Method for producing automobile steel with high scrap ratio from vanadium-containing molten iron and automobile steel

By adopting a combination process of light and thin scrap steel and biomass carbon powder in the production of vanadium-containing iron, the problems of low scrap steel consumption and difficult production are solved, and the production of automobile steel with a high scrap steel ratio is achieved, and resource utilization and production efficiency are improved. , reduces environmental impact.

CN118957196APending Publication Date: 2024-11-15PANZHIHUA IRON & STEEL RES INST OF PANGANG GROUP
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411170865.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing technology is difficult to effectively produce vanadium-containing iron, which leads to low consumption of scrap steel, difficult to produce green steel, and cannot be used in enterprises that directly reduce vanadium-titanium magnetite.

Method used

Through precise process control, thin and light scrap steel is used as coolant for converter vanadium extraction, combined with electrode heating and biomass carbon powder to increase carbonization, optimize the ratio of scrap steel to other metal materials, and achieve high scrap steel ratio production.

Benefits of technology

The proportion of scrap steel used is increased, production costs are reduced, and the production of automobile steel with a high scrap steel ratio is achieved. The product quality is stable, the process is simple, and energy consumption and greenhouse gas emissions are reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957196A_ABST
    Figure CN118957196A_ABST
Patent Text Reader

Abstract

The invention discloses a method for producing automobile steel with a high scrap ratio from vanadium-containing molten iron and the automobile steel. The method comprises the following steps that S1, converter vanadium extraction and blowing desulfurization are conducted, specifically, light and thin scrap steel is adopted as a cooling agent for converter vanadium extraction for temperature control, and the final temperature is controlled to range from 1360 DEG C to 1400 DEG C; s2, LF heating and recarburization are conducted, specifically, the desulfurized molten iron is hoisted to an LF procedure, semisteel heating is conducted in an electrode heating mode, biomass carbon powder is added for semisteel recarburization, and 3-5 kg / (t steel) of silicon iron is added before the molten iron is discharged from a station; s3, converter smelting is conducted, specifically, the heated semisteel is added into a steelmaking converter, high-carbon waste steel is added before iron is added, and the final temperature of the converter is controlled to be 1630-1650 DEG C; and S4, RH forced decarburization, powder spraying desulfurization and continuous casting are conducted. Through accurate process control, the production target of high scrap steel ratio of the coolant is achieved, and the ratio of the scrap steel to other metal materials is optimized, so that the problems of low scrap steel consumption and high green steel production difficulty caused by large loss of heat in the vanadium extraction process are effectively solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of steel smelting, and in particular to a method for producing automobile steel with a high scrap steel ratio from vanadium-containing molten iron and the automobile steel. Background Art

[0002] Green and low-carbon is one of the important development themes of the world's steel industry. Comprehensive decarbonization will be a huge challenge facing the world's steel industry. In order to achieve this goal, the world's major economies have launched their own low-carbon roadmaps for the steel industry, and advanced technologies such as "hydrogen-based reduction-electric furnace steelmaking" and "CO2 capture, recovery and storage" have also emerged. However, these technologies are still in the research and development stage. Especially with the downturn in the international economy, shortage of raw materials and turbulent political situation, there is great uncertainty in technology research and development. Before these technologies mature, transitional technologies are needed to support the steady advancement of low-carbon and green development in the steel industry. Solving the increasingly prominent problems of excessive resource consumption, large carbon emissions and continuous accumulation of metallurgical slag in the steel industry is the only way for the current green, low-carbon and sustainable development of the steel industry. With the implementation of my country's dual-carbon strategy, the operation of the EU Carbon Border Adjustment Mechanism (CBMA), and the promotion of carbon footprint assessment (LCA) of the entire life cycle of steel products, the development of low-carbon emission and green production technologies in the current steel industry is imminent, and domestic and foreign steel companies, universities and research and development institutions have also carried out a lot of work. At present, with the severe shortage of resources such as hydrogen-based direct reduced iron, the production of low-carbon green steel products characterized by social scrap steel + green electricity has become a focus of research and development.

