material. In addition, during the synthesis of the core resin material, the introduction of an appropriate amount of aromatic isocyanate monomers and the increase in the functionality of the synthetic product can significantly improve the repair rate and cross-linking strength of the double-wall microcapsules and two-component single-wall microcapsules, effectively improving the repair effect. DETAILED DESCRIPTION
[0036] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0037] The embodiment of the present invention provides an adhesive with self-repairing function, comprising the following components in parts by weight:
[0038]
[0039] The embodiment of the present invention provides an adhesive with a self-repairing function. Compared with the prior art, it contains a mixture of double-wall microcapsules and single-wall microcapsules. Since the double-wall microcapsules and single-wall microcapsules are respectively encapsulated with a repairing agent, when the mica tape is physically damaged or subjected to high voltage to produce microcracks or electrical tree channels, the double-wall microcapsules and single-wall microcapsules will rupture and release the repairing agent, which will quickly fill the damage through chemical reactions and restore the insulation performance of the mica tape. Therefore, by mixing the double-wall microcapsules and single-wall microcapsules, the self-repairing function of the physical damage and electrical tree channels of the mica tape solid can be achieved, ensuring the rapid release and effective reaction of the repairing agent, and by adjusting the ratio of the double-wall microcapsules to the single-wall microcapsules, the rate and effect of the repair reaction can be controlled.
[0040] Optionally, the particle size of the two-component single-wall microcapsule A is 20-25 μm.
[0041] Optionally, the particle size of the two-component single-wall microcapsule B is 20-25 μm.
[0042] Optionally, the particle size of the double-walled microcapsule is 20-25 μm.
[0043] The embodiment of the present invention also provides a method for preparing an adhesive with a self-repairing function, comprising the following steps:
[0044] Step S01: preparing double-wall microcapsules with a particle size of 20 to 25 μm in a low-temperature dispersion tank at a low temperature of -20 to 5°C;
[0045] Step S02: preparing two-component single-wall microcapsules A with a particle size of 20 to 25 μm under low temperature conditions of -20 to 5° C. in a low temperature dispersion tank;
[0046] Step S03: preparing a two-component single-wall microcapsule B with a particle size of 20 to 25 μm under a low temperature condition of -20 to 5° C. in a low temperature dispersion tank;
[0047] Step S04: Add 4 to 6 parts of double-walled microcapsules, 2 to 4 parts of two-component single-walled microcapsules A and 2 to 3 parts of two-component single-walled microcapsules B into 95 to 100 parts of mica tape adhesive, stir evenly at room temperature, and obtain an adhesive with self-repairing function.
[0048] The embodiment of the present invention provides a method for preparing an adhesive with a self-repairing function. Compared with the prior art, polyurethane and / or polyurea double-wall microcapsules and two-component single-wall microcapsules are prepared under low temperature conditions. Since the viscosity of the polymer liquid resin material increases as the temperature decreases, and then solidifies into a solid core resin material, core material particles can be formed by mechanical methods such as spraying without adding an emulsifier, and the shape of the core material particles can be better maintained under conditions such as stirring and dispersion, which can reduce the requirements for the viscosity of the core material resin. At the same time, under low temperature conditions, the reaction of -NCO and -NH is controlled within a certain range of the core material particle shell, providing a guarantee for the formation of double-wall microcapsules and two-component single-wall microcapsule particles with relatively stable size, shape, and composition.
[0049] At the same time, by using low temperature conditions to prepare polyurethane and / or polyurea double-wall microcapsules and two-component single-wall microcapsules, and carrying out the -NCO and -NH capsule wall generation reaction at a relatively low temperature, the reaction rate can be effectively controlled without excessive restrictions on the type and quantity of functional groups (-NCO) in the core material. In addition, during the synthesis of the core resin material, an appropriate amount of aromatic isocyanate monomers and an increase in the functionality of the synthetic product can significantly increase the repair rate and cross-linking strength of the double-wall microcapsules and two-component single-wall microcapsules, effectively improving the repair effect. At the same time, the capsule wall material prepared with the participation of such core materials also has advantages in strength and coating integrity, can better adapt to the "destruction" in the subsequent application process, and also allow the core resin to have a lower room temperature viscosity and better fluidity.
[0050] In addition, polyurethane and / or polyurea double-wall microcapsules and two-component single-wall microcapsules are prepared under low temperature conditions. Since the dissolution and swelling effects of organic solvents on organic matter are reduced to varying degrees, the stability of core material particles and capsule wall materials will not be affected by organic solvent immersion. At the same time, by selecting and controlling the type of organic solvent and temperature, and taking advantage of the rule that the molecular weight of the material gradually increases and the solubility of the organic solvent decreases, the coagulation of the material is accelerated during the reaction preparation process of the inner and outer core materials and the inner and outer wall materials.
