Aluminum-based composite material with multistage heterostructure and preparation method of aluminum-based composite material
Through ball milling treatment of aluminum powder, magnesium powder and stearic acid and subsequent heat treatment, an aluminum-based composite material with multi-stage heterostructure is formed, which solves the problem of inversion of strength-plastic toughness of aluminum-based composite material, and achieves high strength and high strength Matching effect of plastic toughness.
Patent Information
- Application Number
- CN202411065615.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-05
AI Technical Summary
It is difficult for existing aluminum-based composite materials to maintain high plastic toughness while increasing their strength, and there is a problem of inverted strength-plastic toughness.
By mixing aluminum powder, magnesium powder and stearic acid for ball milling, cold-welded alloy particles are formed, then mixed with copper oxide powder for a second ball milling, followed by cold pressing, sintering, hot extrusion, solid solution and aging treatment. Aluminum-based composite material with a multi-stage heterostructure is formed.
The high strength and plastic toughness matching of aluminum-based composite materials is achieved. By regulating the interface and internal defect density, a heterogeneous sheet structure with fine crystal inlaid coarse crystal strips is formed, which improves the mechanical properties of the material.
Smart Images

Figure CN118957339A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal-based composite materials, and in particular relates to an aluminum-based composite material with a multi-level heterogeneous structure and a preparation method thereof. Background Art
[0002] Aluminum-based composites have excellent properties such as low density and high specific strength, and have broad application prospects in the fields of aerospace, electronic power, etc. The introduction of reinforcements will significantly reduce the plasticity while increasing the strength of aluminum-based composites. Therefore, overcoming the inversion problem of strength-plasticity / toughness in aluminum-based composites is a scientific problem that needs to be solved urgently.
[0003] Existing patent CN109082568A discloses a method for preparing an in-situ synthesized nano CuAl2 / Al2O3 reinforced aluminum-based composite material, wherein aluminum powder and copper oxide powder are ball-milled and sintered to form an aluminum-based composite material with excellent performance. However, this method still does not solve the inverted relationship between strength and plasticity of aluminum-based composite materials. Existing studies have shown that the introduction of alloying elements can change the precipitation type of reinforcement phase and precipitation phase, effectively strengthening the aluminum-based composite material system, wherein the addition of Mg element can not only form a MgO reinforcement phase that is coherently matched with the aluminum matrix, and the size is significantly reduced, but also a multi-component precipitation phase can be formed under certain conditions, thereby improving the mechanical properties of the composite material. However, the Al-Mg-CuO system formed after the introduction of Mg element still has the problem of not being able to have high strength and plastic toughness at the same time.
[0004] Therefore, how to prepare aluminum-based composite materials with both high strength and ductility has become a technical problem that needs to be solved urgently in this field. Summary of the invention
[0005] In order to solve the above technical problems, the present invention proposes an aluminum-based composite material with a multi-level heterogeneous structure and a preparation method thereof.
[0006] To achieve the above object, the present invention provides the following technical solutions:
[0007] The present invention provides a method for preparing an aluminum-based composite material with a multi-level heterogeneous structure, comprising the following steps:
[0008] (1) mixing aluminum powder, magnesium powder and stearic acid and subjecting the mixture to a first ball milling process under a protective atmosphere to obtain cold welding alloy particles; mixing the cold welding alloy particles with copper oxide powder and subjecting the mixture to a second ball milling process to obtain a composite powder;
[0009] (2) The composite powder obtained in step (1) is sequentially subjected to cold pressing, sintering, hot extrusion, solution treatment and aging treatment to obtain an aluminum-based composite material with a multi-level heterogeneous structure.
[0010] Preferably, in step (1), the mass ratio of the aluminum powder, magnesium powder, copper oxide powder and stearic acid is (18.2-18.4):0.8:(0.8-1):(0.1-0.15).
