Method for recovering valuable elements in stone coal vanadium extraction purification slag

By using staged acid addition and flocculation treatment, the problem of recovering valuable elements from vanadium extraction slag in shale coal was solved, achieving efficient recovery of uranium, vanadium, and silicon, and improving production efficiency and economic benefits.

CN118957321APending Publication Date: 2024-11-15BEIJING RESEARCH INSTITUTE OF CHEMICAL ENGINEERING AND METALLURGY
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411035467.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Existing technologies are insufficient to effectively recover valuable elements such as vanadium, uranium, and silicon from vanadium extraction and purification slag from coal shale. The formation of silica gel during the leaching process makes leaching filtration difficult, affecting the extraction rate of valuable elements and the continuity of production.

Method used

A staged acid addition method was adopted to control the amount of acid added and the stirring rate to avoid the formation of silica gel. Solid-liquid separation was achieved through flocculation and aging treatment, and uranium and vanadium were recovered by extraction method to obtain precipitated silica product.

Benefits of technology

This method achieves efficient recovery of uranium, vanadium, and silicon from vanadium extraction and purification slag in coal shale, with a leaching rate of over 99%. It also reduces the SiO2 content in the filtrate, thereby improving the continuity of production and the comprehensive utilization rate of valuable elements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957321A_ABST
    Figure CN118957321A_ABST
Patent Text Reader

Abstract

The invention provides a method for recovering valuable elements in stone coal vanadium extraction purification slag, and relates to the technical field of hydrometallurgy. The method for recovering the valuable elements in the stone coal vanadium extraction purification slag comprises the steps of slurry blending, slurry acidolysis and aging, separation and recovery of silicon in slurry, separation and recovery of uranium in a solution, and separation and recovery of vanadium in the solution. According to the method, through comprehensive regulation and control of silicon concentration and salt concentration in the solution in the purification slag acidolysis process, acid adding amount and acid adding speed control, flocculation silicon removal of the leaching solution, aging and the like, form control of silica sol in the solution is achieved, and the technical problems that after leaching, slurry is poor in solid-liquid separation performance, low in valuable element extraction rate and the like are effectively solved. The method realizes comprehensive recovery of three elements of uranium, vanadium and silicon in the purification slag, and has the advantages of high comprehensive utilization rate and good economic benefit.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of hydrometallurgy, and in particular to a method for recovering valuable elements in stone coal vanadium extraction and purification slag. Background Art

[0002] Stone coal vanadium ore is an important vanadium metal resource, and stone coal vanadium extraction is an important way to obtain metallic vanadium. The main processes for extracting vanadium from stone coal are: stone coal crushing, 700-800℃ decarburization, grinding, 800-900℃ roasting, sulfuric acid leaching, solid-liquid separation, and vanadium extraction from leachate. The main processes for extracting vanadium from leachate are: ion exchange, purification and impurity removal, ammonium salt precipitation of vanadium, and roasting.

[0003] Stone coal vanadium extraction purification slag is the waste slag produced in the solution purification link before vanadium precipitation in the stone coal vanadium extraction process. Its main components are magnesium silicate and magnesium phosphate. In addition, it also contains 2.5-8wt% V2O5 and 0.1-1.0wt% U3O8, which is a typical radioactive waste slag. Patent CN202310044143.1 ("A method for co-treatment of lead-containing wastewater using modified stone coal vanadium extraction smelting waste slag") discloses the use of 880-920℃ high-temperature roasting modification to obtain modified slag with MgO and SiO2 as the main components and good dispersibility, and use it for lead-containing wastewater treatment, achieving harmless treatment of waste slag, solving the pollution of large-scale storage to the environment, and saving the cost of wastewater treatment; but this method does not achieve the recovery of valuable elements in the slag. In addition, attempts were made to mix the purified slag with the roasted material (material roasted at 800-900°C) for leaching to recover the valuable element vanadium. However, it was found that colloidal silicon dioxide (silica gel) was precipitated during the leaching process, making leaching and filtration difficult, and it was still difficult to achieve the recovery of the valuable elements. Summary of the invention

[0004] In view of this, the purpose of the present invention is to provide a method for recovering valuable elements in stone coal vanadium purification slag. The present invention realizes the comprehensive recovery of three valuable elements, uranium, vanadium and silicon, in stone coal vanadium purification slag.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] The present invention provides a method for recovering valuable elements in stone coal vanadium extraction and purification slag, comprising the following steps:

[0007] Mixing the purified slag from vanadium extraction from stone coal with water to obtain purified slag slurry;

[0008] Concentrated sulfuric acid is added to the purified slag slurry for acid reaction to obtain a leachate; the ratio of the amount of H2SO4 in the concentrated sulfuric acid to the amount of SiO2 in the purified slag slurry is (2.8-3.5):1; the acid reaction comprises a first acid reaction and a second acid reaction in sequence, the first acid reaction is to add part of the concentrated sulfuric acid at a first stirring rate, the amount of the part of the concentrated sulfuric acid added is 50-80% of the total mass of the concentrated sulfuric acid, and the second acid reaction is to add the remaining concentrated sulfuric acid at a second stirring rate; the first stirring rate is greater than the second stirring rate, and the addition rate of the part of the concentrated sulfuric acid is less than the addition rate of the remaining concentrated sulfuric acid;

