Method for avoiding material suspension during blow-in of large blast furnace

By accurately calculating the batching and optimizing the loading position, combined with full-port air supply and parameter control, the problems of suspended and collapsing materials during the start-up of large blast furnaces have been solved, achieving stable and smooth start-up and reducing costs.

CN118957181APending Publication Date: 2024-11-15BAOTOU IRON & STEEL (GROUP) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410908289.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

During the start-up of a large blast furnace, improper charging and distribution positions can lead to poor permeability inside the furnace, resulting in phenomena such as suspended material and material collapse, which affect the smoothness of start-up and cost.

Method used

By accurately calculating the batching, optimizing the loading position, controlling the air supply through all vents and parameters, a stable softening zone is formed, ensuring uniform distribution of coal and gas flow, avoiding material suspension, and achieving rapid production.

Benefits of technology

This has enabled stable and smooth operation of large blast furnaces during startup, reduced costs, improved production efficiency, increased output, and reduced fuel consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957181A_ABST
    Figure CN118957181A_ABST
Patent Text Reader

Abstract

The invention discloses a method for avoiding material suspension during blow-in of a large blast furnace. The method comprises the following steps: (1) precise burdening calculation; (2) loading of opening furnace burden; (3) igniting and supplying air; (4) controlling parameters; (5) slag iron is calculated, the air volume is required to be 70-75% of the full air level during first iron tapping, and after first iron tapping, the air volume is increased to 80% of the full air level; (6) load adjustment is conducted, specifically, the load is adjusted every 10 batches of materials from the time after air supply to the time before tapping, and the load is + 0.04 t / t to 0.06 t / t; adjusting according to 0.1-0.15 t / t after tapping, and adjusting according to 0.2 t / t after tapping for the first time. According to the invention, the formation process of the stable soft melting belt is realized by accurately calculating the loaded material, optimizing the loading position and supplying air at the whole tuyere; and the innovative control of the first slag iron tapping time is calculated according to material batches, so that the later-stage gas flow distribution is stabilized, the stable and smooth blow-in of the large blast furnace is promoted, and the purposes of quickly reaching the production and reducing the cost are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of opening a large blast furnace in the metallurgical industry, and in particular relates to a method for preventing hanging materials from opening a large blast furnace. Background Art

[0002] At present, with the requirements of environmental protection and modernization of blast furnace ironmaking, blast furnace ironmaking has gradually become large-scale. The large-scale blast furnace system is relatively complex, especially the start-up and shutdown of the furnace, and the smooth start-up requires high technical reserves. The determination of the proportion of the starting charge of a large blast furnace and the accurate calculation of the parameters are the basis for starting the furnace. The core technology for a smooth start-up is the method and position of loading the charge, which is the key to determining the smooth start-up of the blast furnace.

[0003] The calculation of traditional blast furnace charge takes the slag basicity and Al2O3 content in the slag as important reference indicators, and ensures the air permeability in the furnace by reasonably matching sintered ore, pelletized ore, silica, limestone, etc., to create conditions for rapid air addition and production of the blast furnace. However, due to inappropriate charging and distribution positions, the air permeability in the furnace deteriorates during the formation of the soft melting zone at the start of the furnace, resulting in a gradual reduction in the rhythm and space of air addition, which ultimately leads to the phenomenon of suspended material, collapsed material, and pipeline during the furnace opening process.

[0004] Based on this, the present invention aims to stabilize the soft melting zone formation process and gas flow distribution through innovative control of charging and distribution methods, air supply and slag iron calculation, so as to promote stable and smooth operation of large blast furnaces and achieve the purpose of rapid production and cost reduction. Summary of the invention

[0005] The purpose of the present invention is to provide a method for avoiding hanging materials during the opening of a large blast furnace, and to achieve a stable soft melting zone formation process by accurately calculating the charging material, optimizing the charging position, and supplying air through the entire tuyere; innovative control of the first slag and iron discharge time calculated according to the material batch is adopted, thereby stabilizing the later coal gas flow distribution, and promoting the large blast furnace to achieve stable and smooth opening, and realize the purpose of rapid production and cost reduction.

