Precious metal dispersion strengthening process and application product thereof

By adding Y2O3, ZrO2, Sc and B4C powders to the precious metal matrix for dispersion strengthening process, uniformly distributed dispersed phase particles are formed, which solves the problems of improving the mechanical properties and maintaining characteristics of precious metals in the existing technology, and achieves efficient mechanical properties improvement and large-scale applications.

CN118957350APending Publication Date: 2024-11-15XIANYANG OUYE TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411040241.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

While improving the mechanical properties of the existing precious metal strengthening methods, it is difficult to maintain their original excellent characteristics, such as electrical conductivity and thermal conductivity, and process parameters and equipment conditions limit large-scale promotion and application.

Method used

By using the precious metal dispersion strengthening process, by adding Y2O3, ZrO2, Sc and B4C powders to the precious metal matrix for heating, stirring, pouring, deformation treatment and annealing, uniformly distributed dispersed phase particles are formed, hindering the movement of dislocations, thereby increasing the intensity. and hardness while maintaining conductivity.

Benefits of technology

It significantly improves the tensile strength and elongation of precious metals, maintains conductivity, improves the long-lasting strength of high temperatures, and reduces manufacturing costs, making it suitable for large-scale promotion and application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004972194860000051
    Figure BDA0004972194860000051
  • Figure BDA0004972194860000071
    Figure BDA0004972194860000071
  • Figure BDA0004972194860000081
    Figure BDA0004972194860000081
Patent Text Reader

Abstract

The invention relates to a precious metal dispersion strengthening process and an application product thereof in the field of precious metal strengthening processes, and the precious metal dispersion strengthening process comprises the following steps: weighing preparation materials which comprise the following components in percentage by mass: 0.1-0.3% of Y2O3, 0.05-0.08% of ZrO2, 0.05-0.1% of Sc, 0.08-0.12% of B4C and the balance of matrix precious metal; the Y2O3, the ZrO2, the Sc and the B4C are all powdery, and the particle sizes of the Y2O3, the ZrO2, the Sc and the B4C are all 2-4 microns; heating and smelting the matrix noble metal with the content to obtain noble metal liquid; y2O3, ZrO2, Sc and B4C with the content are added into the precious metal liquid, inert gas is introduced for stirring, alloy liquid is obtained, casting and deformation treatment are performed, annealing treatment is performed, and the dispersion-strengthened precious metal-based material is obtained. The original excellent characteristics of precious metal can be kept, and meanwhile the mechanical property of the precious metal is effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of precious metal strengthening technology, and in particular to a precious metal dispersion strengthening technology and its application products. Background Art

[0002] In the field of metal material processing and treatment, precious metals have always attracted wide attention due to their unique physical and chemical properties, such as high electrical conductivity, high thermal conductivity, excellent corrosion resistance, etc. These properties make precious metals have wide application value in many fields.

[0003] However, the strength, hardness and creep resistance of precious metals are relatively low, which to some extent limits their application in extreme environments such as high load and high precision. In order to improve the mechanical properties of precious metals and meet the growing demand for high performance, technicians in this field have conducted a lot of research and exploration.

[0004] At present, the known methods for strengthening precious metals mainly include alloying, heat treatment, deformation strengthening, etc. Alloying is to add other metal elements to precious metals to form solid solutions or intermetallic compounds, thereby improving their strength and hardness. Heat treatment is to change the internal structure of precious metals by controlling the heating and cooling process of precious metals to achieve the purpose of strengthening. Deformation strengthening is to produce work hardening phenomenon by plastic deformation of precious metals, such as rolling, stretching, compression, etc., so as to improve strength and hardness.

[0005] Although the above methods have improved the mechanical properties of precious metals to a certain extent, there are still some shortcomings. For example, the alloying method may change the original properties of precious metals, such as electrical conductivity and thermal conductivity; the heat treatment and deformation strengthening methods may be limited by factors such as process parameters and equipment conditions, making it difficult to achieve large-scale promotion and application. Therefore, how to effectively improve the mechanical properties of precious metals while maintaining their original excellent properties and reducing manufacturing costs to facilitate large-scale promotion and application is still a technical problem that needs to be solved urgently by those skilled in the art. Summary of the invention

[0006] In order to maintain the original excellent properties of precious metals while effectively improving their mechanical properties, the present application provides a precious metal dispersion strengthening process and its application products.