[0009] The leachate and the flocculant are mixed and flocculated and aged in sequence to obtain an aged slurry;

[0010] The aged slurry is subjected to solid-liquid separation to obtain silicon slag and filtrate;

[0011] The silicon slag is sequentially washed and dried to obtain white carbon black and washing liquid;

[0012] The filtrate and the washing solution are combined, and the obtained solution is subjected to uranium extraction to obtain a uranium product and a vanadium-containing solution.

[0013] Preferably, the mass content of V2O5 in the stone coal vanadium extraction and purification slag is 2.5-8.0%, the mass content of U3O8 is 0.1-1.0%, the mass content of SiO2 is 25-35%, the mass content of P2O5 is 18-25%, and the mass content of MgO is 22-30%.

[0014] Preferably, the mass ratio of the stone coal vanadium extraction purification slag to water is 1:(0.1-0.5).

[0015] Preferably, the mass fraction of the concentrated sulfuric acid is 90-98%.

[0016] Preferably, the first stirring rate is 400-600 rpm; and the adding rate of the portion of concentrated sulfuric acid is 0.1-0.5% of the total mass of concentrated sulfuric acid added per minute.

[0017] Preferably, the first acid reaction is completed until the addition of the portion of concentrated sulfuric acid is completed, and the temperature of the slurry obtained after the addition of the portion of concentrated sulfuric acid is completed is 40-70°C.

[0018] Preferably, the second stirring rate is 280-450 rpm; the addition rate of the remaining concentrated sulfuric acid is 0.3-1.0% of the total mass of concentrated sulfuric acid added per minute.

[0019] Preferably, the second acid reaction further comprises continuing the reaction for 1 to 2 hours after the addition of the remaining concentrated sulfuric acid is completed, and the temperature of the slurry obtained after the addition of the remaining concentrated sulfuric acid is completed is 60 to 85°C.

[0020] Preferably, the flocculant is a cationic polyacrylamide flocculant, the molecular weight of the cationic polyacrylamide flocculant is 1 million to 3 million, the amount of flocculant added to the leachate is 30 to 80 mg / L; the flocculation time is 0.5 to 1.5 hours, the aging temperature is 50 to 75°C, and the time is 3 to 5 hours.

[0021] Preferably, the uranium extraction method comprises: extracting the solution with an extractant to obtain a loaded organic phase and a vanadium-containing solution;

[0022] washing the loaded organic phase to obtain a washed loaded organic phase;

[0023] Using a stripping agent to strip the washed loaded organic phase to obtain a uranium product;

[0024] The extractant is a mixed reagent of di(2-ethylhexyl)phosphoric acid, tributyl phosphate and sulfonated kerosene, wherein the concentration of di(2-ethylhexyl)phosphoric acid in the mixed reagent is 0.15-0.5 mol / L, and the concentration of tributyl phosphate is 0.18-0.72 mol / L;

[0025] The washing reagent used for washing the loaded organic phase is a sulfuric acid solution, and the concentration of the sulfuric acid solution is 0.1-0.5 mol / L;

[0026] The stripping agent is an aqueous solution of (NH4)2CO3, and the concentration of the aqueous solution of (NH4)2CO3 is 1 to 1.5 mol / L.

[0027] The present invention provides a method for recovering valuable elements in stone coal vanadium purification slag. The present invention divides the acid reaction into two stages: the first acid reaction and the second acid reaction. The different acid addition amounts, acid addition rates and stirring rates in the two stages are controlled. The first acid reaction stage is slow acid addition and strong stirring to control the acidity and temperature to avoid the formation of silica gel as much as possible. The second acid reaction stage has crossed the silica gel formation stage, and the acid addition rate is appropriately increased to ensure the reaction temperature and shorten the entire reaction time. The stirring rate is appropriately reduced to form larger particles of silica sol, and then silicon removal is conveniently achieved through subsequent flocculation and aging, which is conducive to the recovery of vanadium and uranium in the subsequent solution. In addition, the present invention combines the filtrate after the solid-liquid separation of the aged slurry with the silicon slag washing liquid, thereby avoiding the crystallization of MgSO4, Mg(H2PO4)2 and other salts in the leaching solution due to excessive concentration, forming scale in pipelines and equipment, and affecting the continuity of production. The present invention avoids the formation of silica gel with Si-O-Si network structure in the acid leaching process by controlling the acid addition amount and acid addition speed, as well as flocculation and silicon removal and aging of the acid leaching solution, and realizes the morphology control of the silica sol in the solution, so that the solid-liquid separation speed (such as vacuum filtration) of the leaching slurry is increased by more than 5 times, the leaching rate of uranium and vanadium in the purified slag reaches more than 99%, and the SiO2 content in the filtrate is reduced to less than 50 mg / L, effectively solving the technical problems of poor solid-liquid separation performance of the slurry after leaching and low extraction rate of valuable elements. The present invention realizes the comprehensive recovery of the three elements of uranium, vanadium and silicon in the purified slag, and has the advantages of high comprehensive utilization rate and good economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The figure is a schematic diagram of a process for recovering valuable elements (uranium, vanadium and silicon) in stone coal vanadium extraction purification slag according to an embodiment of the present invention. DETAILED DESCRIPTION