[0051] Furthermore, in step S01, preparing double-wall microcapsules with a particle size of 20 to 25 μm under low temperature conditions of -20 to 5° C. in a low temperature dispersion tank comprises the following specific steps:
[0052] Step S011: Add isocyanate, HDI adduct and IPDI adduct in a mass ratio of 5:3:2 into a sealed dispersion tank, and disperse at a dispersion rate of 400-420 rpm for 10-15 minutes at a temperature of 93-96°C to obtain an NCO-containing core resin material. Among them, the NCO content of the isocyanate (MDI polymer) is 16%, the NCO content of the HDI adduct is 14.5%, and the NCO content of the IPDI adduct is 8%. The volume of the sealed dispersion tank is 2L, and the total amount of the above resin added to the sealed dispersion tank does not exceed 0.5kg.
[0053] Step S012: Keep the temperature in the sealed dispersion tank at about 95°C, introduce dry high-pressure air into the sealed dispersion tank, so that the pressure in the sealed dispersion tank is maintained at 1.8 to 2.2 times the atmospheric pressure, and spray the liquid in the sealed dispersion tank intermittently into the methyl acetate solvent in the low-temperature dispersion tank through an airless sprayer. The temperature in the low-temperature dispersion tank is controlled at -20°C to obtain core material particles C containing -NCO with a particle size of 5 to 10 μm. Among them, the discharge port of the sealed dispersion tank and the feed port of the small airless sprayer are connected through a hose and a hose connector, and the spray gun is connected to a 30cm extension tube and a nozzle. Granulation and subsequent production processes are basically completed in the low-temperature dispersion tank. The volume of the low-temperature dispersion tank is 5L. The low-temperature dispersion tank has a sealed design and can be subjected to reduced pressure distillation. A feeding port for adding liquid is provided on the upper cover of the low-temperature dispersion tank. A perforation is provided on the top of the low-temperature dispersion tank, so that the spray gun extension tube passes through the sealed perforation, and part of the extension tube and the spray head extend into the tank and are located at the top of the low-temperature dispersion tank. It should be noted that before the liquid material in the sealed dispersion tank is sprayed into the low-temperature dispersion tank by the airless sprayer, 2.5L of methyl acetate is added to the low-temperature dispersion tank, and the temperature in the low-temperature dispersion tank is controlled at -20°C by the low-temperature cooling circulation pump, and the dispersion rate is maintained at 250 rpm. After the spraying is completed, the temperature and dispersion rate in the low-temperature dispersion tank are maintained for more than 20 minutes.
[0054] Step S013: The trifunctional terminal secondary amino polyether, polyamide resin and methyl acetate in a mass ratio of 2:2:1 are uniformly mixed to form amino resin E. After the temperature in the low-temperature dispersion tank is raised to -5°C, the amino resin E is dripped into the low-temperature dispersion tank at a rate of 0.2-0.3 g / min, and the temperature in the low-temperature dispersion tank is raised to 5°C at a rate of 4 min / °C. The total reaction time is 1.5 hours. After the reaction is completed, the temperature in the low-temperature dispersion tank is uniformly reduced to -5°C to form a polyurea inner capsule wall layer on the outer shell of the core material particles under low temperature conditions. Among them, the amine value of the trifunctional terminal secondary amino polyether is 400 mg / KOH / g, and the amine value of the polyamide resin is 420 mg / KOH / g. After the reaction is completed, the dispersion rate of the low-temperature dispersion tank is 150 rpm, and the dispersion is more than 0.5 hours.
[0055] Step S014: a trifunctional terminal secondary amino polyether, a polyamide resin and methyl acetate in a mass ratio of 8:1:1 are uniformly mixed to form an amino resin F. After the temperature in the low-temperature dispersion tank is raised to -5°C, the amino resin F is evenly divided into 3 parts, each part of the amino resin F is dripped into the low-temperature dispersion tank at a rate of 3 to 3.5 g / min. After the dripping of each part of the amino resin F is completed, 1 part of the MDI monomer solution is added until all 3 parts of the amino resin F are dripped into the low-temperature dispersion tank, the temperature in the low-temperature dispersion tank is uniformly reduced to -10 to -15°C, the dispersion rate is 150 rpm, and the dispersion is carried out for more than 0.5h, so as to drip -NH n The resin forms an outer core material on the outer shell of the core material particle C.
[0056] Step S015: dripping the isocyanate solution into the low-temperature dispersion tank at a rate of 1.8-2.1 g / min, and raising the temperature to 5°C at a rate of 1.8-2.1 min / °C, with a total reaction time of not less than 2 hours, so as to add an excess of low-molecular-weight isocyanate resin to the outer shell of the core particle C under low temperature conditions to form an outer capsule wall layer. In the isocyanate solution, the mass ratio of isocyanate to methyl acetate is 13:7, and the NCO content of the isocyanate (MDI polymer) is 16%.
[0057] Step S016: Pass the prepared capsule particles through a 500-mesh sieve, place the screened microcapsules in a sealed reaction tank, add 0.1 parts of deionized water, maintain the reaction temperature at 25°C, and the dispersion rate at 150 rpm. React for 1 hour, filter at low temperature, dry at a moderate temperature, and reinforce the outer capsule wall layer by moisture curing to obtain double-wall microcapsules with a particle size in the range of 20 to 25 μm.