[0007] In the first aspect, the present application provides a precious metal dispersion strengthening process using the following technical solutions: A precious metal dispersion strengthening process comprises the following steps: Weigh the preparation material, which includes the following components and their mass percentages: 0.1-0.3% Y2O3, 0.05-0.08% ZrO2, 0.05-0.1% Sc and 0.08-0.12% B4C, and the balance is matrix precious metals; the Y2O3, ZrO2, Sc and B4C are all in powder form, and the particle sizes of the Y2O3, ZrO2, Sc and B4C are all 2-4μm; the matrix precious metals with the above contents are heated and smelted to obtain precious metal liquid; then the Y2O3, ZrO2, Sc and B4C with the above contents are added to the precious metal liquid, an inert gas is introduced for stirring to obtain an alloy liquid, the alloy liquid is cast, a deformation treatment is performed, and then an annealing treatment is performed to obtain a dispersion-strengthened precious metal-based material.

[0008] By adopting the above technical solution, the second phase particles dissolved in the precious metal matrix will cause the precious metal matrix to be distorted, and this distortion will have a long effect on the dislocation stress, that is, there is interaction energy between the second phase particles and the dislocation. Y2O3, ZrO2, Sc and B4C in the above particle size range are added to the matrix precious metal, and then through deformation treatment, a dispersed phase particle (second phase particle) with uniform structural distribution is formed at the grain boundary of the material. The dispersed phase particles can hinder the movement of dislocations in the matrix precious metal, so that the dislocation density of the matrix precious metal increases, thereby greatly improving the strength and hardness; at the same time, the dispersed phase particles at the grain boundary of the material can hinder the growth of the material grains, and due to the stable grain structure, it has a higher high-temperature endurance strength. In addition, the compounding of the above content of Y2O3, ZrO2 and Sc as a dispersed phase can significantly improve the tensile strength of the precious metal while maintaining a good elongation, so as to further improve the mechanical properties of the dispersion-strengthened precious metal-based material. Moreover, although the dispersed phase formed above will slightly reduce the conductivity of the dispersion-strengthened precious metal-based material, the degree of decrease is still significantly smaller than that of the existing strengthened precious metals, that is, while improving the mechanical properties of the precious metals, the original excellent properties of the precious metals are maintained.

[0009] Optionally, the deformation treatment includes the following steps: subjecting the flat ingot obtained by casting to a first homogenization treatment, then blanking the flat ingot, and cold rolling the flat ingot into a first thin strip; subjecting the first thin strip to a second homogenization treatment, and then cold rolling the flat ingot to obtain a second thin strip.

[0010] By adopting the above technical scheme, through the first homogenization treatment, the second homogenization treatment and other deformation treatments, the dispersed phase particles can be more evenly distributed between the grains and on the grain boundaries of the matrix precious metal, so that the dispersed phase particles can more comprehensively hinder the movement of dislocations in various parts of the material, thereby improving the overall strength of the dispersion-strengthened precious metal-based material.

[0011] Optionally, the thickness of the first thin strip is 0.4-0.5 mm, and the thickness of the second thin strip is 0.05-0.08 mm.

[0012] By adopting the above technical solution, the materials after the first homogenization treatment and the second homogenization treatment are cold rolled into the first thin strip and the second thin strip of the above thickness respectively, which can make the dispersed phase particles evenly distributed in the matrix precious metal and plastically deform the material, thereby causing work hardening, thereby improving the strength and hardness.

[0013] Optionally, the treatment temperature of the first homogenization treatment is 740-760° C., and the treatment time is 1.5-2 h; the treatment temperature of the second homogenization treatment is 700-720° C., and the treatment time is 15-20 min.

[0014] By adopting the above technical solution, the treatment temperature and time of the first homogenization treatment and the second homogenization treatment are controlled within the above range, so that the matrix precious metal can be recrystallized, and the crystal structure formed by the dispersion-strengthened precious metal-based material is more uniform and the grains are smaller. The refined grains and uniform crystal structure can effectively improve the strength, toughness and plasticity of the dispersion-strengthened precious metal-based material.