[0029] The present invention provides a method for recovering valuable elements in stone coal vanadium extraction and purification slag, comprising the following steps:

[0030] Mixing the purified slag from vanadium extraction from stone coal with water to obtain purified slag slurry;

[0031] Concentrated sulfuric acid is added to the purified slag slurry for acid reaction to obtain a leachate; the ratio of the amount of H2SO4 in the concentrated sulfuric acid to the amount of SiO2 in the purified slag slurry is (2.8-3.5):1; the acid reaction comprises a first acid reaction and a second acid reaction in sequence, the first acid reaction is to add part of the concentrated sulfuric acid at a first stirring rate, the amount of the part of the concentrated sulfuric acid added is 50-80% of the total amount of the concentrated sulfuric acid, and the second acid reaction is to add the remaining concentrated sulfuric acid at a second stirring rate; the first stirring rate is greater than the second stirring rate, and the addition rate of the part of the concentrated sulfuric acid is less than the addition rate of the remaining concentrated sulfuric acid;

[0032] The leachate and the flocculant are mixed and flocculated and aged in sequence to obtain an aged slurry;

[0033] The aged slurry is subjected to solid-liquid separation to obtain silicon slag and filtrate;

[0034] The silicon slag is sequentially washed and dried to obtain white carbon black and washing liquid;

[0035] The filtrate and the washing solution are combined, and the obtained solution is subjected to uranium extraction to obtain a uranium product and a vanadium-containing solution.

[0036] In the present invention, unless otherwise specified, the raw materials / components involved are commercially available products well known to those skilled in the art.

[0037] The present invention mixes the stone coal vanadium extraction purification slag with water to obtain a purified slag slurry. In the present invention, the stone coal vanadium extraction purification slag is a uranium-vanadium-containing waste slag, specifically a production line plate-frame filter press slag. In the present invention, the mass content of V2O5 in the stone coal vanadium extraction purification slag is preferably 2.5-8.0%, more preferably 3-6.5%, the mass content of U3O8 is preferably 0.1-1.0%, more preferably 0.5-0.8%, the mass content of SiO2 is preferably 25-35%, more preferably 27-33%, the mass content of P2O5 is preferably 18-25%, more preferably 20-24%, and the mass content of MgO is preferably 22-30%, more preferably 25-29%; the mass content of V2O5, U3O8, SiO2, P2O5, and MgO in the stone coal vanadium extraction purification slag is the content after the corresponding elements in the stone coal vanadium extraction purification slag are converted.

[0038] In the present invention, the mass ratio of the stone coal vanadium purification slag to water is preferably 1:(0.1-0.5), more preferably 1:(0.2-0.3). In the present invention, water is preferably added to the stone coal vanadium purification slag under stirring, and stirred evenly to obtain the purification slag slurry.

[0039] After obtaining the purified slag slurry, the present invention adds concentrated sulfuric acid to the purified slag slurry for acid reaction to obtain a leaching solution.

[0040] In the present invention, the mass fraction of the concentrated sulfuric acid is preferably 90-98%, more preferably 92-95%; the ratio of the amount of H2SO4 in the concentrated sulfuric acid to the amount of SiO2 in the purified slag slurry is (2.8-3.5):1, that is, n(H2SO4) / n(SiO2)=2.8-3.5, more preferably 3.0-3.2. The formation of silica gel is closely related to acidity, temperature, etc. When n(H2SO4) / n(SiO2)<2.8, although a large amount of silica gel will not be formed, the silicon content in the final solution is high, which affects the subsequent process; when n(H2SO4) / n(SiO2)>2.8, silica gel is very easy to form, and controlling the acid addition speed is the key; at the same time, controlling the acid addition speed also utilizes the dilution heat and reaction heat of sulfuric acid addition to make the reaction reach the optimal temperature, which will also affect the morphology of silicon.

[0041] In the present invention, the acid reaction includes sequentially performing a first acid reaction and a second acid reaction.

