Titanium-based composite material, preparation method thereof and 3D printing method
By introducing nano rare earth oxide particles into titanium alloy and using laser powder bed melting 3D printing technology, the problems of low thermal conductivity and accuracy error during titanium alloy processing are solved, and titanium-based composite materials with high strength and high elongation are realized , improves production efficiency and material performance.
Patent Information
- Application Number
- CN202410871100.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-01
- Publication Date
- 2024-11-15
AI Technical Summary
Titanium alloy has low thermal conductivity during processing, which can easily lead to local temperature rise and work hardening, and has a small elastic modulus, resulting in processing accuracy errors and low production efficiency, limiting its application in the national defense industry.
Introduce nano rare earth oxide particles into titanium alloys and regulate the content of aluminum and rare earth oxides. Laser powder bed melting 3D printing technology is used to form titanium-based composite materials, avoid subsequent heat treatment, and directly obtain high strength and high elongation forming .
It realizes the high yield strength and tensile strength of titanium-based composite materials, combines high elongation of break, meets industrial needs, and improves the performance and production efficiency of materials.
Smart Images

Figure CN118957357A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of metal composite materials, and in particular to a titanium-based composite material and a preparation method and a 3D printing method thereof. Background Art
[0002] Titanium accounts for about 0.6% of the total mass of the earth's crust, second only to aluminum, iron, and magnesium. It is a widely used metal material. The density of titanium alloy is 4.5g / mm 3 (about half of that of high-temperature alloys and steel), and high strength. While meeting the material design strength requirements, it greatly reduces the weight of the material and achieves good economic and environmental benefits. Therefore, it is widely used in industrial fields such as aviation, aerospace, military industry, and biomedicine. Titanium alloys represented by Ti-6Al-4V have the advantages of low density, high specific strength (about 3.5 times that of stainless steel), excellent corrosion resistance (about 15 times that of ordinary stainless steel), wide service temperature range (-196℃~600℃), and good biocompatibility.
[0003] However, titanium alloy has low thermal conductivity, which can easily cause local temperature rise during turning, resulting in sticking of the tool and local hardening of the material, making machining difficult and reducing tool durability. In addition, titanium alloy has a small elastic modulus, about half that of iron, and there is a certain amount of deformation and springback during machining, which can easily cause machining accuracy errors. In the actual production process, the production efficiency and material utilization rate of titanium alloy are both low, and the processing cycle is long, which seriously restricts the application of titanium alloy in the defense industry and other fields.
[0004] The emergence of 3D printing technology in recent years has eliminated the turning process of titanium alloys. Among them, Laser Powder Bed Fusion (LPBF), a 3D printing technology with great development prospects and application advantages, has provided a new solution for the rapid manufacturing of complex titanium alloy components due to its advantages such as digitalization, integration, near-net forming, high processing freedom, no restrictions on part complexity, and high material utilization. However, compared with traditional forgings and castings, the Ti-6Al-4V alloy formed parts manufactured by LPBF have poor plasticity. Although subsequent heat treatment can improve the elongation of the material, factors such as grain coarsening will inevitably lead to a decrease in strength, and will significantly increase production costs, limiting the application of this material. Summary of the invention
[0005] The purpose of the present application is to provide a titanium-based composite material and a preparation method and a 3D printing method thereof, which can effectively improve the yield strength and tensile strength of the titanium-based composite material while having a higher elongation at break.
[0006] To achieve the above objectives, the first aspect of the present application provides a titanium-based composite material, comprising the following composition in mass percentage: Al 7.0% to 10.5%, V 3.0% to 4.5%, nano rare earth oxide particles 0.06% to 1.0%, and the rest Ti and unavoidable impurities.
[0007] In some embodiments of the first aspect, the titanium-based composite material comprises the following composition in mass percentage: 7.5% to 8.0% Al, 3.5% to 4.0% V, 0.1% to 0.5% nano rare earth oxide particles, and the rest Ti and unavoidable impurities.
[0008] In some embodiments of the first aspect, the titanium-based composite material comprises the following composition in mass percentage: Al 7.9% to 8.0%, V 3.7% to 3.8%, and nano rare earth oxide particles 0.2% to 0.5%; preferably, the mass ratio of the Al to the nano rare earth oxide particles is 8:0.5.
[0009] In some embodiments of the first aspect, the titanium-based composite material includes Ti-Al-V alloy particles and nano rare earth oxide particles; preferably, the particle size of the Ti-Al-V alloy particles is 15 μm to 53 μm, and the particle size of the nano rare earth oxide particles is 10 nm to 100 nm.
[0010] In some embodiments of the first aspect, the nano rare earth oxide particles include at least one of nano Y2O3 particles, nano La2O3 particles, and nano CeO2 particles.
[0011] The second aspect of the present application provides a method for preparing any of the above-mentioned titanium-based composite materials, comprising: preparing Ti-Al-V alloy particles using sponge titanium and vanadium-aluminum master alloy; mechanically blending the Ti-Al-V alloy particles and nano rare earth oxide particles to obtain the titanium-based composite material.
[0012] In some embodiments of the second aspect, the method for preparing Ti-Al-V alloy particles using sponge titanium and vanadium-aluminum intermediate alloy includes: mixing sponge titanium and vanadium-aluminum intermediate alloy according to the element stoichiometric ratio, pressing them into blocks and using them as smelting electrodes for vacuum smelting to obtain Ti-Al-V alloy ingots; forging the Ti-Al-V alloy ingots into powdered rods; cleaning and drying the powdered rods, and then melting and atomizing them to obtain the Ti-Al-V alloy particles.