[0011] Preferably, in step (1), the ball milling parameters of the first ball milling treatment and the second ball milling treatment are independently: ball-to-material ratio is (10:1) to (15:1), rotation speed is 500 rpm / min, and time is 6 to 8 hours.
[0012] Preferably, in step (2), the cold pressing pressure is 600 MPa and the holding time is 3 min.
[0013] Preferably, in step (2), the sintering heating rate is 10K / min, the temperature is 863K, and the holding time is 1 to 2h.
[0014] Preferably, in step (2), the hot extrusion temperature is 843K, the holding time is 40 min, the pressure is 750 MPa, and the extrusion ratio is 16:1.
[0015] Preferably, in step (2), the temperature of the solution treatment is 793 K, the holding time is 4 h, and the cooling method is water quenching.
[0016] Preferably, in step (2), the aging treatment is carried out at a temperature of 408 K and for a time of 24 h.
[0017] The present invention also provides an aluminum-based composite material with a multi-level heterogeneous structure prepared by the preparation method described in the above technical solution.
[0018] Compared with the prior art, the present invention has the following advantages and technical effects:
[0019] The present invention uses aluminum powder, magnesium powder, stearic acid and copper oxide powder as raw materials and adopts segmented ball milling, and can obtain a grain heterogeneous structure by regulating the defect density difference between the interface and the interior, so as to form a heterogeneous lamellar structure in which a coarse-grained zone is embedded in a fine-grained zone; at the same time, under the influence of the reaction heat effect in the second ball milling process and the original distribution position of CuO, MgO particles are mainly distributed inside the grains in the fine-grained zone, so as to obtain an aluminum-based composite material with a multi-level heterogeneous structure; and the precipitation of the precipitated phase Al2Cu is regulated by a subsequent heat treatment process, so as to obtain an aluminum-based composite material with high strength and plastic toughness. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0021] Figure 1It is the process flow chart of Example 1;
[0022] Figure 2 The morphology of the cold-welded alloy particles (a) in step (1) of Example 1 and the non-cold-welded alloy particles (b) in Comparative Example 1;
[0023] Figure 3 EBSD images of the aluminum-based composite materials prepared in Example 1 and Comparative Example 1;
[0024] Figure 4 The engineering stress-strain curves of the aluminum-based composite materials prepared in Example 1 and Comparative Examples 1-2 are shown. DETAILED DESCRIPTION
[0025] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0027] An embodiment of the present invention provides a method for preparing an aluminum-based composite material having a multi-level heterogeneous structure, comprising the following steps:
[0028] (1) mixing aluminum powder, magnesium powder and stearic acid and subjecting the mixture to a first ball milling process under a protective atmosphere to obtain cold welding alloy particles; mixing the cold welding alloy particles with copper oxide powder and subjecting the mixture to a second ball milling process to obtain a composite powder;
[0029] (2) The composite powder obtained in step (1) is sequentially subjected to cold pressing, sintering, hot extrusion, solution treatment and aging treatment to obtain an aluminum-based composite material with a multi-level heterogeneous structure.
[0030] In a preferred embodiment, in step (1), the mass ratio of the aluminum powder, magnesium powder, copper oxide powder and stearic acid is (18.2-18.4):0.8:(0.8-1):(0.1-0.15). The present invention controls the amount of aluminum powder, magnesium powder, copper oxide powder and stearic acid within the above range, which is beneficial to improving the strength-ductility matching relationship of the aluminum-based composite material with a multi-level heterogeneous structure. The stearic acid in the present invention is used to control the degree of cold welding of the alloy powder. Changing the amount of stearic acid will not result in cold welding alloy particles.
