Leaching and purifying process of cracked ternary battery black powder

Through the leaching purification process of multi-step copper removal and oxidant treatment, the problems of oil content and COD in the black powder of waste ternary lithium battery are solved, and the loss rate of valuable metals is high is achieved, which is suitable for efficient recycling of valuable metals and impurities. Industrialized production.

CN118957273APending Publication Date: 2024-11-15CAMEL GRP RESOURCE CYCLE XIANGYANG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411168285.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the prior art, the black powder produced after the cracking of the waste ternary lithium battery can easily lead to the oil content and COD content in the purification liquid exceeding the standard, and the loss rate of valuable metals is high and the consumption of auxiliary materials is large, resulting in production efficiency. Low and high cost.

Method used

A leach purification process for black powder leaching of 3-cell battery is adopted, including slurrying of black powder with water, adjusting pH value, and performing multiple copper removal treatments through thiosulfate and sulfide compounds, and combining oxidizing agent to remove iron and aluminum to achieve the Effective recovery of valent metals and removal of impurity metals and organic matters.

Benefits of technology

It effectively reduces the oil content and impurity metal ions in the purification liquid, improves the recycling purity and production efficiency of valuable metals, reduces the consumption of auxiliary materials, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957273A_ABST
    Figure CN118957273A_ABST
Patent Text Reader

Abstract

The invention relates to a cracking ternary battery black powder leaching purification process which comprises the following steps: adding water into cracking ternary battery black powder for slurrying to obtain black powder slurry; adding an acid solution into the black powder slurry to adjust the pH value to 0.5-1.0, dropwise adding hydrogen peroxide to adjust the pH value to 1.5-2.0, and separating to obtain a neutral immersion solution; adding thiosulfate into the neutral immersion liquid to carry out one-step copper removal to obtain one-step copper-removed liquid; a sulfur salt compound solution is added into the first-step copper-removed solution for second-step copper removal, and a second-step copper-removed solution is obtained; and an oxidizing agent is added into the second-step copper-removed solution, then the pH is adjusted, iron and aluminum are removed, and a purified solution is obtained. According to the method, valuable metal is leached out through the neutral leaching step, residual oil is washed out, through two-step copper removal and cooperation of the copper removal agent, copper is effectively removed, meanwhile, other metal is prevented from being carried, finally, the purified liquid mainly containing nickel, cobalt, manganese and lithium is obtained through iron and aluminum removal, and follow-up recovery of the main valuable metal is facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of waste batteries, and in particular to a black powder leaching and purification process for cracking ternary batteries. Background Art

[0002] The black powder produced after the cracking of waste ternary lithium batteries contains valuable metals such as nickel, cobalt, manganese, lithium, and copper, and has great recycling value. It can generate huge economic and social value through hydrometallurgical recovery. However, the black powder produced by cracking contains impurity metals, especially iron and aluminum, as well as organic matter that is not fully cracked, which has an adverse effect on the recovery of valuable metals, especially nickel, cobalt, manganese, and lithium.

[0003] At present, the black powder treatment process produced after the cracking of waste ternary lithium batteries mainly includes the following steps: (1) Leaching: After the cracking of the ternary battery black powder, the pH is adjusted to 2.5-3.0 through intermediate leaching to obtain an intermediate leaching solution; (2) Copper precipitation: The copper content is controlled to <10ppm through a one-step copper precipitation; (3) Iron and aluminum precipitation: The pH is adjusted to remove iron and aluminum; Among them, copper precipitation slag and iron and aluminum precipitation slag will carry valuable metals such as nickel, cobalt and manganese. Therefore, copper precipitation slag and iron and aluminum precipitation slag need to be recovered through acid washing and other steps. In particular, iron and aluminum slag usually requires two-step acid washing + one-step water washing.

[0004] However, in the conventional leaching step, the pH of the intermediate leaching is controlled too high, which can easily lead to excessive oil and COD content in the purified liquid; the one-step copper removal method results in a large amount of precipitant used, a large amount of valuable metals entrained, and difficulty in washing the copper slag; the two-step washing method for removing iron and aluminum slag has a high iron and aluminum recovery rate, a large amount of auxiliary material consumption, and a high cost. Summary of the invention

[0005] The purpose of the present invention is to overcome the above-mentioned technical deficiencies, provide a cracking ternary battery black powder leaching purification process, and solve the technical problems in the prior art that the oil and COD content in the purified liquid is easily exceeded, the loss rate of valuable metals is high, and the consumption of auxiliary materials is large.