[0013] In some embodiments of the second aspect, the Ti—Al—V alloy particles and the nano rare earth oxide particles are mechanically blended using a resonant acoustic mixer.
[0014] The third aspect of the present application provides a 3D printing method for titanium-based composite materials, comprising: using any of the titanium-based composite materials described above as a raw material, and using a laser powder bed melting device to perform layer-by-layer melting and deposition to obtain a target printed object.
[0015] In some embodiments of the third aspect, before performing layer-by-layer melting and deposition, the substrate of the laser powder bed melting equipment is preheated to 75°C to 200°C; during the process of layer-by-layer melting and deposition: the power of the laser of the laser powder bed melting equipment is 100W to 200W, and the diameter of the laser beam is 0.05mm to 0.07mm; after the laser scans each layer of raw material, it rotates 60° to 70° and then scans the next layer of raw material, and the scanning speed is 100mm / s to 1500mm / s, and the scanning interval is 0.09mm to 0.15mm; the thickness of each layer of raw material is 30μm to 60μm, and the oxygen content is less than 1300ppm.
[0016] Compared with the prior art, the technical solution of the present application has the following beneficial effects:
[0017] The present application obtains a titanium-based composite material with excellent performance by introducing nano rare earth oxide particles into a titanium alloy and regulating the content of the nano rare earth oxide particles and the aluminum element. When the titanium-based composite material is used for laser powder bed melting printing, a formed part with ultra-high strength and high elongation can be directly obtained without subsequent heat treatment, which can better meet industrial needs. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] The following drawings describe in detail the exemplary embodiments disclosed in this application. The same reference numerals represent similar structures in several views of the drawings. Those skilled in the art will understand that these embodiments are non-limiting, exemplary embodiments, and the drawings are only used for the purpose of illustration and description, and are not intended to limit the scope of this application. Other embodiments may also accomplish the inventive intent in this application. It should be understood that the drawings are not drawn to scale. Among them:
[0019] Figure 1 This is a scanning electron microscope photograph of the Ti-8Al-4V-0.2Y2O3 composite material prepared in Example 1 of the present application;
[0020] Figure 2 A transmission electron microscope photograph of the 3D printing block prepared in Example 1 of the present application;
[0021] Figure 3 The grain orientation distribution diagram of the 3D printing block prepared in Example 1 and Comparative Example 6 of the present application;
[0022] Figure 4The grain width size distribution diagram of the 3D printing block prepared in Example 1 and Comparative Example 6 of the present application;
[0023] Figure 5 The high temperature parent phase grain orientation distribution diagram of the 3D printing block prepared in Example 1 and Comparative Example 6 of the present application;
[0024] Figure 6 This is a test chart of the tensile properties of the 3D printing block materials prepared in Example 1 and Comparative Example 6 of the present application. DETAILED DESCRIPTION
[0025] The following description provides specific application scenarios and requirements of the present application, with the purpose of enabling those skilled in the art to make and use the content in the present application. It will be apparent to those skilled in the art that various local modifications to the disclosed embodiments are apparent, and the general principles defined herein may be applied to other embodiments and applications without departing from the spirit and scope of the present application. Therefore, the present application is not limited to the embodiments shown, but to the widest scope consistent with the claims.
[0026] At present, when LPBF technology is used to process and manufacture Ti-6Al-4V alloy shaped parts, there is a problem of poor plasticity. In order to solve this problem, the inventors of this application tried to introduce boron and carbon elements into titanium alloys in the early exploration. Although it can refine the grains of the alloy to a certain extent and improve the elongation of the alloy, it also brings many new problems, such as insufficient material strength, the yield strength is only 801MPa, and the tensile strength is only 851MPa. After LPBF processing and manufacturing, the material needs to be heat treated at high temperature (600℃~700℃), and the required boron content is high, which increases the cost and is not conducive to industrial production.
[0027] When titanium alloys are processed and manufactured based on LPBF technology, there are problems such as high amount of boron added, difficulty in taking both plasticity and strength into account, and need for heat treatment after processing and manufacturing. The inventors of the present application conducted further exploration and accidentally discovered that when a low content of nano rare earth oxide particles is added and the ratio of each element is within a suitable range, the titanium-based composite material obtained can obtain higher strength and better plasticity after LPBF processing and manufacturing without subsequent heat treatment.
[0028] Specifically, the titanium-based composite material of the present application includes the following compositions in mass percentage: Al (aluminum element) 7.0% to 10.5%, V (vanadium element) 3.0% to 4.5%, nano rare earth oxide particles 0.06% to 1.0%, and the rest Ti (titanium element) and unavoidable impurities.
[0029] In the titanium-based composite material of the present application, Al is a crucial element in the titanium-based composite material, and its mass ratio affects the strength and plasticity of the titanium-based composite material. Al has a relatively high atomic radius, which can significantly increase the lattice distortion, thereby increasing the resistance to dislocation movement, making it difficult to slip, thereby greatly improving the strength of the alloy solid solution. However, when the strength is too high, it will also affect the plasticity of the material.