[0058] Furthermore, in step S02, preparing the two-component single-wall microcapsules A with a particle size of 20 to 25 μm under low temperature conditions of -20 to 5° C. in a low temperature dispersion tank specifically comprises the following steps:
[0059] Step S021: Add isocyanate, HDI adduct and IPDI adduct in a mass ratio of 5:3:2 into a sealed dispersion tank, and disperse at a dispersion rate of 400 to 420 rpm for 10 to 15 minutes at a temperature of 93 to 96°C to obtain an NCO-containing core resin material. Among them, the NCO content of the isocyanate (MDI polymer) is 16%, the NCO content of the HDI adduct is 14.5%, and the NCO content of the IPDI adduct is 8%. The volume of the sealed dispersion tank is 2L, and the total amount of the above resins added to the sealed dispersion tank does not exceed 0.5kg.
[0060] Step S022: Dry high-pressure air is introduced into the sealed dispersion tank so that the pressure in the sealed dispersion tank is maintained at 1.8 to 2.2 times the atmospheric pressure. The liquid in the sealed dispersion tank is sprayed intermittently into the methyl acetate solvent in the low-temperature dispersion tank by an airless sprayer. The temperature in the low-temperature dispersion tank is controlled at -20°C to obtain core material particles C containing -NCO with a particle size of 5 to 10 μm. Among them, the discharge port of the sealed dispersion tank and the feed port of the small airless sprayer are connected through a hose and a hose connector, and the spray gun is connected to a 30 cm extension tube and a nozzle. Granulation and subsequent production processes are basically completed in the low-temperature dispersion tank. The volume of the low-temperature dispersion tank is 5L. The low-temperature dispersion tank has a sealed design and can be subjected to reduced pressure distillation. A feeding port for adding liquid is provided on the upper cover of the low-temperature dispersion tank. A perforation is provided on the top of the low-temperature dispersion tank so that the spray gun extension tube passes through the sealed perforation. Part of the extension tube and the spray head extend into the tank and are located at the top of the low-temperature dispersion tank. It should be noted that before the liquid material in the sealed dispersion tank is sprayed into the low-temperature dispersion tank by the airless sprayer, 2.5L of methyl acetate is added to the low-temperature dispersion tank, and the temperature in the low-temperature dispersion tank is controlled at -20°C by the low-temperature cooling circulation pump, and the dispersion rate is maintained at 250 rpm. After the spraying is completed, the temperature and dispersion rate in the low-temperature dispersion tank are maintained for more than 20 minutes.
[0061] Step S023: The trifunctional secondary amino-terminated polyether, polyamide resin and methyl acetate in a mass ratio of 1:9:5 are uniformly mixed to form amino resin G. After the temperature in the low-temperature dispersion tank is raised to -5°C, the amino resin G is dripped into the low-temperature dispersion tank at a rate of 0.2-0.3 g / min, and the temperature in the low-temperature dispersion tank is raised to 5°C at a rate of 4 min / °C. The total reaction time is 1.5 hours. After the reaction is completed, the temperature in the low-temperature dispersion tank is uniformly reduced to -5°C, the dispersion rate is 150 rpm, and the dispersion is carried out for more than 0.5 hours to form a polyurea capsule wall layer on the outer shell of the core particle C under low temperature conditions. Among them, the amine value of the trifunctional secondary amino-terminated polyether is 400 mg / KOH / g, and the amine value of the polyamide resin is 420 mg / KOH / g.
[0062] Step S024: Pass the prepared capsule particles through a 500-mesh sieve, place the sieved microcapsules in a sealed reaction tank, add 0.02 parts of epoxy resin, maintain the reaction temperature at 25°C, and the dispersion rate at 150 rpm. React for 1 hour, filter at low temperature, dry at a moderate temperature, and reinforce the capsule wall with epoxy functional groups to obtain dual-component single-wall microcapsules A with a particle size in the range of 20 to 25 μm.
[0063] Furthermore, in step S03, preparing the two-component single-wall microcapsules B with a particle size of 20 to 25 μm under low temperature conditions of -20 to 5° C. in a low temperature dispersion tank specifically comprises the following steps:
[0064] Step S031: uniformly mix a trifunctional terminal secondary amino polyether, a polyamide resin, an MDI monomer and methyl acetate in a mass ratio of 5:3:2 to form an amino resin H, and add the amino resin H into a sealed dispersion tank.