[0015] Optionally, the deformation treatment is followed by an internal oxidation treatment, wherein the treatment pressure of the internal oxidation treatment is 0.55-0.60 MPa, the treatment temperature is 1450-1500° C., and the treatment time is 25-28 h.

[0016] By adopting the above technical scheme, the first thin strip obtained after the deformation treatment is internally oxidized, so that Sc and boron carbide in the matrix precious metal can undergo a certain degree of internal oxidation during the internal oxidation treatment to obtain a nanoscale, uniformly distributed oxide dispersion phase. The obtained nanoscale oxide dispersion phase and micron-scale oxide dispersion phases such as Y2O3 and ZrO2 cooperate with each other, which can more fully hinder the dislocation of the matrix precious metal, thereby improving the strength and hardness of the matrix precious metal.

[0017] Optionally, the matrix precious metal includes at least one of gold, silver, platinum, rhodium and yttrium.

[0018] Optionally, the matrix precious metal includes silver and platinum in a mass ratio of 1:(0.25-0.30).

[0019] By adopting the above technical solution, by combining silver and platinum according to the above mass ratio to prepare a dispersion-strengthened precious metal-based material, its mechanical properties can be more effectively improved, while the original excellent conductive properties of the precious metal can be better maintained.

[0020] Optionally, the annealing temperature of the annealing treatment is 820-830° C., and the annealing time is 20-25 min.

[0021] By adopting the above technical solution, by adjusting the annealing temperature and annealing time to the above range, the residual stress in the dispersion-strengthened precious metal-based material can be more effectively eliminated, and the annealing time and temperature in the above range can better improve the plasticity and toughness of the dispersion-strengthened precious metal-based material without reducing the hardness of the dispersion-strengthened precious metal-based material.

[0022] In the second aspect, the present application provides a dispersion-strengthened precious metal-based material obtained by a precious metal dispersion-strengthening process using the following technical solution: A dispersion-strengthened precious metal-based material obtained by a precious metal dispersion strengthening process, with a density of 19.3-19.6 g / cm 3 , melting point ≥1875℃, resistivity ≤18.6μΩ·cm, tensile strength ≥410N / mm at 20℃ 2 , 20℃ elongation ≥45%, annealing hardness ≥135HV, grain size is 140-150μm.

[0023] In the third aspect, the present application provides an application product made by a precious metal dispersion strengthening process using the following technical solution: Application products made by precious metal dispersion strengthening process include glass fiber drawing leak plates, crucible materials, laboratory high-temperature vessels, biological hospital engineering materials and aerospace and marine engineering materials.

[0024] In summary, the present application includes at least one of the following beneficial technical effects: 1. The second phase particles dissolved into the precious metal matrix will cause the precious metal matrix to be distorted. This distortion will have a long effect on dislocation stress, that is, there is interaction energy between the second phase particles and dislocations. Y2O3, ZrO2, Sc and B4C in the above-mentioned particle size range are added to the precious metal matrix, and then deformed to form dispersed phase particles with uniform structural distribution at the grain boundaries of the material. The dispersed phase particles can hinder the movement of dislocations in the precious metal matrix, increase the dislocation density of the precious metal matrix, and thus greatly improve the strength and hardness; at the same time, the dispersed phase particles at the grain boundaries of the material can hinder the growth of the grains of the material, and due to the stable grain structure, it has a higher high-temperature endurance strength; and, although the dispersed phase formed above will slightly reduce the conductivity of the dispersion-strengthened precious metal-based material, the degree of decrease in conductivity is still significantly smaller than that of the existing strengthened precious metals, that is, while improving the mechanical properties of the precious metals, the original excellent properties of the precious metals are maintained. 2. Compounding the above-mentioned contents of Y2O3, ZrO2 and Sc as a dispersed phase can significantly improve the tensile strength of the precious metal while maintaining a good elongation, thereby further improving the mechanical properties of the dispersion-strengthened precious metal-based materials; 3. Through deformation treatments such as the first homogenization treatment and the second homogenization treatment, the dispersed phase particles can be more evenly distributed between the grains and on the grain boundaries of the matrix precious metal, so that the dispersed phase particles can more comprehensively hinder the movement of dislocations in various parts of the material, thereby improving the overall strength of the dispersion-strengthened precious metal-based materials. DETAILED DESCRIPTION