[0042] In the present invention, the first acid reaction is to add part of concentrated sulfuric acid at the first stirring rate, and the amount of the part of concentrated sulfuric acid added is 50-80% of the total mass of concentrated sulfuric acid, preferably 67-75%. In the present invention, the first stirring rate is preferably 400-600rpm, more preferably 550-580rpm; the rate of adding the part of concentrated sulfuric acid is preferably 0.1-0.5% of the total mass of concentrated sulfuric acid added per minute (i.e. the total amount of concentrated sulfuric acid added in the first acid reaction and the second acid reaction), preferably 0.2-0.4%, more preferably 0.3%. In the present invention, the first acid reaction ends when the part of concentrated sulfuric acid is added completely, and the temperature of the slurry obtained after the part of concentrated sulfuric acid is added completely is preferably 40-70°C, more preferably 50-58°C, and further preferably 50-55°C. In the present invention, the first acid reaction is mainly to purify the acid decomposition process of solids in the slag slurry, while avoiding the formation of silica gel, and the reactions involved are as follows (vanadium (sodium vanadate) exists mainly in the adsorbed state in the slag, and dissolves the adsorbents such as phosphates and silicates into the solution):

[0043] Na2U2O7+4H2SO4→2UO2SO4+2NaHSO4+3H2O

[0044] Mg3(PO4)2↓+2H + →3Mg 2+ +2HPO4 2-

[0045] MgSiO3↓+H + →Mg 2+ +HSiO3 - .

[0046] In the present invention, the second acid reaction is to add the remaining concentrated sulfuric acid at the second stirring rate, that is, the part of the concentrated sulfuric acid and the remaining concentrated sulfuric acid constitute all the concentrated sulfuric acid. In the present invention, the first stirring rate is greater than the second stirring rate, and the second stirring rate is preferably 280-450rpm, more preferably 300-420pm, and further preferably 350-360rpm. In the present invention, the addition rate of the part of the concentrated sulfuric acid is less than the addition rate of the remaining concentrated sulfuric acid, and the addition rate of the remaining concentrated sulfuric acid is preferably 0.3-1.0% of the total mass of concentrated sulfuric acid added per minute, and more preferably 0.5-1.0%. In the present invention, the second acid reaction preferably also includes continuing the reaction for 1-2h after the addition of the remaining concentrated sulfuric acid is completed; the temperature of the slurry obtained after the addition of the remaining concentrated sulfuric acid is preferably 60-85°C, more preferably 65-80°C, and further preferably 65-70°C. In the present invention, the continued reaction for 1 to 2 hours is preferably carried out under stirring, and the stirring rate is preferably the same as the stirring rate when the remaining concentrated sulfuric acid is added; continuing the reaction for 1 to 2 hours under stirring can ensure the reaction of silicon, the silicon reaction speed is fast, and it is easy to precipitate completely, reducing the residual silicon concentration in the solution. In the present invention, the second acid reaction is the process of forming silicic acid and silicon polymerization to generate silica sol to obtain the acid reaction solution.

[0047] The present invention adds acid in two stages, and controls the acid addition speed and stirring speed of the two stages differently. In the first stage, the acid addition should be slow and stirred strongly to control the acidity and temperature to avoid the formation of silica gel as much as possible; in the second stage, the silica gel formation stage has been crossed, and the acid addition speed is appropriately increased to ensure the reaction temperature, shorten the entire reaction time, and appropriately reduce the stirring speed to form larger particles of silica sol. The present invention first dissolves the silicate and the acid into the solution, and then undergoes a series of reactions such as polymerization-depolymerization-saturation precipitation to generate silica sol.

[0048] After obtaining the leachate, the present invention mixes the leachate and a flocculant to perform flocculation and aging in sequence to obtain an aged slurry.

[0049] In the present invention, the flocculant is preferably a cationic polyacrylamide flocculant, and the molecular weight of the cationic polyacrylamide flocculant is preferably 1 million to 3 million, more preferably 2 million to 3 million, and the amount of flocculant added to the acid reaction solution is preferably 30 to 80 mg / L, more preferably 50 to 60 mg / L. In the present invention, the flocculant is preferably added to the acid reaction solution under stirring, and the stirring rate is preferably 280 to 400 rpm, more preferably 300 to 380 rpm. In the present invention, the flocculation time is preferably 0.5 to 1.5 hours, more preferably 1 to 1.5 hours, and the flocculation time is calculated from the completion of the addition of the flocculant, and stirring is maintained during the flocculation process.

[0050] In the present invention, the aging temperature is preferably 50-75° C., more preferably 55-60° C., the time is preferably 3-5 h, more preferably 3-4 h, and the aging is carried out under static conditions.

[0051] The present invention adds a cationic polyacrylamide flocculant into the leaching solution. Under the action of electrostatic force, van der Waals force and hydrogen bond, a part of the long-chain polymer is adsorbed on the surface of the colloidal particles, and the other part is adsorbed on the surface of another particle, so that more colloidal particles are adsorbed on a long chain of the polymer, thereby connecting the colloidal particles into large-particle floccules, and then the silicon can be separated from the solution in a solid-liquid manner.

[0052] After obtaining the aged slurry, the present invention performs solid-liquid separation on the aged slurry to obtain silicon slag and filtrate. In the present invention, the solid-liquid separation method is preferably vacuum filtration. In the present invention, during the solid-liquid separation, the temperature of the aged slurry is preferably above 50°C, more preferably 55-70°C.