[0030] In the titanium alloy materials currently commonly used for LPBF, casting and wire feeding additive manufacturing, the mass proportion of Al is usually 6%, and there are also prior arts showing that when the Al content exceeds 7%, due to the large amount of precipitation of Ti3Al phase, the brittleness of the material will increase and the plasticity will decrease significantly. When the mass percentage of Al is 5.5% to 6.5%, the material can obtain better strength and plasticity. For the titanium-based composite material of the present application, when the mass proportion of Al exceeds 7.0%, the titanium-based composite material can have excellent tensile strength and yield strength. At the same time, the inventors of the present application also found that when the mass proportion of Al exceeds 10.5%, it will also lead to a decrease in plasticity. Analyzing the reason, Al still exists in the titanium alloy matrix in the state of solid solution atoms in the titanium alloy material of the present application, so it will not have a significant impact on plasticity. When the mass proportion of Al is too high, it will affect the crystal axis ratio structure, weaken the opening trend of multiple slip systems, and lead to a decrease in plasticity. Therefore, when the mass percentage of Al is 7.0% to 10.5%, the titanium-based composite material of the present application can have both high strength and elongation.
[0031] In some specific embodiments, the mass percentage of Al can be 7.0%, 7.5%, 7.9%, 8.0%, 8.5%, 9.0%, 9.5%, 10.0%, 10.5%, but is not limited to the listed values, and any value within all sub-ranges composed of the above values is acceptable.
[0032] The present application also uses nano rare earth oxide particles with a high melting point as a ceramic phase to strengthen the titanium-based composite material, which is not easy to decompose during the LPBF process, so it still exists in the form of solid particles in the formed part, and will not affect the plasticity of the material. When metal particles with a lower melting point are used, they will be decomposed into metal elements and oxygen elements by heat during the LPBF process and dissolved in the titanium alloy matrix, where the metal elements will be concentrated at the grain boundaries, causing the grain boundaries to crack easily, reducing the ductility of the titanium-based composite material, and the oxygen element, as the most sensitive brittle element in the titanium-based composite material, will cause dislocation plane slip when it is dissolved in the lattice gap, which will reduce the plasticity of the titanium-based composite material.
[0033] At the same time, the nano rare earth oxide particles can also provide distortion, which can form more martensitic grains during the martensitic transformation process, thereby promoting grain refinement, making the grain boundary's blocking effect on dislocation more obvious, and the nano rare earth oxide particles are distributed inside the grains, which can also effectively hinder the movement of dislocations. Since the nano rare earth oxide particles have a high hardness and are not easy to deform, the dislocations are hindered and pinned when they move to the vicinity of the nano rare earth oxide particles, and the dislocation line becomes longer, the radius of curvature increases, and greater stress is required to make the dislocation continue to move, thereby significantly improving the strength of the titanium-based composite material. At the same time, the nano rare earth oxide particles can hinder the advancement of the solidification interface front during the solidification process, refine the high-temperature phase grains, thereby delaying the localization of strain, and helping to maintain the elongation of the material.
[0034] The inventors of the present application have also found that the more mass percentage of the nano rare earth oxide particles, the better. When the mass percentage of the nano rare earth oxide particles is too large, agglomeration is likely to occur, which will lead to a decrease in the elongation of the titanium-based composite material. Preferably, the mass percentage of the nano rare earth oxide particles is 0.06% to 1.0%, such as 0.06%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, but it is not limited to the listed values, and any value within all sub-ranges composed of the above values is acceptable. Further preferably, the mass percentage of the nano rare earth oxide particles does not exceed 0.5%.
[0035] In summary, the present application introduces nano rare earth oxide particles and regulates the content of Al and nano rare earth oxide particles, so that Al and nano rare earth oxide particles can work together and complement each other to jointly change the microstructure of the titanium alloy, regulate the movement behavior of dislocations, and ultimately obtain a titanium-based composite material with high strength and good plasticity.
[0036] In some preferred embodiments, the titanium-based composite material comprises the following compositions in percentage by mass: 7.5% to 8.0% Al, 3.5% to 4.0% V, 0.1% to 0.5% nano rare earth oxide particles, and the remainder being Ti and unavoidable impurities.
[0037] In some preferred embodiments, the titanium-based composite material comprises the following composition by mass percentage: Al 7.9% to 8.0%, V 3.7% to 3.8%, and nano rare earth oxide particles 0.2% to 0.5%. The inventors of the present application have further found that when the mass ratio of Al to nano rare earth oxide particles is 8:0.5, the improvement effect of the tensile strength and yield strength of the material is more significant.
[0038] In some preferred embodiments, the titanium-based composite material includes Ti-Al-V alloy particles and nano rare earth oxide particles. Further preferably, the particle size of the Ti-Al-V alloy particles is 15 μm to 53 μm, and the particle size of the nano rare earth oxide particles is 10 nm to 100 nm. Different from traditional cast titanium alloys, since the martensite grain size of the titanium alloy prepared by LPBF is very small, when the size of the nano rare earth oxide particles is too large, it may cause the nano rare earth oxide particles to be distributed at the grain boundary to form crack sources, which will affect the plasticity of the titanium-based composite material.
[0039] In some preferred embodiments, the nano rare earth oxide particles include at least one of nano Y2O3 particles, nano La2O3 particles, and nano CeO2 particles.
[0040] In some specific embodiments, the unavoidable impurities include Fe≤0.25%, C≤0.08%, N≤0.05%, and H≤0.015%.
[0041] The present application also provides a method for preparing the titanium-based composite material, which may include the following steps:
[0042] S1: Preparation of Ti-Al-V alloy particles using titanium sponge and vanadium-aluminum master alloy;
[0043] S2: Mechanically blending the Ti-Al-V alloy particles and nano rare earth oxide particles to obtain the titanium-based composite material.