[0003] Green steel refers to steel products with low comprehensive carbon emissions per ton of steel produced by using hot metal produced with scrap steel or green non-carbon reducing agents and using green electricity as energy. Benxi Steel has realized the process of producing green automobile plates with 100% scrap steel as raw materials by using the model of electric furnace + green electricity; Shougang Jingtang has achieved continuous production of green steel with a large scrap steel ratio of 50% in the converter, with the number of continuous casting furnaces reaching 7; Hesteel Group has carried out relevant research on the production of green steel based on direct reduced iron + blast furnace hot metal; Posco, South Korea is also developing a complete set of technologies based on direct reduced iron production technology + smelting furnace / electric furnace to produce green steel. However, these technologies cannot be applied to enterprises that use vanadium-containing molten iron for steelmaking. The main reason is that vanadium-titanium magnetite has not been used to directly reduce molten iron, and the carbon content of vanadium-containing molten iron produced by blast furnace is only 4.0%~4.3%, much lower than the 4.5% of ordinary blast furnace molten iron; the content of [Si]+[Mn] in the molten iron is only 0.3%~0.5%, much lower than the content of more than 1.0% in ordinary blast furnace molten iron; the molten iron temperature is only 1450℃, which is also lower than the iron-out temperature of more than 1500℃ of ordinary molten iron; and the vanadium-containing molten iron needs to be blown with oxygen to extract vanadium, and the thermal mass elements are lost, resulting in scrap steel consumption far less than ordinary molten iron. Therefore, it is extremely difficult to produce green steel with vanadium-containing molten iron.

[0004] In view of this, the existing technology should be improved. Summary of the invention

[0005] The main purpose of the present invention is to provide a method for producing high scrap steel ratio automobile steel from vanadium-containing molten iron and a vanadium-iron alloy. Through precise process control, the production target of high scrap steel ratio of coolant is achieved, and the ratio of scrap steel to other metal materials is optimized, thereby effectively coping with the problems of low scrap steel consumption and difficulty in producing green steel caused by large amount of heat loss in the vanadium extraction process.

[0006] According to one aspect of the present invention, a method for producing high scrap ratio automotive steel from vanadium-containing molten iron is provided, which comprises the following steps: S1. Converter vanadium extraction and injection desulfurization: Converter vanadium extraction uses light scrap steel as a coolant for temperature control. The amount of light scrap steel added accounts for 20-40% of the total amount of metal materials added, and the terminal temperature is controlled at 1360-1400℃; S2, LF heating and carbon increase: After desulfurization, the molten iron is hoisted to the LF process, and the semi-steel is heated by electrode heating, and biomass carbon powder is added to increase the carbon of the semi-steel. Before leaving the station, 3~5kg / (t steel) of ferrosilicon is added; S3, converter smelting: after heating, the semi-steel is added into the steelmaking converter, and high carbon scrap steel is added before adding iron, and the final temperature of the converter is controlled at 1630~1650℃; S4, RH forced decarburization, powder spray desulfurization, continuous casting: After steelmaking, the molten steel undergoes RH forced decarburization and powder spray desulfurization, and the continuous casting process is carried out according to the preset steel type.

[0007] According to one embodiment of the present invention, high-carbon scrap steel is scrap steel with a carbon content > 0.75%, and thin scrap steel is small-sized scrap steel after pretreatment. The maximum dimensions of the length, width and height of the thin scrap steel are < 150 mm and the weight of a single piece is < 5 kg.

[0008] According to one embodiment of the present invention, in step S2, the heating time of the electrode heating is 30-60 minutes, and the carbon content of the semi-steel after carburization is ≥4.5%.

[0009] According to one embodiment of the present invention, step S2 further includes adopting a production mode of two LF furnaces corresponding to one steelmaking converter to ensure continuous production of the steelmaking converter.

[0010] According to one embodiment of the present invention, the biomass carbon powder is obtained by high-temperature carbonization of plants using green electricity energy, and the plants include rice husks and / or straws and / or branches and / or leaves.

[0011] According to one embodiment of the present invention, in step S3, the amount of high carbon scrap steel added is 30-50% of the nominal capacity of the converter.

[0012] According to one embodiment of the present invention, in step S2, the amount of biomass carbon powder added is 5-10 kg / t iron.

[0013] According to one embodiment of the present invention, in step S1, the metal material includes solid iron and scrap steel.

[0014] According to one embodiment of the present invention, the electric energy used in the method is clean energy, and the clean energy includes wind power generation and / or photovoltaic power generation.

[0015] According to another aspect of the present invention, a steel for automobile is provided, which is prepared by any method of the above technical solutions.

