Preparation method of low-cost nickel-based single-crystal high-temperature alloy thin-wall casting
By adjusting the alloy composition, optimizing the casting process, and designing the feeding structure, the shrinkage porosity problem in high-temperature alloy thin-walled castings was solved, achieving low-cost and high-efficiency casting preparation and improving the mechanical properties and airtightness of the castings.
Patent Information
- Application Number
- CN202411065013.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-15
AI Technical Summary
Existing technologies are insufficient to effectively reduce the tendency of shrinkage porosity in thin-walled high-temperature alloy castings, especially in directional or single-crystal high-temperature alloy castings with high content of high-melting-point refractory elements and complex structures, which leads to a decrease in the mechanical properties and airtightness of the castings.
By adjusting the alloy composition, especially by adding an appropriate amount of carbon, optimizing the casting process and designing the feeding structure, and combining vacuum melting and heat treatment processes, low-cost nickel-based single-crystal high-temperature alloy thin-walled castings can be prepared, improving the fluidity and feeding ability of the molten metal and reducing shrinkage defects.
It achieves efficient removal of shrinkage porosity at the solidification end of high-melting-point refractory element alloys, reduces production costs, improves the mechanical properties and airtightness of castings, and is suitable for mass production.
Smart Images

Figure CN118957362A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of high-temperature alloy investment casting, and in particular relates to a method for preparing a low-cost nickel-based single crystal high-temperature alloy thin-wall casting. Background Art
[0002] Nickel-based superalloys have excellent creep properties, fatigue strength, good corrosion resistance and environmental stability, and are widely used in the manufacture of hot-end components of major power components in the fields of aviation, aerospace, ships, and energy. Nickel-based superalloys mainly rely on solid solution strengthening and γ′ precipitation strengthening to improve their mechanical properties. Since nickel-based superalloys can obtain a large amount of high-cubic γ′ precipitation phase after solid solution treatment and aging treatment, they still have high fatigue strength and tensile strength without forging. At present, they have become the key manufacturing material for parts under extreme service conditions. In recent decades, a large number of high-melting-point refractory elements, such as W, Mo, Ta, etc., have been added to the alloy design. These refractory elements have the characteristics of high density, high melting point, and low diffusion coefficient. While improving the temperature-bearing capacity of the alloy, they also lead to serious macro-segregation and inter-dendritic convection. Another point is that since the high-temperature alloy solidifies in the form of dendrites, the dendrite arms are relatively developed, and it is easy for them to bridge with each other, which easily blocks the shrinkage feeding channels. In the later stage of solidification, the inter-dendritic area cannot obtain effective shrinkage feeding of the molten metal. In addition, the composition of high-temperature alloys is complex, and the solidification order of different elements is quite different, which makes the high-temperature alloy castings have a significantly higher tendency to loosen, which is particularly obvious in high-temperature alloy thin-walled products.
[0003] The shrinkage content during the solidification process of high-temperature alloys is directly related to the alloy composition, solidification window and preparation process parameters. Low-cycle fatigue cracks usually occur at shrinkage sites, and the fatigue crack growth rate of single-crystal high-temperature alloys is also higher at shrinkage sites between dendrites. In addition, any form of shrinkage in the casting will reduce the effective stress-bearing area of the casting, produce stress concentration at the sharp corners of the shrinkage, and significantly reduce the mechanical properties of the casting; shrinkage will also reduce the airtightness and physical and chemical properties of the casting. Therefore, developing a method to reduce the porosity tendency of high-temperature alloy thin-walled castings is crucial to improving the performance of high-temperature alloy castings. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a low-cost method for preparing nickel-based single crystal high-temperature alloy thin-walled castings in view of the deficiencies of the above-mentioned prior art. The method effectively improves the shrinkage that is easily generated in high-temperature alloy castings, and is particularly suitable for directional and single crystal high-temperature alloy castings with a high content of high-melting point refractory elements, complex structures, and variable cross-sections.