[0044] In some preferred embodiments, in step S1, the method for preparing Ti-Al-V alloy particles using titanium sponge and vanadium aluminum master alloy may include the following steps:
[0045] S11: mixing titanium sponge and vanadium aluminum master alloy according to the element stoichiometric ratio, pressing into blocks and then using them as melting electrodes for vacuum melting to obtain Ti-Al-V alloy ingots;
[0046] S12: forging the Ti-Al-V alloy ingot into a powder-making rod;
[0047] S13: After cleaning and drying the powdered rod, the powdered rod is melted and atomized to obtain the Ti—Al—V alloy particles.
[0048] In some preferred embodiments, in step S11, the method for preparing the Ti-Al-V alloy ingot specifically includes:
[0049] S111: Sponge titanium and vanadium aluminum master alloy are mixed according to the element stoichiometric ratio, and then compacted into blocks using a hydraulic press, and then the obtained blocks are welded on a smelting electrode in an argon-protected plasma welding chamber; further preferably, in the vanadium aluminum master alloy, the mass percentage of V is 30% to 70%.
[0050] S112: Under vacuum protection, a vacuum consumable arc furnace is used to melt the smelting electrode obtained in step S111 to obtain a Ti-Al-V alloy ingot; more preferably, the smelting times are at least three times. As an example, when three smeltings are performed, the smelting electrode is first melted as a consumable electrode to obtain a primary ingot, the primary ingot is inverted, and a secondary smelting is performed in a vacuum consumable arc furnace as a consumable electrode to obtain a secondary ingot, the secondary ingot is inverted, and a third smelting is performed in a vacuum consumable arc furnace as a consumable electrode to obtain a finished ingot.
[0051] In some preferred embodiments, in step S12, the Ti-Al-V alloy ingot is free forged in two passes by a forging press, wherein the first pass of free forging produces a larger diameter bar, preferably with a diameter of 120 mm. The second pass of free forging produces a smaller diameter bar, preferably with a diameter of 53 mm. The temperature range during forging can be 800°C to 950°C. After being processed by a lathe or the like, a powder bar is obtained.
[0052] In some preferred embodiments, step S13 specifically includes the following steps:
[0053] S131: After cleaning and drying the powder rod, place it in an atomization powder making device (it can be prepared by electrode induction melting gas atomization powder making equipment, or other technologies such as two-flow atomization, centrifugal atomization, rotating electrode atomization, etc.), and use inert gas for protection. The cleaning and drying process can be specifically: use alcohol as a cleaning medium to clean for 15 minutes to 30 minutes, and then keep it warm at 120°C for 2 hours for drying.
[0054] S132: Under appropriate vacuum conditions and protective gas conditions, the powder-making rod is heated and melted. The heating power can be 20kW to 40kW. The molten metal liquid falls into the atomizer nozzle and flows out of the nozzle continuously. High-pressure gas is introduced into the tightly coupled nozzle. The high-speed airflow impacts the metal liquid, atomizing and breaking the metal liquid into a large number of fine droplets. The metal droplets cool and solidify in the atomization chamber, and form spherical Ti-Al-V alloy particles under the action of surface tension.
[0055] In some preferred embodiments, the gas atomization process conditions are as follows: the working pressure is 35 bar to 45 bar, the feed rate of the powder rod is 40 mm / min to 60 mm / min, and the melting heating power of the powder rod is 20 kW to 40 kW. By adjusting the working pressure, the gas flow rate of the high-speed gas flow can be adjusted.
[0056] In some preferred embodiments, step S13 specifically further includes step S133: the obtained spherical Ti—Al—V alloy particles are further screened, classified and collected to obtain Ti—Al—V alloy powder with a particle size of 15 μm to 53 μm.
[0057] In some preferred embodiments, when performing step S2, a resonant acoustic mixer is used to mechanically blend the Ti-Al-V alloy particles and the nano rare earth oxide particles so that the two are evenly mixed.
[0058] The raw materials of the above preparation method are easy to obtain, the steps are simple and easy to operate, the preparation conditions are simple and easy to achieve, and it is very suitable for industrial production.
[0059] The present application also provides a 3D printing method for titanium-based composite materials, which specifically uses LPBF technology for printing. LPBF technology uses laser powder bed melting equipment, using a laser heat source to melt the powder layer layer by layer according to a preset path, thereby obtaining a near-net-shape component with high density, which can achieve requirements that cannot be achieved by traditional processes such as forging and casting.
[0060] Specifically, the 3D printing method of the titanium-based composite material of the present application uses the above-mentioned titanium-based composite material as a raw material, and adopts a laser powder bed melting device to melt and accumulate layer by layer to obtain a target printed object.
[0061] When LPBF technology is used for printing, laser is used as the heat source. The cooling rate of the metal is much higher than that of casting, which is not conducive to the precipitation of Ti3Al phase. Al still exists in the titanium alloy matrix in the state of solid solution atoms and will not have a significant impact on plasticity. At the same time, the cooling rate of LPBF technology is fast, which can inhibit the agglomeration of nano rare earth oxide particles, thereby eliminating the need for subsequent heat treatment, and obtaining the target printed object with ultra-high tensile strength and yield strength, and being able to maintain a high elongation at break.