[0065] Step S032: Dry high-pressure air is introduced into the sealed dispersion tank to maintain the pressure in the sealed dispersion tank at 1.8 to 2.2 times the atmospheric pressure, and the liquid material in the sealed dispersion tank is sprayed intermittently into the methyl acetate solvent in the low-temperature dispersion tank by an airless sprayer. The temperature in the low-temperature dispersion tank is controlled at -20°C to obtain a -NH n Core material particles D. Among them, the discharge port of the sealed dispersion tank and the feed port of the small airless sprayer are connected through a hose and a hose connector, and the spray gun is connected to a 30cm extension tube and a nozzle. Granulation and subsequent production processes are basically completed in a low-temperature dispersion tank. The volume of the low-temperature dispersion tank is 5L. The low-temperature dispersion tank has a sealed design and can be subjected to reduced pressure distillation. The upper cover of the low-temperature dispersion tank is provided with a feeding port for adding liquid. The top of the low-temperature dispersion tank is provided with a perforation so that the spray gun extension tube passes through the sealed perforation. Part of the extension tube and the nozzle extend into the tank and are located at the top of the low-temperature dispersion tank. It should be noted that before the liquid in the sealed dispersion tank is sprayed into the low-temperature dispersion tank by the airless sprayer, 2.5L of methyl acetate is added to the low-temperature dispersion tank, and the temperature in the low-temperature dispersion tank is controlled at -20°C by a low-temperature cooling circulation pump, and the dispersion rate is maintained at 250 rpm. After the spraying is completed, the temperature and dispersion rate in the low-temperature dispersion tank are maintained for more than 20 minutes.
[0066] Step S033: dripping the isocyanate solution into the low-temperature dispersion tank at a rate of 1.8-2.1 g / min, and raising the temperature to 5°C at a rate of 1.8-2.1 min / °C, with a total reaction time of not less than 2 hours, so as to form a polyurea capsule wall layer on the outer shell of the core particle D under low temperature conditions. In the isocyanate solution, the mass ratio of isocyanate to methyl acetate is 2:1, and the NCO content of the isocyanate (MDI polymer) is 16%.
[0067] Step S034: Pass the prepared capsule particles through a 500-mesh sieve, place the sieved microcapsules in a sealed reaction tank, add 0.1 parts of deionized water, maintain the reaction temperature at 25°C, and the dispersion rate at 150 rpm. React for 1 hour, filter at low temperature, dry at a moderate temperature, and reinforce the capsule wall by moisture curing reaction to obtain a two-component single-wall microcapsule B with a particle size in the range of 20 to 25 μm.
[0068] Further, the preparation of the mica tape adhesive in step S04 specifically includes the following steps: adding 50 parts of E44 epoxy resin to a 1000ml three-necked flask, heating and stirring, adding 20 parts of E20 epoxy resin when the temperature in the three-necked flask reaches 110°C, keeping warm for 30 minutes, and adding 25 parts of bismaleimide. Heating to 160°C, keeping warm for 30 minutes, adding 80 parts of tung oil and 20 parts of maleic anhydride again, stirring evenly, cooling to 120°C, keeping warm for 20 minutes, and then cooling to room temperature, adding 100 parts of alcohol, and obtaining the mica tape adhesive.
[0069] The preparation of the mica tape in the embodiment of the present invention specifically includes the following steps: applying the above-mentioned adhesive with self-repairing function to mica paper and glass fiber cloth, and compounding with a compounding roller to obtain the mica tape. Among them, the main indicators of the mica tape are: mica paper content ≥85g / m 2 -110g / m 2 , the content of adhesive with self-repair function is 75g / m 2 ~85g / m 2 , glass fiber cloth content is 35g / m 2 -45g / m 2 , dielectric strength>40MV / mm, tensile strength≥100N / 100mm.
[0070] In order to accurately evaluate the self-repairing adhesive in the embodiment of the present invention, a tensile testing machine is used to simulate mechanical damage and create microcracks, and then the self-repairing performance of the self-repairing adhesive is evaluated by measuring the change in the tensile strength of the multi-resin mica tape. The specific test method and repair efficiency evaluation of the self-repairing adhesive are as follows:
[0071] 1. Mechanical damage simulation and microcrack manufacturing:
[0072] 1) Equipment: Use a high-precision tensile testing machine and set appropriate tensile conditions (such as tensile rate, maximum tensile force, etc.) to simulate the mechanical stress in actual applications.
[0073] 2) Sample preparation: Prepare a set of multi-resin mica tape samples to ensure that the samples are of consistent quality and have no obvious defects.
[0074] 3) Microcrack production: Fix the multi-resin mica tape sample on the tensile testing machine, and cyclically load and unload the sample through the preset tensile program until visible microcracks appear on the surface of the multi-resin mica tape sample. Record the maximum tensile force when visible microcracks appear on the surface of the multi-resin mica tape sample, as well as the state of the microcracks.
[0075] 2. Tensile strength measurement:
[0076] 1) Undamaged state measurement: Before making microcracks, first measure the initial tensile strength of the multi-resin mica tape sample, recorded as XN / mm 2 .
[0077] 2) Post-damage state measurement: After creating microcracks, the tensile strength of the multi-resin mica tape sample is immediately re-measured. At this time, due to the presence of microcracks on the multi-resin mica tape sample, the tensile strength will drop to YN / mm 2 .
[0078] 3) Measurement of repaired state: Place the multi-cracked mica tape sample under standard environment and use the microcapsules in the adhesive with self-repairing function to repair it naturally. After a certain period of time (according to the specific repair time setting), measure the tensile strength of the repaired multi-crack mica tape sample again, recorded as ZN / mm 2 .