[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0007] The present invention discloses a method for preventing suspended materials during opening of a large blast furnace, comprising:

[0008] (1) Accurate batching calculation: Scan the entire furnace volume to determine the charging volume, add silica and limestone to the material structure and the starting charge, control the coke ratio of the entire slag, set the average slag basicity at 0.95 to 1.00 times to ensure that the slag has good fluidity; the coke ratio of the entire furnace is controlled at 3.4-3.6t / t, and the first furnace molten iron [Si] is set at 2.9-3.1%; confirm the basicity, load, and compression rate of different parts;

[0009] (2) Loading of furnace materials

[0010] Before blasting, the furnace hearth, furnace belly, furnace waist, furnace body and furnace throat are charged; the charge is charged to the specified charge line; the furnace belly is charged with all clean coke, the furnace waist is charged with empty coke, and it is ensured that all coke is below the furnace waist; the light load charge at the bottom is combined and loaded when it is actually loaded because the ore batch is small; the loading position is the last batch of each section of charge; the furnace body is set with 12 sections of charge according to different loads, basicity and compression rates;

[0011] (3) Ignition and air supply

[0012] After the air is supplied, the soft melting zone is gradually formed. The hot gas generated by the burning of sleepers and coke in the furnace rises, and gradually conducts mass transfer and heat transfer reactions on each section of the furnace charge. The temperature of each section of the furnace charge gradually increases, so that the furnace charge on the upper part of the tuyere zone gradually begins to soften and melt with the increase in temperature, forming a soft melting zone. The key technology to avoid the furnace opening without hanging materials is: opening the central air flow channel to keep the gas channel in the furnace smooth; adopting full-open tuyere air supply, uniform circumferential air intake, which is conducive to the uniform formation of the soft melting zone and uniform material discharge, and can eliminate deviation and collapse of materials;

[0013] (4) Parameter control

[0014] After the air is supplied, the appropriate air volume is controlled and the material is added according to the specified system and material line. The air temperature is set to 750±10℃ and the moisture content is set to 24-26g / m 3 , control the theoretical combustion temperature; in the first 4 hours, the air-adding rhythm can be faster, and during the formation of the soft melting zone, the air-adding rhythm can be slowed down to control the pressure difference. After the soft melting zone is formed 10 hours later, the air-adding rhythm can be faster; to achieve stable control of the thermal system in the furnace during the rising air volume level, effectively avoiding the generation of suspended materials due to the formation of the soft melting zone during the blast furnace opening process, and achieving rapid blast furnace compliance and production;

[0015] (5) Calculation of slag iron

[0016] When tapping the iron for the first time, the air volume is required to be 70-75% of the full air level. After the first tapping, the air volume is increased to 80% of the full air level.

[0017] (6) Load adjustment

[0018] From air supply to iron tapping, adjust the load by +0.04-0.06t / t for every 10 batches of materials; after iron tapping, adjust by 0.1-0.15t / t; after the first iron tapping, adjust by 0.2t / t.

[0019] Furthermore, the coke ratio of the whole furnace is controlled at 3.5t / t, and the [Si] of the first furnace molten iron is set at 3.0%.

[0020] Furthermore, it is ensured that all the material below 22.4m of the material line is coke;.

[0021] Furthermore, the air temperature is set to 750°C and the moisture content is set to 25g / m 3 , control the theoretical combustion temperature.

[0022] Furthermore, the load is adjusted every 10 batches of material, +0.05t / t.

[0023] Compared with the prior art, the beneficial technical effects of the present invention are:

[0024] Through accurate calculation of the charging material, optimization of the charging position and air supply through the entire tuyere, a stable soft melting zone formation process is achieved; innovative control of the first slag and iron discharge time calculated according to the batch of materials stabilizes the distribution of coal gas flow in the later stage, enabling large blast furnaces to achieve stable and smooth start-up, and realize rapid production and cost reduction.

[0025] The present invention optimizes the start-up of large blast furnaces. In April 2023, Baosteel's No. 8 blast furnace was successfully started and reached full production in three days. The completion results are compared with the output and fuel ratio of No. 8 blast furnaces in 2015 as follows:

[0026] In 2015, the average output of the 8 blast furnaces in the first month after opening was 8098t / d, and the fuel ratio was 538.5kg / t; in 2023, the output was 8873t / d, and the fuel ratio was 535.02kg / t. The output of the blast furnaces in 2023 increased by 775t / d, and the fuel ratio decreased by 3.48kg / t;

[0027] Calculated at 3168 yuan per ton of iron, the cost reduction is 775*3168*30=73656000 yuan;

[0028] Calculated at 2.56 yuan per kg of fuel, the cost reduction is 8873*2.56*30=6814464 yuan;

[0029] The total cost reduction is approximately RMB 74.3374 million. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] The present invention will be further described below in conjunction with the accompanying drawings.