[0006] In order to achieve the above technical purpose, the technical solution provided by the present invention is: In a first aspect, the present invention provides a leaching and purification process for cracking ternary battery black powder, comprising the following steps: S1, slurrying the cracked ternary battery black powder with water to obtain black powder slurry; S2, adding acid to the black powder slurry to adjust the pH value to 0.5-1.0, then adding hydrogen peroxide to adjust the pH value to 1.5-2.0, and separating to obtain a medium immersion liquid; S3, adding thiosulfate to the intermediate leaching solution to perform one-step copper removal to obtain a one-step copper removal solution; S4, adding a sulfide compound solution to the first-step copper removal solution to perform second-step copper removal to obtain a second-step copper removal solution; S5, adding an oxidant to the solution after the second step copper removal, and then adjusting the pH to remove iron and aluminum to obtain a purified solution.

[0007] Compared with the prior art, the beneficial effects of the present invention include: The present invention uses a mid-leaching step to leach out valuable metals and wash out residual oil in a solution; in the first-step copper removal, thiosulfate is used as a copper removal agent to first remove more than 95% of copper, and then in the second-step copper removal, a sulfide compound is used to remove the remaining copper in the solution. Through the two-step copper removal and the combination of the copper removal agent, other metals can be avoided from being entrained while copper is effectively removed; finally, ferrous ions are oxidized into trivalent ferric ions by an oxidant, and the pH is adjusted to remove iron and aluminum in the solution to obtain a purified liquid mainly containing nickel, cobalt, manganese and lithium; the present invention can realize the recovery and purification of valuable metals such as copper while removing impure metals and organic matter, and the obtained purified liquid has low oil and impure metal ion content, which is conducive to the subsequent recovery of the main valuable metals nickel, cobalt, manganese and lithium, has high production efficiency, low auxiliary material consumption, and is more suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0008] Figure 1 It is a flow chart of the steps of the leaching and purification process of black powder of cracking ternary battery of the present invention; Figure 2 It is a process flow chart of Example 1 of the present invention. DETAILED DESCRIPTION

[0009] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0010] See also Figure 1 The present invention provides a leaching and purification process for cracking ternary battery black powder, comprising the following steps: S1, black powder slurrying: slurrying the cracked ternary battery black powder with water to obtain black powder slurry; S2, intermediate leaching: adding acid solution to the black powder slurry to adjust the pH value to 0.5-1.0, then adding hydrogen peroxide to adjust the pH value to 1.5-2.0, and separating to obtain intermediate leaching solution and intermediate leaching residue; S3, one-step copper removal: adding thiosulfate to the intermediate leaching solution to perform one-step copper removal, thereby obtaining one-step copper removal slag and one-step copper removal liquid; S4, two-step copper removal: adding a sulfide compound solution to the first-step copper removal solution to perform two-step copper removal to obtain a two-step copper removal slag and a second-step copper removal solution; S5, iron and aluminum removal: adding an oxidant to the liquid after the second step copper removal, and then adjusting the pH to remove iron and aluminum, to obtain the first iron and aluminum slag and purified liquid.

[0011] Preferably, in step S1, the mass ratio of cracking ternary battery black powder and water is 1: (1.8-2.5); the slurrying time is more than 0.5h, and more preferably the slurrying time is 0.5-1.5h.

[0012] Preferably, step S2 specifically includes: S201, adding acid solution to the black powder slurry to adjust the pH value to 0.5-1.0 and maintaining it for more than 10 minutes to obtain a mixed solution; S202, hydrogen peroxide is added dropwise to the mixed solution to adjust the pH value to 1.5-2.0, and the mixture is aged for at least 0.5 h, and the intermediate leaching solution and intermediate leaching residue are obtained by solid-liquid separation.

[0013] Further preferably, in step S201, acid solution is added to adjust the pH value to 0.5-1.0 and maintained for 10-30 minutes; in step S202, the aging time is 0.5-2 hours; wherein a certain aging time is retained to completely decompose the hydrogen peroxide.

[0014] Further preferably, the mass concentration of hydrogen peroxide is 15%.

[0015] Preferably, step S2 further comprises acid leaching the intermediate leaching residue, specifically comprising: S211, using concentrated sulfuric acid to acid-leach the intermediate leaching residue to separate the acid-leach residue and the acid-leach liquid; the acid-leach liquid is reused as acid liquid; S212, washing the acid leaching residue with water to obtain leaching residue and water washing liquid; the water washing liquid is returned to the acid leaching process.

[0016] Further preferably, in the acid leaching treatment, the liquid-to-solid ratio is (2.5-3.5):1; In the acid leaching solution, H + The concentration is 3.0-4.0 mol / L, and the total metal concentration of nickel, cobalt and manganese is less than 30 g / L; The high-valent nickel, cobalt and manganese are reduced by hydrogen peroxide, and 0.5 to 1.0 times the theoretical amount is added. After the reaction is complete, the total content of nickel, cobalt and manganese on a dry basis in the leached residue is less than 1.0%. The theoretical amount refers to the theoretical molar ratio of hydrogen peroxide to nickel, cobalt and manganese of 1:2.

