Filler modifier as well as preparation method and application thereof
By using filler modification agents made of raw materials such as sodium nitrate and sodium carbonate, soil hydration and collulation are promoted, the problem of insufficient freezing performance of filler modification agents in the prior art is solved, and efficient anti-freezing and The anti-seepage performance improves the stability and construction efficiency of the roadbed.
Patent Information
- Application Number
- CN202411050288.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-15
AI Technical Summary
The existing filler improvers have insufficient freezing performance in the roadbed in cold areas, which cannot effectively prevent uneven freezing and uneven settlement of the roadbed after freezing, resulting in damage to the roadbed stability.
Use filler modification agent made of raw materials such as sodium nitrate, sodium carbonate, sodium sulfate, calcium chloride, magnesium oxide, calcium carbonate, lime, calcium carbide and silt, and crushed through calcination and heating to form an odorless and non-existent The poisoned gray powdery solid promotes the hydration, oxidation and collization reaction of soil, and improves the soil's resistance to frost swelling, permeability and compressive strength.
It significantly improves the anti-freeze, permeability and compressive strength of the soil, reduces construction costs, can improve soil strength in the early stage, and can be reinforced later through grouting and reinforcement, significantly reduces the freezing rate and permeability, and improves the The smoothness and stability of the roadbed.
Smart Images

Figure BDA0004974713970000061 
Figure BDA0004974713970000071 
Figure BDA0004974713970000072
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of filler modifiers, and in particular to a filler modifier and a preparation method and application thereof. Background Art
[0002] When the soil used for the foundation or roadbed of structures such as railways and highways is silty sand, silt, silty clay or even clay, due to the excessive fine particle content and poor particle grading, it often causes insufficient compressive strength, excessive water content, easy frost heave in winter, etc., causing uneven deformation of the roadbed and posing a safety hazard to trains or moving vehicles. In order to solve this problem, it is often necessary to improve such fillers. Traditional filler improvements mainly use traditional binding materials such as cement, lime, and fly ash. Such materials can improve the compressive strength and stability of the soil, improve the performance of the soil to a certain extent, and have good economic efficiency.
[0003] However, for cold and even extremely cold regions, especially for high-speed railways, the requirements for roadbed smoothness are extremely high, which determines that there are more stringent requirements for the frost heave resistance of the soil. In order to prevent uneven frost heave of the roadbed and uneven settlement after freezing, and maintain the overall stability of the roadbed, the frost heave of the soil must be controlled below the design requirements. However, after the improvement methods such as cement and lime are improved, the frost heave of the filler is still obvious, and the purpose of frost heave resistance cannot be achieved.
[0004] In recent years, with the development of technology and the growth of demand, some new filler modifiers have emerged one after another. There are many types of new filler modifiers, which can be divided into inorganic compounds, organic compounds, biological enzymes, etc. according to their main components.
[0005] Inorganic compound filler modifiers are generally in powder form, and are mostly made of cement, lime, fly ash, various types of slag, coal gangue and other raw materials. When reinforcing soft soil, the active minerals contained in the modifier quickly hydrolyze and hydrate with the free water in the soil to form a mixture of calcium hydroxide, hardened calcium carbonate and adhesive colloids, which can consume a large amount of free water in the soil or fix it in the form of crystal water. After various hydrates of the filler modifier are generated, as the hydration reaction gradually deepens, the improved soil itself continues to harden, and stable crystalline hydrates that are insoluble in water are gradually generated in the soil, increasing the stability and strength of the solidified soil. The disadvantages of this type of modifier are that it is used in large quantities and the early strength is not high; the advantages are low cost and good stability.
[0006] Organic compound filler modifiers are generally liquid, mainly made of one or more polymer materials such as water glass and epoxy resin, and most of them have certain oxidizing and hydrophobic properties. They mainly exchange the charge in the filler water with the charge of the filler particles through ion exchange, thereby reducing the water absorption caused by the filler capillaries, filler pores and surface tension, and making the filler after ion exchange reaction change from "hydrophilic" to "hydrophobic". The disadvantages of this type of modifier are high price, certain oxidation effect on metals, great environmental impact on solidified fillers, and poor durability; the advantages are small dosage, convenient construction, high early strength and easy control, and suitable for most types of soil.
[0007] Bio-enzyme filler modifiers are generally liquid, mostly made from organic matter through fermentation, and are protein-based multi-enzyme products. Their effect on fillers is mainly to adhere to filler particles through bio-enzyme catalysis, and to compact them through external force, thereby improving the adhesion of filler particles and forming a dense, stable and impermeable structure. The disadvantages of this type of modifier are that it has a short lifespan, is greatly affected by the environment, and its strength will decrease after being immersed in water; its main advantage is that it is non-toxic and will not cause pollution to the filler.