[0031] The magnesium powder in the present invention can not only form a MgO reinforcement phase that is coherently matched with an aluminum matrix, but also form a multi-element precipitation phase, thereby improving the mechanical properties of the aluminum-based composite material; the copper oxide powder can be evenly dispersed on the surface of the cold-welded alloy particles during the ball milling process, and combined with the reaction heat effect during the second ball milling process, the MgO particles are mainly distributed inside the grains in the fine-grained area, thereby obtaining an aluminum-based composite material with a multi-level heterogeneous structure, and at the same time, O atoms can be provided through a replacement reaction, and a precipitation phase Al2Cu is precipitated through subsequent heat treatment aging; stearic acid is used as a process control agent to regulate the structure of the aluminum-based composite material, so as to obtain a heterogeneous lamellar grain structure with fine grains embedded in coarse grains.
[0032] In a preferred embodiment, in step (1), the purity of the aluminum powder is 99.9%; the purity of the magnesium powder is 99.9%; and the purity of the copper oxide powder is 99.9%.
[0033] In a preferred embodiment, in step (1), the ball milling parameters of the first ball milling treatment and the second ball milling treatment are independently: ball-to-material ratio is (10:1) to (15:1), the rotation speed is 500 rpm / min, and the time is 6 to 8 hours. The aluminum-based composite material prepared under the above ball milling conditions of the present invention has good strength and plastic toughness.
[0034] In a preferred embodiment, in step (1), the protective atmosphere is argon. In the present invention, the first ball milling is performed under a protective atmosphere to prevent the aluminum powder and the magnesium powder from being oxidized.
[0035] The present invention performs a first ball milling process under a protective atmosphere, so that aluminum powder and magnesium powder are mechanically alloyed under the control of stearic acid, and then copper oxide powder is added for a second ball milling process, thereby realizing microstructure control of the composite powder and obtaining a heterogeneous lamellar grain structure of fine grains inlaid with coarse grains. At the same time, a nano-MgO reinforcement phase is in-situ generated inside the aluminum matrix grains through a solid phase in-situ reaction.
[0036] In a preferred embodiment, in step (2), the cold pressing pressure is 600 MPa, the holding time is 3 min, and the pressurizing device is a hydraulic press. The present invention performs cold pressing under the above cold pressing pressure and holding time, which is conducive to obtaining a dense aluminum-based composite material block.
[0037] In a preferred embodiment, in step (2), the sintering temperature rise rate is 10K / min, the temperature is 863K, the holding time is 1 to 2 hours, the equipment is a tubular furnace, and the atmosphere is argon. The present invention performs sintering under the above sintering conditions, which is conducive to obtaining an aluminum-based composite sintered body with excellent tensile properties.
[0038] In a preferred embodiment, in step (2), the hot extrusion temperature is 843K, the holding time is 40 min, the pressure is 750 MPa, and the extrusion ratio is 16: 1. The present invention performs hot extrusion under the above hot extrusion conditions, which is beneficial to improving the tensile properties of the aluminum-based composite material.
[0039] In a preferred embodiment, in step (2), the temperature of the solution treatment is 793K, the holding time is 4 hours, and the cooling method is water quenching.
[0040] In a preferred embodiment, in step (2), the aging treatment is carried out at a temperature of 408 K, for a time of 24 h, and by air cooling.
[0041] The present invention regulates the precipitation of the precipitated phase by solid solution treatment and aging treatment, which is conducive to obtaining an aluminum-based composite material with high strength and plasticity.
[0042] The present invention also provides an aluminum-based composite material with a multi-level heterogeneous structure prepared by the preparation method described in the above technical solution.
[0043] The aluminum-based composite material with a multi-level heterogeneous structure provided by the invention has high strength and plastic toughness.
[0044] The room temperature in the embodiments of the present invention refers to "25±2°C".
[0045] Unless otherwise specified, the raw materials in the examples of the present invention were purchased from commercial sources.