[0017] Further preferably, step S3 further comprises: pickling the one-step copper removal slag with dilute sulfuric acid having a pH of 1.0 to 1.5, with a liquid-to-solid ratio of (2.5 to 3.5):1, and a washing time of more than 1 hour, to obtain cuprous sulfide slag and a one-step copper removal pickling solution; and / or, Step S5 also includes: adding water to the first iron-aluminum slag for slurrying, wherein the liquid-solid ratio is (2.5-3.5):1, and the slurrying time is more than 1 hour, until the iron-aluminum slag is completely dispersed, to obtain a first iron-aluminum slag slurry; adjusting the pH value of the first iron-aluminum slag slurry to 1.5-2.0 by concentrated sulfuric acid and stabilizing it for more than 5 minutes, then heating it to 80-85°C for iron-aluminum slag pickling, stopping the reaction when the pH value is 3.0-3.5, and obtaining a second iron-aluminum slag and an iron-aluminum slag pickling solution by solid-liquid separation; washing the second iron-aluminum slag with water to obtain a third iron-aluminum slag and an iron-aluminum water washing solution, and recycling the iron-aluminum water washing solution to the iron-aluminum slag pickling step; and / or, The copper pickling solution and the iron and aluminum slag pickling solution are removed in one step and returned to the acid leaching treatment.

[0018] In the present invention, the one-step copper removal pickling solution is used as the ore pulp solvent for the intermediate leaching residue acid leaching reaction, and the cuprous sulfide residue can be directly sold after filter pressing. The first iron-aluminum slag can be washed with acid once and washed with water once to achieve a total dry basis nickel and cobalt content of ≤1.0% in the iron-aluminum slag.

[0019] More preferably, during the water washing process of the second iron-aluminum slag, the liquid-to-solid ratio is (2.5-3.5):1, the slurrying time is more than 1 hour, and after the slurrying is completed, the third iron-aluminum slag and the iron-aluminum water washing liquid are separated by filtration and pressing, and the water content in the third iron-aluminum slag is <50%.

[0020] Preferably, in step S3, the thiosulfate includes sodium thiosulfate; the molar ratio of sodium thiosulfate to copper ions contained in the intermediate leaching solution is (0.95-1.05):1; and sodium carbonate solution is used in the one-step copper removal to control the reaction pH value to be 2.0-3.0.

[0021] More preferably, in step S3, the pH value of the intermediate infusion is first controlled at 2.0 to 3.0 and the temperature is above 80° C., and then sodium thiosulfate is added to react for 0.5 to 1.0 h.

[0022] Preferably, in step S4, the sulfide compound solution includes a sodium sulfide solution; the molar ratio of sodium sulfide to copper ions in the one-step copper removal solution is (1.4-2.1): 1. The amount of reaction addition varies according to the copper content in the one-step copper removal solution. In the one-step copper removal solution, if the copper content is 100-200 ppm, the molar ratio of sodium sulfide to copper is 1.5:1.0; if the copper content is less than 100 ppm, the molar ratio of sodium sulfide to copper is 2:1.

[0023] Preferably, in step S4, the two-step copper removal slag is slurried with water to obtain a two-step copper removal slurry; the two-step copper removal slurry is combined with the black powder slurry. Since the one-step copper removal slag is washed with a pickling solution with a pH of 1.0 to 1.5 until the total nickel and cobalt content in the copper slag is less than 0.88%, most of the copper has been separated from the system; the two-step copper removal step only needs to remove a trace amount of copper, and the amount of the two-step copper removal slag produced is small and difficult to wash, so the two-step copper removal slag is directly returned to the intermediate leaching reaction.

[0024] In the present invention, sodium thiosulfate is used for one-step copper removal, and the entrainment content of other valuable metals is small; the copper content in the liquid after the one-step copper removal is less than 200 ppm; the cuprous sulfide slag obtained by washing with dilute sulfuric acid in the one-step copper removal slag has a total content of nickel, cobalt and manganese on a dry basis of less than 1.0%.

[0025] Preferably, the iron and aluminum removal in step S5 specifically includes: adding an oxidant to the liquid after the second step copper removal, reacting for more than 0.5h; then heating to 85-90°C, adding sodium carbonate solution to adjust the pH value to above 5.0, reacting for at least 1h, and filtering to obtain the first iron-aluminum slag and purified liquid.

[0026] Further preferably, the oxidant is hydrogen peroxide, and the molar ratio of H2O2 in the hydrogen peroxide to the ferrous ions in the solution after the second-step copper removal is 2:1.