[0008] Chinese patent CN107739613A discloses a composite filler modifier for anti-frost heave, which can improve the compressive strength and compactness of soil, and make the soil impermeable and anti-frost heave, so as to prevent the railway and highway subgrades in cold areas from frost heave and meet the purpose of smoothness of the subgrade. However, the performance of the modifier needs to be further improved. Summary of the invention
[0009] The purpose of the present invention is to provide a filler modifier and a preparation method and application thereof, so as to solve the problem of insufficient performance of the filler modifier in the prior art.
[0010] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0011] The present invention provides a filler improver, which is made of the following raw materials in parts by weight:
[0012] 0.2-1.5 parts of sodium nitrate, 2.0-3.0 parts of sodium carbonate, 2.0-3.0 parts of sodium sulfate, 0.05-0.2 parts of calcium chloride, 0.05-0.15 parts of magnesium oxide, 0.5-1.5 parts of calcium carbonate, 0.2-2 parts of lime, 0.1-2 parts of calcium carbide and 20-50 parts of silt sand.
[0013] Preferably, it is made from the following raw materials in parts by weight:
[0014] 0.6-1.0 parts of sodium nitrate, 2.5-2.8 parts of sodium carbonate, 2.3-3.2 parts of sodium sulfate, 0.1-0.15 parts of calcium chloride, 0.07-0.13 parts of magnesium oxide, 0.8-1.1 parts of calcium carbonate, 0.5-1.5 parts of lime, 0.2-1 parts of calcium carbide and 25-45 parts of silt sand.
[0015] Preferably, the raw material of the filler modifier also includes cement.
[0016] Preferably, the weight proportion of the cement is 20-200 parts.
[0017] The present invention also provides a method for preparing the filler improver, comprising the following steps:
[0018] Calcine carbonate and calcium carbide are mixed and calcined to obtain a calcined product;
[0019] The calcined product is mixed with other raw materials and subjected to a heating treatment to obtain a heated product;
[0020] The heated product is crushed to obtain a filler improver.
[0021] Preferably, the calcination temperature is 800-1000°C.
[0022] Preferably, the calcination time is 1 to 3 hours.
[0023] Preferably, the temperature of the heating treatment is 400-600°C.
[0024] Preferably, the heating treatment time is 1 to 3 hours.
[0025] The present invention also provides the use of the above-mentioned filler improver or the filler improver prepared by the above-mentioned preparation method in improving the frost heave resistance, impermeability, compressive strength and stability of soil.
[0026] Beneficial effects of the present invention:
[0027] After the filler improver provided by the present invention is fully stirred with the filler, a chain chemical reaction of dissolution, crystallization, absorption, diffusion and recrystallization occurs, and then under the action of mechanical load, the soil structure is changed, the capillaries are destroyed, and ordinary soil is improved into dense, uniform, high-strength, durable, impermeable and frost-resistant high-quality improved soil.
[0028] By using the filler improver provided by the present invention, there is no need to replace the original filler, and the filler that does not meet the design requirements can be improved on-site, thereby reducing construction costs; fillers with too high fine particle content such as silt sand, silt soil, silty clay, and clay can be improved; the early strength of the soil body can be improved, thereby improving construction efficiency; the improved filler has impermeability and frost heave resistance; after being fully mixed with the filler, it can be filled in the roadbed or other structures, and can also be filled into the roadbed or floor by grouting at a later stage, playing a role of reinforcement and frost heave resistance. DETAILED DESCRIPTION
[0029] The present invention provides a filler improver, which is made of the following raw materials in parts by weight:
[0030] 0.2-1.5 parts of sodium nitrate, 2.0-3.0 parts of sodium carbonate, 2.0-3.0 parts of sodium sulfate, 0.05-0.2 parts of calcium chloride, 0.05-0.15 parts of magnesium oxide, 0.5-1.5 parts of calcium carbonate, 0.2-2 parts of lime, 0.1-2 parts of calcium carbide and 20-50 parts of silt sand, preferably: 0.6-1.0 parts of sodium nitrate, 2.5-2.8 parts of sodium carbonate, 2.3-3.2 parts of sodium sulfate, 0.1-0.15 parts of calcium chloride, 0.07-0.13 parts of magnesium oxide, 0.8-1.1 parts of calcium carbonate, 0.5-1.5 parts of lime, 0.2-1 parts of calcium carbide and 25-45 parts of silt sand; in the present invention, the raw materials of the filler modifier also preferably include cement, and the weight proportion of the cement is preferably 20-200 parts.