[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for preparing a low-cost nickel-based single crystal high-temperature alloy thin-wall casting, the method comprising:
[0006] S1. According to the chemical composition of the alloy, the raw materials are mixed and poured into a master alloy ingot in a vacuum melting furnace;
[0007] The master alloy ingot is composed of the following raw materials in mass fraction: Cr: 7.50-8.50%, Co: 7.50-8.50%, W: 7.50-8.50%, Mo: 1.50-2.50%, Ta: 5.30-6.70%, Al: 5.00-6.00%, Ti: 0.30-0.80%, C: 0.010-0.020%, and the balance is Ni;
[0008] Among them, Cr: has good oxidation resistance and corrosion resistance, it can improve the hardness, wear resistance and heat resistance of the alloy; Co: can improve the processing performance and corrosion resistance of the alloy, and is close to the atomic number of the matrix Ni, with strong solid solubility, which can improve the alloying degree of the alloy and improve the comprehensive mechanical properties of the alloy; W, Mo, Ta: are all high melting point elements with high density, which can improve the high temperature strength, hardness and heat resistance of the alloy; Al: a light element, at high temperature, Al can form a stable oxide film to protect the alloy surface from further oxidation, and Al is the main constituent element of the γ' phase in nickel-based high temperature alloys, and can form Ni3Al intermetallic compounds with Ni to improve the mechanical properties of the alloy; Ti: can improve the strength, toughness and corrosion resistance of the alloy, and improve the processing performance of the alloy. Ni: one of the main elements in high temperature alloys, nickel can maintain good creep resistance and durability at high temperatures, reduce the cold brittleness of the alloy, improve plasticity and weldability, and is often used to manufacture parts that withstand stress at high temperatures.
[0009] Adding a small amount of C element can help promote the formation of CO2 gas oxides during alloy melting, reduce the content of Al2O3 solid oxides, and effectively improve the fluidity of the molten metal in the later stage of solidification, increase the shrinkage compensation capacity, reduce the shrinkage, and improve the mechanical properties of the castings. The addition of C element can reduce the slag content, reduce the viscosity of the alloy liquid, improve the fluidity of the molten metal in the later stage of solidification, and increase the shrinkage compensation capacity. However, considering the characteristics of C element such as high melting point and easy reaction with impurity gas, when adding C element, it can be added according to specific requirements during subsequent remelting and melted together with the alloy ingot.
[0010] S2, pressing the wax material into a wax mold according to the wax pressing parameters, and using a low melting point wax material to make a shrinkage-feeding structure, and assembling the wax mold after it is completely cooled to obtain an assembled wax mold;
[0011] S3, shell preparation: a surface layer, a transition layer and a back layer are sequentially arranged on the wax mold obtained in S2 from the inside to the outside to obtain a shell; the material of the surface layer slurry is a mixture of corundum powder, silica sol and 5% polyvinyl alcohol reinforcing agent; the material of the transition layer slurry and the back layer slurry is a mixture of EC95 fused mullite, silica sol and 5% polyvinyl alcohol reinforcing agent;
[0012] S4, melting the master alloy ingot obtained in S1 in a vacuum melting furnace, pouring it into the shell obtained in S3, and obtaining a casting after cooling;
[0013] S5. Clean and cut the casting obtained in S4, complete one solution treatment and two aging treatments in a vacuum heat treatment furnace, remove the shrinkage-feeding structure, and smooth the surface of the casting to obtain a low-cost nickel-based single crystal high-temperature alloy thin-wall casting.
[0014] Preferably, the preparation method of the master alloy ingot in S1 is: first place C at the bottom of the crucible in the vacuum melting furnace, and then load other main materials into the furnace, the order of other main materials is Co, W, Mo, Ta, Cr, Ni, start to melt the materials when the vacuum degree in the furnace is ≤5Pa, and carry out the first refining at 1490℃~1530℃. After the first refining is completed, turn off the power to cool the molten metal to a condensed film state, then add Al and Ti through the turret, and then carry out low-temperature refining at 1390℃~1430℃, and pour and discharge from the furnace at 1440℃~1480℃.
[0015] Preferably, when preparing the feeding structure in S2, the diameter of the feeding wax droplets at the thin wall is 3-5 mm and the height is 2-3 mm. Feeding wax drops are added according to the requirement that the interval between wax drops is not less than 5 mm, and all the parts where the feeding wax drops contact the thin wall are smoothly transitioned.
[0016] Preferably, the viscosity of the surface layer slurry in S3 is 40s-45s, the viscosity of the transition layer slurry is 30s-35s, and the viscosity of the back layer slurry is 10s-15s.