[0079] 3. Self-repair performance evaluation:
[0080] The repair rate (RR) is calculated as follows: RR = (ZY) / (XY) × 100%. By comparing the changes in tensile strength before damage, after damage, and after repair, the repair rate can be calculated to evaluate the actual self-repairing effect of the above-mentioned adhesive with self-repairing function.
[0081] In order to more effectively illustrate the technical solution of the present invention, the technical solution of the present invention is described below through specific embodiments.
[0082] Example 1
[0083] 1) Add 5 parts of double-walled microcapsules, 3 parts of two-component single-walled microcapsules A and 3 parts of two-component single-walled microcapsules B to 100 parts of mica tape adhesive, and stir for 30 minutes at room temperature to ensure that the double-walled microcapsules, two-component single-walled microcapsules A and two-component single-walled microcapsules B are evenly distributed in the mica tape adhesive, that is, to ensure that all components are fully mixed to obtain an adhesive with self-healing function;
[0084] 2) The prepared adhesive with self-repairing function is evenly coated on the mica paper and the glass fiber cloth, and the mica paper and the glass fiber cloth are compounded with a compounding stick to obtain a mica tape sample E 1 .
[0085] The tensile strength of the mica tape sample was tested, and the initial tensile strength was 120N / mm 2 ;
[0086] The sample was cyclically loaded using a tensile testing machine until microcracks appeared, and the tensile strength at this time was recorded as 90N / mm 2The sample was placed in a standard environment (25°C, 50% RH) for natural repair. After 7 days, the tensile strength was tested again and was 105N / mm 2 , the repair rate of the adhesive with self-repairing function in Example 1 is calculated to be 50%, indicating that the adhesive with self-repairing function in Example 1 has a certain self-repairing ability.
[0087] Example 2
[0088] 1) adding 6 parts of double-walled microcapsules, 2 parts of two-component single-walled microcapsules A and 2 parts of two-component single-walled microcapsules B to 100 parts of mica tape adhesive, stirring for 30 minutes at room temperature to ensure that the double-walled microcapsules, two-component single-walled microcapsules A and two-component single-walled microcapsules B are evenly distributed in the mica tape adhesive, that is, to ensure that all components are fully mixed to obtain an adhesive with self-healing function;
[0089] 2) The prepared adhesive with self-repairing function is evenly coated on the mica paper and the glass fiber cloth, and the mica paper and the glass fiber cloth are compounded with a compounding stick to obtain a mica tape sample E 2 .
[0090] The tensile strength of the mica tape sample was tested, and the initial tensile strength was 120N / mm 2 ;
[0091] The sample was cyclically loaded using a tensile testing machine until microcracks appeared, and the tensile strength at this time was recorded as 90N / mm 2 The sample was placed in a standard environment (25°C, 50% RH) for natural repair. After 7 days, the tensile strength was tested again and was 110N / mm 2 , the repair rate of the adhesive with self-repairing function in Example 2 is calculated to be 66.67%, indicating that the adhesive with self-repairing function in Example 2 has a certain self-repairing ability.
[0092] Example 3
[0093] 1) adding 4 parts of double-walled microcapsules, 4 parts of two-component single-walled microcapsules A and 2 parts of two-component single-walled microcapsules B to 100 parts of mica tape adhesive, stirring for 30 minutes at room temperature to ensure that the double-walled microcapsules, two-component single-walled microcapsules A and two-component single-walled microcapsules B are evenly distributed in the mica tape adhesive, that is, to ensure that all components are fully mixed to obtain an adhesive with self-repairing function;
[0094] 2) The prepared adhesive with self-repairing function is evenly coated on the mica paper and the glass fiber cloth, and the mica paper and the glass fiber cloth are compounded with a compounding stick to obtain a mica tape sample E 3 .
[0095] The tensile strength of the mica tape sample was tested, and the initial tensile strength was 120N / mm 2 ;
[0096] The sample was cyclically loaded using a tensile testing machine until microcracks appeared, and the tensile strength at this time was recorded as 90N / mm 2 The sample was placed in a standard environment (25°C, 50% RH) for natural repair. After 7 days, the tensile strength was tested again and was 108N / mm 2 , the repair rate of the adhesive with self-repairing function in Example 3 is calculated to be 60%, indicating that the adhesive with self-repairing function in Example 3 has a certain self-repairing ability.
[0097] Example 4
[0098] 1) adding 4 parts of double-walled microcapsules, 4 parts of two-component single-walled microcapsules A and 2 parts of two-component single-walled microcapsules B to 95 parts of mica tape adhesive, stirring for 30 minutes at room temperature to ensure that the double-walled microcapsules, two-component single-walled microcapsules A and two-component single-walled microcapsules B are evenly distributed in the mica tape adhesive, that is, to ensure that all components are fully mixed to obtain an adhesive with self-healing function;
[0099] 2) The prepared adhesive with self-repairing function is evenly coated on the mica paper and the glass fiber cloth, and the mica paper and the glass fiber cloth are compounded with a compounding stick to obtain a mica tape sample E 4 .