[0027] The present invention uses a mid-leaching step to adjust the pH value to 0.5-1.0, and then slowly drips hydrogen peroxide to adjust the pH value to 1.5-2.0 to degrade COD in the solution, leaching valuable metals and washing out residual oil in the solution; through the acid leaching step, the valuable metals in the mid-leaching residue are completely leached to further improve the leaching rate; in the first-step copper removal, more than 95% of copper is removed by a mixed solution of sodium thiosulfate and sodium carbonate, and the copper slag is washed back with a dilute sulfuric acid solution to remove the entrained valuable metals; the remaining copper in the solution is removed by a sodium sulfide solution, and the two-step copper removal slag enters the mid-leaching step. The leaching reaction tank is used as black powder slurry; finally, ferrous ions are oxidized to trivalent ferric ions by hydrogen peroxide, and the pH is adjusted to remove iron and aluminum in the solution to obtain a purified solution mainly containing nickel, cobalt, manganese and lithium; the iron-aluminum slag is washed with concentrated sulfuric acid to remove valuable metals, and then the free valuable metals in the iron-aluminum slag are washed out by a one-step water washing; the present invention can realize the recovery and purification of valuable metals such as copper while removing impurity metals and organic matter, which is beneficial to the subsequent recovery of the main valuable metals nickel, cobalt, manganese and lithium, has high production efficiency, low auxiliary material consumption, and is more suitable for industrial production.

[0028] The present invention is further described in detail below through specific embodiments. To avoid redundancy, the test methods or conditions are described here: (1) Determine the hydrogen ion concentration of the solution by acid-base titration; (2) The valuable metal content is tested by ICP; (3) The moisture content of leached slag, copper slag, and iron and aluminum slag is measured by moisture analyzer, and the metal content is tested on a dry basis after drying; (4) Calculation formula for the mass of components in the filter residue: filter residue mass (g) * (1-water content%) * valuable metal dry basis component content; (5) Calculation formula for valuable metal recovery rate: (mass of valuable metal components in ferroaluminum slag, g - mass of valuable metal components in ferroaluminum slag, acid-washed slag and water-washed slag, g) / mass of valuable metal components in ferroaluminum slag, g.

[0029] Example 1 See also Figure 2 The present invention provides a leaching and purification process for cracking ternary battery black powder, which specifically comprises the following steps: S1, black powder slurrying: the cracked ternary battery black powder and tap water are mixed in a mass ratio of 1:2 and slurried for 0.5h to obtain black powder slurry.

[0030] S2, intermediate leaching: add acid leaching solution to the black powder slurry to adjust the pH value to 0.73 and stabilize it for 15 minutes, then add 15% hydrogen peroxide to adjust the pH value to 1.67, and separate the intermediate leaching solution and intermediate leaching residue after aging for 1.5 hours; The intermediate leaching residue was treated with acid leaching using concentrated sulfuric acid with a liquid-to-solid ratio of 3:1, and the acid leaching residue and the acid leaching solution were separated. After the reaction was complete, the hydrogen ion concentration in the acid leaching solution was controlled to be 3.59 mol / L, and the total metal concentration of nickel, cobalt and manganese was 27 g / L; the acid leaching solution was returned to the intermediate leaching treatment; the acid leaching residue was washed with water to obtain leaching residue and water washing solution; the water washing solution was returned to the acid leaching treatment; the high-valent nickel, cobalt and manganese were reduced by hydrogen peroxide to improve the leaching rate, and the final leaching residue had a low total content of nickel, cobalt and manganese on a dry basis, which was 0.85%.

[0031] S3, one-step copper removal: firstly, the pH value of the intermediate leaching solution is controlled at 2.5-3.0 and the temperature is controlled at 80-85°C, and then sodium thiosulfate is added to remove copper in one step, the molar ratio of sodium thiosulfate to copper ion is 0.95:1, and after reacting for 0.5 h, the one-step copper removal slag and the one-step copper removal liquid are separated; the copper content in the one-step copper removal liquid is 65 ppm; The one-step copper removal slag was pickled with dilute sulfuric acid at a pH of 1.5, with a liquid-to-solid ratio of 3:1 and a washing time of 1.0 h to obtain cuprous sulfide slag and one-step copper removal pickling liquid; the one-step copper removal pickling liquid was returned to the acid leaching treatment and used as a solvent; the total content of nickel, cobalt and manganese on a dry basis of the cuprous sulfide slag was 0.48%.