[0053] After obtaining silicon slag, the present invention sequentially washes and dries the silicon slag to obtain white carbon black and washing liquid. In the present invention, the washing preferably uses hot water at 50 to 70°C to wash the silicon slag in three stages, and the single-stage washing ratio (the ratio of the volume of washing water added to the volume of the solution contained in the silicon slag) is preferably 0.5 to 1.5, and more preferably 0.5 to 1.0. After the washing, wet silicon slag and washing liquid are obtained, and the wet silicon slag is dried. In the present invention, the drying temperature is preferably 110 to 130°C, and the drying is a dehydration process, including free water and partially bound water, and the reaction formula involved is: nSiO2·(m+1)H2O→nSiO2+(m+1)H2O. After drying, white carbon black is obtained, and the mass content of SiO2 in the white carbon black is more than 90%.

[0054] After obtaining the filtrate and the washing solution, the present invention combines the filtrate and the washing solution, and extracts uranium from the obtained solution to obtain a uranium product and a vanadium-containing solution. In the present invention, the uranium extraction method preferably comprises:

[0055] extracting the solution with an extractant to obtain a loaded organic phase and a vanadium-containing solution;

[0056] washing the loaded organic phase to obtain a washed loaded organic phase;

[0057] The washed loaded organic phase is stripped with a stripping agent to obtain a uranium product.

[0058] In the present invention, the extractant is preferably a mixed reagent of di(2-ethylhexyl)phosphoric acid, tributyl phosphate (TBP) and sulfonated kerosene, the concentration of di(2-ethylhexyl)phosphoric acid in the mixed reagent is preferably 0.15-0.5 mol / L, more preferably 0.25-0.35 mol / L, and the concentration of tributyl phosphate is preferably 0.18-0.72 mol / L, more preferably 0.2-0.3 mol / L. In the present invention, the extraction phase ratio A / O of the extraction is preferably (4-5):1, more preferably (4.5-5):1, and the contact time is preferably 3-5 min, more preferably 4-5 min.

[0059] In the present invention, the washing reagent used for washing the loaded organic phase is preferably a sulfuric acid solution, and the concentration of the sulfuric acid solution is preferably 0.1-0.5 mol / L, more preferably 0.1-0.3 mol / L; the washing phase ratio A / O of the washing is preferably 1:(4-5), more preferably 1:(4.5-5), and the contact time is preferably 3-5 min, more preferably 3-4 min.

[0060] In the present invention, the stripping agent is preferably an aqueous (NH4)2CO3 solution, and the concentration of the aqueous (NH4)2CO3 solution is preferably 1-1.5 mol / L, more preferably 1.2-1.4 mol / L; the stripping ratio A / O of the stripping is preferably 1:(8-15), more preferably 1:(10-12), and the contact time is preferably 10-30 min, more preferably 15-20 min. In the present invention, the stripping obtains a uranium product and a lean organic phase, the uranium in the uranium product exists in the form of uranyl ammonium tricarbonate, and the lean organic phase is reused in the extraction as an extractant.

[0061] In the present invention, the vanadium-containing solution obtained after uranium extraction can be directly returned to the existing ion exchange process of extracting vanadium from stone coal to recover vanadium.

[0062] The present invention aims to solve the technical problems that silicon has an adverse effect on leaching and solid-liquid separation and valuable elements cannot be utilized in the leaching process of vanadium extraction and purification slag, and provides a method for recovering uranium, vanadium and silicon in vanadium extraction and purification slag with good treatment effect, efficient utilization of valuable elements and good economic benefits.

[0063] In order to further illustrate the present invention, the method for recovering valuable elements in the stone coal vanadium purification slag provided by the present invention is described in detail below with reference to examples, but they should not be construed as limiting the protection scope of the present invention.

[0064] The process of recovering valuable elements (uranium, vanadium and silicon) from the stone coal vanadium purification slag in the embodiment is as follows: Figure 1 shown.

[0065] Example 1

[0066] A batch of vanadium-extracted purified slag from stone coal has a V2O5 content of 3.45%, a U3O8 content of 0.769%, a SiO2 content of 27.2%, a P2O5 content of 20.5%, and a MgO content of 25.2%.

[0067] (1) Slurry preparation

[0068] The purification residue is the plate and frame filter press residue of the production line. According to the purification residue: water mass ratio = 1:0.2, the purification residue is added into water under stirring condition, stirred evenly, and a slurry is obtained.

[0069] (2) Slurry acidification and aging

[0070] The amount of concentrated sulfuric acid added during the acidolysis process: According to the amount of SiO2 in the purified slag, the total acid requirement for slurry acidolysis is calculated by n(H2SO4) / n(SiO2)=3.0.