[0016] In a method for producing automotive steel with a high scrap steel ratio from vanadium-containing molten iron according to an embodiment of the present invention, the production target of a high scrap steel ratio is achieved through precise process control, and the ratio of scrap steel to other metal materials is optimized, thereby effectively addressing the problems of low scrap steel consumption and difficulty in producing green steel caused by a large amount of heat loss during the vanadium extraction process. This method has the advantages of stable product quality and simple process. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the technical solution of the embodiment of the present invention, the drawings required for use in the embodiment will be briefly introduced below. Obviously, the drawings described below are only some implementation cases of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0018] Figure 1 A process flow chart of a method for producing high scrap steel ratio automobile steel from vanadium-containing molten iron according to an exemplary embodiment of the present invention is shown. DETAILED DESCRIPTION

[0019] The detailed description of the following embodiments is used to exemplify the principles of the present invention, but cannot be used to limit the scope of the present invention. The present invention can be implemented in many different forms and is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.

[0020] The present invention provides these embodiments to make this disclosure thorough and complete, and fully express the scope of the present invention to those skilled in the art. It should be noted that unless otherwise specifically stated, the relative arrangement of the parts and steps, the composition of materials, numerical expressions and numerical values ​​set forth in these embodiments should be interpreted as being merely exemplary, rather than as limiting.

[0021] It should be noted that, in the description of the present invention, unless otherwise specified, the meaning of "multiple" is greater than or equal to two; the terms "upper", "lower", "left", "right", "inner", "outer", etc., indicating the orientation or positional relationship, are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention. When the absolute position of the object being described changes, the relative positional relationship may also change accordingly.

[0022] It should also be noted that in the description of the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected" and "connected" should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be directly connected or indirectly connected through an intermediate medium. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to the specific circumstances. When a specific device is described as being located between a first device and a second device, there may or may not be an intermediate device between the specific device and the first device or the second device.

[0023] All terms used in the present invention have the same meanings as those understood by those of ordinary skill in the art to which the present disclosure belongs, unless otherwise specifically defined. It should also be understood that terms defined in general dictionaries, for example, should be interpreted as having meanings consistent with their meanings in the context of the relevant technology, and should not be interpreted in an idealized or extremely formal sense, unless explicitly defined herein.

[0024] Technologies, methods, and apparatus known to ordinary technicians in the relevant art may not be discussed in detail, but where appropriate, these technologies, methods, and apparatus should be considered part of the specification.

[0025] like Figure 1 As shown, the present invention provides a method for producing high scrap steel ratio automobile steel from vanadium-containing molten iron, which comprises the following steps: S1. Converter vanadium extraction and injection desulfurization: Converter vanadium extraction uses light scrap steel as a coolant for temperature control. The amount of light scrap steel added accounts for 20-40% of the total amount of metal materials added. No other coolant is used for temperature control. The terminal temperature is controlled at 1360-1400°C. The injection desulfurization is still carried out according to the original process; S2. LF heating and carbon increase: After desulfurization, the molten iron is hoisted to the LF process, and the semi-steel is heated by electrode heating, and biomass carbon powder is added for semi-steel carbon increase. Before leaving the station, 3-5kg / (t steel) of ferrosilicon is added. After carburizing, the carbon content of the semi-steel is controlled above 4.5%; S3, converter smelting: after heating, the semi-steel is added into the steelmaking converter, and high-carbon scrap steel is added before adding iron. The final temperature of the converter is controlled at 1630~1650℃; S4, RH forced decarburization, powder spray desulfurization, continuous casting: after steelmaking, the molten steel is subjected to RH forced decarburization and powder spray desulfurization. The steel type can be classified according to standards including chemical composition (such as carbon content) or quality or use or forming method. The steel type needs to be taken into account during the continuous casting process, and the continuous casting process is carried out according to the preset steel type.

[0026] In the method for producing high scrap steel ratio automotive steel from vanadium-containing molten iron according to an embodiment of the present invention, the equipment of existing enterprises can be better utilized, and combined with the characteristics of vanadium-containing molten iron production, the scrap steel ratio of the vanadium-containing molten iron steelmaking process can be greatly improved, which is beneficial to the comprehensive utilization of social scrap steel resources and the production of automotive steel products that meet green steel requirements.