[0062] In some specific embodiments, the method of using a laser powder bed melting device for layer-by-layer melting and deposition includes: drying and sieving the titanium-based composite material powder and placing it in a powder feeding cylinder of the laser powder bed melting device; preheating the substrate of the laser powder bed melting device, and in an inert gas protection environment, using a laser to selectively scan and melt the titanium alloy powder bed layer, and after each layer is scanned, the substrate is lowered by one layer thickness, the powder feeding cylinder is raised by one layer thickness, and a scraper is used to reciprocate to perform a new layer of titanium-based composite material powder. During the processing, the laser is controlled to use a cross-scanning method. After each layer is scanned, it is rotated by a certain angle and then scans the next layer. This operation is repeated until all preset slices are completed and a titanium-based composite material block of a target size is obtained by stacking layer by layer, which is the target print object.
[0063] In some preferred embodiments, the substrate of the laser powder bed melting device is preheated to 75°C to 200°C. During the layer-by-layer melting and deposition process: the power of the laser of the laser powder bed melting device is 100W to 200W, and the diameter of the laser beam is 0.05mm to 0.07mm; after scanning each layer of the raw material, the laser rotates 60° to 70° and scans the next layer of the raw material, and the scanning speed is 100mm / s to 1500mm / s, and the scanning interval is 0.09mm to 0.15mm; the thickness of each layer of the raw material is 30μm to 60μm, and the oxygen content is less than 1300ppm.
[0064] The following will be combined with the embodiments of the present application to clearly and completely describe the technical solution of the present application. Unless otherwise specified, the reagents and raw materials used can be purchased through commercial channels. The experimental methods in the following examples that do not specify specific conditions are selected according to conventional methods and conditions, or according to the product specifications.
[0065] Sponge titanium was purchased from Pangang Group Mining Co., Ltd., model MHT90; vanadium-aluminum master alloy was purchased from Sichuan Lande Industrial Co., Ltd., model AlV55; Y2O3 powder, with a particle size of 20 nm, was purchased from MCC New Materials Co., Ltd.; La2O3 powder, with a particle size of 20 nm, was purchased from MCC New Materials Co., Ltd.; CeO2 powder, with a particle size of 20 nm, was purchased from MCC New Materials Co., Ltd.
[0066] Hydraulic press: Huzhou Machine Tool Factory Co., Ltd., model YD013; vacuum melting equipment: ALD Vacuum Technology Co., Ltd., model EIGA; forging press: Qingdao Qingdu Forging Machinery Co., Ltd., model EP400; electrode induction melting gas atomization powder making equipment: AVIC Matt, model EIGA; resonant sound mixer: Hummingbird Resonant Sound, model HAM100; laser powder bed melting equipment: German Trumpf, model TruPrint 1000.
[0067] Example 1
[0068] Titanium-based composites
[0069] This embodiment provides a Ti-8Al-4V-0.2Y2O3 composite material, which includes the following compositions in mass percentage: Al 7.91%, V 3.71%, Y2O3 mass fraction accounting for 0.2wt%, and the rest being Ti and unavoidable impurities.
[0070] Preparation of titanium matrix composites
[0071] (1) Processing of pulverized rods
[0072] First, titanium sponge and vanadium aluminum master alloy are weighed according to the element mass percentage of 8% Al and 4% V, and the vanadium aluminum master alloy and titanium sponge are evenly mixed to form a mixed material. The mixed material is pressed into a long strip-shaped block using a hydraulic press, and then the block is welded on the smelting electrode in a plasma welding chamber protected by low-pressure argon gas to obtain a consumable electrode.
[0073] Next, the consumable electrode is fixed on the vacuum melting equipment, and the vacuum melting equipment is evacuated. After that, the consumable electrode is connected to the negative pole of the power supply, and the water-cooled copper crystallizer is connected to the positive pole of the power supply. After power is turned on, arc discharge is generated between the two poles. The high temperature generated by the arc melts the consumable electrode, and the electrode molten droplets fall into the water-cooled copper crystallizer and solidify, thereby obtaining a primary ingot. The primary ingot that has been flattened is inverted and welded to the melting electrode again. The vacuum melting equipment is repeatedly operated to obtain a secondary ingot. After that, the secondary ingot that has been flattened is inverted and welded to the melting electrode for a third melting to obtain a finished ingot.
[0074] After the finished ingot is cooled to below 200°C, the finished ingot is taken out of the smelting furnace. When the finished ingot is cooled to room temperature, the two ends of the finished ingot are turned flat on a lathe, and the surface of the finished ingot is turned off to obtain a finished ingot that meets the forging requirements.
[0075] The finished ingot is forged twice by a forging press at a forging temperature of 850°C. After the first hot forging, a bar with a diameter of 120 mm is obtained. After the second hot forging, a rod blank with a diameter of 53 mm is obtained. The rod blank completed by the second forging is turned by a lathe to finally obtain a powder-making rod with a diameter of 50 mm.
[0076] (2) Preparation of Ti-Al-V alloy powder
[0077] Use a lathe to turn one end of the powder rod into a conical shape, which is conducive to the convergence of molten droplets when the powder rod is melted. The turned powder rod is ultrasonically cleaned with alcohol as the cleaning medium for 15 minutes. After cleaning, the powder rod is placed in an oven with the oven temperature set to 120°C and kept warm for 2 hours for drying.
[0078] After drying, the powder rods are sent into the high-frequency induction melting furnace of the electrode induction melting gas atomization powder making equipment by the lifting and rotating mechanism of the electrode induction melting gas atomization powder making equipment. The melting furnace of the electrode induction melting gas atomization powder making equipment is evacuated, and high-purity protective inert gas is filled after the evacuation is completed. Start the heating power supply, and the powder rods are melted under the heating action of the annular induction coil in the melting furnace, and the heating power is 30kW. At the same time, the powder rods rotate slowly during the melting process and maintain a certain feed rate to ensure that uninterrupted metal solution can be obtained. The feed rate of the powder rods is 40mm / min.