[0025] The embodiments of the present invention will be described in detail below in conjunction with examples. However, those skilled in the art will understand that the following examples are only used to illustrate the present invention and should not be construed as limiting the scope of the present invention. The specific conditions not specified in the examples are carried out according to conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used without indicating the manufacturer are all conventional products that can be purchased commercially.

[0026] 1. Implementation Embodiment 1: A precious metal dispersion strengthening process comprises the following steps: Weigh the preparation material, which includes the following components and their mass percentages: 0.1% Y2O3, 0.05% ZrO2, 0.05% Sc and 0.08% B4C, the balance is matrix precious metals; Y2O3, ZrO2, Sc and B4C are all in powder form, the particle size of Y2O3, ZrO2, Sc and B4C powders is 3μm, and the purity of Y2O3, ZrO2, Sc and B4C is more than 99.7%; The matrix precious metal includes at least one of gold, silver, platinum, rhodium and yttrium, and the present application preferably uses silver and platinum in a mass ratio of 1:0.28; The above-mentioned contents of silver and platinum are added into a vacuum medium frequency furnace under the condition of vacuum degree ≤2.0kPa for heating and smelting to obtain precious metal liquid, and then the above-mentioned contents of Y2O3, ZrO2, Sc and B4C are added into the precious metal liquid to obtain alloy liquid, and nitrogen is introduced for stirring to obtain alloy liquid; casting is carried out under nitrogen protection to obtain a platinum-silver alloy ingot containing a dispersed phase, and then the platinum-silver alloy ingot is deformed.

[0027] The deformation treatment includes the following steps: subjecting the platinum-silver alloy flat ingot to a first homogenization treatment at a treatment temperature of 750°C and a treatment time of 1.7 hours; after the treatment is completed, the ingot is opened and then cold-rolled into a first thin strip with a thickness of 0.45 mm; the first thin strip is subjected to a second homogenization treatment at a treatment temperature of 710°C and a treatment time of 18 minutes; after the treatment is completed, the ingot is cold-rolled into a second thin strip with a thickness of 0.06 mm.

[0028] The second thin strip was subjected to internal oxidation treatment, and the treatment pressure of the internal oxidation treatment was 0.58 MPa, the treatment temperature was 1480° C., and the treatment time was 27 h.

[0029] After the internal oxidation treatment is completed, the second thin strip is subjected to annealing treatment, the annealing temperature of the annealing treatment is 825° C., and the annealing time is 22 minutes. After the annealing is completed, a dispersion-strengthened precious metal-based material is obtained.

[0030] Embodiment 2-3: A precious metal dispersion strengthening process, the differences from Example 1 are shown in Table 1.

[0031] Table 1: Embodiment 4: A precious metal dispersion strengthening process, which is different from Example 2 in that the mass ratio of silver to platinum in the matrix precious metal is 1:0.25.

[0032] Embodiment 5: A precious metal dispersion strengthening process, which is different from Example 2 in that the mass ratio of silver to platinum in the matrix precious metal is 1:0.30.

[0033] Embodiment 6: A precious metal dispersion strengthening process, which is different from Example 2 in that the base precious metal is silver.

[0034] Embodiment 7: A precious metal dispersion strengthening process, which is different from Example 2 in that the base precious metal is platinum.

[0035] Embodiment 8: A precious metal dispersion strengthening process, which is different from Example 2 in that the particle size of Y2O3, ZrO2, Sc and B4C is 2μm.

[0036] Embodiment 9: A precious metal dispersion strengthening process, which is different from Example 2 in that the particle size of Y2O3, ZrO2, Sc and B4C is 4 μm.

[0037] Embodiment 10: A precious metal dispersion strengthening process, which is different from Example 2 in that: the thickness of the first thin strip is 0.4 mm.

[0038] Embodiment 11: A precious metal dispersion strengthening process, which is different from Example 2 in that: the thickness of the first thin strip is 0.5 mm.