[0017] Preferably, during pouring in S4, the heating temperature of the upper zone of the vacuum melting furnace is 1480-1520°C; the heating temperature of the lower zone is 1530-1570°C; the pouring temperature is 1530-1570°C; and the crystal pulling rate is 3mm / min-4mm / min.
[0018] Compared with the prior art, the present invention has the following advantages:
[0019] The present invention provides a method for preparing a low-cost nickel-based single crystal high-temperature alloy and a thin-walled casting thereof. The design concept is to remove a large amount of slag existing in the alloy by adjusting the C element content, thereby improving the fluidity of the molten metal and increasing the shrinkage compensation capacity; further, by changing the casting process, the shrinkage depth is reduced; finally, the shallow shrinkage defects generated at the end of solidification are completely removed by the shrinkage compensation structure. The present invention solves the problem that alloys with high contents of high-melting-point refractory elements W, Mo, and Ta are prone to shrinkage at the end of solidification by the synergistic effect of adjusting the alloy composition, designing the shrinkage compensation structure, and changing the melting and casting process. The provided method for preparing a low-cost nickel-based single crystal high-temperature alloy and a thin-walled casting thereof is simple to operate, easy to implement, and highly efficient, which reduces production costs and is suitable for mass production.
[0020] The present invention is further described in detail below with reference to the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 (a) and (b) are respectively the slag of the molten metal without adding C and the slag of the molten metal after adding C in Example 1 of the present invention.
[0022] Figure 2 This is the micro-shrinkage of the casting in Example 1 of the present invention.
[0023] Figure 3 (a), (b), and (c) are the micro-shrinkage conditions of the castings in Comparative Examples 1, 2, and 3 of the present invention, respectively. DETAILED DESCRIPTION
[0024] Example 1
[0025] The method for preparing a low-cost nickel-based single crystal high-temperature alloy thin-wall casting of this embodiment is as follows:
[0026] S1. According to the chemical composition of the alloy, the raw materials are mixed and poured into a master alloy ingot in a vacuum melting furnace;
[0027] The master alloy ingot is composed of the following raw materials in mass fraction: Cr: 8.0%, Co: 8.0%, W: 8.0%, Mo: 1.8%, Ta: 6.2%, Al: 5.5%, Ti: 0.6%, C: 0.018%, and the balance is Ni;
[0028] The alloy has excellent mechanical properties. The yield strength and tensile strength at 800℃ can reach about 940MPa and 1200MPa respectively, while the elongation and shrinkage can be maintained at about 20%; the endurance performance at 1093℃ and 158MPa can still be greater than 60h. It is much higher than the equiaxed and directional columnar crystal high-temperature alloys under the same test conditions. The high-temperature ultimate strength of most equiaxed alloys can only reach about 1000MPa, the elongation is about 5%, the shrinkage is only about 15%, and the high-temperature endurance time is about 50h, such as K465 alloy; the ultimate strength of most directional alloys at high temperature is about 1100MPa, and the high-temperature endurance performance is about 40h, such as DZ125 alloy;
[0029] The preparation method of the master alloy ingot is as follows: after the furnace charge is prepared, the master alloy is smelted. Since the melting point of C element is high, C is first placed at the bottom of the crucible in the vacuum melting furnace, and then other main materials are loaded into the furnace. The order of the other main materials is Co, W, Mo, Ta, Cr, and Ni. When the vacuum degree in the furnace is ≤5Pa, the material is melted. In this embodiment, the vacuum degree after the alloy is melted is 1Pa, the first refining temperature is 1510°C, and the refining time is 10min. After the first refining is completed, the power is turned off and the temperature is lowered to make the metal liquid to a condensed film state. The power outage time is 15min, Al and Ti are added through a turret, and then low-temperature refining at 1410°C is performed for 8min. The pouring temperature is 1460°C, and after the pouring is completed, it needs to be left to stand for 10min before being taken out of the furnace. Figure 1 (a) and (b) are the slag conditions of the molten metal before and after adding C, that is, Figure 1 (a) shows the slag after smelting of the existing master alloy (i.e. without C added). Figure 1 (b) is the slag of the master alloy after adjusting the C content in this embodiment;
[0030] S2, the wax material is pressed into a wax mold according to the wax pressing parameters. After the wax mold is pressed, it needs to be fully cooled, and the cooling time is about 30 minutes. After it is completely cooled, a low melting point wax material (red wax) is used to make a shrinkage-feeding structure. After the wax mold is completely cooled, the wax mold is assembled. When the wax mold is assembled, the casting needs to be completely perpendicular to the chassis to obtain an assembled wax mold;
[0031] When preparing the feeding structure, the diameter of the feeding wax droplet at the thin wall is 5 mm and the height is 2 mm. Feeding wax drops are added according to the requirement that the interval between the wax drops is not less than 5 mm. All the parts where the feeding wax drops contact the thin wall need to have a smooth transition without pits or protrusions.