[0027] Using thin scrap steel as a coolant achieves resource recycling, reduces the mining of new resources, and thus reduces damage to the environment. Thin scrap steel can quickly absorb heat during the smelting process, effectively reducing the furnace temperature, thereby maintaining the stability of the smelting process. It has a wide range of sources and low cost, which can reduce smelting costs.

[0028] In some specific embodiments, high carbon scrap steel is scrap steel with a carbon content of> 0.75%, and light scrap steel is small-sized scrap steel after pretreatment, and the maximum length, width and height of light scrap steel is <150mm and the weight of a single piece is <5kg. In order to save resources and reduce the waste of scrap steel, high carbon scrap steel and light scrap steel are derived from scrap steel recycled by society. After recycling, in order to ensure the carbon content after the converter, the scrap steel will be preliminarily screened, and the scrap steel with a carbon content of> 0.75% will be defined as high carbon scrap steel, and high carbon scrap steel will be added before adding iron. When light scrap steel is processed into a small size, its surface area to volume ratio increases, so that the surface area in contact with vanadium-containing molten iron is larger, thereby improving the efficiency of heat exchange and helping to react more quickly. Small-sized light scrap steel, as a coolant, can more effectively absorb excess heat in the converter during the melting process, which not only reduces energy consumption, but also helps to reduce the emission of greenhouse gases such as carbon dioxide. Due to the improvement of cooling efficiency, the smelting cycle of the converter is shortened, thereby also improving production efficiency. In addition, small-sized and thin scrap steel is more easily penetrated by the slag in the converter, reducing the possibility of secondary oxidation and further improving smelting efficiency.

[0029] On the basis of the above embodiments, in step S2, the heating time of the electrode heating is 30 to 60 minutes, and the carbon content of the semi-steel after carburization is ≥ 4.5%. By means of electrode heating, the temperature of the semi-steel can be quickly and evenly increased, thereby shortening the heating time and improving production efficiency. In addition, precise temperature control also helps to reduce energy waste and reduce production costs. When the electrode is heated, the heat energy transferred to the discharge point will diffuse to other parts of the electrode, avoiding or reducing the centralized heating of the electrode, reducing the loss of the electrode, which has a positive effect on reducing production costs and improving economic benefits. In order to ensure complete heating, the heating time of the electrode heating is 30 to 60 minutes.

[0030] The carbon content in steel is one of the important factors affecting its mechanical properties. Within a certain range, increasing the carbon content in semi-steel can improve the strength and hardness of the steel. This is because carbon can strengthen the crystal structure of steel, making it denser and harder. By increasing the carbon content of semi-steel to more than 4.5%, the hardness, wear resistance and toughness of the semi-steel roll will be improved. The increase in carbon content also helps to control the morphology and distribution of carbides in the semi-steel roll, thereby further improving its surface quality and service life.

[0031] Adding biomass carbon powder can increase the carbon element lost during the smelting process. When the carbon content in the smelting process does not meet the expected requirements, adding a certain proportion of carburizer can effectively increase the carbon content in the molten steel, thereby smelting ideal steel. The carburizer in this application is biomass carbon powder.

[0032] In some specific embodiments, step S2 also includes a production mode of using two LF furnaces to correspond to one steel-making converter to ensure the continuous production of the steel-making converter. Through the coordinated use of two LF furnaces and one steel-making converter, continuous refining of molten steel can be achieved, waiting time can be reduced, and overall production efficiency can be improved. Through the reasonable arrangement of the production process, the production rhythm between the converter and the LF furnace can be better coordinated to achieve the continuity and stability of the production process. In this application, in order to ensure the continuous production of the steel-making converter, other ratios can be used for the quantity ratio of the LF furnace and the steel-making converter, such as 3:2 and 4:3, etc., as long as the final usage quantity meets the actual production needs.

[0033] On the basis of the above embodiments, biomass carbon powder is obtained by high-temperature carbonization of plants using green electricity energy, and the plants include rice husks and / or straws and / or branches and / or leaves. Biomass carbon powder comes from renewable resources, such as agricultural and forestry biomass waste, etc., specifically including one or more of rice husks, straws, branches and leaves, and is converted into carbon powder through high-temperature carbonization, thereby achieving effective utilization of resources and reducing environmental pollution. Biomass carbon powder combines with semi-steel at high temperature to form solid solution structure and carbide structure, thereby improving the strength and hardness of steel. The main role of carbon in steel is to form these structures, thereby enhancing the mechanical properties of the material. Biomass carbon powder can be easily mixed with other raw materials and added to semi-steel, which is convenient for realizing automated production. At the same time, its carbonization process is compatible with existing steel production processes and is easy to integrate into existing production lines.