[0046] Example 1
[0047] A method for preparing an aluminum-based composite material with a multi-level heterogeneous structure, the process flow is as follows Figure 1 As shown, the specific steps are as follows:
[0048] (1) 18.2 g aluminum powder, 0.8 g magnesium powder and 0.11 g stearic acid were placed in a 250 mL ball mill, and the first ball milling treatment was performed under argon protection. The ball milling parameters were as follows: the ball-to-material ratio was 15:1, the ball milling speed was 500 rpm / min, and the ball milling time was 8 h to obtain cold welding alloy particles; then 1.0 g copper oxide powder was added to the above cold welding alloy particles, and the second ball milling treatment was performed. The ball milling parameters were as follows: the ball-to-material ratio was 15:1, the ball milling speed was 500 rpm / min, and the ball milling time was 6 h to obtain a composite powder.
[0049] (2) placing the composite powder obtained in step (1) in a cold pressing mold, applying a pressure of 600 MPa using a hydraulic press, maintaining the pressure for 3 min, and then placing it in a tubular furnace with argon gas for sintering. After sintering, hot extrusion is performed in a conical extrusion mold to obtain an aluminum-based composite material block with a multi-level heterogeneous structure; the sintering process parameters are: heating rate 10 K / min, temperature 863 K, and holding time 1 h; the hot extrusion process parameters are: temperature 843 K, holding time 40 min, pressure 750 MPa, and extrusion ratio 16:1.
[0050] (3) The aluminum-based composite material block with a multi-level heterogeneous structure obtained in step (2) is solution treated at 793 K for 4 hours and water quenched, then aged at 408 K for 24 hours and air-cooled to obtain an aluminum-based composite material with a multi-level heterogeneous structure.
[0051] Comparative Example 1
[0052] (1) 18.2 g aluminum powder, 0.8 g magnesium powder and 0.2 g stearic acid were placed in a 250 mL ball mill, and the first ball milling treatment was performed under argon protection, and the ball milling parameters were: ball-to-material ratio of 15:1, ball milling speed of 500 rpm / min, and ball milling time of 8 h to obtain un-cold-welded alloy particles; then 1.0 g copper oxide powder was added to the un-cold-welded alloy particles, and the second ball milling treatment was performed, and the ball milling parameters were: ball-to-material ratio of 15:1, ball milling speed of 500 rpm / min, and ball milling time of 6 h to obtain composite powder;
[0053] Steps (2)-(3) are the same as in Example 1.
[0054] Comparative Example 2
[0055] (1) 18.4 g aluminum powder, 0.8 g magnesium powder and 0.11 g stearic acid were placed in a 250 mL ball mill, and the first ball milling treatment was performed under argon protection. The ball milling parameters were as follows: the ball-to-material ratio was 15:1, the ball milling speed was 500 rpm / min, and the ball milling time was 8 h to obtain cold welding alloy particles; then 0.8 g copper powder was added to the above cold welding alloy particles, and the second ball milling treatment was performed. The ball milling parameters were as follows: the ball-to-material ratio was 15:1, the ball milling speed was 500 rpm / min, and the ball milling time was 6 h to obtain a composite powder.
[0056] Steps (2)-(3) are the same as in Example 1.
[0057] Figure 2 Figure 1 is a morphology diagram of the cold-welded alloy particles (a) in step (1) of Example 1 and the uncold-welded alloy particles (b) in step (1) of Comparative Example 1. Figure 2 It can be seen that the cold welded alloy particles are welded together in blocks due to the mechanical alloying during the ball milling process.
[0058] Figure 3 EBSD images of the aluminum-based composite materials prepared in Example 1 and Comparative Example 1, wherein (a) is Comparative Example 1 and (b) is Example 1. Figure 3 It can be seen that the aluminum-based composite material prepared in Example 1 has a multi-level heterogeneous structure of fine grains embedded in coarse grains, while the aluminum-based composite material prepared in Comparative Example 1 has a uniform structure.
[0059] The aluminum-based composite materials prepared in Example 1 and Comparative Examples 1-2 were wire cut to be processed into standard tensile specimens, and the tensile properties were tested in a universal tensile testing machine, wherein the tensile rate was 0.5 mm / min. The test results are shown in FIG. Figure 4 .