[0032] S4, two-step copper removal: adding a 10% sodium sulfide solution to the first-step copper removal solution for two-step copper removal, wherein the molar ratio of sodium sulfide to copper is 2.0:1.0; obtaining a two-step copper removal slag and a second-step copper removal solution; The second-step copper removal slag is slurried with water and then enters the intermediate leaching reaction tank for use as black powder slurry.

[0033] S5, iron and aluminum removal: hydrogen peroxide is added to the liquid after the second step copper removal, the molar ratio of H2O2 to ferrous ions in the liquid after the second step copper removal is 2:1, and the oxidation reaction is carried out for 0.5h. After the oxidation reaction is completed, the temperature is raised to 85-90°C, sodium carbonate solution is added to adjust the pH value to 5.2-5.5, and iron and aluminum are removed. After the reaction is carried out for 1.5h, the first iron and aluminum slag and the purified liquid are obtained by filtration; The first iron-aluminum slag is slurried with water, wherein the liquid-solid ratio is 3:1, and the slurrying time is 1.0h, until the iron-aluminum slag is completely dispersed, to obtain a first iron-aluminum slag slurry; the pH value of the first iron-aluminum slag slurry is adjusted to 1.5-1.8 by concentrated sulfuric acid and stabilized for more than 5min, and then the temperature is raised to 85°C for iron-aluminum slag pickling, the reaction is stopped when the pH value is 3.5, and a second iron-aluminum slag and an iron-aluminum slag pickling liquid are obtained by solid-liquid separation; the second iron-aluminum slag is washed with water to obtain a third iron-aluminum slag and an iron-aluminum water washing liquid, and the iron-aluminum water washing liquid is reused in the iron-aluminum slag pickling step; The first iron-aluminum slag liquid is washed with acid and with water at a solid ratio of 3:1 to achieve a total dry nickel and cobalt content of 0.72% (both less than 1%) in the iron-aluminum slag.

[0034] Example 2 In order to investigate the influence of the intermediate leaching process, the difference between this embodiment and embodiment 1 is that acid leaching solution is added to the black powder slurry to adjust the pH value to 5.27, 3.12, 1.83 and 0.91, and the other steps and conditions are the same as those in embodiment 1.

[0035] The oil content and COD of the intermediate immersion liquid were tested, and the results are shown in Table 1 below.

[0036] Table 1 Effect of solution pH on oil content and COD

[0037] From the data in Table 1, it can be seen that: (1) the addition of hydrogen peroxide will increase the pH. The purpose of adding hydrogen peroxide is to accelerate the reaction as a catalyst and degrade COD. Therefore, the pH of the solution must be controlled at <3.0 before adding hydrogen peroxide to degrade COD. When the pH of the solution is >3.0, the COD in the intermediate leaching solution is >1300ppm, and the oil content in the intermediate leaching solution is >55ppm. At this time, no hydrogen peroxide is added; (2) When the pH of the solution is between 0.5 and 1, the pH is adjusted to 1.5 and 2.0 with hydrogen peroxide, and the COD in the solution is <800ppm, and the oil content is <10ppm; (3) During the preferred intermediate leaching reaction, the hydrogen ion concentration provided by the acid leaching solution needs to reach 80-90% of the theoretical amount of black powder leaching. The pH in the solution is controlled at 0.50-1.0, and then the hydrogen peroxide catalytic reaction can achieve the effect of effectively degrading COD and separating oil.

[0038] Example 3 In order to investigate the effect of the liquid-to-solid ratio on the leaching rate under the condition of quantitative sulfuric acid in the acid leaching process, the difference between this embodiment and embodiment 1 is that the liquid-to-solid ratio of the intermediate leaching residue for acid leaching with concentrated sulfuric acid is adjusted to 2:1 and 4:1, and the other steps and conditions are the same as those in embodiment 1.

[0039] The hydrogen ion concentration and the total metal concentration of nickel, cobalt and manganese in the acid leaching solution were tested, and the dry basis nickel, cobalt and manganese of the leached residue were calculated. The results are shown in Table 2 below.

[0040] Table 2 Effect of liquid-solid ratio on leaching rate in acid leaching process

[0041] From the data in Table 2, it can be seen that: (1) Under the condition of liquid-solid ratio of 2:1, the hydrogen ion concentration is greater than 4 mol / L. Since the total concentration of nickel, cobalt and manganese in the solution is greater than 30 g / L, the total content of nickel, cobalt and manganese in the washing residue is greater than 1.0%, the acid leaching effect is not good; (2) When the liquid-solid ratio is 3:1, the hydrogen ion concentration is 3.59 mol / L, the nickel, cobalt and manganese concentration in the solution is less than 30 g / L, and the total content of nickel, cobalt and manganese on a dry basis in the washing residue is 0.85% less than 1.0%, and the acid leaching effect meets the requirements; (3) When the liquid-solid ratio is 4:1, the hydrogen ion concentration is less than 3.0 mol / L, and the total content of nickel, cobalt and manganese in the washing residue is 1.38% greater than 1.0, and the acid leaching effect is not good; (4) When the acid leaching liquid-solid ratio is controlled to 3:1, the hydrogen ion concentration is 3-4 mol / L, and the acid leaching effect is the best; (5) Since this process leaches more than 80% of valuable metals during the intermediate leaching reaction, the acid leaching reaction can achieve leaching using a reducing agent less than 1 times the theoretical amount.