[0031] Figure 1 This is the trend interface of 8# blast furnace;

[0032] Figure 2 The material list and material distribution angle for the 8# blast furnace;

[0033] Figure 3 This is the charge distribution angle for the 8# blast furnace. DETAILED DESCRIPTION

[0034] In order to better explain the present invention, the main contents of the present invention are further explained below in combination with the opening process of Baotou Steel's No. 8 blast furnace at the end of March, but the contents of the present invention are not limited to the following embodiments.

[0035] The effective volume of Baosteel's 8# blast furnace is 4150m 3 , 38 tuyere and 4 iron mouth. The furnace was started on October 12, 2015. Due to the design of the hot blast pipe system, the blast furnace was shut down on February 7, 2023 using an empty material line to lower the material level. The repair took 52 days. The hot blast pipe system was replaced and the lining was sprayed from the tuyere belt to the lower edge of the steel bricks at the throat of the blast furnace.

[0036] Before opening the furnace, the material structure of the furnace is

[0037] (1) Accurate batching calculation: Scan the entire furnace volume to determine the charging volume, add silica and limestone to the material structure and the starting charge, control the coke ratio of the entire slag, and set the average slag basicity at 0.95 to 1.00 times to ensure that the slag has good fluidity. The coke ratio of the entire furnace is controlled at 3.5t / t, and the first furnace molten iron [Si] is set at 3.0%. The basicity, load, and compression rate of different parts are confirmed, as shown in Table 1.

[0038] Table 1 Parameter settings

[0039]

[0040] (2) Loading

[0041] Table 28# Blast Furnace Start-up Materials List

[0042]

[0043] Based on the quantitative principles of furnace start-up technology and combined with the specific conditions of blast furnace start-up, the nodes and control principles of each stage in the furnace start-up process were calculated and planned, and the various parameters of the start-up process were detailed.

[0044] Before blasting, the furnace hearth, furnace belly, furnace waist, furnace body and furnace throat are charged; the charge is charged to the specified charge line. The furnace belly is charged with all clean coke, and the furnace waist is charged with empty coke, and it is ensured that all coke is below the furnace waist (charge line 22.4m). The lower light load charge is combined and loaded when it is actually loaded because the ore batch is small. The loading position is the last batch of each section of the charge. The furnace body is set with 12 sections of charge according to different loads, basicity and compression rates.

[0045] See the material list and material distribution angle of 8# blast furnace opening Figure 2 ; 8# blast furnace opening charge angle see Figure 3 .

[0046] (3) Ignition and air supply

[0047] After the air is supplied, the soft melting zone is gradually formed, and the hot gas generated by the burning of the sleepers and coke in the furnace hearth rises, gradually conducting mass transfer and heat transfer reactions on each section of the charge. The temperature of each section of the charge gradually increases, causing the charge on the upper part of the tuyere zone to gradually soften and melt as the temperature rises, forming a soft melting zone. The key technology to avoid the furnace being opened without hanging charge is to open the central air flow channel, thereby keeping the gas channel in the furnace smooth. Fully open the tuyere to supply air, and the circumferential air intake is uniform, which is conducive to the uniform formation of the soft melting zone and uniform material discharge, and can eliminate deviation and collapse of the material. Figure 1 shown.

[0048] (4) Parameter control

[0049] After the air is supplied, the appropriate air volume is controlled and the material is added according to the specified system and material line. The air temperature is set to 750℃ and the moisture content is set to 25g / m 3 , control the theoretical combustion temperature. In the first 4 hours, the air-adding rhythm can be faster. During the formation of the soft melting zone, slow down the air-adding and control the pressure difference. After the soft melting zone is formed 10 hours later, the air-adding rhythm can be faster. Stable control of the thermal system in the furnace is achieved during the rising of the air volume level, effectively avoiding the generation of suspended materials due to the formation of the soft melting zone during the blast furnace opening process, and achieving the blast furnace to quickly reach the standard and production.