[0079] The molten beam droplets fall into the tightly coupled nozzle of the atomizer, and the nozzle is connected to the melting furnace and the atomization chamber. At the same time, the nozzle of the electrode induction melting gas atomization powder making equipment is introduced with high-pressure inert gas, and the working pressure is set to 35 bar. The high-speed airflow impacts and breaks the molten metal that continuously flows out of the tightly coupled nozzle, atomizing it into fine metal droplets. The metal droplets fall into the atomization chamber, and the flying droplets are transformed into spherical droplets by the action of surface tension. The spherical droplets are rapidly cooled and solidified into powder in the atomization chamber. The powder is then graded and collected with the help of an airflow classification system, and finally Ti-Al-V alloy powder is obtained. The Ti-Al-V alloy powder produced by the above-mentioned gas atomization process has a high degree of sphericity, and the average particle size of the powder particles is 35.79μm.
[0080] (3) Preparation of Ti-8Al-4V-0.2Y2O3 composite materials
[0081] Weigh 1g of nano Y2O3 powder and 499g of the Ti-Al-V alloy powder prepared above, place them in a glass jar of a resonant acoustic mixer, and place the glass jar in the resonant acoustic mixer. Set it to vibrate for two minutes and then cool for one minute, which is one cycle. Start the machine and perform four cycles to complete the mixing. Take out the uniformly mixed titanium-based composite material and seal it in a vacuum.
[0082] 3D Printing
[0083] First, the Ti-8Al-4V-0.2Y2O3 composite material prepared above was dried, the oven temperature was set to 120°C, the insulation time was 2 hours, and argon was used for protection. After that, it was poured into a sieve with an aperture of 53 μm to obtain a powder that meets the standard of "BD32 / T3599-2019 Powder for Laser Selection of Titanium Alloy Parts". The screened Ti-8Al-4V-0.2Y2O3 composite material was placed in the powder feeding cylinder of the laser powder bed melting equipment.
[0084] Next, install the substrate used by the laser powder bed melting equipment and calibrate the substrate working platform. After the substrate is debugged, close the working chamber door of the laser powder bed melting equipment. Then, turn on the laser powder bed melting equipment, use the laser powder bed melting equipment to preheat the substrate, set the preset temperature to 150°C, and pass high-purity argon gas into the equipment at the same time. Use high-purity argon gas to wash the laser powder bed melting equipment to reduce the oxygen content in the laser powder bed melting equipment to below 500ppm to avoid oxidation of titanium alloy during 3D printing. While introducing argon gas to reduce the oxygen content of the equipment, the import of 3D printing slice data can be carried out at the same time. When the oxygen content meets the equipment requirements and the 3D printing file is imported, pre-powdering can be performed. Pre-powdering can ensure good fusion between the first layer of powder and the substrate.
[0085] After the pre-powder preparation is completed, 3D printing can be carried out. During the 3D printing process, argon gas is always introduced to ensure that the oxygen content of the equipment is always at a normal working level. During the 3D printing process, the parameters of the laser powder bed melting equipment are set as follows: laser power is 170W, scanning speed is 1100mm / s, powder layer thickness is 30μm, spot diameter is 0.06mm, scanning spacing is 0.1mm, and the scanning mode is strip scanning.
[0086] The specific 3D printing process can be described as follows: after the laser heat source completes the scanning of the previous layer of metal powder, the substrate drops a layer thickness (30μm), the powder feeding cylinder rises a layer thickness (30μm), and the scraper movement is used to spread the new powder layer. After the powder is spread, the laser adjusts the angle of the scanning path by rotating 67° relative to the previous layer scanning path, and then starts scanning the next layer, repeating the powder spreading-scanning operation until all preset slices are completed. The metal powder is accumulated layer by layer to finally obtain 80*100*10mm 3 After 3D printing is completed, the 3D printed block and substrate are separated by wire cutting.
[0087] Example 2
[0088] This embodiment provides a Ti-8Al-4V-0.5Y2O3 composite material, including the following composition in mass percentage: Al 7.91%, V 3.71%, Y2O3 0.5wt%, and the rest being Ti and unavoidable impurities.
[0089] The preparation method and 3D printing process of the Ti-8Al-4V-0.5Y2O3 composite material can refer to Example 1.
[0090] Example 3
[0091] This embodiment provides a Ti-8Al-4V-0.2La2O3 composite material, including the following composition in mass percentage: Al 7.91%, V 3.71%, La2O3 0.2wt%, and the rest being Ti and unavoidable impurities.
[0092] The preparation method and 3D printing process of the Ti-8Al-4V-0.2La2O3 composite material can refer to Example 1.
[0093] Example 4
[0094] This embodiment provides a Ti-8Al-4V-0.2CeO2 composite material, including the following composition in mass percentage: Al 7.91%, V 3.71%, CeO2 0.2wt%, and the rest being Ti and unavoidable impurities.
[0095] The preparation method and 3D printing process of the Ti-8Al-4V-0.2CeO2 composite material can refer to Example 1.
[0096] Comparative Example 1
[0097] This comparative example provides a Ti-8Al-4V composite material, which includes the following composition in mass percentage: Al 7.91%, V 3.71%, and the remainder Ti and inevitable impurities.
[0098] The preparation method and 3D printing process of the Ti-8Al-4V composite material can be referred to Example 1.