[0042] Example 4 In order to investigate the effect of the amount of sodium thiosulfate in one-step copper removal, the difference between this embodiment and embodiment 1 is only that the molar ratio of sodium thiosulfate to copper ion is adjusted to 0.8:1, 1.05:1, 1.1:1, 1.2:1 and 1.3:1, and the other steps and conditions are the same as those in embodiment 1.

[0043] The copper content in the solution before and after one-step copper removal and the nickel and cobalt content in the cuprous sulfide slag were tested, and the results are shown in Table 3 below.

[0044] Table 3 Effect of sodium thiosulfate dosage in one-step copper removal

[0045] It can be seen from the data in Table 3 that: (1) with the increase of the amount of sodium thiosulfate added, the copper content in the solution after one-step copper removal shows a decreasing trend; (2) when the sodium thiosulfate addition ratio coefficient is greater than 0.95, the copper content in the solution is 185ppm<200ppm; (3) when the sodium thiosulfate addition ratio coefficient is increased to 1.05, the copper content in the solution decreases from 185ppm to 127ppm, and the decrease is not obvious; (4) when the sodium thiosulfate ratio coefficient is greater than 1.1, the copper content in the solution is less than 100ppm; (5) after the sodium thiosulfate ratio coefficient is greater than 1.1, the total nickel and cobalt entrainment in the pickled copper slag is 1.26%>1.0%, and when the sodium thiosulfate ratio coefficient is increased, the nickel and cobalt entrainment amount gradually increases, so the preferred sodium thiosulfate to copper ion molar ratio of 0.95 to 1.05 has the best effect.

[0046] Example 5 In order to investigate the effect of the amount of sodium sulfide in the two-step copper removal, the difference between this embodiment and embodiment 1 is only that the molar ratio of sodium sulfide to copper ion is adjusted to 1.0:1 and 1.5:1, and the other steps and conditions are the same as those in embodiment 1.

[0047] The same treatment was performed on the one-step copper removal solution (obtained at a sodium thiosulfate:copper molar ratio of 1.1:1) with a copper content of 65 ppm in Example 4; the copper content in the solution before and after the two-step copper removal and the nickel and cobalt content in the cuprous sulfide slag were tested, and the results are shown in Table 4 below.

[0048] Table 4 Effect of sodium sulfide dosage in two-step copper removal

[0049] It can be seen from the data in Table 4 that: (1) after the initial one-step copper removal, the copper content of the liquid is less than 100ppm, the sodium sulfide addition ratio coefficient is greater than 2.0, and the copper content of the liquid after copper removal is 5ppm<10ppm; (2) after the initial one-step copper removal, the copper content of the liquid is between 100 and 200ppm, the sodium sulfide addition ratio coefficient is greater than 1.5, and the copper content of the liquid after copper removal is 4ppm<10ppm; (3) according to the different copper content ratios, the sodium sulfide addition ratio coefficient needs to be adjusted. When the copper content in the solution is greater than 200ppm, sodium thiosulfide is used to remove copper; when the copper content in the solution is 100 to 200ppm, sodium sulfide is used to remove copper, and the sodium sulfide addition ratio coefficient is preferably controlled to be 1.5 times; when the copper content in the solution is less than 100ppm, sodium sulfide is used to remove copper, and the sodium sulfide addition ratio coefficient is controlled to be 2.0 times.