[0031] In the present invention, sodium nitrate undergoes double decomposition with inorganic salts in the filler to play an oxidizing role; sodium carbonate can undergo double decomposition with alkali such as calcium hydroxide in the soil to generate precipitates and sodium hydroxide; sodium carbonate can undergo double decomposition with calcium salts, barium salts, etc. in the soil to generate precipitates; sodium sulfate can generate cement hydration products more quickly, thereby accelerating the hydration and hardening speed of cement; calcium chloride aqueous solution can accelerate the hardening of cement and increase the cold resistance of cement mortar, and has an antifreeze effect; calcium carbonate has a good affinity with the gel in the soil, which can accelerate the cross-linking reaction of the gel and enhance the stability of the soil; magnesium oxide is mixed with minerals in the soil to generate gel hardening; cement provides a variety of active minerals; silt sand provides a skeleton attachment effect, and each component combines with calcium carbide to play a synergistic role, which can enable the filler improver to achieve the best effect.
[0032] The present invention also provides a preparation method of the above-mentioned filler improver, comprising the following steps: mixing calcium carbonate and calcium carbide and calcining to obtain a calcined product; mixing the calcined product with other raw materials and performing heat treatment to obtain a heated product; crushing the heated product to obtain a filler improver; the calcination temperature of the present invention is preferably 800-1000°C; the calcination time is preferably 1-3h; the heating treatment temperature is preferably 400-600°C; and the heating treatment time is preferably 1-3h.
[0033] The filler modifier obtained by the preparation method of the present invention is an odorless, non-toxic gray powder solid, which works through the following three reactions:
[0034] First, the hydration of cement particles in the soil is accelerated and the cement is nearly completely hydrated: after the filler composite modifier is added to the cement, electrolytes are produced, which weakens the tension between water molecules, accelerates the rupture of cement particles, and increases the specific surface area of cement, thereby accelerating the hydration of cement and ultimately making the cement completely hydrated. At the same time, the formation of a large amount of cement slurry increases the density of the soil.
[0035] Secondly, accelerate the oxidation reaction of metal components in the soil: the filler composite modifier can produce an oxidation reaction with the metal elements contained in the cement or filler, and the concentration of the produced electrolyte will increase as the oxidation proceeds. The higher the concentration of the electrolyte solution, the faster the metal elements in the filler oxidize, and the better the solidification effect of the soil.
[0036] Finally, the mixed soil in the filler is gelled: the cement particles are completely hydrated to form a high-concentration cement slurry, which acts on the soil particles. As time goes by, a large amount of colloidal components and crystalline hydrates with high chemical inertness and plastic strength are formed in the soil. These colloidal components and crystalline hydrates serve as fillings for pores, cracks, and holes in strata or soil, and also as cementing materials for soil particles.
[0037] The technical solution provided by the present invention produces the effects of solidifying soil and resisting frost heaving from two aspects. First, the sodium nitrate, sodium carbonate, calcium carbonate, magnesium oxide and the like in its components react with substances in the soil and components in cement to play a role in reinforcing fillers and resisting frost heaving; second, sodium carbonate, sodium sulfate, calcium chloride and the like can stimulate and promote the cement hydration reaction, so that the cement is nearly completely hydrated in a short period of time (when cement is used normally, the cement hydration reaction does not occur sufficiently in a short period of time, and it usually takes decades or even hundreds of years to be completely hydrated), giving full play to the performance of cement, improving the consolidation degree of the soil being acted on, and making the soil more solidified, stronger and more resistant to frost heaving in a short period of time.
[0038] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0039] Example 1
[0040] 1. The proportion of each component: 0.6kg sodium nitrate, 2.5kg sodium carbonate, 3.1kg sodium sulfate, 0.1kg calcium chloride, 0.11kg magnesium oxide, 1kg calcium carbonate, 45kg cement, 0.6kg lime, 0.35kg calcium carbide, and 40kg silt sand.
[0041] 2. First, grind the block and granular raw materials, namely calcium chloride, magnesium oxide, calcium carbonate and calcium carbide into powder for later use.
[0042] 3. Mix calcium carbonate and calcium carbide in proportion and heat to 900°C, maintain for 2 hours, and fully calcine. After cooling, add sodium nitrate, sodium carbonate, sodium sulfate, cement and silt sand in proportion, mix, heat from room temperature to 450°C, and maintain this temperature for 2 hours;
[0043] 4. The calcined mixture is ground into powder again and fully stirred in a stirring device to complete the preparation of the improver.
[0044] Example 2
[0045] 1. Proportion of each component: 1.0kg sodium nitrate, 2.8kg sodium carbonate, 2.4kg sodium sulfate, 0.13kg calcium chloride, 0.13kg magnesium oxide, 0.8kg calcium carbonate, 65kg cement, 1.5kg lime, 0.9kg calcium carbide, 30kg silt sand.
[0046] 2. First, grind the block and granular raw materials, namely calcium chloride, magnesium oxide, calcium carbonate and calcium carbide into powder for later use.