[0032] S3, shell preparation: the wax mold obtained in S2 is cleaned and blown dry before shell preparation, and a surface layer, a transition layer and a back layer are sequentially arranged on the wax mold from the inside to the outside to obtain a shell; the material of the surface layer slurry is a mixture of 320# corundum powder, silica sol and 5% polyvinyl alcohol reinforcing agent; the material of the transition layer slurry and the back layer slurry is a mixture of 320# EC95 powder (EC95 fused mullite), silica sol and 5% polyvinyl alcohol reinforcing agent; the viscosity of the surface layer slurry is 40s, and the sanding particle size is 100#; the viscosity of the transition layer slurry is 30s, and the sanding particle size is 46#; the viscosity of the back layer slurry is 10s, and the sanding particle size is 24#;
[0033] In this embodiment, sand sprinkling means that after the mold is dipped in slurry, sand is poured onto the mold that has been dipped in slurry to combine the sand with the slurry. This is the process of preparing the mold shell.
[0034] S4, melting the master alloy ingot obtained in S1 in a vacuum melting furnace, pouring it into the shell obtained in S3, and obtaining a casting after cooling;
[0035] The material is cut according to the weight of the casting assembly, and the material weight is 2.7kg. After the material is cut, the surface of the master alloy ingot needs to be polished smooth to remove surface inclusions and oxide scale produced by cutting. When the casting is melted, the specific process parameters are as follows:
[0036] The heating temperature of the upper zone of the vacuum melting furnace is 1500℃; the heating temperature of the lower zone is 1550℃; the vacuum degree is 7Pa when power is supplied; the vacuum degree after the alloy is melted is 0.9Pa; the refining temperature is 1580℃; the refining time is 3min; the pouring temperature is 1550℃; the crystal pulling rate is 3mm / min; and the crystal pulling height is 270mm.
[0037] S5. After the casting is completely cooled, the casting obtained in S4 is cleaned of the mold shell and the pouring and riser are removed. To avoid recrystallization when removing the process subsidy, a solid solution and two aging are completed in a vacuum heat treatment furnace. The total heat treatment time is 58 hours. After completion, a special polishing tool is used to remove the shrinkage structure and the casting surface is smoothed. The removal amount during smoothing is 50μm to 70μm. Finally, the fluorescent defects and shrinkage depth are inspected to obtain a low-cost nickel-based single crystal high-temperature alloy thin-walled casting.
[0038] Figure 2 This is the micro-shrinkage of the casting stored in this embodiment. After fluorescence inspection and observation under an optical microscope, no shrinkage occurs at the end of solidification of the casting, which meets the standard requirements.
[0039] Comparative Example 1
[0040] For further explanation, in this comparative example, no C element is added, and the other parameters are consistent with those in Example 1. Specifically, the furnace charge preparation and the master alloy preparation are performed. The ingredients are prepared according to the chemical composition, in weight percentage, Cr: 8.0%, Co: 8.0%, W: 8.0%, Mo: 1.8%, Ta: 6.2%, Al: 5.5%, Ti: 0.6%,
[0041] After the preparation of the charge is completed, the master alloy is smelted. The order of the main materials is cobalt, tungsten, molybdenum, tantalum, chromium, and nickel. When the vacuum degree and temperature meet the requirements, the chemical process, the first refining, the addition of aluminum and titanium small materials, low-temperature refining, pouring, and unloading are carried out in sequence. The vacuum degree after the alloy is melted is 1Pa; the first refining temperature is 1510℃, and the refining time is 10min; after the first refining, the power is turned off to cool down until the film condenses on the surface of the molten metal, and the power outage time is 15min, and aluminum and titanium are added through the turret; the low-temperature refining temperature is 1410℃, and the refining time is 8min; the pouring temperature is 1460℃, and after pouring, it needs to stand for 10min before unloading.