[0050] Example 6 The first iron-aluminum slag obtained in Example 1 is washed, the first iron-aluminum slag contains 64.84% water, and includes iron hydroxide, aluminum hydroxide, nickel sulfate, cobalt sulfate, and manganese sulfate (wherein the dry basis components include cobalt: 1.95%, 41.14g; nickel: 5.77%, 121.73g; manganese: 3.58, 75.52g; aluminum: 8.3%, 175.1g; iron: 1.13%, 23.84g); comprising the following steps: (1) 6000 g of the first ferroaluminum slag was slurried with water, wherein the liquid-to-solid ratio was 3:1 and the slurrying time was 1.0 h to obtain the first ferroaluminum slag slurry; (2) The first iron-aluminum slag slurry is treated by rapidly adding concentrated sulfuric acid to reduce the pH of the solution to 1.8-2.0, thereby changing the colloidal structure of the iron-aluminum slag and releasing the adsorbed nickel, cobalt and manganese (when adding acid, the acidity in the local area is too high, which affects the iron-aluminum washing rate. In order to reduce the iron-aluminum washing rate, the pH is adjusted at room temperature) (3) After pH adjustment, steam direct heating was used to accelerate the reaction rate. The temperature was raised to 80-85°C and the reaction was continued for 2.5 hours until the endpoint pH was stabilized at 3.2. (4) After the first iron-aluminum slag is pickled, it is filtered to obtain the second iron-aluminum slag and the iron-aluminum slag pickling liquid; the second iron-aluminum slag is washed with water to control the slurry liquid-solid ratio to 3:1, so that the free nickel, cobalt and manganese valuable metals in the slag can be washed out, and the slurrying time is 1.0h. After the slurrying is completed, the third iron-aluminum slag (containing solid iron hydroxide and aluminum hydroxide) is completely separated from the nickel, cobalt and manganese valuable metals by pressing.

[0051] After one-step acid washing and one-step water washing, the first iron-aluminum slag, the second iron-aluminum slag and the third iron-aluminum slag were tested for components, and the results are shown in Table 5 below; and the washing recovery rate of each component was calculated: cobalt washing recovery rate: 89.67%, nickel washing recovery rate: 92.24%, manganese washing recovery rate: 95.10, aluminum washing recovery rate: 11.36%, iron washing recovery rate 6.92%.

[0052] Table 5 Iron and aluminum slag washing data

[0053] Comparative Example 1 The only difference from Example 1 is that the raw materials for the two-step copper removal are replaced, and sodium sulfide is used to remove copper in one step for the intermediate leaching solution with a copper content of 1800 ppm. The other steps and conditions are the same as those in Example 1.

[0054] Table 6 Effect of using sodium sulfide as copper removal agent in one-step copper removal

[0055] From the data in Comparative Example 1, it can be analyzed that the addition ratio coefficient of sodium sulfide of 1.0 can remove the copper content in the solution to <100ppm, but the filter residue after sodium sulfide copper removal contains valuable metals of nickel, cobalt and manganese with a content of >14%, which cannot be recovered by acid washing. Therefore, sodium thiosulfate is used as the copper removal agent in the one-step copper removal.

[0056] Therefore, it has been verified that the removal of copper by sodium sulfide will result in the entrainment of a large amount of valuable metals such as nickel and cobalt, and the recovery rate is low. Therefore, sodium sulfide is suitable for removing trace copper. The copper removal slurry directly enters the intermediate leaching reaction tank without considering the problem of filter residue washing.

[0057] Comparative Example 2 The only difference from Example 1 is that the raw materials for the two-step copper removal are replaced, sodium thiosulfate is used for the second step of copper removal (the one-step copper removal liquid is the one-step copper removal liquid obtained by the second group in Comparative Example 1), and the other steps and conditions are the same as those in Example 1.

[0058] Table 7 Effect of using sodium thiosulfate as copper removal agent in two-step copper removal

[0059] It can be analyzed from the data in Comparative Example 2 that for a solution with a copper content of <100 ppm, a sodium thiosulfate addition ratio coefficient of >3.0 can achieve a copper content in the solution after copper removal of <10 ppm, but the amount of nickel, cobalt and manganese entrained in the two-step copper removal slag is >3.0%. The defect of Comparative Example 2 compared to Example 5 is that the amount of auxiliary material added is 1.5 times the theoretical amount of sodium sulfide, and the copper content in the two-step copper removal slag exceeds the standard.

[0060] Comparative Example 3 The only difference from Example 3 is that the hydrogen peroxide in the intermediate immersion step is removed, and the other steps and conditions are the same as those in Example 3.

[0061] Table 8 Effect of removing hydrogen peroxide in the intermediate leaching step on acid leaching

[0062] Comparison of Comparative Example 3 with Example 3 shows that, without the addition of hydrogen peroxide, the metal leaching rate in the slag is low, so hydrogen peroxide is required in the acid leaching.

[0063] The specific implementation of the present invention described above does not constitute a limitation on the protection scope of the present invention. Any other corresponding changes and modifications made based on the technical concept of the present invention should be included in the protection scope of the claims of the present invention.