[0071] The first stage of acid addition reaction: the amount of concentrated sulfuric acid added in the first stage is 67% of the total amount of acid added, and the concentration of concentrated sulfuric acid is 98wt%; under the stirring condition of 550rpm, the concentrated sulfuric acid is added by using a metering pump, and the acid addition speed is controlled at 0.3wt% / min (that is, 0.3% of the total acid amount is added per minute, the same as in the following embodiments), and the slurry temperature after acid addition is 55°C;

[0072] Second stage of acid addition reaction: After the first stage of acid addition reaction is completed, concentrated sulfuric acid is continued to be added for the second stage of reaction. The amount of concentrated sulfuric acid added in the second stage is 33% of the total amount of acid added, and the concentration of concentrated sulfuric acid is 98wt%; under the stirring condition of 350rpm, the concentrated sulfuric acid is added by a metering pump, and the acid addition speed is controlled at 0.5wt% / min (that is, 0.5% of the total acid amount is added per minute, the same as in the following embodiments), and the slurry temperature after acid addition is 65℃; after all the concentrated sulfuric acid is added, continue stirring for 2h;

[0073] The third stage is flocculation and aging: under the stirring condition of 350rpm, add cationic polyacrylamide flocculant (molecular weight 2.8 million) at 60mg / L and stir for 1.5h; after the flocculation reaction is completed, keep it at 60℃ and let it stand for 3h.

[0074] (3) Separation and recovery of silicon in the slurry: The aged slurry was filtered by vacuum filtration, and the slurry temperature was maintained at 55°C; after filtration, the silicon slag was washed in three stages with hot water at 70°C, with a single-stage washing ratio of 0.5. The washing liquid and the filtrate were combined for subsequent uranium and vanadium recovery. The silicon slag was dried at 130°C to obtain white carbon with a SiO2 content of 91.2wt%.

[0075] (4) Separation and recovery of uranium in solution: Uranium in solution was separated by extraction. The extractant was 0.3 mol / L di(2-ethylhexyl)phosphoric acid + 0.3 mol / L TBP + sulfonated kerosene, the extraction phase ratio was A / O = 4.5:1, and the contact time was 5 min; the loaded organic phase was washed with 0.1 mol / L H2SO4 solution, the washing phase ratio was A / O = 1:4, and the contact time was 3 min; after washing, the loaded organic phase was stripped of uranium with 1.2 mol / L (NH4)2CO3 aqueous solution, the stripping phase ratio was A / O = 1:10, and the contact time was 15 min, to obtain uranamide tricarbonate product and lean organic phase, and the lean organic phase was reused as the extractant.

[0076] (5) Separation and recovery of vanadium in solution: After uranium extraction, the vanadium in the solution is directly returned to the existing ion exchange process for vanadium extraction from stone coal to recover vanadium.

[0077] The uranium content in the uranium tricarbonate amide product is 45.1wt%, and the uranium recovery rate is 97.2%; the vanadium recovery rate is 98.5%; the SiO2 content in the white carbon black is 91.2wt%, and the silicon recovery rate is 96.8%.

[0078] Example 2

[0079] A batch of stone coal vanadium extraction purification slag, the mass content of V2O5 in the purified slag is 6.5%, the mass content of U3O8 is 0.641%, the mass content of SiO2 is 30.34%, the mass content of P2O5 is 22.89%, and the mass content of MgO is 26.78%.

[0080] (1) Slurry preparation

[0081] The purification residue is the plate and frame filter press residue of the production line. According to the purification residue: water mass ratio = 1:0.25, the purification residue is added into water under stirring condition, stirred evenly, and a slurry is obtained.

[0082] (2) Slurry acidification and aging

[0083] The amount of concentrated sulfuric acid added during the acidolysis process: According to the amount of SiO2 in the purified slag, the total acid requirement for slurry acidolysis is calculated by n(H2SO4) / n(SiO2)=3.2.

[0084] The first stage of acid addition reaction: the amount of concentrated sulfuric acid added in the first stage is 75% of the total amount of acid added, and the concentration of concentrated sulfuric acid is 92wt%; under the stirring condition of 600rpm, the concentrated sulfuric acid is added by a metering pump, the acid addition speed is controlled at 0.26wt% / min, and the slurry temperature after acid addition is 50°C;

[0085] Second stage of acid addition reaction: After the first stage of acid addition reaction is completed, continue to add concentrated sulfuric acid for the second stage of reaction. The amount of concentrated sulfuric acid added in the second stage is 25% of the total amount of acid added, and the concentration of concentrated sulfuric acid is 92wt%; under the stirring condition of 420rpm, the concentrated sulfuric acid is added by a metering pump, and the acid addition speed is controlled at 0.8wt% / min. The slurry temperature after acid addition is 70℃; after all the concentrated sulfuric acid is added, continue stirring for 2h;

[0086] The third stage of flocculation and aging: under the stirring condition of 300rpm, add cationic polyacrylamide flocculant (molecular weight 2.8 million) according to 50mg / L and stir for 1.5h; after the flocculation reaction is completed, keep it at 60℃ and let it settle for 3h.