[0034] Based on the above embodiment, in step S3, the amount of high carbon scrap steel added is 30-50% of the nominal capacity of the converter. The nominal capacity refers to the standard capacity claimed by the product for market promotion and consumer selection. In this application, the amount of high carbon scrap steel added is 30-50% of the nominal capacity of the converter. Preferably, the amount added is 40% of the nominal capacity.

[0035] On the basis of the above embodiment, in step S2, the addition amount of biomass carbon powder is 5~10kg / (t iron). Compared with other carburizers, biomass carbon powder has lower cost, especially when its raw material source is extensive and easy to obtain. In addition, its carburizing effect is stable, which can reduce waste in the production process. The carburizing process of biomass carbon powder can accurately control the carbon content in steel, and adjust the carbon content according to the different requirements of steel to balance the strength, hardness, plasticity and toughness of steel. In this application, in order to obtain better carburizing effect, the addition amount of biomass carbon powder is 6~8kg / (t iron). By accurately controlling the addition amount of biomass carbon powder, it is possible to achieve accurate adjustment of steel performance, thereby improving the quality of the product. This is of great significance for producing high-performance, high-quality steel products.

[0036] On the basis of the above embodiments, in step S1, the metal material includes solid iron and scrap steel. As raw materials, solid iron and scrap steel can directly participate in the steelmaking process, reducing the secondary processing and conversion of raw materials, thereby improving the production efficiency of steelmaking. In addition, the recycling of scrap steel can also reduce the mining of new resources and reduce production costs. In the converter vanadium extraction, solid iron and scrap steel can be used as reducing agents to participate in the reduction reaction of vanadium, thereby improving the recovery rate and extraction efficiency of vanadium. In addition, the vanadium element that may be contained in the scrap steel can also be recycled in the vanadium extraction process, further improving the resource utilization rate.

[0037] On the basis of the above embodiments, the electric energy used in the method is clean energy, and the clean energy includes wind power generation and / or photovoltaic power generation. Wind power generation and photovoltaic power generation are clean renewable energy sources that do not produce greenhouse gas and harmful substance emissions. The use of these two energy sources for smelting can significantly reduce the emission of pollutants such as sulfur dioxide and nitrogen oxides, which helps to protect the atmospheric environment and has a significant effect on improving the environment, reducing pollution and reducing greenhouse gas emissions. In addition, the use of wind energy and solar energy can reduce dependence on fossil fuels, thereby saving limited natural resources. Especially in today's increasingly serious energy crisis and environmental pollution, the use of renewable energy for smelting has important strategic significance.

[0038] The present invention also provides a steel for automobiles, which is prepared by any method of the above technical solutions.

[0039] The solution of the present application is described below through specific embodiments.

[0040] Example 1 The production process is "converter vanadium extraction → injection desulfurization → LF heating and carbonization → converter smelting → RH forced decarburization, powder spray desulfurization → continuous casting". The 220t converter vanadium extraction uses light scrap steel as a coolant for temperature control. The proportion of light scrap steel added accounts for 40% of the total amount of metal materials added. No other coolant is used for temperature control, and the terminal temperature is controlled at 1360℃. The injection desulfurization is still carried out according to the original process. After desulfurization, the molten iron is hoisted to the LF process, and the semi-steel is heated by electrode heating, and 6kg / kg of biomass carbon powder is added. (t iron) is used for semi-steel carbonization, the heating time is controlled at 60min, the carbon content of semi-steel after carbonization is controlled at 4.5%, and 1200kg / (t steel) of ferrosilicon is added before leaving the station; after heating, 155t semi-steel is added to the steelmaking converter, and 85t high-carbon scrap steel is added before adding iron, and the final temperature of the converter is controlled at 1630℃; after steelmaking, the molten steel enters the RH for forced decarburization, powder spraying desulfurization and other treatments; the continuous casting process is carried out according to the preset steel type requirements; the electricity involved comes from clean energy such as wind power and photovoltaic power generation, and the high-carbon scrap steel comes from social recycled scrap steel. The scrap steel ratio of the whole process reaches 58.9%.