Claims

1. A leaching and purification process for cracking ternary battery black powder, characterized in that: The following steps are involved: S1, slurrying the cracked ternary battery black powder with water to obtain black powder slurry; S2, adding acid to the black powder slurry to adjust the pH value to 0.5-1.0, then adding hydrogen peroxide to adjust the pH value to 1.5-2.0, and separating to obtain a medium immersion liquid; S3, adding thiosulfate to the intermediate leaching solution to perform one-step copper removal to obtain a one-step copper removal solution; S4, adding a sulfide compound solution to the one-step copper removal solution to perform two-step copper removal to obtain a two-step copper removal solution; S5, adding an oxidant to the solution after the copper removal in the second step, and then adjusting the pH to remove iron and aluminum to obtain a purified solution.

2. The leaching and purification process for cracking ternary battery black powder according to claim 1 is characterized in that: In step S1, the mass ratio of the cracked ternary battery black powder to water is 1: (1.8-2.5); the slurrying time is more than 0.5h.

3. The leaching and purification process for cracking ternary battery black powder according to claim 1, characterized in that: In step S2, acid solution is added to the black powder slurry to adjust the pH value to 0.5-1.0 and maintained for more than 10 minutes, and then hydrogen peroxide is added dropwise to adjust the pH value to 1.5-2.0, and the mixture is aged for at least 0.5 hours to obtain an intermediate leaching solution and intermediate leaching residue through solid-liquid separation.

4. The leaching and purification process for cracking ternary battery black powder according to claim 3 is characterized in that: The process further includes subjecting the intermediate leaching residue to acid leaching treatment, wherein the acid leaching treatment specifically includes: The intermediate leaching residue is subjected to acid leaching treatment with concentrated sulfuric acid to separate the acid leaching residue and the acid leaching liquid; the acid leaching liquid is reused as acid liquid; The acid leaching residue is washed with water to obtain leaching residue and water washing liquid; the water washing liquid is returned to the acid leaching treatment.

5. The leaching and purification process for cracking ternary battery black powder according to claim 4 is characterized in that: Step S3 also includes: pickling the one-step copper removal slag obtained by the one-step copper removal with dilute sulfuric acid having a pH of 1.0 to 1.5, with a liquid-to-solid ratio of (2.5 to 3.5):1, and a washing time of more than 1 hour to obtain cuprous sulfide slag and a one-step copper removal pickling solution; and / or, Step S5 also includes: slurrying the first iron-aluminum slag obtained by removing iron and aluminum with water to obtain a first iron-aluminum slag slurry; adjusting the pH value of the first iron-aluminum slag slurry to 1.5-2.0 by concentrated sulfuric acid and stabilizing it for more than 5 minutes, then heating it to 80-85°C to carry out iron-aluminum slag pickling, stopping the reaction when the pH value is 3.0-3.5, and obtaining a second iron-aluminum slag and an iron-aluminum slag pickling liquid by solid-liquid separation; washing the second iron-aluminum slag with water to obtain a third iron-aluminum slag and an iron-aluminum water washing liquid, and recycling the iron-aluminum water washing liquid to the iron-aluminum slag pickling step; and / or, The one-step copper removal pickling solution and the iron-aluminum slag pickling solution are returned to the acid leaching process.

6. The leaching and purification process for cracking ternary battery black powder according to claim 1, characterized in that: In step S3, the thiosulfate includes sodium thiosulfate; the molar ratio of the sodium thiosulfate to the copper ions contained in the intermediate leaching solution is (0.95-1.05):1; In the one-step copper removal, the pH value of the intermediate leaching solution is first controlled at 2.0-3.0 and the temperature is above 80° C., and then sodium thiosulfate is added to react for 0.5-1.0 h.

7. The leaching and purification process for cracking ternary battery black powder according to claim 1, characterized in that: In step S4, the sulfide compound solution includes a sodium sulfide solution; the molar ratio of the sodium sulfide to the copper ions in the solution after one-step copper removal is (1.4-2.1):

1.

8. The leaching and purification process for cracking ternary battery black powder according to claim 7, characterized in that: When the copper content in the solution after one-step copper removal is 100-200 ppm, the molar ratio of sodium sulfide to copper is 1.5:1.0; when the copper content in the solution after one-step copper removal is less than 100 ppm, the molar ratio of sodium sulfide to copper is 2:

1.

9. The leaching and purification process for cracking ternary battery black powder according to claim 1, characterized in that: In step S4, water is added to the two-step copper removal slag obtained by the two-step copper removal to be slurried to obtain a two-step copper removal slurry; and the two-step copper removal slurry is combined with the black powder slurry.

10. The leaching and purification process for cracking ternary battery black powder according to claim 1, characterized in that: The iron and aluminum removal in step S5 specifically includes: adding an oxidant to the liquid after the second step copper removal, reacting for more than 0.5 hours; then heating to 85-90°C, adding sodium carbonate solution to adjust the pH value to above 5.0, reacting for at least 1 hour, and filtering to obtain the first iron-aluminum slag and the purified liquid.