[0087] (3) Separation and recovery of silicon in the slurry: The aged slurry was filtered by vacuum filtration, and the slurry temperature was maintained at 60°C; after filtration, the silicon slag was washed in three stages with hot water at 65°C, with a single-stage washing ratio of 0.5. The washing liquid and the filtrate were combined for subsequent uranium and vanadium recovery. The silicon slag was dried at 130°C to obtain white carbon black with a SiO2 content of 92.0%.

[0088] (4) Separation and recovery of uranium in solution: Uranium in solution was separated by extraction. The extractant was 0.35 mol / L di(2-ethylhexyl)phosphoric acid + 0.3 mol / L TBP + sulfonated kerosene, the extraction phase ratio was A / O = 4:1, and the contact time was 5 min; the loaded organic phase was washed with 0.15 mol / L H2SO4 solution, the washing phase ratio was A / O = 1:4, and the contact time was 3 min; after washing, the loaded organic phase was stripped of uranium with 1.2 mol / L (NH4)2CO3 aqueous solution, the stripping phase ratio was A / O = 1:10, and the contact time was 20 min, to obtain uranamide tricarbonate product and lean organic phase, and the lean organic phase was reused as the extractant.

[0089] (5) Separation and recovery of vanadium in solution: After uranium extraction, the vanadium in the solution is directly returned to the existing ion exchange process for vanadium extraction from stone coal to recover vanadium.

[0090] The uranium content in the uranium tricarbonate amide product is 44.9wt%, and the uranium recovery rate is 96.8%; the vanadium recovery rate is 97.5%; the SiO2 content in the white carbon black is 92.0wt%, and the silicon recovery rate is 96.0%.

[0091] Example 3

[0092] A batch of stone coal vanadium extraction purification slag, the mass content of V2O5 in the purified slag is 2.89%, the mass content of U3O8 is 0.558%, the mass content of SiO2 is 32.8%, the mass content of P2O5 is 23.6%, and the mass content of MgO is 28.5%.

[0093] (1) Slurry preparation

[0094] The purification residue is the plate and frame filter press residue of the production line. According to the purification residue: water mass ratio = 1:0.5, the purification residue is added into water under stirring condition, stirred evenly, and a slurry is obtained.

[0095] (2) Slurry acidification and aging

[0096] The amount of concentrated sulfuric acid added during the acidolysis process: According to the amount of SiO2 in the purified slag, the total acid requirement for slurry acidolysis is calculated by n(H2SO4) / n(SiO2)=3.5.

[0097] The first stage of acid addition reaction: the amount of concentrated sulfuric acid added in the first stage is 80% of the total amount of acid added, and the concentration of concentrated sulfuric acid is 95wt%; under the stirring condition of 580rpm, the concentrated sulfuric acid is added by a metering pump, the acid addition speed is controlled at 0.4wt% / min, and the slurry temperature after acid addition is 58°C;

[0098] Second stage of acid addition reaction: After the first stage of acid addition reaction is completed, continue to add concentrated sulfuric acid for the second stage of reaction. The amount of concentrated sulfuric acid added in the second stage is 20% of the total amount of acid added, and the concentration of concentrated sulfuric acid is 95wt%; under the stirring condition of 360rpm, the concentrated sulfuric acid is added by a metering pump, and the acid addition speed is controlled at 0.8wt% / min. The slurry temperature after acid addition is 80℃; after all the concentrated sulfuric acid is added, continue stirring for 2h;

[0099] The third stage of flocculation and aging: under the stirring condition of 300rpm, add cationic polyacrylamide flocculant (molecular weight 2.8 million) according to 80mg / L and stir for 0.5h; after the flocculation reaction is completed, keep it at 75℃ and let it settle for 4h.

[0100] (3) Separation and recovery of silicon in the slurry: The aged slurry was filtered by vacuum filtration, and the slurry temperature was maintained at 70°C; after filtration, the silicon slag was washed in three stages with hot water at 50°C, with a single-stage washing ratio of 1.0. The washing liquid and the filtrate were combined for subsequent uranium and vanadium recovery. The silicon slag was dried at 120°C to obtain white carbon black with a SiO2 content of 90.5%.

[0101] (4) Separation and recovery of uranium in solution: Uranium in solution was separated by extraction. The extractant was 0.25 mol / L di(2-ethylhexyl)phosphoric acid + 0.2 mol / L TBP + sulfonated kerosene, the extraction phase ratio was A / O = 5:1, and the contact time was 4 min; the loaded organic phase was washed with 0.3 mol / L H2SO4 solution, the washing phase ratio was A / O = 1:4.5, and the contact time was 4 min; after washing, the loaded organic phase was stripped of uranium with 1.4 mol / L (NH4)2CO3 aqueous solution, the stripping phase ratio was A / O = 1:12, and the contact time was 25 min, to obtain uranamide tricarbonate product and lean organic phase, and the lean organic phase was reused as the extractant.

[0102] (5) Separation and recovery of vanadium in solution: After uranium extraction, the vanadium in the solution is directly returned to the existing ion exchange process for vanadium extraction from stone coal to recover vanadium.