[0060] Figure 4 The engineering stress-strain curves of the aluminum-based composite materials prepared in Example 1 and Comparative Examples 1-2 are shown.
[0061] Among them, the multi-level heterogeneous structure is Example 1, the uniform structure is Comparative Example 1, and the alloy is Comparative Example 2. Figure 4 It can be seen that the aluminum-based composite material with a multi-level heterogeneous structure prepared by the present invention has an excellent strength-plasticity-toughness matching relationship and has excellent work hardening ability.
[0062] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.
Claims
1. A method for preparing an aluminum-based composite material having a multi-level heterogeneous structure, It is characterized in that The following steps are involved: (1) mixing aluminum powder, magnesium powder and stearic acid and subjecting the mixture to a first ball milling process under a protective atmosphere to obtain cold welding alloy particles; mixing the cold welding alloy particles with copper oxide powder and subjecting the mixture to a second ball milling process to obtain a composite powder; (2) The composite powder obtained in step (1) is sequentially subjected to cold pressing, sintering, hot extrusion, solution treatment and aging treatment to obtain an aluminum-based composite material with a multi-level heterogeneous structure.
2. The method for preparing the aluminum-based composite material having a multi-level heterogeneous structure according to claim 1, It is characterized in that In step (1), the mass ratio of the aluminum powder, magnesium powder, copper oxide powder and stearic acid is (18.2-18.4):0.8:(0.8-1):(0.1-0.15).
3. The method for preparing the aluminum-based composite material having a multi-level heterogeneous structure according to claim 1, It is characterized in that In step (1), the ball milling parameters of the first ball milling treatment and the second ball milling treatment are independently: ball-to-material ratio is (10:1) to (15:1), rotation speed is 500 rpm / min, and time is 6 to 8 hours.
4. The method for preparing the aluminum-based composite material having a multi-level heterogeneous structure according to claim 1, It is characterized in that In step (2), the cold pressing pressure is 600 MPa and the holding time is 3 min.
5. The method for preparing the aluminum-based composite material having a multi-level heterogeneous structure according to claim 1, It is characterized in that In step (2), the sintering heating rate is 10K / min, the temperature is 863K, and the holding time is 1 to 2h.
6. The method for preparing the aluminum-based composite material having a multi-level heterogeneous structure according to claim 1, It is characterized in that In step (2), the hot extrusion temperature is 843K, the holding time is 40min, the pressure is 750MPa, and the extrusion ratio is 16:
1.
7. The method for preparing the aluminum-based composite material having a multi-level heterogeneous structure according to claim 1, It is characterized in that In step (2), the temperature of the solution treatment is 793K, the holding time is 4h, and the cooling method is water quenching.
8. The method for preparing the aluminum-based composite material having a multi-level heterogeneous structure according to claim 1, It is characterized in that In step (2), the aging treatment is carried out at a temperature of 408 K and for a time of 24 h.
9. An aluminum-based composite material with a multi-level heterogeneous structure prepared by the preparation method according to any one of claims 1 to 8.
Citation Information
Patent Citations
Powder metallurgy preparation method for nano-particle reinforced ultra-fine grain metal-matrix composite
CN106312057A
Preparation method for in-situ generation of MgO dispersion strengthened ultra-fine grain Al-Mg alloy
CN108359823A
Preparation method for nano CuAl2 / Al2O3 reinforced aluminum matrix composite material by in-situ synthesis
CN109082568A
Preparation method for nanometer magnesium oxide (MgO) aluminum alloy matrix composite by means of in-situ synthesis
CN110541083A
Nanoparticle reinforced aluminum alloy and preparation method thereof
CN115961184A
Cited By
Solute cluster reinforced aluminum alloy material as well as preparation method and application thereof
CN122105205A