[0041] Example 2 The production process is "converter vanadium extraction → injection desulfurization → LF heating and carbonization → converter smelting → RH forced decarburization, powder spray desulfurization → continuous casting". The 120t converter vanadium extraction uses light scrap steel as a coolant for temperature control. The proportion of light scrap steel added accounts for 35% of the total amount of metal materials added. No other coolant is used for temperature control, and the terminal temperature is controlled at 1400℃. The injection desulfurization is still carried out according to the original process. After desulfurization, the molten iron is hoisted to the LF process, and the semi-steel is heated by electrode heating, and 10kg / kg of biomass carbon powder is added. (t iron) is used for semi-steel carbonization, the heating time is controlled at 40min, the carbon content of semi-steel after carbonization is controlled at 4.6%, and 1000kg / (t steel) of ferrosilicon is added before leaving the station; after heating, 85t semi-steel is added to the steelmaking converter, and 50t high-carbon scrap steel is added before adding iron, and the final temperature of the converter is controlled at 1650℃; after steelmaking, the molten steel enters the RH for forced decarburization, powder spraying desulfurization and other treatments; the continuous casting process is carried out according to the preset steel type requirements; the electricity involved comes from clean energy such as wind power and photovoltaic power generation, and the high-carbon scrap steel comes from social recycled scrap steel. The scrap steel ratio of the whole process reaches 59.1%.

[0042] Example 3 The production process is "converter vanadium extraction → injection desulfurization → LF heating and carbonization → converter smelting → RH forced decarburization, powder spray desulfurization → continuous casting". The 120t converter vanadium extraction uses light scrap steel as a coolant for temperature control. The proportion of light scrap steel added accounts for 20% of the total amount of metal materials added. No other coolant is used for temperature control, and the terminal temperature is controlled at 1400℃. The injection desulfurization is still carried out according to the original process. After desulfurization, the molten iron is hoisted to the LF process, and the semi-steel is heated by electrode heating, and 5kg / kg of biomass carbon powder is added. (t iron) is used for semi-steel carbonization, the heating time is controlled at 40min, the carbon content of semi-steel after carbonization is controlled at 4.6%, and 1800kg / (t steel) of ferrosilicon is added before leaving the station; 85t semi-steel is added to the steelmaking converter after heating, and 50t high-carbon scrap steel is added before adding iron, and the final temperature of the converter is controlled at 1650℃; after steelmaking, the molten steel enters the RH for forced decarburization, powder spraying desulfurization and other treatments; the continuous casting process is carried out according to the preset steel type requirements; the electricity involved comes from clean energy such as wind power and photovoltaic power generation, and the high-carbon scrap steel comes from social recycled scrap steel. The scrap steel ratio of the whole process reaches 58.5%.

[0043] After the implementation of the present invention, at least the following beneficial effects are achieved: (1) Making full use of the LF heating function can not only effectively increase the temperature of the molten steel, ensuring that it reaches the smelting temperature required by the process, thereby ensuring the quality and performance of the steel. At the same time, by precisely controlling the heating process, the carbon content in the semi-steel can be appropriately increased to meet the specific carbon content requirements of different steel grades. This measure not only optimizes the production process, but also improves production efficiency, providing a strong guarantee for the production of high-quality steel.

[0044] (2) During the smelting process, light and thin scrap steel is used to control the temperature of the converter for vanadium extraction. This method aims to effectively adjust and control the temperature in the converter by adding light and thin scrap steel to ensure the stability of the smelting process. At the same time, the addition of scrap steel also increases the proportion of scrap steel used, reduces production costs, and achieves effective resource utilization and environmental emission reduction. This not only reflects the importance attached to environmental protection and resource conservation, but also demonstrates the innovation ability and technical level in the field of steel production.

[0045] (3) In the entire production process, the electricity used is all green energy. This means that the production activities not only meet the production needs, but also actively respond to the national call for energy conservation and emission reduction, and make positive contributions to protecting the environment and promoting sustainable development. By adopting clean energy and environmental protection technology, the negative impact on the environment is reduced, achieving a win-win situation of economic and environmental benefits.