[0042] The wax mold is pressed according to the given wax pressing parameters. After the wax mold is pressed, it needs to be fully cooled. The cooling time is about 30 minutes. After it is completely cooled, low melting point wax is used to make the shrinkage compensation structure. The diameter of the shrinkage compensation wax droplet at the thin wall is 5mm and the height is 2mm. It is added according to the requirement that the wax droplet interval is not less than 5mm. All the parts where the shrinkage compensation wax droplets contact the thin wall must be smoothly transitioned, and no pits or protrusions should appear. After that, the wax mold is assembled. When the wax mold is assembled, the casting must be completely perpendicular to the chassis.
[0043] The assembled wax mold is cleaned and blown dry before preparing the shell. When preparing the shell, the surface layer uses 320# corundum powder + silica sol, which contains a polymer reinforcing agent. The transition layer and back layer use 320# EC95 powder + silica sol + 5% polyvinyl alcohol reinforcing agent; the surface layer slurry viscosity is 40s, and the sand particle size is 100#; the transition layer slurry viscosity is 30s, and the sand particle size is 46#; the back layer slurry viscosity is 10s, and the sand particle size is 24#.
[0044] The material is cut according to the weight of the casting assembly, and the material weight is 2.7kg. After the material is cut, the surface of the master alloy ingot needs to be polished smooth to remove surface inclusions and oxide scale produced by cutting. When the casting is melted, the specific process parameters are as follows:
[0045] The heating temperature of the upper zone is 1500℃; the heating temperature of the lower zone is 1550℃; the vacuum degree is 7Pa when power is supplied; the vacuum degree after the alloy is melted is 0.9Pa; the refining temperature is 1580℃; the refining time is 3min; the pouring temperature is 1550℃; the pouring speed is 6s; the standing time is 2min; the crystal pulling rate is 3mm / min; the crystal pulling height is 270mm.
[0046] After the casting is completely cooled, the shell is cleaned and the pouring and riser are removed. To avoid recrystallization when removing the process subsidy, it is necessary to first perform a solid solution treatment and two aging treatments in a vacuum high-pressure gas quenching furnace. The total heat treatment time is 58 hours. After completion, a special polishing tool is used to remove the shrinkage structure. After removal, the surface of the casting with the shrinkage structure needs to be smoothed. The removal amount during smoothing is 50μm. Finally, the fluorescent defects and shrinkage depth are inspected.
[0047] After fluorescence inspection and observation under an optical microscope, shrinkage appeared at the end of solidification of the casting, and the shrinkage depth was about 300μm ( Figure 3 a).
[0048] Comparative Example 2
[0049] Compared with Example 1, this comparative example not only does not add C element, but also does not add shrinkage-feeding structure, and the remaining steps and process parameters are consistent with the example.
[0050] After fluorescence inspection and observation under an optical microscope, it was found that the shrinkage was quite serious, and the shrinkage depth at the end of coagulation reached 600μm ( Figure 3 b).
[0051] Comparative Example 3
[0052] Compared with Example 1, this comparative example does not add C element and feeding structure. At the same time, the pouring process does not adopt the preferred process described in the present invention. The specific pouring process is as follows:
[0053] The heating temperature of the upper zone is 1420℃; the heating temperature of the lower zone is 1470℃; the vacuum degree is 7Pa when power is supplied; the vacuum degree after the alloy is melted is 0.9Pa; the refining temperature is 1580℃; the refining time is 3min; the pouring temperature is 1470℃; the pouring speed is 6s; the standing time is 2min; the crystal pulling rate is 5mm / min; the crystal pulling height is 270mm.
[0054] The remaining steps and process parameters remain the same as those in the embodiment.
[0055] After fluorescence inspection and observation under an optical microscope, it was found that the shrinkage was quite serious, and the shrinkage depth at the end of coagulation reached 2500μm ( Figure 3 c), seriously affecting the mechanical properties of castings.