[0047] 3. Mix calcium carbonate and calcium carbide in proportion and heat to 900°C, maintain for 2 hours, and fully calcine. After cooling, add sodium nitrate, sodium carbonate, sodium sulfate, cement and silt sand in proportion, mix, heat from room temperature to 450°C, and maintain this temperature for 2 hours;
[0048] 4. The calcined mixture is ground into powder again and fully stirred in a stirring device to complete the preparation of the improver.
[0049] Experimental example
[0050] After the silt sand was improved with the improver, the unconfined compressive strength, permeability test and frost heave test were carried out. The test plan is as follows:
[0051] Test mix ratio
[0052] The improved raw materials are made of silt sand and clay, the mass ratio of silt sand and clay is 7:3, and the maximum dry density is 1.92g / cm 3The optimum moisture content is 12.5%, the compaction coefficient of the test piece is K=0.95, the cement content is 8.0% of the total mass of silt sand and clay, and the modifier content of Example 1 of the present invention is 2.0% of the cement mass.
[0053] According to the "Railway Engineering Geotechnical Test Code" (TB10102-2010), the following tests are carried out:
[0054] ①7-day saturated unconfined compressive strength
[0055] ②12 freeze-thaw cycles of unconfined compressive strength test of chemically improved soil: Freeze-thaw cycle conditions for unconfined compressive strength: freezing at -20℃ for 24h, immersion in water at 25℃ for 24h, which is one freeze-thaw cycle.
[0056] ③6 freeze-thaw cycle frost heave rate tests: Freeze-thaw cycle conditions of frost heave test: After completing the frost heave test, soak in water at 25℃ for 24h, and then carry out the next test, which is a freeze-thaw cycle frost heave rate test.
[0057] ④ Permeability test after 28 days of curing
[0058] The results are shown in Table 1 below:
[0059] Table 1 Test results of unconfined compressive strength, permeability test and frost heave test
[0060]
[0061]
[0062] Table 2 Results of frost heave rate test after 6 freeze-thaw cycles
[0063]
[0064] The test results show that after 12 freeze-thaw cycles, the strength of the silt sand treated with the improver did not decrease, but increased by 14.8% to 2.25 MPa; after 6 freeze-thaw cycles, the frost heave rate showed no upward trend, and the average frost heave rate of 6 freeze-thaw cycles was only 0.29%, with almost no frost heave; in addition, the permeability coefficient of the improved silt sand was 10 -4 cm / s-10 -5 cm / s level, with good anti-seepage effect.
[0065] In summary, the improver provided by the present invention has excellent anti-frost heave and anti-permeability properties, as well as the effect of improving the strength of the filler. The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be regarded as the protection scope of the present invention.
Claims
1. A filler improver, It is characterized in that Made from the following raw materials in parts by weight: 0.2-1.5 parts of sodium nitrate, 2.0-3.0 parts of sodium carbonate, 2.0-3.0 parts of sodium sulfate, 0.05-0.2 parts of calcium chloride, 0.05-0.15 parts of magnesium oxide, 0.5-1.5 parts of calcium carbonate, 0.2-2 parts of lime, 0.1-2 parts of calcium carbide and 20-50 parts of silt sand.
2. The filler modifier according to claim 1, It is characterized in that Made from the following raw materials in parts by weight: 0.6-1.0 parts of sodium nitrate, 2.5-2.8 parts of sodium carbonate, 2.3-3.2 parts of sodium sulfate, 0.1-0.15 parts of calcium chloride, 0.07-0.13 parts of magnesium oxide, 0.8-1.1 parts of calcium carbonate, 0.5-1.5 parts of lime, 0.2-1 parts of calcium carbide and 25-45 parts of silt sand.
3. The filler modifier according to claim 1, It is characterized in that The raw material of the filler modifier also includes cement.
4. The filler modifier according to claim 3, It is characterized in that The weight proportion of the cement is 20-200 parts.
5. A method for preparing the filler modifier according to any one of claims 1 to 4, It is characterized in that The following steps are involved: Calcine carbonate and calcium carbide are mixed and calcined to obtain a calcined product; The calcined product is mixed with other raw materials and subjected to a heating treatment to obtain a heated product; The heated product is crushed to obtain a filler improver.
6. The preparation method according to claim 5, It is characterized in that The calcination temperature is 800-1000°C.
7. The preparation method according to claim 6, It is characterized in that The calcination time is 1 to 3 hours.
8. The preparation method according to claim 5, It is characterized in that The temperature of the heating treatment is 400-600°C.
9. The preparation method according to claim 8, It is characterized in that The heating treatment time is 1 to 3 hours.
10. Use of the filler modifier according to any one of claims 1 to 4 or the filler modifier prepared by the preparation method according to claims 5 to 9 in improving the frost heave resistance, impermeability, compressive strength and stability of soil.