[0099] Comparative Example 2
[0100] This comparative example provides a Ti-4Al-4V-0.2Y2O3 composite material, which includes the following compositions in percentage by mass: 3.80% Al, 3.75% V, 0.2wt% Y2O3, and the remainder Ti and unavoidable impurities.
[0101] The preparation method and 3D printing process of the Ti-4Al-4V-0.2Y2O3 composite material can refer to Example 1.
[0102] Comparative Example 3
[0103] This comparative example provides a Ti-6Al-4V-0.2Y2O3 composite material, which includes the following compositions in percentage by mass: 5.75% Al, 3.85% V, 0.2wt% Y2O3, and the remainder Ti and unavoidable impurities.
[0104] The Ti-6Al-4V-0.2Y2O3 composite material and 3D printing process can refer to Example 1.
[0105] Comparative Example 4
[0106] This comparative example provides a Ti-8Al-4V-0.05Y2O3 composite material, which includes the following compositions in mass percentage: Al 7.91%, V 3.71%, Y2O3 0.05wt%, and the rest Ti and unavoidable impurities.
[0107] The preparation method and 3D printing process of the Ti-8Al-4V-0.05Y2O3 composite material can refer to Example 1.
[0108] Comparative Example 5
[0109] This comparative example provides a Ti-8Al-4V-1.5Y2O3 composite material, which includes the following compositions in mass percentage: Al 7.91%, V 3.71%, Y2O3 1.5wt%, and the rest Ti and inevitable impurities.
[0110] The preparation method and 3D printing process of the Ti-8Al-4V-1.5Y2O3 composite material can refer to Example 1.
[0111] Comparative Example 6
[0112] This comparative example provides a Ti-6Al-4V alloy powder purchased from Suzhou Beifeng Intelligent Technology Co., Ltd. in Jiangsu Province. The alloy powder number is R56400, and its element composition is Ti Bal, Al 5.50-6.75wt%, V 3.50-4.50wt%, Fe≤0.16wt%, and the powder diameter is 15μm-53μm. The 3D printing process can refer to Example 1.
[0113] Scanning electron microscope test
[0114] The Ti-8Al-4V-0.2Y2O3 composite material powder prepared in Example 1 was subjected to a scanning electron microscope test. The test method was as follows: a small amount of sample powder was adhered to the conductive adhesive, and the conductive adhesive with the sample powder was attached to the sample stage, and then placed in a TESCANGAIA3 scanning electron microscope for observation using a 5kv voltage. The results are shown in FIG. Figure 1 As shown. Figure 1 It can be seen that the sphericity of the Ti-8Al-4V-0.2Y2O3 composite material powder prepared in Example 1 remains intact.
[0115] Transmission electron microscope test
[0116] The 3D printing block prepared in Example 1 was tested by transmission electron microscopy. The test method is as follows: a small amount of sample powder is adhered to the conductive adhesive, and the conductive adhesive with the sample powder is attached to the sample stage, and then placed in a TESCAN GAIA3 scanning electron microscope for observation using a 5kv voltage. The results are as follows: Figure 2 shown.
[0117] Depend on Figure 2 It can be seen that the nano Y2O3 particles are observed as white dots in the high-angle annular dark field scanning transmission mode. It can also be observed in the figure that the martensitic grains of the titanium alloy are arranged in a lath-like manner, which is a typical feature of LPBF titanium alloys. The grain width is about a few hundred nanometers, which is significantly smaller than the grains of traditional cast titanium alloys (tens of microns). The size of the nano Y2O3 particles is tens of nanometers, distributed in the grains, and has a good interface bonding with the matrix. No debonding and cracks are observed, so it will not affect the plasticity of the material.
[0118] Electron Backscatter Diffraction (EBSD)
[0119] The 3D printing blocks prepared in Example 1 and Comparative Example 6 were subjected to an electron backscatter diffraction test, and the test method was as follows: the samples were cut into small blocks of 5 mm*5 mm*3 mm for easy observation, inlaid with conductive resin, and surface ground with 320 mesh, 1000 mesh and 2000 mesh sandpaper respectively, and then polished with 3 μm, 1 μm and 0.02 μm diamond suspension polishing liquid, and finally vibrated polished with 0.02 μm diamond suspension polishing liquid to remove the stress layer to obtain a sample that can be used for EBSD observation, and the EBSD experiment was carried out using a TESCAN GAIA3 scanning electron microscope using a voltage of 20 kV.
[0120] Combination Figure 3 and Figure 4 , (a) is the test diagram of Example 1, and (b) is the test diagram of Comparative Example 6. The average short axis width of the grains in Example 1 is 1.47 μm, which is smaller than that in Comparative Example 6 (1.59 μm). This is because nano Y2O3 particles are introduced into the titanium-based composite material of Example 1, and the nano Y2O3 particles can provide distortion, so that more martensitic grains are formed during the martensitic transformation process, thereby promoting grain refinement. The smaller the short axis width of the grains of the material, the more conducive it is to improving the strength of the material.
[0121] like Figure 5 As shown, (a) is the test diagram of Example 1, and (b) is the test diagram of Comparative Example 6. The nano Y2O3 particles of Example 1 can hinder the advancement of the solidification interface front during the solidification process and refine the high-temperature phase grains. The refined high-temperature phase grains can delay the localization of strain and help maintain the elongation of the material. Therefore, the 3D printing material prepared in Example 1 has the characteristics of ultra-high strength and high elongation. The 3D printing material prepared in Comparative Example 6 has coarse columnar high-temperature phase grains, whose internal orientation distribution is relatively close, and it is difficult to form an effective barrier to dislocations, resulting in a lower strength of the 3D printing material.