[0056] Example 2
[0057] The method for preparing a low-cost nickel-based single crystal high-temperature alloy thin-wall casting of this embodiment is as follows:
[0058] S1. According to the chemical composition of the alloy, the raw materials are mixed and poured into a master alloy ingot in a vacuum melting furnace;
[0059] The master alloy ingot is composed of the following raw materials by mass fraction: Cr: 7.50%, Co: 8.50%, W: 7.50%, Mo: 1.50%, Ta: 5.30%, Al: 5.00%, Ti: 0.300%, C: 0.020%, and the balance is Ni. The preparation method of the master alloy ingot is as follows: after the furnace charge is prepared, the master alloy is smelted. Since the C element has a high melting point, C is first placed at the bottom of the crucible in the vacuum melting furnace, and then other main materials are loaded into the furnace. The order of other main materials is Co, W, Mo, Ta, Cr, Ni. When the vacuum degree in the furnace is 5Pa, the material is started to be quenched. The first refining temperature is 1490℃ and the refining time is 8min. After the first refining is completed, the power is turned off to cool down the molten metal to a condensed film state. The power outage time is 15min. Al and Ti are added through the turret. Then, low-temperature refining at 1390℃ is carried out for 6min. The pouring temperature is 1440℃. After pouring, it needs to stand for 15min before being taken out of the furnace.
[0060] S2, the wax material is pressed into a wax mold according to the wax pressing parameters. After the wax mold is pressed, it needs to be fully cooled, and the cooling time is about 30 minutes. After it is completely cooled, a low melting point wax material (red wax) is used to make a shrinkage-feeding structure. After the wax mold is completely cooled, the wax mold is assembled. When the wax mold is assembled, the casting needs to be completely perpendicular to the chassis to obtain an assembled wax mold;
[0061] When preparing the feeding structure, the diameter of the feeding wax droplet at the thin wall is 3mm and the height is 3mm. Feeding wax drops are added according to the requirement that the interval between the wax drops is not less than 5mm. All the parts where the feeding wax drops contact the thin wall need to have a smooth transition without pits or protrusions.
[0062] S3, shell preparation: the wax mold obtained in S2 is cleaned and dried before shell preparation, and a surface layer, a transition layer and a back layer are sequentially arranged on the wax mold from the inside to the outside to obtain a shell; the material of the surface layer slurry is a mixture of 320# corundum powder, silica sol and 5% polyvinyl alcohol reinforcing agent; the material of the transition layer slurry and the back layer slurry is a mixture of 320# EC95 powder (EC95 fused mullite), silica sol and 5% polyvinyl alcohol reinforcing agent;
[0063] The viscosity of the surface layer slurry is 45s, and the sand particle size is 100#; the viscosity of the transition layer slurry is 35s, and the sand particle size is 46#; the viscosity of the back layer slurry is 15s, and the sand particle size is 24#;
[0064] S4, melting the master alloy ingot obtained in S1 in a vacuum melting furnace, pouring it into the shell obtained in S3, and obtaining a casting after cooling;
[0065] The material is cut according to the weight of the casting assembly, and the material weight is 2.71kg. After the material is cut, the surface of the master alloy ingot needs to be polished smooth to remove surface inclusions and oxide scale produced by cutting. When the casting is melted, the specific process parameters are as follows:
[0066] The heating temperature of the upper zone of the vacuum melting furnace is 1480℃; the heating temperature of the lower zone is 1530℃; the vacuum degree is 7Pa when power is supplied; the vacuum degree after the alloy is melted is 0.8Pa; the refining temperature is 1580℃; the refining time is 3min; the pouring temperature is 1530℃; the crystal pulling rate is 4mm / min; and the crystal pulling height is 270mm.
[0067] S5. After the casting is completely cooled, the casting obtained in S4 is cleaned of the mold shell and the pouring and riser are removed. To avoid recrystallization when removing the process subsidy, a solid solution and two aging are completed in a vacuum heat treatment furnace. The total heat treatment time is 58 hours. After completion, a special polishing tool is used to remove the shrinkage structure and the casting surface is smoothed. The removal amount during smoothing is 70μm. Finally, the fluorescent defects and shrinkage depth are inspected to obtain a low-cost nickel-based single crystal high-temperature alloy thin-wall casting.