[0100] The tensile strength of the mica tape sample was tested, and the initial tensile strength was 120N / mm 2 ;
[0101] The sample was cyclically loaded using a tensile testing machine until microcracks appeared, and the tensile strength at this time was recorded as 90N / mm 2 The sample was placed in a standard environment (25°C, 50% RH) for natural repair. After 7 days, the tensile strength was tested again and was 108N / mm 2 , the repair rate of the adhesive with self-repairing function in Example 4 is calculated to be 60%, indicating that the adhesive with self-repairing function in Example 4 has a certain self-repairing ability.
[0102] Example 5
[0103] 1) adding 6 parts of double-walled microcapsules, 2 parts of two-component single-walled microcapsules A and 2 parts of two-component single-walled microcapsules B to 98 parts of mica tape adhesive, stirring for 30 minutes at room temperature to ensure that the double-walled microcapsules, two-component single-walled microcapsules A and two-component single-walled microcapsules B are evenly distributed in the mica tape adhesive, that is, to ensure that all components are fully mixed to obtain an adhesive with self-healing function;
[0104] 2) The prepared adhesive with self-repairing function is evenly coated on the mica paper and the glass fiber cloth, and the mica paper and the glass fiber cloth are compounded with a compounding stick to obtain a mica tape sample E 5 .
[0105] The tensile strength of the mica tape sample was tested, and the initial tensile strength was 120N / mm 2 ;
[0106] The sample was cyclically loaded using a tensile testing machine until microcracks appeared, and the tensile strength at this time was recorded as 90N / mm 2 The sample was placed in a standard environment (25°C, 50% RH) for natural repair. After 7 days, the tensile strength was tested again and was 110N / mm 2 , the repair rate of the adhesive with self-repairing function in Example 5 is calculated to be 66.67%, indicating that the adhesive with self-repairing function in Example 5 has a certain self-repairing ability.
[0107] Comparative Example 1
[0108] 1) adding 10 parts of double-walled microcapsules to 100 parts of mica tape adhesive and stirring for 30 minutes at room temperature to ensure that the double-walled microcapsules are evenly distributed in the mica tape adhesive, that is, to ensure that all ingredients are fully mixed to obtain an adhesive with self-healing function;
[0109] 2) The prepared adhesive with self-repairing function is evenly coated on the mica paper and the glass fiber cloth, and the mica paper and the glass fiber cloth are compounded with a compounding stick to obtain a mica tape sample E 6 .
[0110] The tensile strength of the mica tape sample was tested, and the initial tensile strength was 120N / mm 2 ;
[0111] The sample was cyclically loaded using a tensile testing machine until microcracks appeared, and the tensile strength at this time was recorded as 90N / mm 2 The sample was placed in a standard environment (25°C, 50% RH) for natural repair, and the tensile strength was tested again after 7 days and was 100N / mm 2 , the repair rate of the adhesive with self-repairing function in comparative example 1 is 33.33% through calculation, indicating that the adhesive with self-repairing function in comparative example 1 has certain self-repairing ability.
[0112] Comparative Example 2
[0113] 1) adding 10 parts of two-component single-wall microcapsules A to 100 parts of mica tape adhesive and stirring for 30 minutes at room temperature to ensure that the two-component single-wall microcapsules A are evenly distributed in the mica tape adhesive, that is, to ensure that all components are fully mixed to obtain an adhesive with self-healing function;
[0114] 2) The prepared adhesive with self-repairing function is evenly coated on the mica paper and the glass fiber cloth, and the mica paper and the glass fiber cloth are compounded with a compounding stick to obtain a mica tape sample E 7 .
[0115] The tensile strength of the mica tape sample was tested, and the initial tensile strength was 120N / mm 2 ;
[0116] The sample was cyclically loaded using a tensile testing machine until microcracks appeared, and the tensile strength at this time was recorded as 90N / mm 2 The sample was placed in a standard environment (25°C, 50% RH) for natural repair. After 7 days, the tensile strength was tested again and was 102N / mm 2 , the repair rate of the adhesive with self-repairing function in comparative example 2 is 40% through calculation, indicating that the adhesive with self-repairing function in comparative example 2 has certain self-repairing ability.
[0117] Comparative Example 3
[0118] 1) Add 10 parts of two-component single-wall microcapsules B to 100 parts of mica tape adhesive and stir for 30 minutes at room temperature to ensure that the two-component single-wall microcapsules B are evenly distributed in the mica tape adhesive, that is, to ensure that all components are fully mixed to obtain an adhesive with self-healing function;
[0119] 2) The prepared adhesive with self-repairing function is evenly coated on the mica paper and the glass fiber cloth, and the mica paper and the glass fiber cloth are compounded with a compounding stick to obtain a mica tape sample E 8 .
[0120] The tensile strength of the mica tape sample was tested, and the initial tensile strength was 120N / mm 2 ;
[0121] The sample was cyclically loaded using a tensile testing machine until microcracks appeared, and the tensile strength at this time was recorded as 90N / mm 2 The sample was placed in a standard environment (25°C, 50% RH) for natural repair. After 7 days, the tensile strength was tested again and was 102N / mm 2 , the repair rate of the adhesive with self-repairing function in comparative example 3 is calculated to be 40%, indicating that the adhesive with self-repairing function in comparative example 3 has a certain self-repairing ability.