[0039] Embodiment 12: A precious metal dispersion strengthening process, which is different from Example 2 in that: the thickness of the second thin strip is 0.05 mm.

[0040] Embodiment 13: A precious metal dispersion strengthening process, which is different from Example 2 in that: the thickness of the second thin strip is 0.08 mm.

[0041] Embodiment 14: A precious metal dispersion strengthening process, which is different from Example 2 in that the treatment temperature of the first homogenization treatment is 740° C. and the treatment time is 1.5 h.

[0042] Embodiment 15: A precious metal dispersion strengthening process, which is different from Example 2 in that the treatment temperature of the first homogenization treatment is 760° C. and the treatment time is 2 hours.

[0043] Embodiment 16: A precious metal dispersion strengthening process, which is different from Example 2 in that the treatment temperature of the second homogenization treatment is 700° C. and the treatment time is 15 minutes.

[0044] Embodiment 17: A precious metal dispersion strengthening process, which is different from Example 2 in that the treatment temperature of the second homogenization treatment is 720° C. and the treatment time is 20 min.

[0045] Embodiment 18: A precious metal dispersion strengthening process, which is different from Example 2 in that the treatment pressure of the internal oxidation treatment is 0.55 MPa, the treatment temperature is 1450° C., and the treatment time is 25 h.

[0046] Embodiment 19: A precious metal dispersion strengthening process, which is different from Example 2 in that the treatment pressure of the internal oxidation treatment is 0.60 MPa, the treatment temperature is 1500° C., and the treatment time is 28 hours.

[0047] Embodiment 20: A precious metal dispersion strengthening process, which is different from Example 2 in that the annealing temperature of the annealing treatment is 820° C. and the annealing time is 20 min.

[0048] Embodiment 22: A precious metal dispersion strengthening process, which is different from Example 2 in that the annealing temperature of the annealing treatment is 830° C. and the annealing time is 25 min.

[0049] 2. Comparison Comparative Example 1: The difference from Example 2 is that ZrO2 is replaced by Y2O3 in equal amounts.

[0050] Comparative Example 2: The difference from Example 2 is that Sc is replaced by Y2O3 in equal amounts.

[0051] Comparative Example 3: The difference from Example 2 is that B4C is replaced by Y2O3 in equal amounts.

[0052] Comparative Example 4: Difference from Example 2: The particle size of Y2O3, ZrO2, Sc and B4C is 6 μm.

[0053] 3. Performance test 1) The resistivity of the dispersion-strengthened precious metal-based materials obtained in Examples 1-22 and Comparative Examples 1-4 was measured using a SW-200 resistivity tester. The measurement results are shown in Table 2.

[0054] 2) The 20°C tensile strength and 20°C elongation of the dispersion-strengthened precious metal-based materials obtained in Examples 1-22 and Comparative Examples 1-4 were measured using an FPZ2100 electronic tensile testing machine. The measurement results are shown in Table 2.

[0055] 3) The annealing hardness of the dispersion-strengthened precious metal-based materials obtained in Examples 1-22 and Comparative Examples 1-4 was measured using an M-type Vickers hardness tester. The measurement results are shown in Table 2.

[0056] 4) With reference to the document “Dispersion Strengthened Pt25Au—A New Crucible Vessel Material”, the sustained fracture life of the dispersion strengthened precious metal-based materials obtained in Examples 1-22 and Comparative Examples 1-4 at 1300°C and 5MPa stress was measured. The measurement results are shown in Table 2.

[0057] Table 2: 4. Results Analysis and Summary Combining Examples 1-3 and Table 2, it can be seen that the contents of each component of the prepared materials of Examples 1-3 are all different. It can be seen from Table 2 that the resistivity of the dispersion-strengthened precious metal-based materials prepared in Examples 1-3 is all ≤18.6μΩ·cm, the tensile strength is all ≥410N / mm2, the elongation is all ≥45%, the annealing hardness is ≥135HV, and the sustained fracture life is all ≥32h. The resistivity, tensile strength, elongation, annealing hardness and sustained fracture life of the dispersion-strengthened precious metal-based materials prepared in Example 2 are all better than those in Example 1 and Example 3.