[0068] After fluorescence inspection and observation under an optical microscope, no shrinkage was found at the end of solidification of the casting, which meets the standard requirements.
[0069] Example 3
[0070] The method for preparing a low-cost nickel-based single crystal high-temperature alloy thin-wall casting of this embodiment is as follows:
[0071] S1. According to the chemical composition of the alloy, the raw materials are mixed and poured into a master alloy ingot in a vacuum melting furnace;
[0072] The master alloy ingot is composed of the following raw materials by mass fraction: Cr: 8.50%, Co: 7.50%, W: 8.50%, Mo: 2.50%, Ta: 6.70%, Al: 6.00%, Ti: 0.80%, C: 0.010%, and the balance is Ni; the preparation method of the master alloy ingot is: after the furnace charge is prepared, the master alloy is smelted, and since the C element has a high melting point, C is first placed at the bottom of the crucible in the vacuum melting furnace, and then other main materials are loaded into the furnace, and the master alloy is smelted. The order of the main materials is Co, W, Mo, Ta, Cr, Ni. When the vacuum degree in the furnace is 2Pa, the material is quenched. The first refining temperature is 1530℃ and the refining time is 12min. After the first refining is completed, the power is turned off to cool the metal liquid to a condensed film state. The power outage time is 15min. Al and Ti are added through the turret. Then, low-temperature refining at 1430℃ is carried out for 10min. The pouring temperature is 1480℃. After pouring, it needs to stand for 12min before being taken out of the furnace.
[0073] S2, the wax material is pressed into a wax mold according to the wax pressing parameters. After the wax mold is pressed, it needs to be fully cooled, and the cooling time is about 30 minutes. After it is completely cooled, a low melting point wax material (red wax) is used to make a shrinkage-feeding structure. After the wax mold is completely cooled, the wax mold is assembled. When the wax mold is assembled, the casting needs to be completely perpendicular to the chassis to obtain an assembled wax mold;
[0074] When preparing the feeding structure, the diameter of the feeding wax droplet at the thin wall is 4 mm and the height is 2 mm. Feeding wax drops are added according to the requirement that the interval between the wax drops is not less than 5 mm. All the parts where the feeding wax drops contact the thin wall need to have a smooth transition without pits or protrusions.
[0075] S3, shell preparation: the wax mold obtained in S2 is cleaned and blown dry before shell preparation, and a surface layer, a transition layer and a back layer are sequentially arranged on the wax mold from the inside to the outside to obtain a shell; the material of the surface layer slurry is a mixture of 320# corundum powder, silica sol and 5% polyvinyl alcohol reinforcing agent; the material of the transition layer slurry and the back layer slurry is a mixture of 320# EC95 powder (EC95 fused mullite), silica sol and 5% polyvinyl alcohol reinforcing agent; the viscosity of the surface layer slurry is 40s, and the sanding particle size is 100#; the viscosity of the transition layer slurry is 30s, and the sanding particle size is 46#; the viscosity of the back layer slurry is 10s, and the sanding particle size is 24#;
[0076] S4, melting the master alloy ingot obtained in S1 in a vacuum melting furnace, pouring it into the shell obtained in S3, and obtaining a casting after cooling;
[0077] The material is cut according to the weight of the casting assembly, and the material weight is 2.72kg. After the material is cut, the surface of the master alloy ingot needs to be polished smooth to remove surface inclusions and oxide scale produced by cutting. When the casting is melted, the specific process parameters are as follows:
[0078] The heating temperature of the upper zone of the vacuum melting furnace is 1520℃; the heating temperature of the lower zone is 1570℃; the vacuum degree is 9Pa when power is supplied; the vacuum degree after the alloy is melted is 0.8Pa; the refining temperature is 1580℃; the refining time is 3min; the pouring temperature is 1570℃; the crystal pulling rate is 4mm / min; and the crystal pulling height is 270mm.
[0079] S5. After the casting is completely cooled, the casting obtained in S4 is cleaned of the mold shell and the pouring and riser are removed. To avoid recrystallization when removing the process subsidy, a solid solution and two aging treatments are completed in a vacuum heat treatment furnace. The total heat treatment time is 58 hours. After completion, a special polishing tool is used to remove the shrinkage structure and the casting surface is smoothed. The removal amount during smoothing is 100μm. Finally, the fluorescent defects and shrinkage depth are inspected to obtain a low-cost nickel-based single crystal high-temperature alloy thin-wall casting.