[0046] The above are exemplary embodiments disclosed in the present invention. The order disclosed in the above embodiments of the present invention is for description only and does not represent the advantages and disadvantages of the embodiments. However, it should be noted that the discussion of any of the above embodiments is only exemplary and is not intended to imply that the scope disclosed in the embodiments of the present invention (including the claims) is limited to these examples. Various changes and modifications may be made without departing from the scope defined in the claims. The functions, steps and / or actions of the method claims according to the disclosed embodiments described herein do not need to be performed in any particular order. In addition, although the elements disclosed in the embodiments of the present invention may be described or required in individual form, they may also be understood as multiple unless explicitly limited to the singular.

[0047] A person skilled in the art should understand that the discussion of any of the above embodiments is only exemplary and is not intended to imply that the scope of the disclosure of the embodiments of the present invention (including the claims) is limited to these examples; under the concept of the embodiments of the present invention, the technical features in the above embodiments or different embodiments can also be combined, and there are many other changes in different aspects of the embodiments of the present invention as described above, which are not provided in detail for the sake of simplicity. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the embodiments of the present invention should be included in the protection scope of the embodiments of the present invention.

Claims

1. A method for producing high scrap ratio automobile steel from vanadium-containing hot metal, It is characterized in that The following steps are involved: S1. Converter vanadium extraction and injection desulfurization: The converter vanadium extraction uses light and thin scrap steel as a coolant for temperature control. The amount of light and thin scrap steel added accounts for 20-40% of the total amount of metal material added, and the terminal temperature is controlled at 1360-1400°C; S2, LF heating and carbon increase: After desulfurization, the molten iron is hoisted to the LF process, and the semi-steel is heated by electrode heating, and biomass carbon powder is added to increase the carbon of the semi-steel. Before leaving the station, 3~5kg / (t steel) of ferrosilicon is added; S3, converter smelting: after heating, the semi-steel is added into the steelmaking converter, and high carbon scrap steel is added before adding iron, and the final temperature of the converter is controlled at 1630~1650℃; S4, RH forced decarburization, powder spray desulfurization, continuous casting: After steelmaking, the molten steel undergoes RH forced decarburization and powder spray desulfurization, and the continuous casting process is carried out according to the preset steel type.

2. The method for producing high scrap ratio automobile steel from vanadium-containing molten iron according to claim 1, It is characterized in that The high-carbon scrap steel refers to scrap steel with a carbon content of >0.75%, and the light and thin scrap steel refers to small-sized scrap steel that has been pre-treated. The maximum dimensions of the light and thin scrap steel in length, width and height are <150mm and the weight of a single piece is <5kg.

3. The method for producing high scrap ratio automobile steel from vanadium-containing molten iron according to claim 1, It is characterized in that In step S2, the heating time of the electrode heating is 30-60 minutes, and the carbon content of the semi-steel after carburization is ≥4.5%.

4. The method for producing high scrap ratio automobile steel from vanadium-containing molten iron according to claim 1, It is characterized in that Step S2 also includes adopting a production mode of two LF furnaces corresponding to one steelmaking converter to ensure continuous production of the steelmaking converter.

5. The method for producing high scrap ratio automobile steel from vanadium-containing molten iron according to claim 1, It is characterized in that The biomass carbon powder is obtained by high-temperature carbonization of plants using green electricity energy, and the plants include rice husks and / or straws and / or branches and / or leaves.

6. The method for producing high scrap ratio automobile steel from vanadium-containing molten iron according to claim 1, It is characterized in that In step S3, the amount of high carbon scrap steel added is 30-50% of the nominal capacity of the converter.

7. The method for producing high scrap ratio automobile steel from vanadium-containing molten iron according to claim 6, It is characterized in that In step S2, the amount of biomass carbon powder added is 5-10 kg / t iron.

8. The method for producing high scrap ratio automobile steel from vanadium-containing molten iron according to claim 1, It is characterized in that In step S1, the metal material includes solid iron and scrap steel.

9. The method for producing high scrap ratio automobile steel from vanadium-containing molten iron according to claim 1, It is characterized in that The electric energy used in the method is clean energy, which includes wind power generation and / or photovoltaic power generation.

10. A kind of steel for automobiles, It is characterized in that The method is prepared by any one of claims 1 to 9.

Citation Information

Cited By

  • Composite carrier roller and preparation method thereof

    CN119429503A

  • Short-process electric arc furnace smelting method for high-quality green steel with high scrap ratio of 80%