[0122] The relevant performance test results of the adhesives with self-repairing function in the above Examples 1 to 5 and Comparative Examples 1 to 3 are respectively listed in the following Table 1.
[0123] Table 1 Test results of adhesives with self-repairing function in Examples 1 to 5 and Comparative Examples 1 to 3
[0124]
[0125]
[0126] From the analysis of Table 1 above, it can be seen that the self-repairing adhesives in Examples 1 to 5 have a significantly improved repair rate compared with the self-repairing adhesives in Comparative Examples 1 to 3, indicating that the self-repairing adhesives in Examples 1 to 5 have a good repair effect on the microcracks or electrical tree channels caused by physical damage to the mica tape, and the repair effect is significantly improved. In addition, compared with Example 1 and Example 3, Example 2 increases the proportion of double-wall microcapsules in Example 2 and reduces the proportion of two-component single-wall microcapsules. The repair rate of the self-repairing adhesive in Example 2 for physical damage to the mica tape is increased to 66.67%, indicating that adjusting the proportion of microcapsules can effectively improve the repair effect. Compared with Example 1 and Example 2, since the double-wall microcapsules are reduced and the two-component single-wall microcapsules A are increased in Example 3, the repair rate of the physical damage of the mica tape by the adhesive with self-repairing function in Example 3 is still maintained at a high level (60%), indicating that by adjusting the proportion of three different types of microcapsules, namely double-wall microcapsules, two-component single-wall microcapsules A and two-component single-wall microcapsules B, the repair performance of the adhesive with self-repairing function can be affected differently, so that the proportion of double-wall microcapsules, two-component single-wall microcapsules A and two-component single-wall microcapsules B can be adjusted according to specific needs to optimize the repair effect.
[0127] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. An adhesive with self-repairing function, characterized in that: The composition comprises the following components in parts by weight:
2. The adhesive with self-repairing function according to claim 1, characterized in that: The particle size of the two-component single-wall microcapsule A is 20-25 μm.
3. The adhesive with self-repairing function according to claim 1, characterized in that: The particle size of the two-component single-wall microcapsule B is 20-25 μm.
4. The adhesive with self-repairing function according to claim 1, characterized in that: The particle size of the double-wall microcapsule is 20-25 μm.
5. A method for preparing an adhesive with self-repairing function, characterized in that: The steps include: Step S01: preparing double-wall microcapsules with a particle size of 20 to 25 μm in a low-temperature dispersion tank at a low temperature of -20 to 5°C; Step S02: preparing two-component single-wall microcapsules A with a particle size of 20 to 25 μm under low temperature conditions of -20 to 5° C. in a low temperature dispersion tank; Step S03: preparing two-component single-wall microcapsules B with a particle size of 20 to 25 μm under low temperature conditions of -20 to 5° C. in a low temperature dispersion tank; Step S04: Add 4 to 6 parts of double-walled microcapsules, 2 to 4 parts of two-component single-walled microcapsules A and 2 to 3 parts of two-component single-walled microcapsules B into 95 to 100 parts of mica tape adhesive, stir evenly at room temperature, and obtain an adhesive with self-repairing function.
6. The method for preparing an adhesive with self-repairing function according to claim 5, characterized in that: The step S01 includes the following steps: Step S011: adding isocyanate, HDI adduct and IPDI adduct in a mass ratio of 5:3:2 into a sealed dispersion tank, dispersing at a temperature of 93 to 96° C. and a dispersion rate of 400 to 420 rpm for 10 to 15 minutes to obtain an -NCO-containing core material resin material; Step S012: introducing dry high-pressure air into the sealed dispersion tank so that the pressure in the sealed dispersion tank is maintained at 1.8 to 2.2 times the atmospheric pressure, and spraying the liquid in the sealed dispersion tank intermittently into the methyl acetate solvent in the low-temperature dispersion tank by an airless sprayer, wherein the temperature in the low-temperature dispersion tank is controlled at -20°C, to obtain core particles C containing -NCO; Step S013: uniformly mixing a trifunctional terminal secondary amino polyether, a polyamide resin and methyl acetate in a mass ratio of 2:2:1 to form an amino resin E; after the temperature in the low-temperature dispersion tank is raised to -5°C, dripping the amino resin E into the low-temperature dispersion tank at a rate of 0.2-0.3 g / min, and simultaneously raising the temperature in the low-temperature dispersion tank to 5°C at a rate of 4 min / °C; the total reaction time is 1.5 h; after the reaction is completed, uniformly lowering the temperature in the low-temperature dispersion tank to -5°C to form a polyurea inner capsule wall layer on the outer shell of the core material particles under low temperature conditions; Step S014: a trifunctional terminal secondary amino polyether, a polyamide resin and methyl acetate in a mass ratio of 8:1:1 are uniformly mixed to form an amino resin F. After the temperature in the low-temperature dispersion tank is raised to -5°C, the amino resin F is evenly divided into 3 portions, each portion of the amino resin F is dripped into the low-temperature dispersion tank at a rate of 3 to 3.5 g / min. After the dripping of each portion of the amino resin F is completed, 1 portion of the MDI monomer solution is added until all 3 portions of the amino resin F are dripped into the low-temperature dispersion tank, the temperature in the low-temperature dispersion tank is uniformly reduced to -10 to -15°C, and a -NH n Resin to form an outer core material on the outer shell of the core material particle C; Step S015: dripping the isocyanate solution into the low-temperature dispersion tank at a rate of 1.8-2.1 g / min, and raising the temperature to 5°C at a rate of 1.8-2.1 min / °C, with a total reaction time of not less than 2 hours, so as to add an excess of low-molecular-weight isocyanate resin to the outer shell of the core particle C under low temperature conditions to form an outer capsule wall layer; Step S016: Pass the prepared capsule particles through a 500-mesh sieve, place the sieved microcapsules in a sealed reaction tank, add 0.1 parts of deionized water, maintain the reaction temperature at 25°C, and the dispersion rate at 150 rpm. React for 1 hour to obtain double-wall microcapsules with a particle size range of 20 to 25 μm.