[0058] And combined with Comparative Examples 1-3, it can be seen that in Comparative Example 1, ZrO2 is replaced by Y2O3 in equal amounts, in Comparative Example 2, Sc is replaced by Y2O3 in equal amounts, and in Comparative Example 3, B4C is replaced by Y2O3 in equal amounts. As can be seen from Table 2, the resistivity, tensile strength, elongation, annealing hardness, and endurance fracture life of the dispersion-strengthened precious metal-based materials obtained in Comparative Examples 1-3 are significantly inferior to those in Example 2.

[0059] From the above, it can be concluded that compounding Y2O3, ZrO2, Sc, B4C and the matrix precious metal according to the contents of Example 2 can significantly improve the conductivity, strength, toughness, hardness and high temperature resistance of the dispersion-strengthened precious metal-based materials.

[0060] Combining Example 2, Examples 4-7 and Table 2, it can be seen that the mass ratio of silver and platinum in the base precious metal of Example 4-5 is different from that of Example 2, while Examples 6-7 use silver and platinum as base precious metals respectively. From Table 2, it can be seen that the resistivity of the dispersion-strengthened precious metal-based materials obtained in Examples 4-7 is ≤18.6μΩ·cm, the tensile strength is ≥410N / mm2, the elongation is ≥45%, the annealing hardness is ≥135HV, and the lasting fracture life is ≥32h. However, it can be seen that the resistivity, tensile strength, elongation, annealing hardness and lasting fracture life of Examples 4-5 are better than those of Examples 6-7.

[0061] Combining Example 2, Examples 8-9 and Table 2, it can be seen that the particle sizes of Y2O3, ZrO2, Sc and B4C in Examples 8-9 are different from those in Example 2. From Table 2, it can be seen that the resistivity of the dispersion-strengthened precious metal-based materials obtained in Examples 8-9 is ≤18.6μΩ·cm, the tensile strength is ≥410N / mm2, the elongation is ≥45%, the annealing hardness is ≥135HV, and the sustained fracture life is ≥32h. And combined with Comparative Example 4, the particle sizes of Y2O3, ZrO2, Sc and B4C in Comparative Example 4 are 6μm. From Table 2, it can be seen that the resistivity, tensile strength, elongation, annealing hardness and sustained fracture life of the dispersion-strengthened precious metal-based materials obtained in Comparative Example 4 are significantly inferior to those in Example 2.

[0062] It can be concluded from the above that the particle sizes of Y2O3, ZrO2, Sc and B4C are within the scope of this application, and the obtained dispersion-strengthened precious metal-based material has good conductivity, strength, toughness, hardness and high temperature resistance.

[0063] Combining Example 2, Examples 10-13 and Table 2, it can be seen that the thickness of the first thin strip in Examples 10-11 is different from that in Example 2, and the thickness of the second thin strip in Examples 12-13 is different from that in Example 2. As can be seen from Table 2, the resistivity of the dispersion-strengthened precious metal-based materials prepared in Examples 10-13 is ≤18.6μΩ·cm, and the tensile strength is ≥410N / mm 2, elongation ≥ 45%, annealing hardness ≥ 135HV, and endurance fracture life ≥ 32h. It can be seen from the above that in the first homogenization treatment and the second homogenization treatment, the thickness of the first thin strip and the second thin strip is controlled within the range of the present application, and the obtained dispersion-strengthened precious metal-based material has good conductivity, strength, toughness, hardness and high temperature resistance.

[0064] Combining Example 2, Examples 14-17 and Table 2, it can be seen that the treatment temperature and time of the first homogenization treatment in Examples 14-15 are different from those in Example 2, and the treatment temperature and time of the second homogenization treatment in Examples 16-17 are different from those in Example 2. As can be seen from Table 2, the resistivity of the dispersion-strengthened precious metal-based materials obtained in Examples 14-17 is ≤18.6μΩ·cm, the tensile strength is ≥410N / mm2, the elongation is ≥45%, the annealing hardness is ≥135HV, and the sustained fracture life is ≥32h. It can be seen from the above that the treatment temperature and time in the first homogenization treatment and the second homogenization treatment are controlled within the scope of this application, and the obtained dispersion-strengthened precious metal-based materials have good conductivity, strength, toughness, hardness and high temperature resistance.