[0122] Tensile properties test
[0123] The 3D printing blocks prepared in Examples 1 to 4 and Comparative Examples 1 to 6 were subjected to wire cutting to obtain tensile specimens with a gauge length of 17 mm*3.8 mm*1.5 mm, and tensile performance tests were performed on the tensile specimens. The test method is as follows: the tensile specimens were placed in an MTS E43 tensile machine for a room temperature uniaxial tensile test at a strain rate of 0.5 mm / s. Figure 6 The tensile property test graphs of Example 1 (curve a) and Comparative Example 6 (curve b) are shown, and Table 1 shows the tensile property test results of Examples 1-4 and Comparative Examples 1-6.
[0124] Table 1 Tensile properties test results
[0125]
[0126] Compared with Comparative Examples 1 to 6, the titanium-based composite material of the embodiment of the present application can have both ultra-high strength and good elongation when formed, which is more in line with industrial needs. The main reason is that the reasonable regulation of Al and rare earth oxides causes changes in the microstructure of the alloy, among which the appropriate addition of Al significantly increases the lattice distortion, thereby increasing the resistance to dislocation movement, making it difficult to slip, thereby increasing the strength of the alloy solid solution and improving the material strength. The addition of an appropriate amount of high-melting-point rare earth oxide particles can still exist in the form of particles in the formed parts obtained by LPBF processing, effectively playing a role in refining the high-temperature phase grains and improving the strength of the formed parts without having a significant impact on the plasticity of the material. At the same time, the smaller-sized rare earth oxide particles can have a good interface bonding with the matrix, further weakening the impact on the plasticity of the material.
[0127] The above description of the embodiments is to facilitate those of ordinary skill in the art to understand and apply the present application. It is obvious that those familiar with the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without having to pay creative labor. Therefore, the present application is not limited to the embodiments herein, and improvements and modifications made by those skilled in the art based on the contents disclosed in the present application without departing from the scope and spirit of the present application are within the scope of the present application.
Claims
1. A titanium-based composite material, characterized in that: The invention comprises the following compositions in mass percentage: 7.0% to 10.5% of Al, 3.0% to 4.5% of V, 0.06% to 1.0% of nano rare earth oxide particles, and the rest of Ti and inevitable impurities.
2. The titanium-based composite material according to claim 1, characterized in that: The titanium-based composite material comprises the following components in percentage by mass: 7.5% to 8.0% Al, 3.5% to 4.0% V, 0.1% to 0.5% nano rare earth oxide particles, and the rest being Ti and inevitable impurities.
3. The titanium-based composite material according to claim 1, characterized in that: The titanium-based composite material comprises the following components in percentage by mass: 7.9% to 8.0% Al, 3.7% to 3.8% V, and 0.2% to 0.5% nano rare earth oxide particles; preferably, the mass ratio of the Al to the nano rare earth oxide particles is 8:0.
5.
4. The titanium-based composite material according to claim 1, characterized in that: The titanium-based composite material comprises Ti-Al-V alloy particles and nano rare earth oxide particles; preferably, the particle size of the Ti-Al-V alloy particles is 15 μm to 53 μm, and the particle size of the nano rare earth oxide particles is 10 nm to 100 nm.
5. The titanium-based composite material according to any one of claims 1 to 4, characterized in that: The nano rare earth oxide particles include at least one of nano Y2O3 particles, nano La2O3 particles and nano CeO2 particles.
6. A method for preparing the titanium-based composite material according to any one of claims 1 to 5, characterized in that: include: Ti-Al-V alloy particles are prepared using titanium sponge and vanadium-aluminum master alloy; The Ti-Al-V alloy particles and nano rare earth oxide particles are mechanically blended to obtain the titanium-based composite material.
7. The method for preparing the titanium-based composite material according to claim 6, characterized in that: The method for preparing Ti-Al-V alloy particles by using titanium sponge and vanadium-aluminum master alloy comprises: The titanium sponge and the vanadium-aluminum master alloy are mixed according to the element stoichiometric ratio, pressed into blocks, and then used as a smelting electrode for vacuum smelting to obtain a Ti-Al-V alloy ingot; Forging the Ti-Al-V alloy ingot into a powder-making rod; The powdered rod is cleaned and dried, and then melted and atomized to obtain the Ti-Al-V alloy particles.
8. The method for preparing the titanium-based composite material according to claim 6, characterized in that: The Ti-Al-V alloy particles and the nano rare earth oxide particles are mechanically blended by using a resonant acoustic mixer.
9. A 3D printing method for titanium-based composite materials, characterized in that: include: The titanium-based composite material according to any one of claims 1 to 5 is used as a raw material, and a laser powder bed melting device is used to perform layer-by-layer melting and deposition to obtain a target printed object.
10. The 3D printing method of titanium-based composite material according to claim 9, characterized in that: Before performing layer-by-layer melting and deposition, the substrate of the laser powder bed melting equipment is preheated to 75°C to 200°C; during the process of layer-by-layer melting and deposition: the power of the laser of the laser powder bed melting equipment is 100W to 200W, and the diameter of the laser beam is 0.05mm to 0.07mm; after scanning each layer of raw material, the laser rotates 60° to 70° and then scans the next layer of raw material, and the scanning speed is 100mm / s to 1500mm / s, and the scanning interval is 0.09mm to 0.15mm; the thickness of each layer of raw material is 30μm to 60μm, and the oxygen content is less than 1300ppm.