[0103] The uranium content in the uranium tricarbonate amide product is 44.8wt%, and the uranium recovery rate is 96.2%; the vanadium recovery rate is 97.3%; the SiO2 content in the white carbon black is 90.5wt%, and the silicon recovery rate is 95.2%.

[0104] It can be seen from the above embodiments that the present invention realizes the comprehensive recovery of the three elements of uranium, vanadium and silicon in the purified slag, and has the advantages of high comprehensive utilization rate and good economic benefits.

[0105] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be regarded as the protection scope of the present invention.

Claims

1. A method for recovering valuable elements in stone coal vanadium purification slag, characterized in that: The following steps are involved: Mixing the purified slag from vanadium extraction from stone coal with water to obtain purified slag slurry; Concentrated sulfuric acid is added to the purified slag slurry for acid reaction to obtain a leachate; the ratio of the amount of H2SO4 in the concentrated sulfuric acid to the amount of SiO2 in the purified slag slurry is (2.8-3.5):1; the acid reaction comprises a first acid reaction and a second acid reaction in sequence, the first acid reaction is to add part of the concentrated sulfuric acid at a first stirring rate, the amount of the part of the concentrated sulfuric acid added is 50-80% of the total mass of the concentrated sulfuric acid, and the second acid reaction is to add the remaining concentrated sulfuric acid at a second stirring rate; the first stirring rate is greater than the second stirring rate, and the addition rate of the part of the concentrated sulfuric acid is less than the addition rate of the remaining concentrated sulfuric acid; The leachate and the flocculant are mixed and flocculated and aged in sequence to obtain an aged slurry; The aged slurry is subjected to solid-liquid separation to obtain silicon slag and filtrate; The silicon slag is sequentially washed and dried to obtain white carbon black and washing liquid; The filtrate and the washing solution are combined, and the obtained solution is subjected to uranium extraction to obtain a uranium product and a vanadium-containing solution.

2. The recycling method according to claim 1, characterized in that: The mass content of V2O5 in the stone coal vanadium purification slag is 2.5-8.0%, the mass content of U3O8 is 0.1-1.0%, the mass content of SiO2 is 25-35%, the mass content of P2O5 is 18-25%, and the mass content of MgO is 22-30%.

3. The recycling method according to claim 1, characterized in that: The mass ratio of the stone coal vanadium extraction purification slag to water is 1:(0.1-0.5).

4. The recycling method according to claim 1, characterized in that: The mass fraction of the concentrated sulfuric acid is 90-98%.

5. The recycling method according to claim 1, characterized in that: The first stirring rate is 400-600 rpm; the adding rate of the part of concentrated sulfuric acid is 0.1-0.5% of the total mass of concentrated sulfuric acid added per minute.

6. The recycling method according to claim 1, 4 or 5, characterized in that: The first acid reaction is completed when the addition of the portion of concentrated sulfuric acid is completed, and the temperature of the slurry obtained after the addition of the portion of concentrated sulfuric acid is completed is 40-70°C.

7. The recycling method according to claim 1, characterized in that: The second stirring rate is 280-450 rpm; the addition rate of the remaining concentrated sulfuric acid is 0.3-1.0% of the total mass of the concentrated sulfuric acid added per minute.

8. The recovery method according to claim 1, 4 or 7, characterized in that: The second acid reaction also includes continuing the reaction for 1 to 2 hours after the remaining concentrated sulfuric acid is added, and the temperature of the slurry obtained after the remaining concentrated sulfuric acid is added is 60 to 85°C.

9. The recycling method according to claim 1, characterized in that: The flocculant is a cationic polyacrylamide flocculant, the molecular weight of the cationic polyacrylamide flocculant is 1 million to 3 million, the amount of flocculant added to the leaching solution is 30 to 80 mg / L; the flocculation time is 0.5 to 1.5 hours, the aging temperature is 50 to 75° C., and the time is 3 to 5 hours.

10. The recycling method according to claim 1, characterized in that: The uranium extraction method comprises: extracting the solution with an extractant to obtain a loaded organic phase and a vanadium-containing solution; washing the loaded organic phase to obtain a washed loaded organic phase; Using a stripping agent to strip the washed loaded organic phase to obtain a uranium product; The extractant is a mixed reagent of di(2-ethylhexyl)phosphoric acid, tributyl phosphate and sulfonated kerosene, wherein the concentration of di(2-ethylhexyl)phosphoric acid in the mixed reagent is 0.15-0.5 mol / L, and the concentration of tributyl phosphate is 0.18-0.72 mol / L; The washing reagent used for washing the loaded organic phase is a sulfuric acid solution, and the concentration of the sulfuric acid solution is 0.1-0.5 mol / L; The stripping agent is an aqueous solution of (NH4)2CO3, and the concentration of the aqueous solution of (NH4)2CO3 is 1 to 1.5 mol / L.

Citation Information

Patent Citations

  • Method for cooperatively treating lead-containing wastewater by using modified stone coal vanadium extraction smelting waste slag