[0080] After fluorescence inspection and observation under an optical microscope, no shrinkage was found at the end of solidification of the casting, which meets the standard requirements.
[0081] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A method for preparing a low-cost nickel-based single crystal high-temperature alloy thin-wall casting, characterized in that: The method is: S1. According to the chemical composition of the alloy, the raw materials are mixed and poured into a master alloy ingot in a vacuum melting furnace; The master alloy ingot is composed of the following raw materials by mass fraction: Composition: Cr: 7.50-8.50%, Co: 7.50-8.50%, W: 7.50-8.50%, Mo: 1.50-2.50%, Ta: 5.30-6.70%, Al: 5.00-6.00%, Ti: 0.30-0.80%, C: 0.010-0.020%, the balance is Ni; S2, pressing the wax material into a wax mold according to the wax pressing parameters, and using a low melting point wax material to make a shrinkage-feeding structure, and assembling the wax mold after it is completely cooled to obtain an assembled wax mold; S3, shell preparation: a surface layer, a transition layer and a back layer are sequentially arranged on the wax mold assembled in S2 from the inside to the outside to obtain a shell; the material of the surface layer slurry is a mixture of corundum powder, silica sol and 5% polyvinyl alcohol reinforcing agent; The materials of the transition layer slurry and the back layer slurry are a mixture of EC95 fused mullite, silica sol and 5% polyvinyl alcohol reinforcing agent; S4, melting the master alloy ingot obtained in S1 in a vacuum melting furnace, pouring it into the shell obtained in S3, and obtaining a casting after cooling; S5. Clean and cut the casting obtained in S4, complete one solution treatment and two aging treatments in a vacuum heat treatment furnace, remove the shrinkage-feeding structure, and smooth the surface of the casting to obtain a low-cost nickel-based single crystal high-temperature alloy thin-wall casting.
2. A method for preparing a low-cost nickel-based single crystal high-temperature alloy thin-wall casting according to claim 1, characterized in that: The preparation method of the master alloy ingot described in S1 is: first place C at the bottom of the crucible in the vacuum melting furnace, and then load other main materials into the furnace. The order of the other main materials is Co, W, Mo, Ta, Cr, and Ni. When the vacuum degree in the furnace is ≤5Pa, the material is started to be smelted, and the first refining is carried out at 1490℃~1530℃. After the first refining is completed, the power is turned off and the temperature is lowered to allow the molten metal to reach a condensed film state, and then Al and Ti are added through a turret, followed by low-temperature refining at 1390℃~1430℃, and pouring and unloading at 1440℃~1480℃.
3. The method for preparing a low-cost nickel-based single crystal high-temperature alloy thin-wall casting according to claim 1, characterized in that: When preparing the feeding structure in S2, the diameter of the feeding wax droplets at the thin wall is 3-5 mm and the height is 2-3 mm. Feeding wax drops are added according to the requirement that the interval between wax drops is not less than 5 mm, and all the parts where the feeding wax drops contact the thin wall are smoothly transitioned.
4. The method for preparing a low-cost nickel-based single crystal high-temperature alloy thin-wall casting according to claim 1, characterized in that: The viscosity of the surface layer slurry in S3 is 40s-45s, the viscosity of the transition layer slurry is 30s-35s, and the viscosity of the back layer slurry is 10s-15s.
5. The method for preparing a low-cost nickel-based single crystal high-temperature alloy thin-wall casting according to claim 1, characterized in that: During pouring in S4, the heating temperature of the upper zone of the vacuum melting furnace is 1480-1520°C; the heating temperature of the lower zone is 1530-1570°C; the pouring temperature is 1530-1570°C; and the crystal pulling rate is 3mm / min-4mm / min.
Citation Information
Cited By
Method for reducing mixed crystals and recrystallization at abrupt change position of section of nickel-based single crystal superalloy
CN119772103A
A method for reducing mischcrystal and recrystallization at cross-section discontinuities in nickel-based single crystal superalloys
CN119772103B