[0050] (5) Calculation of slag iron

[0051] The traditional blast furnace slag iron is calculated by the cumulative air volume, which is greatly affected by the accuracy of the air volume meter and the time of gas delivery. In addition, due to the influence of the furnace load, the air consumption per ton of coke varies greatly, which easily leads to a large gap between the slag iron and the theoretical amount, and the iron-tapping time cannot be accurately determined. When the iron is tapped for the first time, the air volume is required to be 70-75% of the full air level. After the first iron tapping, the air volume is increased to 80% of the full air level.

[0052] (6) Load adjustment

[0053] From air supply to iron tapping, adjust the load by +0.05t / t every 10 batches of materials; after iron tapping, adjust by 0.1-0.15t / t; after the first iron tapping, adjust by 0.2t / t.

[0054] The air volume during this furnace opening was relatively large and stable, the furnace condition did not fluctuate, and active retreat was carried out when the soft melting zone was formed, achieving accurate iron tapping and reaching full production in three days in the later stage.

[0055] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for preventing hanging materials during the opening of a large blast furnace, characterized in that: include: (1) Accurate batching calculation: Scan the entire furnace volume to determine the charging volume, add silica and limestone to the material structure and the starting charge, control the coke ratio of the entire slag, set the average slag basicity at 0.95 to 1.00 times to ensure that the slag has good fluidity; the coke ratio of the entire furnace is controlled at 3.4-3.6t / t, and the first furnace molten iron [Si] is set at 2.9-3.1%; confirm the basicity, load, and compression rate of different parts; (2) Loading of furnace materials Before blasting, the furnace hearth, furnace belly, furnace waist, furnace body and furnace throat are charged; the charge is charged to the specified charge line; the furnace belly is charged with all clean coke, the furnace waist is charged with empty coke, and it is ensured that all coke is below the furnace waist; the light load charge at the bottom is combined and loaded when it is actually loaded because the ore batch is small; the loading position is the last batch of each section of charge; the furnace body is set with 12 sections of charge according to different loads, basicity and compression rates; (3) Ignition and air supply After the air is supplied, the soft melting zone is gradually formed. The hot gas generated by the burning of sleepers and coke in the furnace rises, and gradually conducts mass transfer and heat transfer reactions on each section of the furnace charge. The temperature of each section of the furnace charge gradually increases, so that the furnace charge on the upper part of the tuyere zone gradually begins to soften and melt with the increase in temperature, forming a soft melting zone. The key technology to avoid the furnace opening without hanging materials is: opening the central air flow channel to keep the gas channel in the furnace smooth; adopting full-open tuyere air supply, uniform circumferential air intake, which is conducive to the uniform formation of the soft melting zone and uniform material discharge, and can eliminate deviation and collapse of materials; (4) Parameter control After the air is supplied, the appropriate air volume is controlled and the material is added according to the specified system and material line. The air temperature is set to 750±10℃ and the moisture content is set to 24-26g / m 3 , control the theoretical combustion temperature; in the first 4 hours, the air-adding rhythm can be faster, and during the formation of the soft melting zone, the air-adding rhythm can be slowed down to control the pressure difference. After the soft melting zone is formed 10 hours later, the air-adding rhythm can be faster; to achieve stable control of the thermal system in the furnace during the rising air volume level, effectively avoiding the generation of suspended materials due to the formation of the soft melting zone during the blast furnace opening process, and achieving rapid blast furnace compliance and production; (5) Calculation of slag iron When tapping the iron for the first time, the air volume is required to be 70-75% of the full air level. After the first tapping, the air volume is increased to 80% of the full air level. (6) Load adjustment From air supply to iron tapping, adjust the load by +0.04-0.06t / t for every 10 batches of materials; after iron tapping, adjust by 0.1-0.15t / t; after the first iron tapping, adjust by 0.2t / t.

2. The method for avoiding hanging materials during opening of a large blast furnace according to claim 1, characterized in that: The coke ratio of the entire furnace is controlled at 3.5t / t, and the [Si] of the first furnace molten iron is set at 3.0%.

3. The method for avoiding hanging materials during opening of a large blast furnace according to claim 1, characterized in that: And ensure that all the material below 22.4m of the material line is coke.

4. The method for avoiding hanging materials during opening of a large blast furnace according to claim 1, characterized in that: The air temperature is set to 750°C and the moisture content is set to 25g / m 3 , control the theoretical combustion temperature.

5. The method for avoiding hanging materials during opening of a large blast furnace according to claim 1, characterized in that: Adjust the load every 10 batches of materials, +0.05t / t.