[0065] Combining Example 2, Example 18-19 and Table 2, it can be seen that the treatment pressure, temperature and time of the internal oxidation treatment in Example 18-19 are different from those in Example 2. From Table 2, it can be seen that the resistivity of the dispersion-strengthened precious metal-based materials obtained in Example 18-19 is ≤18.6μΩ·cm, the tensile strength is ≥410N / mm2, the elongation is ≥45%, the annealing hardness is ≥135HV, and the sustained fracture life is ≥32h. It can be obtained from the above that the treatment pressure, temperature and time of the internal oxidation treatment are controlled within the scope of this application, and the conductivity, strength, toughness, hardness and high temperature resistance of the obtained dispersion-strengthened precious metal-based materials are all good.

[0066] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.

Claims

1. A precious metal dispersion strengthening process, characterized in that: The following steps are involved: Weigh the preparation material, which includes the following components and their mass percentages: 1-0.3% Y2O3, 0.05-0.08% ZrO2, 0.05-0.1% Sc and 0.08-0.12% B4C, the balance being matrix precious metals; the Y2O3, ZrO2, Sc and B4C are all in powder form, and the particle sizes of the Y2O3, ZrO2, Sc and B4C are all 2-4 μm; The matrix noble metal with the above content is heated and smelted to obtain noble metal liquid; then the above content of Y2O3, ZrO2, Sc and B4C are added to the noble metal liquid, an inert gas is introduced for stirring to obtain alloy liquid, the alloy liquid is poured, a deformation treatment is performed, and then an annealing treatment is performed to obtain a dispersion-strengthened noble metal-based material.

2. A noble metal dispersion strengthening process according to claim 1, characterized in that: The deformation treatment comprises the following steps: subjecting the flat ingot obtained by casting to a first homogenization treatment, then blanking the flat ingot, and cold rolling the flat ingot into a first thin strip; subjecting the first thin strip to a second homogenization treatment, and then cold rolling the first thin strip to obtain a second thin strip.

3. A noble metal dispersion strengthening process according to claim 5, characterized in that: The thickness of the first thin strip is 0.4-0.5 mm, and the thickness of the second thin strip is 0.05-0.08 mm.

4. A noble metal dispersion strengthening process according to claim 1, characterized in that: The treatment temperature of the first homogenization treatment is 740-760° C., and the treatment time is 1.5-2 hours; the treatment temperature of the second homogenization treatment is 700-720° C., and the treatment time is 15-20 minutes.

5. A noble metal dispersion strengthening process according to claim 1, characterized in that: After the deformation treatment, an internal oxidation treatment is performed, wherein the treatment pressure of the internal oxidation treatment is 0.55-0.60 MPa, the treatment temperature is 1450-1500° C., and the treatment time is 25-28 hours.

6. A noble metal dispersion strengthening process according to claim 1, characterized in that: The matrix precious metal includes at least one of gold, silver, platinum, rhodium and yttrium.

7. A noble metal dispersion strengthening process according to claim 1, characterized in that: The matrix precious metal includes silver and platinum in a mass ratio of 1:(0.25-0.30).

8. A noble metal dispersion strengthening process according to claim 1, characterized in that: The annealing temperature of the annealing treatment is 820-830° C., and the annealing time is 20-25 min.

9. A dispersion-strengthened precious metal-based material obtained by the precious metal dispersion-strengthening process according to any one of claims 1 to 8, characterized in that: Density: 19.3-19.6g / cm 3 , melting point ≥1875℃, resistivity ≤18.6μΩ·cm, tensile strength ≥410N / mm at 20℃ 2 , 20℃ elongation ≥45%, annealing hardness ≥135HV, grain size is 140-150μm.

10. An applied product obtained by using the precious metal dispersion strengthening process according to any one of claims 1 to 8, characterized in that: Including glass fiber drawing leak plates, crucible materials, laboratory high-temperature vessels, biological hospital engineering materials and aerospace and marine engineering materials.