7. The method for preparing an adhesive with self-repairing function according to claim 5, characterized in that: The step S02 includes the following steps: Step S021: adding isocyanate, HDI adduct and IPDI adduct in a mass ratio of 5:3:2 into a sealed dispersion tank, dispersing at a temperature of 93 to 96° C. and a dispersion rate of 400 to 420 rpm for 10 to 15 minutes to obtain an -NCO-containing core material resin material; Step S022: introducing dry high-pressure air into the sealed dispersion tank so that the pressure in the sealed dispersion tank is maintained at 1.8 to 2.2 times the atmospheric pressure, and spraying the liquid in the sealed dispersion tank intermittently into the methyl acetate solvent in the low-temperature dispersion tank by an airless sprayer, wherein the temperature in the low-temperature dispersion tank is controlled at -20°C, to obtain core material particles C containing -NCO; Step S023: uniformly mixing a trifunctional terminal secondary amino polyether, a polyamide resin and methyl acetate in a mass ratio of 1:9:5 to form an amino resin G; after the temperature in the low-temperature dispersion tank is raised to -5°C, dripping the amino resin G into the low-temperature dispersion tank at a rate of 0.2-0.3 g / min, and simultaneously raising the temperature in the low-temperature dispersion tank to 5°C at a rate of 4 min / °C; the total reaction time is 1.5 h; after the reaction is completed, uniformly lowering the temperature in the low-temperature dispersion tank to -5°C to form a polyurea capsule wall layer on the outer shell of the core particle C under low temperature conditions; Step S024: Pass the prepared capsule particles through a 500-mesh sieve, place the sieved microcapsules in a sealed reaction tank, add 0.02 parts of epoxy resin, maintain the reaction temperature at 25°C, and the dispersion rate at 150 rpm. React for 1 hour to obtain two-component single-wall microcapsules A with a particle size in the range of 20 to 25 μm.
8. The method for preparing an adhesive with self-repairing function according to claim 5, characterized in that: The step S03 includes the following steps: Step S031: uniformly mixing a trifunctional secondary amino-terminated polyether, a polyamide resin, an MDI monomer and methyl acetate in a mass ratio of 5:3:2 to form an amino resin H, and adding the amino resin H into a sealed dispersion tank; Step S032: Dry high-pressure air is introduced into the sealed dispersion tank to maintain the pressure in the sealed dispersion tank at 1.8 to 2.2 times the atmospheric pressure, and the liquid material in the sealed dispersion tank is sprayed intermittently into the methyl acetate solvent in the low-temperature dispersion tank by an airless sprayer, and the temperature in the low-temperature dispersion tank is controlled at -20°C to obtain a -NH n Core material particles D; Step S033: dripping the isocyanate solution into the low-temperature dispersion tank at a rate of 1.8-2.1 g / min, and raising the temperature to 5°C at a rate of 1.8-2.1 min / °C, with a total reaction time of not less than 2 hours, so as to form a polyurea capsule wall layer on the outer shell of the core particle D under low temperature conditions; Step S034: Pass the prepared capsule particles through a 500-mesh sieve, place the sieved microcapsules in a sealed reaction tank, add 0.1 parts of deionized water, maintain the reaction temperature at 25°C, and the dispersion rate at 150 rpm. React for 1 hour to obtain dual-component single-wall microcapsules B with a particle size in the range of 20 to 25 μm.
9. The method for preparing an adhesive with self-repairing function according to any one of claims 6 to 8, characterized in that: The amine value of the trifunctional secondary amino-terminated polyether is 400 mg / KOH / g, and the amine value of the polyamide resin is 420 mg / KOH / g.
10. The method for preparing an adhesive with self-repairing function according to any one of claims 6 to 8, characterized in that: The NCO content of the isocyanate was 16%.
Citation Information
Cited By
Evaluation method for self-repairing performance of epoxy self-repairing resin
CN121068434A